Forging-rolling-heat treatment coordinated regulation and control grain refining and homogenizing method for large ring piece

Through the coordinated control method of forging-rolling-heat treatment, the problem of uneven temperature and deformation in the molding of large ring parts is solved, and the fine grain homogenization is achieved, and the performance and quality of ring parts are improved.

CN119061248APending Publication Date: 2024-12-03WUHAN UNIV OF TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411201659.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Large ring parts are prone to uneven temperature and deformation problems during the forming process, resulting in coarse crystals and mixed crystals in the forgings, affecting the quality.

Method used

The forging-rolling-heat treatment collaborative control method is adopted to obtain the blank through four upsetting and three draw-out treatments. The S-type rolling curve and outer diameter length velocity curve are designed for rolling, and combined with low-temperature pretreatment and solid solution heat treatment. Regulates grain size and structure.

Benefits of technology

The grain fine homogenization and forming of large austenitic stainless steel ring parts is achieved, which improves the performance and quality of the forgings and avoids uneven temperature and deformation problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061248A_ABST
    Figure CN119061248A_ABST
Patent Text Reader

Abstract

The invention provides a large ring piece forging-rolling-heat treatment coordinated regulation and control grain refining and homogenizing method, and belongs to the field of metal component manufacturing. A bar is subjected to four times of upsetting and three times of drawing-out treatment to obtain a blank; an S-shaped rolling curve is designed according to the change conditions of the required product size parameters of the ring piece and the size parameters of the blank, an outer diameter growth speed curve of the ring piece is designed, the blank is rolled according to the S-shaped rolling curve and the outer diameter growth speed curve, and a forged piece is obtained; and heat treatment: performing low-temperature pretreatment on the forge piece, and combining a solid solution heat treatment means to obtain a final product. According to the method, the grain size is regulated and controlled through collaborative matching of forging and rolling heat treatment process parameters, blank grains are refined and homogenized through multi-directional matching deformation in the blank manufacturing process, ring piece grains are refined and homogenized through multi-parameter collaborative rolling in the ring rolling process, and ring piece grain structures are regulated and controlled through low-temperature pretreatment combined with solid solution heat treatment in the heat treatment process; and grain refining and homogenizing forming of the large austenitic stainless steel ring piece is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal component manufacturing, and in particular to a method for coordinated regulation of grain refinement and homogenization of large ring parts by forging-rolling-heat treatment. Background Art

[0002] Large rings are key components of major equipment such as nuclear power, wind power, and aerospace, and their performance directly affects the reliability and safety of equipment operation. With the development trend of large-scale nuclear power equipment, the new generation of nuclear power requires ultra-large austenitic stainless steel rings with a diameter of more than 5 meters. The working and service conditions are harsh, and extremely high requirements are placed on the performance of the rings. The manufacture of high-performance large rings requires seamless forging structure, and seamless forging structure often needs to be obtained through overall plastic forming. Therefore, the ring rolling process is the main method for manufacturing high-performance large rings. In addition, ensuring that the grains inside the ring are small and uniform is an important way to further improve the performance of the ring.

[0003] CN102489639A of China discloses a fine-grained rolling forming method for large high-alloy steel rings, which is manufactured by radial-axial rolling forming process. Ring rolling is an advanced plastic processing technology for producing large rings. It can obtain high-performance rings with high geometric accuracy and dense structure in a short time through continuous rotational plastic deformation. The principle is that the ring blank is continuously bitten into the radial rolling pass formed by the driving roller and the core roller under the action of the rotation of the driving roller and the linear feeding of the core roller; at the same time, the ring is clamped up and down by two tapered rollers and rotated to provide up and down feeding; the ring blank is continuously subjected to the action of the radial and axial rolling pass, resulting in continuous local plastic deformation to reduce its wall thickness and height, expand its diameter, and form the cross-sectional profile, and finally obtain the specified shape and size. However, for large rings, due to the heavy weight of the forgings and the generally large cross-sectional size, problems such as temperature and uneven deformation are prone to occur during the forming process, resulting in problems such as coarse grains and mixed grains in the rings, which seriously affects the quality of the forgings. Summary of the invention

[0004] In view of this, the present invention proposes a method for coordinated regulation of grain refinement and homogenization of large ring forging-rolling-heat treatment, which is used to solve the problem that the current large ring forming method easily causes uneven temperature and deformation of the forgings, resulting in coarse grains and mixed grains in the rings, thereby seriously affecting the quality of the forgings.

