Bulk type catalytic proppant as well as preparation method and application thereof
By combining modified clay with SO3H groups in catalytic proppants with additives, the problem of poor conversion activity of organic matter in high clay shales is solved, and efficient oil shale resource utilization and oil quality improvement are achieved , meets the needs of shale fracturing and in-situ catalysis.
Patent Information
- Application Number
- CN202310623409.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-30
AI Technical Summary
The existing catalytic proppants have poor organic matter hydrocarbon generation conversion activity in high clay shale reservoirs and have low conversion efficiency, which cannot meet the needs of oil shale crack support and in-situ catalytic conversion.
The modified clay with SO3H groups is combined with additives to prepare catalytic proppants through acid activation, thiolation, wet ball mill grafting and oxidation reactions to form a bulk catalytic proppants with high acid amount and acid strength. Used for shale fracturing micro-slit support and in-situ catalysis.
It significantly improves the utilization rate and recovery rate of oil shale resources, improves oil quality, and has environmentally friendly processes, controllable particle size, and is easy to prepare on a large scale, meeting national standards.
Smart Images

Figure CN119060716A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of shale fracturing functionalized proppants, and in particular to a bulk catalytic proppant and a preparation method and application thereof. Background Art
[0002] At present, the common types of proppants are mainly quartz sand, artificial ceramsite, and resin-coated sand, which can be used for more than 95% of the total amount. Among them, artificial ceramsite is widely used in medium-deep wells because of its good sphericity, high strength, corrosion resistance, and best flow conductivity.
[0003] With the development of oil shale hydraulic fracturing technology, higher requirements are put forward for the strength, surface properties and conductivity of proppants, especially for the development of proppants with catalytic active centers. Catalytic proppants not only need to have the performance of ceramsite proppants, but also have catalytic active centers that can convert organic matter such as kerogen in the reservoir into crude oil.
[0004] my country's continental shale clay has the formation characteristics of high content, but the existing catalytic proppants have problems such as poor organic matter hydrocarbon conversion activity and low conversion efficiency. Therefore, it is necessary to develop efficient bulk catalytic functional proppants suitable for shale reservoirs with high clay content, in order to achieve the integrated technology of oil shale fracture support and in-situ catalytic conversion of organic matter, and improve oil shale recovery and oil quality. Summary of the invention
[0005] The purpose of the present invention is to overcome the problems of the existing catalytic proppants in the prior art, such as insufficient acid or weak acid strength, poor conversion activity of organic matter to hydrocarbons, low conversion efficiency, etc., and to provide a bulk catalytic proppant and a preparation method and application thereof.
[0006] In order to achieve the above-mentioned object, the present invention provides a bulk catalytic proppant in the first aspect, wherein the catalytic proppant comprises: a catalyst having SO 3 H group-modified clay and additives; wherein the SO 3 In the H-group modified clay, clay and SO 3 The weight ratio of H groups is 5-20:1.
[0007] A second aspect of the present invention provides a method for preparing a bulk catalytic proppant, which comprises the following steps:
[0008] (1) After the clay is activated with acid, a thiol-forming agent is added to perform wet ball milling grafting;
[0009] (2) reacting the product obtained in step (1) with an oxidant to obtain a 3 H group modified clay;
[0010] (3) The SO3 The modified clay with H group and the auxiliary agent are mixed, granulated and calcined to obtain the bulk catalytic proppant.
[0011] A third aspect of the present invention provides an application of the bulk catalytic proppant in shale fracturing micro-fracture support.
[0012] Through the above technical solution, the bulk catalytic proppant of the present invention has the following technical advantages:
[0013] (1) The bulk catalytic proppant of the present invention has the performance of shale micro-fracture support and in-situ catalytic hydrocarbon conversion, which significantly improves the utilization rate of oil shale resources.
