Coal-based high-performance road asphalt, concrete mineral aggregate and road construction method

The preparation of coal-based high-performance road asphalt through physical and chemical methods has solved the problems of insufficient utilization and poor compatibility of direct liquefied coal residues, realized the preparation of high-performance asphalt, met the technical indicators of high-speed asphalt construction specifications, and improved the asphalt Stability and road performance.

CN119060550APending Publication Date: 2024-12-03RES INST OF HIGHWAY MINIST OF TRANSPORT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310634334.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the prior art, when the coal liquefied residue is used as road asphalt raw material, it is insufficiently utilized and has poor compatibility with matrix asphalt and rubber oil. Long-term storage will cause chromatography, which will affect the performance of use.

Method used

The coal-based high-performance road asphalt is prepared by physical and chemical methods. By mixing the coal directly liquefied residue, waste tire powder and dispersant, and adding matrix asphalt and coupling agent under high temperature and high shear conditions, a high compatibility coal-based high is formed. Performance road asphalt, using coupling agents and dispersants to improve the molecular structure and compatibility of asphalt components.

Benefits of technology

It has achieved high utilization rate, long-term storage stability and good road performance of coal-based high-performance road asphalt, meets the technical indicators of the "Technical Specifications for Highway Asphalt Pavement Construction", and has significant rut resistance and shear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a road asphalt modifier as well as a preparation method and application thereof. The road asphalt modifier comprises the following components in percentage by weight: 10-55% of coal pitch; 10%-30% of coal liquefaction residues; and the balance of additive naphtha. According to the invention, coal pitch, coal liquefaction residues and naphtha are used as main raw materials, and react at 150-200 DEG C for 1-3 hours to obtain a blend, and then the blend is added into petroleum pitch for modification. A large amount of residues are generated by coal liquefaction, the consumption of petroleum asphalt is reduced, and the modifier is good in modification effect, low in production cost, beneficial to environmental protection, capable of meeting the technical specification requirements of road asphalt construction and capable of providing a new way for reutilization of the coal residues.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of highway traffic technology, and in particular relates to a coal-based high-performance road asphalt. In addition, the present invention also relates to a concrete mineral aggregate prepared by using the coal-based high-performance road asphalt and a method for road construction using the concrete mineral aggregate. Background Art

[0002] Transportation is an important basic industry of the national economy, and has a strategic and overall impact on economic and social development. my country's transportation has continued to develop rapidly, forming a comprehensive transportation network with "five vertical and five horizontal" as the main framework, and the transportation capacity has been greatly improved. In recent years, the country has built a number of major transportation engineering projects, and transportation in key areas has accelerated development and achieved breakthroughs, which generally meet the development of my country's economy and society. With the rise of urban agglomerations, the requirements for improving basic public transportation services and transportation safety guarantee systems and building urban agglomeration transportation networks are increasingly on the agenda.

[0003] Asphalt is one of the important components of pavement materials and acts as a binder. However, due to the temperature sensitivity of asphalt itself, road asphalt directly from crude oil or heavy traffic road asphalt itself cannot meet the requirements. In order to improve the performance of road asphalt pavement, the use of modified asphalt is an important method to solve this problem. Modified asphalt is a uniform asphalt mixture after adding modifiers to conventional road asphalt. At present, most highways are paved with modified asphalt. Additives used for asphalt modification can be divided into two categories: polymers and non-polymers. The former mainly includes thermoplastic elastomers, resins and rubbers, such as SBS, PE, etc. SBS is currently the most widely used type. However, polymer additives are non-polar polymer substances with a large relative molecular mass. Compared with petroleum asphalt, due to differences in structure and properties, modified asphalt is prone to segregation during hot storage. The latter mainly includes fillers, natural asphalt, fibers, anti-stripping agents, anti-aging agents and antioxidants, such as sulfur, carbon black and Trinidad Lake asphalt (TLA). Among non-polymer additives, TLA is widely used in countries around the world for its excellent modification performance. Many important projects in China also use TLA, such as Jiangyin Bridge, the west runway of Beijing Capital International Airport, and the Ziyang section of Chengdu-Chongqing Expressway. With the construction of expressways in China and the improvement of the grade of ordinary roads, the demand for TLA will further increase. However, due to the limitation of TLA sources, the import price is expensive and rising, which seriously affects the construction of my country's basic public transportation service network and transportation safety guarantee system.

[0004] Coal tar is the residue of coal tar produced during coal coking and gasification after vacuum distillation, accounting for about 55% of coal tar. As a major coal producer, my country produces a large amount of coal tar as a by-product every year. As early as the 1960s and 1980s, coal tar was used as road asphalt abroad. There are also studies and applications of coal tar as road asphalt in China. For example, Chinese patent CN101705003B discloses a coal tar for high-grade roads. It is composed of 85-90 parts by weight of coal tar, 6-10 parts of modifier (SBS, waste plastics, star-shaped fluorene polymers), and 4-5 parts of cosolvent (polyphosphoric acid). The invention found that coal tar has strong tensile strength, good temperature resistance, low production cost, and improves the use value of coal tar. For another example, Chinese patent CN102653631A discloses a mixed asphalt for roads and a preparation method thereof. The invention prepares a mixed asphalt by using medium-temperature coal tar, petroleum asphalt and modified additives, thereby improving the high-temperature performance of ordinary road petroleum asphalt and the adhesion of the asphalt mixture. The invention also has a simple preparation process, a low production temperature, and convenient product transportation, making it suitable for road construction projects.