[0005] The technical solution of the present invention is implemented as follows: The present invention provides a method for coordinated regulation of grain refining and homogenization of large rings by forging-rolling-heat treatment, comprising the following steps: step one, forging: subjecting the bar to four upsetting and three drawing treatments to obtain a blank; step two, rolling: designing an S-shaped rolling curve in combination with the required product size parameters of the ring and the changes in the size parameters of the blank, and designing an outer diameter growth rate curve of the ring, rolling the blank according to the S-shaped rolling curve and the outer diameter growth rate curve to obtain a forging; step three, heat treatment: performing low-temperature pretreatment on the forging and combining it with solid solution heat treatment to obtain the final product.

[0006] On the basis of the above technical scheme, preferably, in step one, the bar is columnar, with the axial direction of the bar as the z direction, and the two directions perpendicular to each other on the radial section of the bar as the x direction and the y direction, and the bar is forged in the following order: upsetting in the z direction, drawing in the x direction, upsetting in the x direction, drawing in the y direction, upsetting in the y direction, drawing in the z direction, and upsetting in the z direction; during the last upsetting, the bar is forged to the height of the blank, and then rounded, punched, and the end face is flattened to obtain the blank.

[0007] More preferably, the deformation amount of each upsetting is controlled between 50% and 70%, and the deformation amount of each stretching is controlled between 35% and 55%.

[0008] On the basis of the above technical solution, preferably, in step 2, the S-shaped rolling curve is a three-segment rolling curve, which has a straight line of segment I, a straight line of segment II and a straight line of segment III connected in sequence, and the formula of the three-segment rolling curve is,

[0009]

[0010] Among them, Δb and Δh are the radial and axial deformation of the blank and forging before and after the ring rolling, respectively; b0 and b f Respectively represent the wall thickness of the blank and forging; h0 and h f They represent the height of the blank and the forging respectively; K is defined as the radial-axial deformation ratio, which represents the ratio of Δb and Δh; k1 and k2 are the slopes of the first and third straight lines respectively; μ1 and μ2 are the wall thickness reduction coefficients of the first and second straight lines respectively.

[0011] More preferably, when the size parameters of the blank are converted according to the required product size parameters of the ring, the required product size parameters of the ring are the same as the size parameters of the forging. According to the principle of constant volume, the blank height h0, thickness b0 and inner radius r0 can be converted to be, respectively,

[0012]

[0013]

[0014]

[0015] Where, λ is defined as the ratio of the cross-sectional area of ​​the blank to that of the forging, r f The inner radius of the required product for the ring.

[0016] More preferably, λ≥2.

[0017] On the basis of the above technical solution, preferably, the rolling process in step 2 is divided into five stages: biting hole type, overall forging, stable rolling, shaping and sizing. At the end of each stage, the outer radius of the ring should reach the corresponding design size R i , the calculation formula of the ring growth rate curve is:

[0018] R i =R0+β i (R f -R0) (i=1,2,3,4),

[0019] Among them, R0 is the outer radius of the blank, R f is the outer radius of the forging; β1 ranges from 0.05 to 0.1, β2 ranges from 0.15 to 0.2, β3 ranges from 0.7 to 0.85, and β4 ranges from 0.95 to 0.98.

[0020] More preferably, during the rolling process, the ring is driven by the rolling equipment to rotate with a ring speed V Di , when biting into the hole type, it is the initial rolling stage, and the ring speed increase V at the beginning of the initial rolling stage D1 The ring speed V at the beginning of the overall forging stage is 1-2 mm / s. D2 The main rolling stage is 2-5 mm / s, and the ring speed increase V in the main rolling stage is D3 The ring speed V at the end of the shaping stage and the sizing stage is 10-20 mm / s. D4 0.5~3mm / s.

[0021] On the basis of the above technical scheme, preferably, in step three, the forgings after rolling are first subjected to low-temperature pretreatment, heated to the low-temperature preheating temperature of the material and kept warm, and then cooled by furnace cooling; then solution heat treatment is performed, heated to the solution heating temperature of the material and kept warm, and then quickly cooled to room temperature by water cooling.

