High-density lanthanum-lead intermetallic compound LaPb3 and preparation method thereof
Through the rapid molding of the cold crucible magnetic levitation vacuum smelting and water-cooled casting, the density problem of the lanthanum-lead intermetallic compound LaPb3 is solved, and the preparation of high-density LaPb3 ingots is achieved, which meets the performance requirements of nuclear fusion neutron multiplier and reduces production cost.
Patent Information
- Application Number
- CN202411573281.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-11-06
AI Technical Summary
It is difficult to prepare high-density lanthanum lead intermetallic compound LaPb3 in the prior art. Conventional smelting methods have problems with raw material volatility, segregation and pores, and cannot meet the performance requirements of nuclear fusion neutron multiplier.
The cold crucible magnetic levitation vacuum smelting equipment is used for suspension and smelting, combined with water-cooled casting and rapid molding, the raw material ratio and high-frequency magnetic field stirring are regulated, the raw material volatility and segregation are avoided, and the raw material is achieved, and sufficient reaction and stable molding are achieved.
LaPb3 ingots with a density greater than 90% were prepared to meet the functional needs of neutron multiplier and provide an economical and feasible large-scale industrial production solution.
Smart Images

Figure CN119061276A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of new material technology, specifically to the field of nuclear fusion material technology, and in particular to a high-density lanthanum-lead intermetallic compound LaPb 3 and a preparation method thereof. Background Art
[0002] The nuclear fusion reaction process is based on the reaction of deuterium (D) and tritium (T) to produce helium (He) and 14.1 MeV neutrons (D+T→He+n). T needs to be continuously supplied during the reaction, but this element cannot be directly obtained in the natural environment. Tritium needs to be produced by neutron irradiation of tritium breeder materials, that is, neutrons react with Li elements to produce T to achieve tritium self-sustaining in fusion reactors. Not all neutrons from fusion reactions can be used for T generation, and some of them are lost due to parasitic absorption of structural materials and non-functional materials. Therefore, neutron multiplication is required to produce additional neutrons to compensate for the lost neutrons.
[0003] At present, the two most widely studied neutron multiplication metal materials in the world are beryllium and lead. Beryllium has a sufficiently high (n, 2n) neutron multiplication reaction rate (the threshold is about 1.86 MeV) and a high melting point (1287°C), so it can be used in solid form in the solid blanket of the fusion demonstration reactor (DEMO). However, Be-based multipliers also have many disadvantages, such as limited natural reserves, high cost, and strong toxicity. Compared with Be, the lead (n, 2n) neutron multiplication reaction threshold is higher (about 6.76 MeV), but for 14.1MeV fusion neutrons, lead has a higher reaction cross section than Be. At the same time, lead-based materials are widely used as neutron multipliers because of their abundant reserves and low prices. LaPb 3 Since the melting point is above 1100℃, it can be used in solid form and is one of the most promising lead-based solid compounds for solid neutron multipliers. In terms of cost, compared with solid blankets using solid Be-based neutron multipliers, dense LaPb 3 The material will significantly reduce the economic cost of the fusion reactor DEMO.
[0004] The neutron multiplier of DEMO solid blanket needs to have a high density to meet the performance requirements. 3 The material can be prepared by induction melting and arc melting. Conventional induction melting methods do not react fully in a short period of time, and mechanical stirring is required to promote the reaction of the raw materials. Long-term heating will aggravate the volatilization and burning of the raw materials. The arc melting method uses plasma discharge to instantly heat to a high temperature zone. The raw metal lead has a low melting point, and the instantaneous high temperature will cause violent volatilization. The prepared material has serious segregation and porosity. Therefore, the preparation processes that have been reported cannot produce the bulk material performance requirements required for solid neutron multipliers.