[0014] (2) The bulk catalytic proppant of the present invention has the advantages of large acid content, high acid strength, controllable particle size, and easy large-scale preparation, which can improve the oil recovery rate of oil shale and improve the quality of produced oil.
[0015] (3) The method for preparing the bulk catalytic support of the present invention can avoid the step of refluxing the organic solvent, and the process is environmentally friendly.
[0016] (4) The method for preparing the bulk catalytic proppant of the present invention can control the acid content of the proppant according to the processing requirements, thereby adjusting the optimal catalytic proppant dosage for oil shale hydrocarbon generation conversion.
[0017] (5) The fine particle proppant with a particle size of 0.1-2 mm prepared by the present invention can ensure effective support for fracturing micro-cracks and narrow cracks.
[0018] (6) The bulk catalytic proppant used in the present invention has high strength and low acid solubility, meeting national standards.
[0019] (7) The process of the present invention is simple, no waste acid is discharged, and a large-scale oil shale catalytic proppant production line can be quickly formed. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is an electron microscope scanning image of the catalytic proppant of Example 1 of the present invention;
[0021] Figure 2 is an electron microscope scanning image of the catalytic proppant of Example 2 of the present invention;
[0022] Figure 3 is an electron microscope scanning image of the catalytic proppant of Example 3 of the present invention;
[0023] Figure 4 This is an electron microscope scanning image of the catalytic support agent of Example 4 of the present invention. DETAILED DESCRIPTION
[0024] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0025] The first aspect of the present invention provides a bulk catalytic proppant, wherein the catalytic proppant comprises: a catalyst having SO 3 H group-modified clay and additives; wherein the SO 3 In the H-group modified clay, clay and SO 3 The weight ratio of H groups is 5-20:1.
[0026] Clay with SO 3 The H groups generate sulfur-doped carbon quantum dots in the proppant pores, which maintain the acid properties and have high hydrothermal stability, which is the unique advantage of the prepared catalytic proppant. This makes the bulk catalytic proppant have high acid density, controllable acid amount, and good controllability of particle size. At the same time, the present application controls the clay and SO 3 The weight ratio of H groups is 5-20:1, so that SO 3 The modified clay with H groups added to the catalytic proppant has the characteristics of large acid content and high acid strength, which can effectively solve the problem of poor in-situ conversion and hydrocarbon generation performance of resources such as medium and low maturity shale oil and oil shale due to small acid content and low acid strength, and at the same time overcome the defect of insufficient support of expanded clay proppant for narrow cracks and tiny gaps.
[0027] In the present invention, by adding SO 3 H group-modified clay, i.e., sulfonic acid group-modified acid catalyst, can not only catalyze hydrocarbon conversion in situ during fracturing, but also SO 3 The modified clay of H group can also be used as a proppant to work together with additives such as kaolin, bauxite, dolomite, etc. to support the shale micro-cracks during the fracturing process; at the same time, the catalytic proppant of the present invention has the characteristics of large acid content and high acid strength, which can effectively solve the problem of poor in-situ conversion and hydrocarbon generation performance of resources such as medium and low maturity shale oil and oil shale due to small acid content and low acid strength, and overcome the defect of insufficient support of ceramsite proppant for narrow cracks and tiny gaps.
[0028] In some specific embodiments of the present invention, the auxiliary agent includes an additive and a structural auxiliary agent, wherein the additive is selected from one or more of kaolin, bauxite, and dolomite. Adding a certain amount of the above additives to the proppant can improve the strength of the proppant. The structural auxiliary agent is selected from one or more of citric acid, cellulose, and starch. Adding a certain amount of the above structural auxiliary agent to the proppant plays a role in bonding and pore formation, increases the surface area of the proppant, and improves the catalytic and supporting performance. Among the auxiliary agents, the structural auxiliary agent is 5-15wt%.
[0029] In some specific embodiments of the present invention, the SO 3 The weight ratio of the modified clay with H group to the auxiliary agent is 1-10:1. Within this weight ratio range, the prepared proppant has a high acid density.