[0005] Although coal tar is cheap and has the advantages of low temperature stability, good adhesion and good anti-corrosion performance when used as road asphalt, the application practice at home and abroad shows that coal tar has poor weather resistance and plasticity, and contains toxic polycyclic aromatic hydrocarbons. Therefore, since coal tar pollutes the environment and harms human health, its promotion and application as a road paving material at home and abroad is greatly restricted. In recent years, people have been seeking new coal-based materials as road asphalt materials.

[0006] Direct coal liquefaction residue (DCLR) is a byproduct of direct high-temperature pyrolysis of coal. Since it undergoes hydrogenation treatment at a temperature of more than 500°C during the reaction, the heteroatoms that can cause environmental pollution are basically removed, and the volatile components it contains are extremely low, so it is an environmentally friendly raw material. Coal liquefaction residue is mainly composed of inorganic matter (about 20%) and organic matter (about 80%). Among them, inorganic matter includes minerals in coal and added iron-based catalysts; organic matter includes heavy oil and asphalt as well as unconverted coal, of which asphalt-like substances account for about 50%. It can be seen that the considerable amount of asphalt components in coal liquefaction residue has the potential to be used as road asphalt.

[0007] In China, Shenhua Ordos Coal-to-Oil Branch was the first to conduct preliminary exploration and research on "how to use coal direct liquefaction residue directly as road asphalt material through modification". For example, Chinese patent CN 103173025 B invented a method for preparing road asphalt using coal direct liquefaction residue. The method first uses coal tar to extract low softening point asphaltene in coal direct liquefaction residue; then uses the principle of low-temperature phase separation of asphaltene and coal tar during the cooling process to separate asphaltene from coal tar; then the extracted asphaltene, coal direct liquefaction residue and petroleum asphalt are prepared in different proportions to form road asphalt that can meet different road performance requirements. This method makes full use of the characteristics of coal direct liquefaction residue containing certain asphaltene components, but the disadvantage is that the coal direct liquefaction residue needs to be separated first, and then the extracted asphaltene is used as a blending raw material to prepare road asphalt. For another example, Chinese patent CN 104559253 A discloses a road asphalt modifier, which is prepared by adding 5%-10% granular coal direct liquefaction residue and 2%-3% rubber oil to base asphalt, and stirring at high temperature to prepare a low-cost coal direct liquefaction residue-based asphalt modifier. The price of this modifier to improve asphalt performance is much lower than the price of traditional SBS to improve asphalt performance, with low production cost and good economic benefits. However, the compatibility between coal direct liquefaction residue and base asphalt and rubber oil is poor, and long-term storage will produce chromatography. Summary of the invention

[0008] In order to solve the technical problems of insufficient raw material utilization when using coal direct liquefaction residue as raw material for road asphalt, poor compatibility between coal direct liquefaction residue and matrix asphalt and rubber oil, and chromatography phenomenon caused by long-term storage, the purpose of the present invention is to provide a coal-based high-performance road asphalt prepared by a physical and chemical method. The various technical indicators of the coal-based high-performance road asphalt prepared by the method of the present invention meet the requirements of the "Technical Specifications for Highway Asphalt Pavement Construction" (JTG F40-2004).

[0009] The invention discloses a coal-based high-performance road asphalt, which comprises the following components by weight: 10-55 parts of coal direct liquefaction residue, 10-30 parts of waste tire powder, 0.05-0.3 parts of coupling agent, 1-4.5 parts of dispersant and 10-35 parts of base asphalt; the coal-based high-performance road asphalt is prepared by first mixing the coal direct liquefaction residue, the waste tire powder and the dispersant according to the weight ratio, stirring the mixture at 100-150°C for 0.5-1.5h, and then feeding the mixture into a high-speed shearing machine, adding base asphalt and coupling agent in sequence, and subjecting the mixture to high-speed shearing for 0.5-1.5h at a shearing temperature of 140-180°C and a shearing rate of 1000-3000rpm to obtain a coal-based high-performance road asphalt.

[0010] Preferably, the coupling agent is a composite additive consisting of diethylenetriamine and carbon disulfide in a mass ratio of 1:1-1:3, and is added to the mixture by first adding diethylenetriamine to the mixture and then gradually adding carbon disulfide at a certain addition rate.

[0011] Preferably, the dispersant is a three-dimensional graphene powder. More preferably, the three-dimensional graphene is exfoliated graphene or reduced oxidized graphene, or a mixture of the two.

[0012] Preferably, the coal direct liquefaction residue is a coal residue discharged from a vacuum distillation device after direct coal liquefaction, with a softening point of no higher than 180°C and a solid content of no more than 50% by weight. More preferably, the sum of the heavy oil content and the asphaltene content in the coal liquefaction residue is higher than 50%.