[0005] Want to prepare high-density intermetallic compound LaPb 3 The block material is very difficult to obtain, and there are no related reports at home and abroad. This is because the raw metal lead and metal lanthanum are volatile, and conventional rare earth alloys or lead-based alloys are generally smelted with melting points close to or with trace amounts of doping. LaPb 3 The system contains a large amount of metallic lanthanum and metallic lead, and the melting point difference between the two metal raw materials is huge. Excessive temperature treatment will cause uncontrollable volatilization and burning of the raw materials. Metal lanthanum is prone to agglomeration, and the raw materials need to be fully in contact and react during the smelting process. The binding energy of lanthanum-lead intermetallic compounds is low. Long-term heat treatment or high-temperature treatment may cause decomposition or volatilization of the material. In short, excessive volatilization and burning, metal lanthanum agglomeration and decomposition reactions in the reaction between metallic lanthanum and metallic lead will lead to the formation of pores in the casting process, seriously affecting the density of the ingot. It is difficult to prepare lanthanum-lead intermetallic compounds LaPb with a density greater than 90%. 3 Ingot. Summary of the invention
[0006] The purpose of the present invention is to provide a high-density lanthanum-lead intermetallic compound LaPb 3 The invention relates to a preparation process of a lanthanum-lead intermetallic compound LaPb with a density greater than 90%. The invention discloses a method for preparing a lanthanum-lead intermetallic compound LaPb with a density greater than 90%. The method is designed to achieve full reaction of suspension smelting and rapid molding of water-cooled casting, regulate the volatilization and burning loss of raw metal lead and metal lanthanum, avoid the segregation and agglomeration behavior of metal lanthanum elements and the high-temperature decomposition of intermetallic compounds, and obtain a lanthanum-lead intermetallic compound LaPb with a density greater than 90%. 3 Ingot casting meets the functional requirements of solid neutron multipliers. This provides an economically feasible large-scale industrial production solution for the research and development of lead-based neutron multipliers. The technical solution adopted by the present invention is:
[0007] A high-density lanthanum-lead intermetallic compound LaPb 3 And a preparation method thereof, comprising the following steps:
[0008] (1) Using metallic lead and metallic lanthanum as raw materials;
[0009] (2) Use cold crucible magnetic levitation vacuum melting equipment for suspension melting;
[0010] (3) Water-cooled mold casting to obtain a high-density lanthanum-lead intermetallic compound ingot;
[0011] As one of the preferred embodiments of the present invention, in step (1), the raw materials of lead and lanthanum are mixed in a molar ratio of 3:1.05-1.15, preferably 3:1.1. Micro-control of the raw material ratio can compensate for the different degrees of volatilization and burning loss of the raw materials of lead and lanthanum during the sintering process. Both the raw materials of lanthanum and lead are easy to volatilize, and there is volatilization and burning loss during the high-temperature sintering process. The burning loss of lanthanum is more serious. Therefore, it is necessary to adjust the raw materials to an excessive amount of lanthanum in order to achieve sufficient reaction to obtain the pure phase of the intermetallic compound LaPb 3 Too much Pb in the raw material will lead to the presence of metallic Pb residue in the product. The low melting point of metallic Pb will seriously affect the intermetallic compound LaPb 3 The La content is too high, which will lead to the presence of metallic La residue in the product. The melting point of metallic La is lower than 1110℃ and it is unstable in the air. It will react quickly with water and oxygen, causing the compound to hydrolyze and deteriorate, seriously affecting the intermetallic compound LaPb 3 Stability and its application functions.
[0012] As one of the preferred embodiments of the present invention, in step (1), the size of the block material is less than 2 cm. Raw materials that are too large cannot be fully stirred in a short time after being melted.
[0013] As one of the preferred embodiments of the present invention, in step (2), a cold crucible magnetic suspension vacuum melting equipment is used for melting, and the melting environment gas is one or more of nitrogen, argon and helium.
[0014] As one of the preferred embodiments of the present invention, in step (2), the temperature is raised and smelted by the high-frequency magnetic field of a cold crucible magnetic suspension vacuum melting device. After reaching the melting point of the raw material (reaching the melting point of lanthanum, 920°C, i.e., both the raw material metal lead and the metal lanthanum are melted), the temperature is continued to be raised to overheat by 50-60°C to reach the melting temperature.
[0015] As one of the preferred embodiments of the present invention, in the step (2), the melting temperature is reached and the mixture is kept warm and stirred continuously for 10-20 minutes using magnetic flux lines.