[0030] In some specific embodiments of the present invention, the particle size of the proppant is 0.1-2 mm, and the particle size distribution can be adjusted according to production requirements, so that the prepared proppant has adjustable acid content and particle size.
[0031] In some specific embodiments of the present invention, the SO 3 The H-group modified clay is obtained by acid activation, thiolization, wet ball milling grafting and oxidation of clay. 3 H group-modified clay, i.e., sulfonic acid group-modified acid catalyst, can not only catalyze hydrocarbon conversion in situ during fracturing, but also SO 3 The modified clay of H group can also be used as a proppant to work together with additives such as kaolin, bauxite, dolomite, etc. to support the shale micro-cracks during the fracturing process; at the same time, the catalytic proppant of the present invention has the characteristics of large acid content and high acid strength, which can effectively solve the problem of poor in-situ conversion and hydrocarbon generation performance of resources such as medium and low maturity shale oil and oil shale due to small acid content and low acid strength, and overcome the defect of insufficient support of ceramsite proppant for narrow cracks and tiny gaps.
[0032] In some specific embodiments of the present invention, the control of the SO 3 The weight ratio of the modified clay with H group to the auxiliary agent is 1-10:1, and the acid amount is adjusted according to the amount of thiol grafting so that the acid amount of the proppant is greater than 1 mmol / g.
[0033] In some specific embodiments of the present invention, the acid content of the proppant is determined by a base adsorption method.
[0034] A second aspect of the present invention provides a method for preparing a bulk catalytic proppant, which comprises the following steps:
[0035] (1) Activating the clay with acid, adding a thiol-forming agent, and performing wet ball milling grafting;
[0036] (2) reacting the product obtained in step (1) with an oxidant to obtain a 3 H group modified clay;
[0037] (3) The SO 3 The modified clay with H group and the auxiliary agent are mixed, granulated and calcined to obtain the bulk catalytic proppant.
[0038] In some specific embodiments of the present invention, in step (1), the acid is selected from one or more of hydrochloric acid, nitric acid and sulfuric acid.
[0039] In some specific embodiments of the present invention, the clay is selected from attapulgite clay and / or zeolite, wherein the zeolite is preferably clinoptilolite.
[0040] In some specific embodiments of the present invention, in step (1), the clay is activated with acid, stirred at 40° C. for a period of time, filtered, and dried.
[0041] In some specific embodiments of the present invention, the thiolating agent is selected from one or more of 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-mercaptopropyldimethoxysilane.
[0042] In some specific embodiments of the present invention, in step (1), after adding the thiol-forming agent, a small amount of water is added, wet ball milling grafting is performed using a ball mill, and the mixture is washed with distilled water and dried.
[0043] In some specific embodiments of the present invention, the oxidant is selected from one or more of hydrogen peroxide, nitric acid, sodium hypochlorite, and peracetic acid.
[0044] In some specific embodiments of the present invention, the auxiliary agent is selected from one or more of kaolin, bauxite and dolomite.
[0045] In some specific embodiments of the present invention, the proppant additive further comprises a structural additive, and the structural additive is selected from one or more of citric acid, cellulose, and starch. A certain amount of the structural additive is added to the proppant to play a role in bonding and pore formation, increase the surface area of the proppant, and improve the catalytic and supporting performance. Among the additives, the structural additive is 5-15wt%.
[0046] In some specific embodiments of the present invention, in step (2), after reacting with an oxidant, washing with distilled water and drying are performed to obtain a product having SO 3 H group modified clay.
[0047] In some specific embodiments of the present invention, the SO 3 H-group modified clay and additives need to be ground before mixing.
[0048] In some specific embodiments of the present invention, the weight ratio of the clay to the auxiliary agent is 1-10:1.
[0049] In some specific embodiments of the present invention, the mass ratio of the clay to the acid, the thiol-forming agent, and the oxidant is 1:3-6:0.3-3:1-9.