[0013] In the formula of the coal-based high-performance road asphalt disclosed in the present invention, waste tire powder is used as an additive component to improve the colloidal structure of the asphalt in the product, thereby improving the viscoelasticity and thixotropy of the coal-based high-performance road asphalt product; in the formula, the coal direct liquefaction residue component is beneficial to promoting the dissolution of the waste tire powder in the matrix asphalt and promoting the modification reaction of the matrix asphalt; the coupling agent is a composite additive composed of diethylenetriamine and carbon disulfide in a mass ratio of 1:1-1:3, and is added to the mixture by first adding diethylenetriamine to the mixture and then gradually adding carbon disulfide at a certain adding rate; under heating and high shear conditions, the carbon disulfide is decomposed to continuously generate sulfur bonds and sulfur free radical coordination atoms, thereby promoting the chelating effect between the molecular structures of the coal liquefaction residue, the waste tire powder and the matrix asphalt in the formula of the present invention through the diethylenetriamine, thereby improving the molecular arrangement of the asphalt components in the mixture and enhancing the cohesion of the asphalt components in the product formula. At the same time, the coal liquefaction residue has a certain dissolving effect on other components in the formula, forming a colloid-like substance, which greatly improves the road performance indicators such as the chemical stability and anti-aging performance of the product. The introduction of graphene powder in the dispersant introduces polar functional groups (such as carboxyl, hydroxyl, epoxy, etc.) into the mixed material of the formula, thereby further promoting the formation of a bridge structure between the matrix asphalt and the coal liquefaction residue, promoting the cross-linking reaction between the coal liquefaction residue and the matrix asphalt, and improving the component compatibility and stability of the coal-based high-performance road asphalt product, and greatly improving the use performance of the coal-based high-performance road asphalt product prepared based on the coal liquefaction residue. In addition, the coal-based high-performance road asphalt provided by the present invention has high dynamic stability and Marshall strength, has significant anti-rutting performance and anti-shear performance, and ensures that the paved road surface has good comprehensive road performance.

[0014] A concrete mineral aggregate prepared using the above-mentioned coal-based high-performance road asphalt, characterized in that it is a mixture of coal-based high-performance road asphalt and ore according to a mix ratio determined by design and experiment.

[0015] The coal-based high-performance road asphalt in the concrete mineral aggregate is composed of the following components in parts by mass: 10-55 parts of coal direct liquefaction residue, 10-30 parts of waste tire powder, 0.05-0.3 parts of coupling agent, 1-4.5 parts of dispersant and 10-35 parts of base asphalt; the coal-based high-performance road asphalt is firstly prepared by mixing the coal direct liquefaction residue, the waste tire powder and the dispersant according to the mass ratio, stirring them at 100-150°C for 0.5-1.5h, and then feeding them into a high-speed shearing machine, adding base asphalt and coupling agent in turn, and high-speed shearing for 0.5-1.5h at a shear temperature of 140-180°C and a shear rate of 1000-3000rpm to obtain a coal-based high-performance road asphalt.

[0016] The coupling agent is a composite additive composed of diethylenetriamine and carbon disulfide in a mass ratio of 1:1-1:3, and is added to the mixture by first adding diethylenetriamine to the mixture, and then gradually adding carbon disulfide at a certain addition rate; the dispersant is a three-dimensional graphene powder. More preferably, the three-dimensional graphene is exfoliated graphene or reduced oxidized graphene, or a mixture of the two.

[0017] In the above-mentioned formulation of coal-based high-performance road asphalt, the coal direct liquefaction residue is preferably a coal residue discharged from a vacuum distillation device after direct coal liquefaction, with a softening point of no more than 180°C and a solid content of no more than 50% by weight. More preferably, the sum of the heavy oil content and the asphaltene content in the coal liquefaction residue is higher than 50%.

[0018] The present invention also relates to a road construction method, comprising the steps of mixing a mixture, transporting the mixture, spreading the mixture, rolling the mixture, and treating a transverse construction joint, and is characterized in that:

[0019] Step 1: Mixing the mixture

[0020] The road asphalt modifier is crushed to less than 3 microns, and according to the mix ratio determined by design and test, it is sent into the mixer with the stone at a temperature of 150-180℃ and fully mixed until the aggregate particles are completely covered with the asphalt film and the asphalt is completely and evenly mixed into the aggregate. The time and mixing temperature for mixing a cylinder of qualified mixture during large-scale construction are determined through the construction of the test section pavement; if the mixture is found to be unevenly mixed during construction, the mixing is stopped immediately and the cause is analyzed;

[0021] Step 2: Mixed material transportation

[0022] Before the construction of the test section, the transport vehicle will be washed, and the isolation agent of 1:1 vegetable oil and detergent will be applied to the bottom plate of the carriage. There will be no liquid accumulation in the carriage. When loading, move in the order of front, back and middle. During the construction process, the paved road surface is kept 10-30cm away from the front of the paver, and the paver is pushed forward to unload, and the temperature of the mixture is kept at 150-180℃;

[0023] Step 3: Spreading the mixture

[0024] During the mixture paving process, the paver travel speed is controlled at 2-3m / min, and the ironing board is preheated at a temperature of not less than 100℃ for 1 hour in advance. During paving, ensure that there is no less than 2 / 3 of the mixture in the spiral feeder; use non-contact balance beam for leveling, and use the automatic leveling system to control the longitudinal and transverse slopes from both sides of the paving layer; use manual filling and leveling at 10-15cm on both sides of the paver;

[0025] Step 4: Mixture rolling

[0026] After the asphalt mixture of the test section is paved, it is rolled by a combination of a double steel wheel vibratory roller and a tire roller. Before rolling, the rubber wheels are coated with a 1:1 ratio of vegetable oil and detergent. The initial rolling temperature is controlled to be ≥150℃ and the final rolling temperature is ≥90℃.