[0022] More preferably, during the rolling process of step 2, the temperature range of the forging is controlled to be 1180-1220°C, and the outer surface temperature range of the forging is controlled to be 850-900°C at the end of rolling. After rolling, the forging is transferred to a water pool for cooling within 2 minutes, and the forging is cooled until the surface temperature of the forging drops below 100°C before being taken out of the water.

[0023] The large ring forging-rolling-heat treatment coordinated control grain refining and homogenization method of the present invention has the following beneficial effects compared with the prior art:

[0024] This patent controls the grain size by coordinated matching of forging-rolling-heat treatment process parameters. In the billet making process, the billet grains are refined and homogenized through multi-directional matching deformation. In the ring rolling process, the ring grains are refined and homogenized through multi-parameter coordinated rolling. In the heat treatment process, the grain structure of the ring is controlled by low-temperature pretreatment combined with solution heat treatment, thereby realizing the fine and homogenized grain forming of large austenitic stainless steel rings. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 Schematic diagram of the method of the present invention, wherein (a) is step one, (b) is step two, and (c) is step three;

[0027] Figure 2 1 is a schematic flow diagram of the four-upsetting and three-drawing process in step 1 of the method of the present invention, wherein (1) is a three-dimensional schematic diagram of a bar material, and (2) to (8) are schematic diagrams of four upsetting and three drawing steps respectively;

[0028] Figure 3 It is a side cross-sectional view of the ring of the present invention, wherein the upper figure is a blank, and the lower figure is a ring of the required size of the product;

[0029] Figure 4 is a rolling curve diagram of the method of the present invention;

[0030] Figure 5 The figure is a ring growth rate curve diagram of the method of the present invention.

[0031] In the figure: 1. Ring; 2. Bar; 3. Blank; 4. Forging. DETAILED DESCRIPTION

[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] like Figure 1 As shown, a large ring forging-rolling-heat treatment coordinated control grain refining and homogenization method of the present invention comprises the following steps:

[0034] Step 1, forging: After the bar is heated and kept warm, the bar 2 is subjected to four upsetting and three drawing processes, and then rounded, punched, and flattened to obtain a blank 3. The purpose of this step is to achieve the purpose of fine and homogenous blank grains through multi-directional matching deformation of the bar 2.

[0035] Step 2, rolling: Based on the required product size parameters of the ring 1, according to the size, rolling ratio and radial-axial deformation ratio of the ring 1, the size parameters of the blank 3 are converted, and a simplified S-shaped rolling curve is designed in combination with the required product size parameters of the ring 1 and the changes in the size parameters of the blank 3 to control the size evolution process from the section of the blank 3 to the section of the target forging 4, and a reasonable outer diameter growth rate curve of the ring 1 is designed. The blank 3 is rolled according to the S-shaped rolling curve and the outer diameter growth rate curve to obtain the forging 4. The motion control of each roller is determined by the rolling curve and the outer diameter growth rate curve of the ring 1; the temperature of the ring 1 is coordinated to be within the required range at the beginning and end of the rolling, and the forging 4 is quickly transferred to the water pool for rapid cooling after the rolling is completed. The purpose of this step is to achieve the purpose of fine and homogenized billet grains through multi-parameter coordinated rolling of the bar 2.

[0036] Step 3, heat treatment: The final product is obtained by combining low-temperature pretreatment with solution heat treatment on the forging 4, which can effectively suppress the coarse grain and mixed grain defects of the solution heat treatment caused by uneven deformation of austenitic stainless steel.

[0037] exist Figure 2 In a preferred embodiment shown, in step one, the bar 2 is columnar, preferably cylindrical, with the axial direction of the bar 2 as the z direction, and the two directions perpendicular to each other on the radial circular section of the bar 2 as the x direction and the y direction, respectively, and the bar 2 is forged in the following order: upsetting in the z direction, stretching in the x direction, upsetting in the x direction, stretching in the y direction, upsetting in the y direction, stretching in the z direction, and upsetting in the z direction; during the last upsetting, the bar 2 is forged to the height of the blank 3, and then rounded, punched, and flattened to obtain the blank 3.

[0038] exist Figure 2 In a preferred embodiment shown, the deformation amount of each upsetting is controlled between 50 and 70%, and the deformation amount of each drawing is controlled between 35 and 55%, which can achieve the purpose of refining and homogenizing the grains of the billet.