[0050] In some specific embodiments of the present invention, in step (3), the calcination temperature is 750-1100° C., and the calcination time is 0.5-3 h.
[0051] The third aspect of the present invention provides an application of the bulk catalytic proppant in shale fracturing micro-fracture support.
[0052] The catalytic proppant prepared by the present invention is applied to the in-situ catalytic conversion of oil shale. In a 100mL intermittent reactor in the laboratory, oil shale, water and the catalytic proppant are added, the temperature is raised to 280-350°C at a certain heating rate, maintained for 4 hours, the reactor is cooled to room temperature, and the product is taken out for product property analysis.
[0053] The present invention will be described in detail below through examples.
[0054] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be obtained through commercial channels.
[0055] Example 1
[0056] 2 g of attapulgite was acidified with 20 mL of 6 mol / L hydrochloric acid, stirred at 40 ° C for a period of time, filtered and dried, and the acidified attapulgite, 2.6 g of 3-mercaptopropyltrimethoxysilane, 10 mL of water and 50 g of agate medium balls were added to a 50 mL resin jar, and ball milled at 300 rpm for 2.5 h using a planetary ball mill. After the reaction was completed, it was washed with distilled water 3 times to remove the unreacted 3-mercaptopropyltrimethoxysilane, and then dried at 85 ° C for 12 h to obtain thiol-modified attapulgite; the prepared thiol-modified attapulgite was added to 50 mL (15%) of an aqueous solution of hydrogen peroxide, stirred at room temperature for 12 h, then washed with distilled water, and dried at 85 ° C to obtain a sulfhydryl-modified attapulgite with SO 3 H group modified clay.
[0057] 40 g of the prepared 3The modified clay with H group and 10g of additives (20wt% kaolin, 65wt% bauxite, 5wt% dolomite, 9wt% cellulose, 1wt% citric acid) were ground separately to obtain kaolin powder, bauxite powder, dolomite powder and SO 3 The mixture of the modified clay powder of H group. After the powder is evenly mixed, it is placed in a spray granulator for granulation. The pellets are placed in an oven for drying. The dried pellets are subjected to programmed temperature calcination, rising to 800°C at 50°C / min, calcining for 90min, and then rising to 1100°C at 50°C / min, calcining for 60min.
[0058] Among them, the obtained proppant contains clay and SO 3 The weight ratio of H groups is 5:1, and the 3 The weight ratio of the H-group modified clay to the auxiliary agent is 4:1, and the acid content of the proppant is 1.496 mmol / g.
[0059] Example 2
[0060] 2 g of attapulgite was acidified with 20 mL of 6 mol / L hydrochloric acid, stirred at 40 ° C for a period of time, filtered and dried, attapulgite, 1.6 g of 3-mercaptopropyltrimethoxysilane, 10 mL of water and 50 g of agate medium balls were added to a 50 mL resin jar, and ball milled at 300 rpm for 2.5 h using a planetary ball mill. After the reaction was completed, it was washed with distilled water 3 times to remove unreacted 3-mercaptopropyltrimethoxysilane, and then dried at 85 ° C for 12 h to obtain mercapto-modified attapulgite; the prepared mercapto-modified attapulgite was added to 30 mL (15%) of an aqueous solution of hydrogen peroxide, stirred at room temperature for 12 h, then washed with distilled water, and dried at 85 ° C to obtain a sulfhydryl-modified attapulgite with SO 3 H group modified clay.
[0061] 40 g of the prepared 3 The modified clay with H group and 10g of additives (30wt% kaolin, 55wt% bauxite, 5wt% dolomite, 9wt% cellulose, 1wt% citric acid) were ground separately to obtain kaolin powder, bauxite powder, dolomite powder and SO 3 The mixture of the modified clay powder of H group. After the powder is evenly mixed, it is placed in a spray granulator for granulation. The pellets are placed in an oven for drying. The dried pellets are subjected to programmed temperature calcination, rising to 800°C at 50°C / min, calcining for 90min, and then rising to 1100°C at 50°C / min, calcining for 60min.