[0016] As one of the preferred embodiments of the present invention, in step (2), after smelting is completed, heating is stopped and the material is allowed to cool naturally to room temperature in the crucible. The cooled and formed ingot is mechanically reversed to complete the ingot turning. The cumulative number of ingot turnings is greater than or equal to 2 times. For example, when the raw material reaches the melting point, it continues to be heated to 50-60°C, kept warm and stirred continuously for 10-20 minutes using magnetic flux lines, and then the heating is stopped to allow the material to cool naturally in the crucible. The cooled and formed ingot is mechanically reversed to complete an ingot turning. Then continue to repeat the heating treatment until the melting point is overheated by 50-60°C, kept warm and stirred continuously for 10-20 minutes using magnetic flux lines, and then turned over for the second time after cooling. Then repeat the high-frequency magnetic field heating treatment until the melting point is overheated by 50-60°C, kept warm and stirred continuously for 10-20 minutes using magnetic flux lines.
[0017] As one of the preferred embodiments of the present invention, in the step (3), the molten liquid is cast into a mold, and the mold material can be one or more of copper, stainless steel, and graphite.
[0018] As one of the preferred embodiments of the present invention, in step (3), a water-cooled mold is used for casting, and the mold temperature during the casting process is lower than 60°C.
[0019] The present invention reduces the burning loss caused by the low melting point and volatility of the raw material metal lanthanum and metal lead through the full reaction of suspension smelting and rapid molding by water-cooling casting, and avoids the LaPb 3 The lanthanum-lead intermetallic compound LaPb was prepared by decomposition and segregation of lanthanum elements. 3 The density of the ingot is greater than 90%, which meets the performance requirements of nuclear fusion neutron multiplier materials. The preparation method designed by the present invention is simple and can achieve high-density lanthanum-lead intermetallic compound LaPb at a low economic cost. 3 Large-scale batch production. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The high-density lanthanum-lead intermetallic compound LaPb obtained in Example 1 3 Appearance morphology diagram;
[0021] Figure 2 The high-density lanthanum-lead intermetallic compound LaPb obtained in Example 1 3 XRD pattern of
[0022] Figure 3 The high-density lanthanum-lead intermetallic compound LaPb obtained in Example 1 3 SEM images of
[0023] Figure 4 The high-density lanthanum-lead intermetallic compound LaPb obtained in Example 1 3EDS element analysis diagram;
[0024] Figure 5 This is the appearance morphology of the sample ingot obtained in Comparative Example 1;
[0025] Figure 6 This is the SEM image of the sample ingot obtained in Comparative Example 1;
[0026] Figure 7 This is the appearance morphology of the sample ingot obtained in Comparative Example 2. DETAILED DESCRIPTION
[0027] The present invention is further described below in conjunction with specific implementation examples so that those skilled in the art can better understand the present invention. However, the protection scope of the present invention is not limited to the following embodiments, and the scope of rights of the present invention shall be subject to the scope of the claims.
[0028] Example 1
[0029] A high-density lanthanum-lead intermetallic compound LaPb 3 The preparation process is:
[0030] (1) Using metallic lead and metallic lanthanum particles as raw materials; the metallic lead and metallic lanthanum raw materials are mixed in a molar ratio of 3:1.1; and the size of the metallic lead and metallic lanthanum raw materials is less than 2 cm.
[0031] (2) Use cold crucible magnetic levitation vacuum melting equipment for melting. Under the protection of high-purity nitrogen, place the prepared raw materials in the copper crucible of the melting furnace and start heating and melting under the action of high-frequency magnetic field. After the raw materials reach the melting point, continue to heat up by 50°C, keep warm and stir continuously for 15 minutes using magnetic flux lines, then stop heating and let the material cool naturally to room temperature in the crucible. Mechanically reverse the cooled ingot to complete one ingot flipping. Then continue to repeat the heating treatment until the melting point is overheated by 50°C, keep warm and stir continuously for 15 minutes using magnetic flux lines, and then turn the ingot over for the second time after cooling. Then repeat the high-frequency magnetic field heating treatment until the melting point is overheated by 50°C, keep warm and stir continuously for 15 minutes using magnetic flux lines.
[0032] (3) The molten metal after smelting in stage (2) is cast into a mold using a stainless steel water-cooled mold. The mold temperature is kept below 60°C. LaPb is obtained after casting. 3 Ingot.