[0027] Rolling is carried out in three stages: initial compaction, secondary compaction and final compaction. For the upper layer: initial compaction uses a double steel wheel roller to roll from low to high, with static pressure forward and vibration backward; secondary compaction uses a 30t rubber wheel roller to follow up; final compaction uses double steel wheels for rolling; for the lower layer: initial compaction uses two rubber wheels to roll alternately; both secondary compaction and final compaction use two double steel wheel vibratory rollers to roll alternately; rolling is carried out longitudinally, with each rolling section of 30m, moving slowly and evenly forward from low to high, overlapping by 1 / 3-1 / 2 of the wheel width to avoid missed compaction and over-compaction.

[0028] Step 5: Horizontal construction joint treatment

[0029] Flat joint treatment is adopted. A three-meter ruler is used to position the joint along the longitudinal direction. At the end of the paving, it is cantilevered and the joint position is determined by the point where the paving layer and the ruler are out of contact. It is cut with a saw and then scraped off. When paving continues, the mortar left by sawing is wiped clean and a small amount of tack coat asphalt is applied. The paving machine ironing plate starts paving from the joint. When rolling, a steel wheel roller is used for lateral compaction, and rolling is carried out from the first paved road surface gradually across the lateral construction joint to the newly paved surface layer.

[0030] Compared with the prior art, the beneficial technical progress achieved by the present invention is:

[0031] Compared with the prior art Chinese patent CN 103173025 B, in the technical solution of the present invention, the coal direct liquefaction residue is directly utilized without component separation, so the utilization rate of the coal direct liquefaction residue is high and the process is simpler. Compared with the prior art Chinese patent CN 104559253 A, the formula of the coal-based high-performance road asphalt disclosed in the present invention has high compatibility between components, can be stored for a long time without chromatography, and has good product performance. DETAILED DESCRIPTION

[0032] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments.

[0033] In the following examples, the number of components and percentages are all by weight. Among them, the coal direct liquefaction residue used is from the Shenhua Group's coal direct liquefaction continuous test device, the waste tire powder number is 10-100, and the matrix asphalt is selected from Zhonghai 90# (ZH90) and Qinhuangdao 90# (QHD90) two 90 needle penetration grade heavy traffic asphalt as the matrix asphalt. The heated stirring kettle adopts a slurry-type industrial stainless steel reactor produced by Shandong Environmental Protection Technology Co., Ltd. (heating temperature 100-200°C, stirring speed 0-130rpm, working pressure 0.6MPa); the high shear dispersion equipment uses a YA90 high shear emulsifier produced by Shanghai Machinery Equipment Co., Ltd. (power: 1500W, power supply: 220V 50Hz / 60HZ, speed range: 300-6000rpm variable frequency speed regulation).

[0034] Example 1

[0035] 50 parts of coal direct liquefaction residue, 10 parts of waste tire powder and 3 parts of dispersant are mixed evenly and loaded into a stainless steel reactor. At a shear temperature of 120℃±10℃ and a stirring rate of 80rpm, the mixing treatment is carried out for 1h. Then the reaction materials are transferred to a high shear emulsifier, and the shear temperature and shear rate are set to 170℃±10℃ and 2000rpm. 30 parts of base asphalt ZH90 and 0.05 parts of diethylenetriamine are added in sequence. Finally, 0.05 parts of carbon disulfide are gradually added to the aforementioned mixture at an addition rate of 1ml / min. After the addition is completed, high-speed shearing is continued for 1.5h to obtain a coal-based high-performance road asphalt.

[0036] Example 2

[0037] 35 parts of coal direct liquefaction residue, 15 parts of waste tire powder and 1 part of dispersant are mixed evenly and loaded into a stainless steel reactor. At a shear temperature of 70℃±10℃ and a stirring rate of 80rpm, the mixing treatment is carried out for 1.5h. Then the reaction material is transferred to a high shear emulsifier, and the shear temperature and shear rate are set to 200℃±10℃ and 4000rpm. 15 parts of base asphalt ZH90 and 0.05 parts of diethylenetriamine are added in sequence. Finally, 0.15 parts of carbon disulfide are gradually added to the aforementioned mixture at an addition rate of 1ml / min. After the addition is completed, high-speed shearing is continued for 0.5h to obtain a coal-based high-performance road asphalt.