[0039] exist Figure 4 In a preferred embodiment shown in FIG. 1 , in step 2, the S-shaped rolling curve is a three-segment rolling curve, which is formed by sequentially connecting the first segment straight line, the second segment straight line and the third segment straight line. The formula of the three-segment rolling curve is:

[0040]

[0041] Wherein, Δb and Δh are the radial and axial deformations of the blank 3 and the forging 4 before and after the ring 1 is rolled, respectively; b0 and b f Respectively represent the wall thickness of the blank 3 and the forging 4; h0 and h f They represent the height of the blank 3 and the forging 4 respectively; K is defined as the radial-axial deformation ratio, which represents the ratio of Δb and Δh; k1 and k2 are the slopes of the first and third straight lines respectively; μ1 and μ2 are the wall thickness reduction coefficients of the first and third straight lines respectively, and their value ranges are 0 to 1. By selecting appropriate k1, k2, μ1, and μ2, a ​​three-stage rolling curve can be obtained.

[0042] exist Figure 3 In a preferred embodiment shown in the figure, when the size parameters of the blank 3 are converted according to the required product size parameters of the ring 1, the required product size parameters of the ring 1 are the same as the size parameters of the forging 4. According to the principle of constant volume, the height h0, thickness b0 and inner radius r0 of the blank 3 can be converted respectively.

[0043]

[0044]

[0045]

[0046] Among them, λ defines the rolling ratio, which represents the ratio of the cross-sectional area of ​​the blank 3 to the forging 4, r f It is the inner radius of the required product of the ring 1.

[0047] The radial-axial deformation ratio K represents the ratio of Δb to Δh. Specifically,

[0048]

[0049] For the ratio λ of the cross-sectional area of ​​the blank 3 and the forging 4, specifically,

[0050]

[0051] exist Figure 3 In a preferred embodiment shown in the figure, the ring blank size can be obtained by selecting a suitable rolling ratio and radial-axial deformation ratio. Usually, to obtain a dense grain structure, λ≥2 should be taken; the radial-axial deformation ratio K is determined according to the radial and axial force energy of the equipment and the height-to-thickness ratio of the forging 4.

[0052] exist Figure 5In a preferred embodiment shown in FIG. 1 , the rolling process in step 2 is divided into five stages: biting hole type, overall forging, stable rolling, shaping and sizing. At the end of each stage, the outer radius of the ring 1 should reach the corresponding design size R i , the calculation formula for the growth rate curve of ring 1 is:

[0053] R i =R0+β i (R f -R0) (i=1,2,3,4),

[0054] Among them, R0 is the outer radius of blank 3, R f is the outer radius of forging 4; β1 ranges from 0.05 to 0.1, β2 ranges from 0.15 to 0.2, β3 ranges from 0.7 to 0.85, and β4 ranges from 0.95 to 0.98.

[0055] exist Figure 5 In a preferred embodiment shown in the figure, during the rolling process, the ring 1 is driven by the rolling equipment to rotate with a ring speed V. Di , when biting into the hole type, it is the initial rolling stage, and the ring speed increase V at the beginning of the initial rolling stage D1 The ring speed V at the beginning of the overall forging stage is 1-2 mm / s. D2 The main rolling stage is 2-5 mm / s, and the ring speed increase V in the main rolling stage is D3 The ring speed V at the end of the shaping stage and the sizing stage is 10-20 mm / s. D4 The core roller radial feed speed V can be obtained from the designed rolling curve and the growth rate curve of the ring 1. f and the tapered roller axial feed speed V a , thereby controlling the movement of the rolls during the rolling process.

[0056] exist Figure 1 In a preferred embodiment shown, in step three, the forging 4 after rolling is first subjected to low-temperature pretreatment, heated to the low-temperature preheating temperature of the material and kept warm, and then cooled by furnace cooling; then solution heat treatment is performed, heated to the solution heating temperature of the material and kept warm, and then quickly cooled to room temperature by water cooling. Before the final solution heat treatment, the deformation energy storage distribution inside the grains of the material is homogenized by low-temperature pretreatment, which can effectively suppress the coarse grain and mixed grain defects caused by uneven deformation of austenitic stainless steel during forging and rolling.