[0033] After the above steps, high-density LaPb 3 Ingot, appearance and morphology Figure 1 shown.
[0034] The obtained LaPb 3 The ingot was subjected to phase characterization, and its XRD results are shown in Figure 2 As shown, the characteristic peak matches PDF#65-7232, and the sample is LaPb 3 structure.
[0035] The obtained LaPb 3 The ingot was subjected to microstructural analysis, and its SEM morphology is as follows Figure 3 As shown in Figure 1, the surface of the micro-scale sample is dense. The ESD element analysis results of the sample are shown in Figure 1. Figure 4 As shown, the elements lanthanum and lead are evenly distributed without element segregation and agglomeration.
[0036] The obtained LaPb 3 The density of the ingot was analyzed by using the water displacement method (using alcohol and water as the medium) to determine the sample density. The sample volume was converted by the mass product of the liquid displacement, and the density of the sample ingot was calculated. The density of the sample was obtained by comparing the theoretical density of the material. The results are shown in Table 1, and the density of the materials is greater than 90%.
[0037] Table 1 LaPb 3 Ingot density determination
[0038] medium Sample mass (dry weight), m, (g) Weight gain of sample in medium, Δm, (g) <![CDATA[Volume of medium displaced by the sample, v = Δm / ρ, (cm 3 ).]]> <![CDATA[Sample density, ρ = m / v, (g / cm 3 ).]]> <![CDATA[Apparent density (LaPb 3 Theoretical density 10.72 g / cm 3 )(%)]]> Alcohol 1.776 0.135 0.171 10.387 96.9 water 0.301 0.030 0.030 10.092 94.1
[0039] Comparative Example 1
[0040] Preparation of LaPb by induction melting 3 Ingot. 3 The ingot preparation process is as follows:
[0041] Using lead and lanthanum as raw materials, the surface of the raw materials is cleaned, and the surface of the tooling is purified. A vacuum induction melting furnace is used for production, and the smelting is performed at a vacuum degree below 10Pa. After the lead liquid is heated to 950°C, the lanthanum metal begins to melt. After it is completely melted at 1250°C, it is left to stand for 10 minutes, and the temperature is repeated 3 times. The liquid stirring is strengthened to ensure the alloying of the liquid. After the alloy temperature rises to 1350°C, it is kept still and cast into the mold. After solidification and cooling for 3 hours, it is taken out of the furnace and demolded.
[0042] After the above steps, LaPb 3 Ingot, appearance and morphology Figure 5 As shown in Figure 2, the surface of the ingot is uneven, and there are many pits and holes.
[0043] The obtained LaPb 3 The ingot was subjected to microstructural analysis, and its SEM morphology was as follows Figure 6 As shown, there is obvious element segregation on the surface of the microscopic sample, and there is an obvious porous structure in the lanthanum agglomeration area.
[0044] The obtained LaPb 3The density of the ingot was analyzed by using the drainage method (using alcohol and water as the medium) to determine the sample density. The sample volume was converted using the mass product of the liquid that was drained, and the density of the sample ingot was calculated. The theoretical density of the material was used to determine the density of the sample. The results are shown in Table 2, and the density of the materials was less than 90%.
[0045] This experiment proves that induction heating melting and conventional mold casting cannot produce high-density LaPb 3 This is because the method cannot quickly achieve sufficient reaction between the raw material metal lanthanum and metal lead and the LaPb in the slow cooling process. 3 Possible decomposition reactions, the escape of these atmospheres and element segregation will lead to obvious pore structures in the ingot, resulting in low density of the ingot and failure to meet the performance requirements of the neutron multiplier.