[0038] Example 3

[0039] 10 parts of coal direct liquefaction residue, 20 parts of waste tire powder and 1 part of dispersant are mixed evenly and loaded into a stainless steel reactor. At a shear temperature of 130℃±10℃ and a stirring rate of 80rpm, the mixing treatment is carried out for 0.5h. Then the reaction material is transferred to a high shear emulsifier, and the shear temperature and shear rate are set to 150℃±10℃ and 4000rpm. 30 parts of base asphalt ZH90 and 0.05 parts of diethylenetriamine are added in sequence. Finally, 0.05 parts of carbon disulfide are gradually added to the aforementioned mixture at an addition rate of 1ml / min. After the addition is completed, high-speed shearing is continued for 1h to obtain a coal-based high-performance road asphalt.

[0040] Example 4

[0041] 55 parts of coal direct liquefaction residue, 20 parts of waste tire powder and 4 parts of dispersant are mixed evenly and loaded into a stainless steel reactor. At a shear temperature of 140℃±10℃ and a stirring rate of 80rpm, the mixing treatment is carried out for 1h. Then the reaction materials are transferred to a high shear emulsifier, and the shear temperature and shear rate are set to 200℃±10℃ and 3000rpm. 25 parts of base asphalt ZH90 and 0.15 parts of diethylenetriamine are added in sequence. Finally, 0.15 parts of carbon disulfide are gradually added to the aforementioned mixture at an addition rate of 1ml / min. After the addition is completed, high-speed shearing is continued for 1.5h. After the reaction is completed, the product in the high shear emulsifier is collected to obtain a coal-based high-performance road asphalt product.

[0042] Example 5

[0043] 40 parts of coal direct liquefaction residue, 10 parts of waste tire powder and 1.4 parts of dispersant are mixed evenly and loaded into a stainless steel reactor. At a shear temperature of 120℃±10℃ and a stirring rate of 80rpm, the mixing treatment is carried out for 1.5h. Then the reaction materials are transferred to a high shear emulsifier, and the shear temperature and shear rate are set to 170℃±50℃ and 4000rpm. 25 parts of base asphalt QHD90 and 0.05 parts of diethylenetriamine are added in sequence. Finally, 0.05 parts of carbon disulfide are gradually added to the aforementioned mixture at an addition rate of 1ml / min. After the addition is completed, high-speed shearing is continued for 1h. After the reaction is completed, the product in the high shear emulsifier is collected to obtain a coal-based high-performance road asphalt product.

[0044] Example 6

[0045] 50 parts of coal direct liquefaction residue, 25 parts of waste tire powder and 4.5 parts of dispersant are mixed evenly and loaded into a stainless steel reactor. At a shear temperature of 140℃±10℃ and a stirring rate of 80rpm, the mixing treatment is carried out for 1h. Then the reaction materials are transferred to a high shear emulsifier, and the shear temperature and shear rate are set to 200℃±10℃ and 5000rpm. 35 parts of base asphalt QHD90 and 0.1 parts of diethylenetriamine are added in sequence. Finally, 0.2 parts of carbon disulfide are gradually added to the aforementioned mixture at an addition rate of 1ml / min. After the addition is completed, high-speed shearing is continued for 1.5h. After the reaction is completed, the product in the high shear emulsifier is collected to obtain a coal-based high-performance road asphalt product.

[0046] Basic performance test of coal-based high-performance road asphalt products. According to the test method of "Highway Engineering Asphalt and Asphalt Mixture Test Procedure JTG E20-2011", the asphalt mixtures of Examples 1 to 6 and using a single base asphalt (ZH90, QHD90) were tested. The specific test content, test method and results are as follows.

[0047] The changes in properties such as penetration, softening point, and ductility of the residue after heating of the coal-based high-performance road asphalt product obtained in this embodiment are measured to evaluate the aging resistance of the asphalt. Among them: 1) The penetration is measured using the national standard GB / T4509-1998 (petroleum asphalt penetration measurement method). Penetration is an index of the consistency of asphalt, reflecting the degree of hardness and softness of asphalt under certain conditions, and actually characterizes the viscosity of asphalt at that temperature. The smaller the penetration, the harder the asphalt. 2) The asphalt softening point is measured using the national standard GB / T4507-1999 (petroleum asphalt softening point measurement method). The asphalt softening point measurement method uses the ring and ball method. The so-called ring and ball method is that the sample is placed in a copper ring of specified size with a copper ball of specified size and weight in water or glycerin, and the heating rate is increased by 5°C per minute until the asphalt softens. The water temperature when the steel ball sinks to a specified distance is the softening point of the asphalt, expressed in °C. 3) The ductility test adopts the national standard GB / T4508-1999 (Method for determining the ductility of petroleum asphalt). The method for testing the ductility of asphalt is to pour the melted asphalt into a pre-prepared ductility mold of a certain size, and after a certain treatment, stretch the two ends of the standard test piece at a certain temperature and stretching rate (5cm / min) until it breaks. The length of the fracture position is the ductility of the asphalt at this temperature. 4) The film oven test adopts the national standard GB / T5304-1985, which is used to determine the mass loss of road asphalt film after heating, so as to evaluate the construction performance of asphalt products.

[0048] The test results are shown in Table 1.