[0062] Among them, the obtained proppant contains clay and SO 3 The weight ratio of H groups is 8:1, and the 3The weight ratio of the H-group modified clay to the auxiliary agent is 4:1, and the acid content of the proppant is 1.253 mmol / g.
[0063] Example 3
[0064] 2 g of clinoptilolite was acidified with 20 mL of 6 mol / L hydrochloric acid, stirred at 40° C. for a period of time, filtered and dried, and the acidified clinoptilolite, 3 g of 3-mercaptopropyltrimethoxysilane, 10 mL of water and 50 g of agate medium balls were added to a 50 mL resin jar, and ball milled at 300 rpm for 2.5 h using a planetary ball mill. After the reaction was completed, it was washed with distilled water for 3 times to remove the unreacted 3-mercaptopropyltrimethoxysilane, and then dried at 85° C. for 12 h to obtain the mercapto-modified clinoptilolite; the prepared mercapto-modified clinoptilolite was added to 25 mL (15%) of an aqueous solution of hydrogen peroxide, stirred at room temperature for 12 h, then washed with distilled water, and dried at 85° C. to obtain a sulfhydryl-modified clinoptilolite with SO 3 H group modified clay.
[0065] 40 g of the prepared 3 The modified clay with H group and 10g of additives (35wt% kaolin, 50wt% bauxite, 5wt% dolomite, 9wt% cellulose, 1wt% citric acid) were ground separately to obtain kaolin powder, bauxite powder, dolomite powder and SO 3 The mixture of the modified clay powder of H group. After the powder is evenly mixed, it is placed in a spray granulator for granulation. The pellets are placed in an oven for drying. The dried pellets are subjected to programmed temperature calcination, rising to 800°C at 50°C / min, calcining for 90min, and then rising to 1100°C at 50°C / min, calcining for 60min.
[0066] Among them, the obtained proppant contains clay and SO 3 The weight ratio of H groups is 10:1, and the 3 The weight ratio of the H-group modified clay to the auxiliary agent is 4:1, and the acid content of the proppant is 1.187 mmol / g.
[0067] Example 4
[0068] 2 g of clinoptilolite was acidified with 20 mL of 6 mol / L hydrochloric acid, stirred at 40° C. for a period of time, filtered and dried, and the acidified clinoptilolite, 0.65 g of 3-mercaptopropyltrimethoxysilane, 10 ml of water and 50 g of agate medium balls were added to a 50 mL resin jar, and ball milled at 300 rpm for 2.5 h using a planetary ball mill. After the reaction was completed, it was washed with distilled water for 3 times to remove the unreacted 3-mercaptopropyltrimethoxysilane, and then dried at 85° C. for 12 h to obtain the mercapto-modified clinoptilolite; the prepared mercapto-modified clinoptilolite was added to 20 mL (15%) of an aqueous solution of hydrogen peroxide, stirred at room temperature for 12 h, then washed with distilled water, and dried at 85° C. to obtain a sulfhydryl-modified clinoptilolite with SO 3 H group modified clay.
[0069] 40 g of the prepared 3 The modified clay with H group and 10g of additives (kaolin 40wt%, bauxite 45wt%, dolomite 5wt%, cellulose 9wt%, citric acid 1wt%) were ground separately to obtain kaolin powder, bauxite powder, dolomite powder and SO 3 The mixture of the modified clay powder of H group. After the powder is evenly mixed, it is placed in a spray granulator for granulation. The pellets are placed in an oven for drying. The dried pellets are subjected to programmed temperature calcination, rising to 800°C at 50°C / min, calcining for 90min, and then rising to 1100°C at 50°C / min, calcining for 60min.