[0057] exist Figure 1In a preferred embodiment shown in the figure, during the rolling process of step 2, the temperature range of the forging 4 is controlled to be 1180-1220°C to avoid excessive temperature causing serious grain coarsening of the ring 1; at the end of rolling, the outer surface temperature range of the forging 4 is controlled to be 850-900°C; after rolling, the forging 4 is transferred to a water pool for cooling within 2 minutes, and is cooled until the surface temperature of the forging 4 drops below 100°C before being taken out of the water to avoid the core of the ring 1 being in a high temperature state for a long time at the end of rolling, which may cause serious grain growth in the core.

[0058] Taking a certain 316H stainless steel super-large ring 1 as an example, the ring 1 is manufactured by the method of the present application.

[0059] Target product forging 4 wall thickness b f =443mm, height h f =790mm, inner radius r f =7557mm. The forging-rolling-heat treatment coordinated control grain refinement and homogenization process method includes the following steps:

[0060] Step 1: Calculate the blanking weight according to the target forging size, heat the bar 2 to a temperature within the range of 1180-1220°C and keep it warm for 2 hours, then perform four upsetting and three drawing treatments in sequence along the x, y, and z axes of the bar 2 to obtain a rolled blank 3.

[0061] Step 2, first calculate the size of blank 3, take K = 3.7462, λ = 2.4448, and get the size of blank 3 b0 = 930mm, h0 = 920mm, r0 = 3014mm; then design the rolling curve, take k1 = k2 = 0.2, μ1 = 0.2, μ2 = 0.8, then the rolling curve expression is,

[0062]

[0063] Then design the growth rate curve of ring 1, that is, the ring speed-increasing curve, taking β1 = 0.1, β2 = 0.15, β3 = 0.8, β4 = 0.95, then R1 = 4349.6mm, R2 = 4552.4mm, R3 = 7188.8mm, R4 = 7797.2mm; V D1 =2mm / s, V D2 =4mm / s, V D3 =15mm / s, V D4 =1mm / s; From the designed rolling curve and ring speed-increasing curve, the radial feed speed V of the core roller can be obtained. f and the tapered roller axial feed speed V a , thereby controlling the movement of the rollers during rolling and ensuring that the outer surface temperature is within the range of 850-900°C at the end of rolling.

[0064] Step three, the ring 1 after rolling is subjected to low-temperature pretreatment and solution heat treatment to adjust the grain structure of the ring. First, the deformation energy storage distribution inside the material grains is homogenized through low-temperature pretreatment. The specific measures are heating to 940°C and then keeping it warm for 6 hours, and then furnace cooling. Then, the final solution heat treatment is carried out. The specific measures are heating to 1020°C and then keeping it warm for 3 hours, and then rapid cooling by water cooling is adopted.

[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for coordinated regulation of grain refinement and homogenization of large rings by forging, rolling and heat treatment, characterized in that: The following steps are included: Step 1, forging: subjecting the bar material (2) to four upsetting processes and three drawing processes to obtain a blank (3); Step 2, rolling: designing an S-shaped rolling curve based on the required product size parameters of the ring (1) and the changes in the size parameters of the blank (3), and designing an outer diameter growth rate curve of the ring (1), rolling the blank (3) according to the S-shaped rolling curve and the outer diameter growth rate curve to obtain the forging (4); Step three, heat treatment: performing low temperature pretreatment on the forging (4) and combining it with solid solution heat treatment to obtain the final product.

2. The method for coordinated grain refinement and homogenization of large ring forging-rolling-heat treatment according to claim 1 is characterized in that: In the step 1, the bar (2) is columnar, with the axial direction of the bar (2) being the z direction, and the two mutually perpendicular directions on the radial section of the bar (2) being the x direction and the y direction, respectively, and the bar (2) is forged in the following order: upsetting in the z direction, drawing in the x direction, upsetting in the x direction, drawing in the y direction, upsetting in the y direction, drawing in the z direction, and upsetting in the z direction; during the last upsetting, the bar (2) is forged to the height of the blank (3), and then rounded, punched, and flattened to obtain the blank (3).

3. The method for coordinated regulation of grain refinement and homogenization of large ring forging-rolling-heat treatment according to claim 2 is characterized in that: The deformation amount of each upsetting is controlled between 50 and 70%, and the deformation amount of each drawing is controlled between 35 and 55%.