[0049] Table 1 Performance of coal-based high-performance road asphalt products prepared under different conditions

[0050]

[0051] As can be seen from Table 1, within the test conditions, the higher the shear temperature, the better the basic performance of the product. This is mainly because as the shear temperature increases, the fluidity of the coal liquefaction residue in the raw material is higher, and it is easier to react physically and chemically with the waste tire powder and the matrix asphalt molecules, thereby greatly improving the product performance. At the same time, as the shear temperature increases, the reactants in the mixture are more easily activated, and carbon disulfide is added at a certain rate under heating and high shear conditions, and then sulfur bonds and sulfur radical coordination atoms are continuously generated, thereby promoting the chelating effect between the molecular structure of the coal liquefaction residue, the waste tire powder and the matrix asphalt in the formula of the present invention through diethylenetriamine. At the same time, the coal liquefaction residue has a certain dissolving effect on other components, forming a colloid-like substance, which greatly improves the road performance indicators such as the chemical stability and anti-aging performance of the product.

[0052] The following examples further illustrate in detail the concrete mineral aggregate prepared using the above-mentioned coal-based high-performance road asphalt of the present invention, and the method of using the concrete mineral aggregate for road construction.

[0053] Example 7

[0054] In this example, the coal-based high-performance road asphalt prepared in Example 5 was used as raw material to prepare concrete mineral aggregate. The mineral aggregate gradation was carried out in accordance with the "Technical Specifications for Highway Asphalt Pavement Construction" (JTG F40-2004). The specific mineral aggregate gradation design is shown in Table 2.

[0055] Table 2 Mineral material gradation design table

[0056]

[0057] The optimal asphalt-stone ratio of concrete mineral aggregate coal-based high-performance road asphalt was estimated. Five different asphalt-stone ratios were taken at intervals of 0.5% to form Marshall specimens. The indicators and related mechanical indicators were measured, with the asphalt-stone ratio as the horizontal axis and the various volume indicators as the vertical axis. The test results are shown in Table 3.

[0058] Table 3 Marshall test results of concrete mineral aggregates

[0059]

[0060] It can be seen from Table 3 that when the asphalt-to-stone ratio is 4.3%, the concrete mineral aggregate prepared by using the coal-based high-performance road asphalt provided by the present invention has the best road performance and the best construction performance.

[0061] Example 8

[0062] This example further verifies the use effect of the road paving material prepared by using the coal-based high-performance road asphalt provided by the present invention as raw material through high-temperature stability evaluation of the concrete mineral aggregate obtained in Example 7. The main test methods for evaluating the high-temperature stability of asphalt mixtures include: small rutting test, uniaxial static creep test, ring road test, APA rutting test, etc. This example evaluates the high-temperature stability of the mixed asphalt mixture through rutting test, and the test results are shown in Table 4.

[0063] Table 4 Asphalt mixture rutting test results

[0064]

[0065] By comparing the dynamic stability of the matrix asphalt mixture in Table 4 and the concrete mineral aggregate prepared with the coal-based high-performance road asphalt of the present invention, it can be found that with the addition of coal tar, the dynamic stability of the mixed asphalt with different addition ratios of coal tar is slightly improved. The experiment shows that in the concrete mineral aggregate, with the increase of the content of coal-based high-performance road asphalt, the high-temperature performance of the concrete mineral aggregate is higher than that of the concrete mineral aggregate prepared with a single matrix petroleum asphalt, which is consistent with the law of the high-temperature performance index reaction in the mixed asphalt road performance we studied in the previous stage.

[0066] Example 9

[0067] This example is to evaluate the low temperature crack resistance of the concrete mineral aggregate obtained in Example 7 by mixing it with asphalt mixture to further verify the technical effect of using the coal-based high-performance road asphalt provided by the present invention as raw material for road paving materials.

[0068] The low-temperature crack resistance of asphalt mixture is directly related to the low-temperature performance of the pavement and is one of the most important road performances of asphalt mixture. In addition to evaluating the low-temperature performance of asphalt, the low-temperature crack resistance of the mixture should also be evaluated. At present, the main methods for evaluating the low-temperature crack resistance of asphalt mixtures are: direct tensile test, indirect tensile test, creep test, bending test and stress relaxation test. This embodiment uses a low-temperature beam bending test to evaluate the low-temperature crack resistance of the modified asphalt mixture.

[0069] The test block used in the beam bending test was made by rolling the rutting asphalt mixture specimen (wheel rolling method) into a prismatic beam with a length of 250mm±2.0mm, a width of 30mm±2.0mm, and a height of 50mm±2.0 mm, and a span of 200mm±0.5mm. The test temperature used in this test was -10℃±0.5℃, and the constant temperature water tank used a 1:1 methanol-water solution as the coolant medium, and circulated back. The low-temperature bending test results of the modified asphalt mixture beams with two ratios are shown in Table 5.

[0070] Table 5 Results of low temperature bending test of asphalt mixture beams

[0071]

[0072] The low-temperature flexural tensile strength of asphalt mixture reflects the low-temperature crack resistance. The larger the index is under low-temperature conditions, the stronger its low-temperature crack resistance is. As shown in Table 5, as the content of coal-based high-performance road asphalt in the mixture increases, the flexural tensile strength of the asphalt mixture decreases, but the decrease is not large, about 2%-4%. The failure strain mainly reflects the deformation ability at low temperature. The larger the ultimate strain, the stronger its low-temperature deformation ability. As shown in Table 5, with the failure strain as the evaluation index, the failure strain of 15% coal-based high-performance road asphalt mixture is equivalent to that of the matrix asphalt, and the failure strain of 30% coal-based high-performance road asphalt mixture is about 4% lower than that of the matrix asphalt. It can be seen that the addition of coal asphalt has little effect on the low-temperature performance of asphalt mixture, which is basically the same as the matrix asphalt.