[0070] Among them, the obtained proppant contains clay and SO 3 The weight ratio of H groups is 20:1, and the 3 The weight ratio of the H-group modified clay to the auxiliary agent is 4:1, and the acid content of the proppant is 1.046 mmol / g.
[0071] Comparative Example 1
[0072] 2 g of attapulgite was acidified with 20 mL of 6 mol / L hydrochloric acid, stirred at 40 ° C for a period of time, filtered and dried, and the acidified attapulgite, 4.5 g of 3-mercaptopropyltrimethoxysilane, 10 mL of water and 50 g of agate medium balls were added to a 50 mL resin jar, and ball milled at 300 rpm for 2.5 h using a planetary ball mill. After the reaction was completed, it was washed with distilled water three times to remove the unreacted 3-mercaptopropyltrimethoxysilane, and then dried at 85 ° C for 12 h to obtain mercapto-modified attapulgite; the prepared mercapto-modified attapulgite was added to 80 mL (15%) of an aqueous solution of hydrogen peroxide, stirred at room temperature for 12 h, then washed with distilled water, and dried at 85 ° C to obtain a sulfhydryl-modified attapulgite with SO 3 H group modified clay.
[0073] 40 g of the prepared 3 The modified clay with H group and 10g of additives (20wt% kaolin, 65wt% bauxite, 5wt% dolomite, 9wt% cellulose, 1wt% citric acid) were ground separately to obtain kaolin powder, bauxite powder, dolomite powder and SO 3 The mixture of the modified clay powder of H group. After the powder is evenly mixed, it is placed in a spray granulator for granulation. The pellets are placed in an oven for drying. The dried pellets are subjected to programmed temperature calcination, rising to 800°C at 50°C / min, calcining for 90min, and then rising to 1100°C at 50°C / min, calcining for 60min.
[0074] Among them, the obtained proppant contains clay and SO 3 The weight ratio of H groups is 3:1, and the 3 The weight ratio of the H-group modified clay to the auxiliary agent is 4:1, and the acid content of the proppant is 1.539 mmol / g.
[0075] Comparative Example 2
[0076] 2 g of clinoptilolite was acidified with 20 mL of 6 mol / L hydrochloric acid, stirred at 40° C. for a period of time, filtered and dried, and the acidified clinoptilolite, 0.43 g of 3-mercaptopropyltrimethoxysilane, 10 ml of water and 50 g of agate medium balls were added to a 50 mL resin jar, and ball milled at 300 rpm for 2.5 h using a planetary ball mill. After the reaction was completed, it was washed with distilled water for 3 times to remove the unreacted 3-mercaptopropyltrimethoxysilane, and then dried at 85° C. for 12 h to obtain the mercapto-modified clinoptilolite; the prepared mercapto-modified clinoptilolite was added to an aqueous solution of 15 mL (15%) hydrogen peroxide, stirred at room temperature for 12 h, then washed with distilled water, and dried at 85° C. to obtain a sulfhydryl-modified clinoptilolite with SO 3 H group modified clay.
[0077] 40 g of the prepared 3 The modified clay with H group and 10g of additives (kaolin 40wt%, bauxite 45wt%, dolomite 5wt%, cellulose 9wt%, citric acid 1wt%) were ground separately to obtain kaolin powder, bauxite powder, dolomite powder and SO 3 The mixture of the modified clay powder of H group. After the powder is evenly mixed, it is placed in a spray granulator for granulation. The pellets are placed in an oven for drying. The dried pellets are subjected to programmed temperature calcination, rising to 800°C at 50°C / min, calcining for 90min, and then rising to 1100°C at 50°C / min, calcining for 60min.
[0078] Among them, the obtained proppant contains clay and SO 3The weight ratio of H groups is 30:1, and the 3 The weight ratio of the H-group modified clay to the auxiliary agent is 4:1, and the acid content of the proppant is 0.875 mmol / g.