[0046] Table 2 LaPb prepared by induction melting 3 Ingot density determination
[0047] medium Sample mass (dry weight), m, (g) Weight gain of sample in medium, Δm, (g) <![CDATA[Volume of medium displaced by the sample, v = Δm / ρ, (cm 3 ).]]> <![CDATA[Sample density, ρ = m / v, (g / cm 3 ).]]> <![CDATA[Apparent density (LaPb 3 Theoretical density 10.72 g / cm 3 )(%)]]> water 5.511 0.607 0.607 9.079 84 Alcohol 7.125 0.617 0.782 9.114 85
[0048] Comparative Example 2
[0049] Preparation of LaPb by Arc Melting 3 Ingot casting, the preparation process is:
[0050] Lead and lanthanum are used as raw materials and mixed in a ball mill under inert gas protection. A vacuum arc melting furnace is used for preparation, and the vacuum degree is maintained below 10 Pa. The raw materials are melted at high temperature in the form of plasma arc discharge, and then cooled and demolded.
[0051] After the above steps, LaPb 3 Ingot, appearance and morphology Figure 7 As shown in the figure, the surface of the ingot is uneven and there is serious raw material segregation. This is because the low-melting-point metal lead undergoes violent volatilization and burning at the instantaneous high temperature of arc melting.
[0052] This experiment proves that the arc melting method cannot produce high-density LaPb 3 Ingot casting. This is because the raw material metal lead has a low melting point, and instantaneous high temperature will cause violent volatilization and burning of the raw material, resulting in serious element segregation in the sample, poor density, and failure to meet the performance requirements of the neutron multiplier.
[0053] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high-density lanthanum-lead intermetallic compound LaPb 3 The preparation method of It is characterized in that The following steps are involved: (1) Using metallic lead and metallic lanthanum as raw materials; (2) Use cold crucible magnetic levitation vacuum melting equipment for suspension melting; (3) Water-cooled mold casting to obtain high-density lanthanum-lead intermetallic compound LaPb 3 Ingot.
2. The high density lanthanum-lead intermetallic compound LaPb according to claim 1 3 The preparation method of It is characterized in that In step (1), the metal lead and the metal lanthanum are in a molar ratio of 3:1.05-1.
15.
3. The high density lanthanum-lead intermetallic compound LaPb according to claim 1 3 The preparation method of It is characterized in that In step (1), the metal lead and the metal lanthanum are both metal blocks with a size less than 2 cm.
4. The high density lanthanum-lead intermetallic compound LaPb according to claim 1 3 The preparation method of It is characterized in that In step (2), the ambient gas for suspension smelting is one or more of high-purity nitrogen, argon, and helium.
5. The high density lanthanum-lead intermetallic compound LaPb according to claim 1 3 The preparation method of It is characterized in that In step (2), the temperature is raised and melted by the high-frequency magnetic field of the cold crucible magnetic levitation vacuum melting equipment. After reaching the melting point of the raw material, the temperature is further raised by 50-60°C to reach the melting temperature. The temperature is kept and stirred continuously for 10-20 minutes using magnetic flux lines. After the melting is completed, the heating is stopped and the material is allowed to cool naturally to room temperature in the crucible. The cooled and formed ingot is mechanically reversed to complete the ingot turning.
6. The high density lanthanum-lead intermetallic compound LaPb according to claim 5 3 The preparation method of It is characterized in that The cumulative number of ingot turning is greater than or equal to 2 times.
7. The high density lanthanum-lead intermetallic compound LaPb according to claim 1 3 The preparation method of It is characterized in that In step (3), the molten metal is cast into a mold, and the mold material is one or more of copper, stainless steel, and graphite.
8. The high density lanthanum-lead intermetallic compound LaPb according to claim 1 3 The preparation method of It is characterized in that In step (3), a water-cooled mold is used for casting, and the mold temperature during the casting process is lower than 60°C.
9. A high-density lanthanum-lead intermetallic compound LaPb 3 Ingot, It is characterized in that The preparation method is used as described in any one of claims 1 to 8.
Citation Information
Patent Citations
High strength lead alloy and manufacturing method thereof
CN101476057A
Smelting preparation method of large-sized titanium-aluminum intermetallic ingot
CN104388714A
Lead-based neutron multiplier suitable for fusion reactor solid cladding
CN114708991A
Production Method for High-Purity Lanthanum, High-Purity Lanthanum, Sputtering Target Composed of High-Purity Lanthanum, and Metal Gate Film Containing High-Purity Lanthanum as Main Component
US20130241010A1
Additively manufactured high-temperature aluminum alloys, and feedstocks for making the same
US20200199716A1