[0073] It can be seen from Examples 7 to 9 that the technical indicators of the coal-based high-performance road asphalt product obtained by the method of the present invention all meet the relevant technical requirements in the Technical Specifications for Highway Asphalt Pavement Construction (JTG F40-2004).

[0074] Example 10

[0075] This embodiment provides a method for paving a road surface using the coal-based high-performance road asphalt mixture provided by the present invention. The specific method is as follows:

[0076] Step 1: Mixing the mixture

[0077] The mixture is mixed strictly according to the mix ratio determined by design and test, and the aggregate and the coal-based high-performance road asphalt of the present invention crushed to less than 3 microns are fed into the mixer and fully mixed until the aggregate particles are completely covered by the asphalt film and the asphalt is completely and evenly mixed into the aggregate. The time and mixing temperature for mixing a cylinder of qualified mixture during large-scale construction are determined through the test section pavement construction. During the test section construction process, the mixing uniformity of the mixture needs to be checked, and problems such as white stones, dull yellow and gray colors should not appear. If the mixture is found to be unevenly mixed during large-scale construction, the mixing should be stopped immediately and the cause should be analyzed.

[0078] Step 2: Transportation of Mixture

[0079] Before the construction of the test section, the transport vehicle will be washed, and the bottom plate of the carriage will be painted with a 1:1 vegetable oil and detergent release agent to prevent the mixture from sticking. After spraying the release agent, the carriage will be raised to empty the accumulated liquid. When loading, in order to avoid segregation of the mixture, it must be moved strictly in the order of front, back, and middle. Before paving, it must be directed by a dedicated person, stop 10-30cm in front of the paver, and rely on the paver to push forward to unload.

[0080] Use a mercury thermometer to measure the temperature of the mixture at the construction site and strictly check the mixing quality. It can only be used for construction after passing the test.

[0081] Step 3: Spreading the mixture

[0082] Under the condition that the production and transportation of the mixture are normal, the paving consumption of the mixture is basically matched with the production speed, the flatness and density of the surface construction are guaranteed, and the travel speed of the paver is controlled to be 2-3m / min. Preheat the screed plate at a temperature not lower than 100℃ for 1 hour in advance. Before starting, place a pad with the same height as the loose paving elevation at the bottom of the screed plate. After the pad passes smoothly, open the screed plate and tamper. When paving, ensure that there is no less than 2 / 3 of the mixture in the spiral feeder to ensure that the paver does not have segregation of the full width section.

[0083] A non-contact balance beam is used for leveling, and an automatic leveling system is used to control the longitudinal and transverse slopes from both sides of the paving layer. Manual material filling and leveling are used at about 12cm on both sides of the paver.

[0084] Step 4: Rolling of the mixture

[0085] After the asphalt mixture of the test section is paved, it is rolled by a combination of a double steel wheel vibratory roller and a tire roller. Before rolling, apply a 1:1 ratio of vegetable oil and detergent to the rubber wheel. The initial rolling temperature is controlled to be ≥150℃, and the final rolling temperature is ≥90℃.

[0086] It is carried out in three stages: initial compaction, secondary compaction and final compaction. For the upper layer: the initial compaction is carried out by a double steel wheel roller from low to high, with static pressure forward and vibration backward; the secondary compaction is carried out by a 30t rubber wheel roller; the final compaction is carried out by double steel wheels. For the lower layer: the initial compaction is carried out by two rubber wheels alternatingly; the secondary compaction and final compaction are carried out by two double steel wheel vibratory rollers alternatingly.

[0087] The rolling is carried out longitudinally, with each rolling section being 30m, moving forward slowly and evenly from low to high, overlapping by 1 / 3-1 / 2 wheel width to avoid missing and over-pressing.

[0088] Step 5: Horizontal construction joint treatment

[0089] All horizontal construction joints are treated with flat joints. Use a three-meter ruler to cantilever along the longitudinal position at the end of the paving, and determine the joint position where the paving layer and the ruler are out of contact. Cut it with a saw and then remove it. When continuing to pave, clean the mortar left by sawing, apply a small amount of tack coat asphalt, and start paving from the joint with the paving machine screed. When rolling, use a steel wheel roller to compact horizontally, and gradually cross the horizontal construction joint from the first paved road surface to roll to the new paved surface layer.

[0090] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been presented as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A coal-based high-performance road asphalt, which is prepared by physical and chemical reaction of five raw materials consisting of 10-55 parts of coal direct liquefaction residue, 10-30 parts of waste tire powder, 0.05-0.3 parts of coupling agent, 1-4.5 parts of dispersant and 10-35 parts of base asphalt in a certain adding order.

2. The coal-based high-performance road asphalt according to claim 1, characterized in that: The coal direct liquefaction residue is the residue discharged from the vacuum distillation device after the coal direct liquefaction, with a softening point not higher than 180° C. and a solid content not exceeding 50% by weight.