4. The method for coordinated regulation of grain refinement and homogenization of large ring forging-rolling-heat treatment according to claim 1 is characterized in that: In the step 2, the S-shaped rolling curve is a three-segment rolling curve, which is formed by connecting the first segment straight line, the second segment straight line and the third segment straight line in sequence. The formula of the three-segment rolling curve is: Wherein, Δb and Δh are respectively the radial and axial deformations of the blank (3) and the forging (4) before and after the ring (1) is rolled; b0 and b f represent the wall thickness of the blank (3) and the forging (4) respectively; h0 and h f They respectively represent the heights of the blank (3) and the forging (4); K is defined as the radial-axial deformation ratio, which represents the ratio of Δb and Δh; k1 and k2 are respectively the slopes of the first and third straight lines; μ1 and μ2 are respectively the wall thickness reduction coefficients of the first and third straight lines.

5. The method for coordinated regulation of grain refinement and homogenization of large ring forging-rolling-heat treatment according to claim 4 is characterized in that: When the size parameters of the blank (3) are converted based on the required product size parameters of the ring (1), the required product size parameters of the ring (1) are the same as the size parameters of the forging (4). Based on the principle of constant volume, the height h0, thickness b0 and inner radius r0 of the blank (3) can be converted to be respectively: Wherein, λ defines the rolling ratio, which is expressed as the ratio of the cross-sectional area of ​​the blank (3) to the cross-sectional area of ​​the forging (4), and r f is the inner radius of the required product of the ring (1).

6. The method for coordinated regulation of grain refinement and homogenization of large ring forging-rolling-heat treatment according to claim 5 is characterized in that: λ≥2.

7. The method for coordinated regulation of grain refinement and homogenization of large ring forging-rolling-heat treatment according to claim 1 is characterized in that: The rolling process in step 2 is divided into five stages: biting hole type, overall forging, stable rolling, shaping and sizing. At the end of each stage, the outer radius of the ring (1) should reach the corresponding design size R i The calculation formula of the growth rate curve of the ring (1) is: R i =R0+β i (R f -R0)(i=1,2,3,4), Wherein, R0 is the outer radius of the blank (3), R f is the outer radius of the forging (4); β1 has a value range of 0.05 to 0.1, β2 has a value range of 0.15 to 0.2, β3 has a value range of 0.7 to 0.85, and β4 has a value range of 0.95 to 0.

98.

8. The method for coordinated regulation of grain refinement and homogenization of large ring forging-rolling-heat treatment according to claim 7 is characterized in that: During the rolling process, the ring (1) is driven by the rolling equipment to rotate with a ring speed V. Di , when biting into the hole type, it is the initial rolling stage, and the ring speed increase V at the beginning of the initial rolling stage D1 The ring speed V at the beginning of the overall forging stage is 1-2 mm / s. D2 The main rolling stage is 2-5 mm / s, and the ring speed V in the main rolling stage is D3 The ring speed V at the end of the shaping stage and the sizing stage is 10-20 mm / s. D4 0.5~3mm / s.

9. The method for coordinated regulation of grain refinement and homogenization of large ring forging-rolling-heat treatment according to claim 1, characterized in that: In the step three, the forging (4) after rolling is first subjected to low-temperature pretreatment, heated to the low-temperature preheating temperature of the material and kept warm, and then cooled by furnace cooling; then solution heat treatment is performed, heated to the solution heating temperature of the material and kept warm, and then quickly cooled to room temperature by water cooling.

10. The method for coordinated regulation of grain refinement and homogenization of large ring forging-rolling-heat treatment according to claim 9, characterized in that: During the rolling process of step 2, the temperature of the forging (4) is controlled to be in the range of 1180-1220° C., and at the end of rolling, the outer surface temperature of the forging (4) is controlled to be in the range of 850-900° C. After rolling, the forging (4) is transferred to a water pool for cooling for a period of less than 2 minutes, and is cooled until the surface temperature of the forging (4) drops below 100° C. before being taken out of the water.

Citation Information

Cited By

  • Forging process for improving grain size of GH4145 high-temperature alloy

    CN119794233A

  • Martensite ring piece production method

    CN120190302A