[0079] The catalytic supports prepared in Examples 1-4 were scanned by electron microscope, and the results were as follows: Figure 1-4 As shown, it can be seen that the prepared proppant has high sphericity and a pore structure.
[0080] The prepared catalytic proppant was used to evaluate the catalytic conversion performance of oil shale in a laboratory batch reactor.
[0081] Test Example 1:
[0082] 8 g of shale powder, 2 g of the catalytic proppant prepared in Example 1, and 20 mL of water were added into a reactor and reacted at 300° C. for 4 h.
[0083] Test Example 2:
[0084] 8 g of shale powder, 2 g of the catalytic proppant prepared in Example 2, and 20 mL of water were added into a reactor and reacted at 300° C. for 4 h.
[0085] Test Example 3:
[0086] 8 g of shale powder, 2 g of the catalytic proppant prepared in Example 3, and 20 mL of water were added into a reactor and reacted at 300° C. for 4 h.
[0087] Test Example 4:
[0088] 8 g of shale powder, 2 g of the catalytic proppant prepared in Example 4, and 20 mL of water were added into a reactor and reacted at 300° C. for 4 h.
[0089] Test Example 5:
[0090] 8 g of shale powder, 2 g of the catalytic proppant prepared in Comparative Example 1, and 20 mL of water were added into a reactor and reacted at 300° C. for 4 h.
[0091] Test Example 6:
[0092] 8 g of shale powder, 2 g of the catalytic proppant prepared in Comparative Example 2, and 20 mL of water were added into a reactor and reacted at 300° C. for 4 h.
[0093] Test Example 7:
[0094] The comparative example is the thermal conversion of pure oil shale without any catalyst. 10 g of shale powder and 20 mL of water were added to a reactor and reacted at 300° C. for 4 h.
[0095] The oil and gas production from pyrolysis of oil shale after adding different catalytic proppants was evaluated by measuring the product oil yield. The results are shown in Table 1.
[0096] Table 1
[0097] project Residue (%) Oil yield (%) Gas production rate (%) Test Example 1 20.8 32.8 46.4 Test Example 2 19.5 31.5 49.5 Test Example 3 20.1 37.8 42.1 Test Example 4 18.3 33.9 47.8 Test Example 5 20.3 33.2 46.5 Test Example 6 24.7 29.8 45.5 Test Example 7 26.2 28.4 45.4
[0098] The results in Table 1 show that compared with the thermal conversion of oil shale without catalytic proppant, the oil yield of the catalytic conversion product of oil shale is significantly increased and the residue rate is significantly reduced after adding catalytic proppant, indicating that the addition of catalytic proppant increases the oil yield. 3 When the weight ratio of H groups is less than 5:1, the catalytic activity of the catalyst proppant is not significantly improved, and the manufacturing cost increases. 3 When the weight ratio of H groups is greater than 20:1, the catalytic activity of the catalyst is significantly weakened. 3 The weight ratio of the H group maintains the acidic properties in the range of 5-20:1, and has high hydrothermal stability. It can effectively solve the problem of poor in-situ conversion and hydrocarbon generation performance of resources such as medium and low maturity shale oil and oil shale due to small acid amount and low acid strength, and overcome the defect of insufficient support of expanded clay proppants for narrow cracks and tiny gaps.
[0099] The elemental analysis of the oil produced by pyrolysis of oil shale after adding different catalytic proppants is shown in Table 2.