3. The coal-based high-performance road asphalt according to claim 2, characterized in that: The sum of the heavy oil content and the asphaltene content in the coal liquefaction residue is higher than 50%.

4. The coal-based high-performance road asphalt according to claim 1, characterized in that: The coupling agent is a composite additive composed of diethylenetriamine and carbon disulfide in a mass ratio of 1:1-1:

3.

5. The coal-based high-performance road asphalt according to claim 1, characterized in that: The dispersant is graphene powder.

6. The coal-based high-performance road asphalt according to claim 5, characterized in that: The graphene powder is any one of exfoliated graphene or reduced oxidized graphene or a mixture of the two.

7. A method for preparing coal-based high-performance road asphalt, characterized in that: Firstly, the coal direct liquefaction residue and waste tire powder are crushed into 60-100 meshes respectively to obtain coal direct liquefaction residue powder and waste tire powder; then, the coal direct liquefaction residue powder, waste tire powder and dispersant are mixed according to the mass fraction ratio of coal direct liquefaction residue: waste tire powder: dispersant = 10-55:10-30:1-4.5, and the mixture is fully stirred at 60-150°C for 0.5-1.5h, and then sent to a high-speed shearing machine, 10-35 parts of base asphalt and 0.05-0.3 parts of coupling agent are added in sequence, and high-speed shearing is performed for 0.5-1.5h at a shear temperature of 120-220°C and a shear rate of 1000-5000rpm to obtain a coal-based high-performance road asphalt.

8. The method for preparing coal-based high-performance road asphalt according to claim 7, characterized in that: The coupling agent is a composite additive composed of diethylenetriamine and carbon disulfide in a mass ratio of 1:1-1:3, and is added to the mixture by first adding diethylenetriamine to the mixture and then gradually adding carbon disulfide at a certain adding rate.

9. A concrete mineral aggregate, characterized in that: The coal-based high-performance road asphalt described in any one of claims 1 to 6 is mixed with ore according to a mix ratio determined by design and experiment.

10. A road construction method, comprising the steps of mixing a mixture, transporting the mixture, spreading the mixture, rolling the mixture, and treating a transverse construction joint, characterized in that: Step 1: Mixing the mixture The road asphalt modifier is crushed to less than 3 microns, and according to the mix ratio determined by design and test, it is sent into the mixer with the stone at a temperature of 150-180℃ and fully mixed until the aggregate particles are completely covered with the asphalt film and the asphalt is completely and evenly mixed into the aggregate. The time and mixing temperature for mixing a cylinder of qualified mixture during large-scale construction are determined through the construction of the test section pavement; if the mixture is found to be unevenly mixed during construction, the mixing is stopped immediately and the cause is analyzed; Step 2: Mixed material transportation Before the construction of the test section, the transport vehicle will be washed, and the isolation agent of 1:1 vegetable oil and detergent will be applied to the bottom plate of the carriage. There will be no liquid accumulation in the carriage. When loading, move in the order of front, back and middle. During the construction process, the paved road surface is kept 10-30cm away from the front of the paver, and the paver is pushed forward to unload, and the temperature of the mixture is kept at 150-180℃; Step 3: Spreading the mixture During the mixture paving process, the paver travel speed is controlled at 2-3m / min, and the ironing board is preheated at a temperature of not less than 100℃ for 1 hour in advance. During paving, ensure that there is no less than 2 / 3 of the mixture in the spiral feeder; use non-contact balance beam for leveling, and use the automatic leveling system to control the longitudinal and transverse slopes from both sides of the paving layer; use manual filling and leveling at 10-15cm on both sides of the paver; Step 4: Mixture rolling After the asphalt mixture of the test section is paved, it is rolled by a combination of a double steel wheel vibratory roller and a tire roller. Before rolling, the rubber wheels are coated with a 1:1 ratio of vegetable oil and detergent. The initial rolling temperature is controlled to be ≥150℃ and the final rolling temperature is ≥90℃. Rolling is carried out in three stages: initial compaction, secondary compaction and final compaction. For the upper layer: initial compaction uses a double steel wheel roller to roll from low to high, with static pressure forward and vibration backward; secondary compaction uses a 30t rubber wheel roller to follow up; final compaction uses double steel wheels for rolling; for the lower layer: initial compaction uses two rubber wheels to roll alternately; both secondary compaction and final compaction use two double steel wheel vibratory rollers to roll alternately; rolling is carried out longitudinally, with each rolling section of 30m, moving slowly and evenly forward from low to high, overlapping by 1 / 3-1 / 2 of the wheel width to avoid missed compaction and over-compaction. Step 5: Horizontal construction joint treatment Flat joint treatment is adopted. A three-meter ruler is used to position the joint along the longitudinal direction. At the end of the paving, it is cantilevered and the joint position is determined by the point where the paving layer and the ruler are out of contact. It is cut with a saw and then scraped off. When paving continues, the mortar left by sawing is wiped clean and a small amount of tack coat asphalt is applied. The paving machine ironing plate starts paving from the joint. When rolling, a steel wheel roller is used for lateral compaction, and rolling is carried out from the first paved road surface gradually across the lateral construction joint to the newly paved surface layer.