[0100] Table 2
[0101]
[0102]
[0103] The results in Table 2 show the effect of the catalytic proppant on the properties of the oil product from oil shale conversion. The elemental analysis of the product oil shows that the addition of the catalytic proppant in Examples 1-4 improves the H / C ratio of the product oil, and the output oil saturation is higher. At the same time, it shows excellent deoxygenation and denitrification modification effects, which improves the quality of the product oil. In Comparative Example 1, the clay and SO used in Test Example 5 are 3 The weight ratio of H groups is 3:1. 3 When the H group content is high, the effect is not obvious, but the cost increases greatly; for Comparative Example 2, that is, the clay and SO used in Test Example 6 3 The weight ratio of H groups is 30:1, and its deoxidation and denitrification modification effect is poor. Therefore, the clay and SO in the catalytic proppant 3 The weight ratio of H groups in the range of 5-20:1 maintains the acidic properties, produces higher oil saturation, and exhibits excellent deoxygenation and denitrification modification effects.
[0104] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A bulk catalytic proppant, characterized in that: The catalytic support comprises: modified clay with SO3H groups and an auxiliary agent; wherein, in the modified clay with SO3H groups, the weight ratio of clay to SO3H groups is 5-20:
1.
2. The catalytic proppant according to claim 1, characterized in that: The weight ratio of the modified clay with SO3H groups to the auxiliary agent is 1-10:1; Preferably, the auxiliary agent includes an additive and a structural auxiliary agent, wherein the additive is selected from one or more of kaolin, bauxite, and dolomite, and the structural auxiliary agent is selected from one or more of citric acid, cellulose, and starch; Preferably, in the auxiliary agent, the content of the structural auxiliary agent is 5-15wt%, and the content of the additive is 85-95wt%.
3. The catalytic proppant according to claim 1 or 2, characterized in that: The particle size of the catalytic proppant is 0.1-2 mm; Preferably, the modified clay with SO3H groups is obtained by sequentially subjecting clay to acid activation, thiolization, wet ball milling grafting and oxidation; Preferably, the acid content of the proppant is greater than 1 mmol / g.
4. A method for preparing a bulk catalytic proppant, characterized in that: The following steps are involved: (1) After the clay is activated with acid, a thiol-forming agent is added to perform wet ball milling grafting; (2) reacting the product obtained in step (1) with an oxidant to obtain a modified clay having a SO3H group; (3) The modified clay with SO3H groups and the auxiliary agent are mixed, and the bulk catalytic support is obtained by granulation and calcination.
5. The preparation method according to claim 4, characterized in that: In step (1), the acid is selected from one or more of hydrochloric acid, nitric acid and sulfuric acid; Preferably, the clay is selected from attapulgite and / or zeolite; Preferably, the zeolite is clinoptilolite.
6. The preparation method according to claim 4 or 5, characterized in that: The mercapto group-forming agent is selected from one or more of 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-mercaptopropyldimethoxysilane; Preferably, the oxidant is selected from one or more of hydrogen peroxide, nitric acid, sodium hypochlorite and peracetic acid.
7. The preparation method according to any one of claims 4 to 6, characterized in that: The auxiliary agents include additives and structural auxiliary agents; Preferably, the additive is selected from one or more of kaolin, bauxite, and dolomite, and the structural additive is selected from one or more of citric acid, cellulose, and starch; Preferably, in the auxiliary agent, the content of the structural auxiliary agent is 5-15wt%, and the content of the additive is 85-95wt%.
8. The preparation method according to any one of claims 4 to 7, characterized in that: The weight ratio of the modified clay with SO3H group to the auxiliary agent is 1-10:1; Preferably, the mass ratio of the clay to the acid, the thiol-forming agent, and the oxidant is 1:3-6:0.3-3:1-9.
9. The preparation method according to any one of claims 4 to 8, characterized in that: In step (3), the calcination temperature is 750-1100° C. and the calcination time is 0.5-3 h.
10. Use of the bulk catalytic proppant described in any one of claims 1 to 3 and the bulk catalytic proppant prepared by the preparation method described in any one of claims 4 to 9 in shale fracturing micro-fracture support.
Citation Information
Patent Citations
Dual function proppants
CN103764945A
Double-layer high-strength fracturing propping agent and preparing method thereof
CN105131934A
PROPPANT
RU2011141386A