Porous degradable iron-manganese alloy bone scaffold material as well as preparation method and application thereof
The preparation of porous degradable iron-manganese alloy bone stents through electrode induction smelting and 3D printing technology solves the problem of insufficient mechanical properties and biocompatibility of bone stent materials, and achieves effective bone defect repair and new bone formation in the weight-bearing area.
Patent Information
- Application Number
- CN202411084129.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-12-03
AI Technical Summary
The existing bone stent materials have shortcomings in mechanical properties and biocompatibility, and cannot be effectively used for the repair of bone defects, especially in the weight-bearing area, which is difficult to form new bones.
Electrode induction smelting is used to prepare porous degradable iron-manganese alloy bone scaffold material. Through a combination of 3D printing and heat treatment, a mesh structure is designed to regulate porosity and pore structure, ensuring that the mechanical properties of the material match the bones in the intended repair area, and Surface polishing is achieved through cleaning treatment.
It achieves good biocompatibility of the material, quantitative adjustment of the degradation rate, and improves the mechanical properties after degradation, and is suitable for bone defect repair in the weight-bearing area.
Smart Images

Figure BDA0004984675130000141 
Figure BDA0004984675130000151
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of degradable alloy bone scaffolds, and relates to a porous degradable iron-manganese alloy bone scaffold material and a preparation method and application thereof. Background Art
[0002] Bone tissue is the hardest connective tissue in the human body and plays an irreplaceable role in maintaining body functions. As the scaffold of the human body, bones are responsible for supporting, maintaining, bearing weight, hematopoiesis, calcium storage and metabolism. The treatment of bone defects has long been a major problem that has plagued mankind. Clinically proven, autologous bone transplantation is the best way to treat bone defects, but at the expense of healthy tissue. Allogeneic bone transplantation has superior histological characteristics, but there is an immune rejection reaction, it is susceptible to virus infection, and the cost of sample preparation, processing and storage is high.
[0003] The emergence of tissue engineering has provided a new option for the clinical treatment of bone defects. Using three-dimensional digital preparation technology, a three-dimensional digital model of the bone defect site can be constructed before surgery, which can "tailor-make" high-precision implant bone scaffold products and surgical plans for patients, thereby improving the success rate of surgery and making the surgery more precise and safer. At the same time, three-dimensional digital technology can manufacture non-standard and personalized bone scaffolds with complex structural shapes and integrated gradient performance designs to meet the needs of different patients.
[0004] Ceramic bone scaffolds have been widely studied because they do not dissolve metal ions and do not cause allergic reactions. At present, ceramic-based bone scaffolds based on hydroxyapatite, β-tricalcium phosphate or composite with polymers have good biocompatibility, but their mechanical properties and long-term stability need to be improved, and they cannot be used to repair bone defects in weight-bearing areas. Medical metal materials such as tantalum and titanium have good mechanical properties and biocompatibility, but they cannot be degraded, and it is difficult to form new bone during the bone defect repair process.
[0005] In summary, providing a degradable bone scaffold material with excellent mechanical properties and biocompatibility and a preparation method thereof is an urgent problem to be solved by those skilled in the art. Summary of the invention
[0006] The purpose of the present invention is to provide a porous degradable iron-manganese alloy bone scaffold material and a preparation method and application thereof. The porous degradable iron-manganese alloy bone scaffold material prepared by combining electrode induction smelting and powder making, 3D printing and heat treatment has good biocompatibility, quantitatively adjustable degradation rate, good mechanical properties and bone ingrowth in vivo after degradation.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a method for preparing a porous degradable iron-manganese alloy bone scaffold material, the preparation method comprising the following steps:
[0009] (1) subjecting the iron-manganese pre-alloy to electrode induction melting to obtain an iron-manganese pre-alloy powder;
[0010] (2) designing a mesh structure of a 3D printing model of an iron-manganese alloy bone scaffold material, then performing layered slicing, and importing the layered slicing results into a 3D printing program;
[0011] The porosity of the network structure is 37.89-77.17%, for example, it can be 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, 62%, 65%, 68%, 70%, 72% or 75%, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0012] (3) sequentially performing 3D printing, heat treatment and cleaning on the iron-manganese pre-alloyed powder obtained in step (1);
[0013] There is no particular order in which steps (1) and (2) are performed.
[0014] In the present invention, the layered slicing is to layer the 3D printed structure model along the height direction, and each slice generated by the layered slicing is parallel to the reference plane of the slice; the thickness of the slice is 30-50 μm.
[0015] The preparation method provided by the present invention adopts a one-step electrode induction melting gas atomization method to prepare powder, and the obtained iron-manganese pre-alloy powder has less element burnout, better fluidity, more uniform composition and less impurities introduced; by designing a mesh structure and adopting a combination of 3D printing and heat treatment, an iron-manganese alloy bone scaffold material matching the shape of the bone defect can be customized, and while achieving quantitative adjustment of the porosity and pore structure, it is ensured that the mechanical properties of the iron-manganese alloy match the mechanical properties of the bone in the area to be repaired, thereby solving the problem of mutual restriction between high porosity and mechanical properties of the bone scaffold material; finally, the obtained iron-manganese alloy is cleaned, and the surface of the iron-manganese alloy can be polished while cleaning.
[0016] As a preferred technical solution of the present invention, the iron-manganese pre-alloy in step (1) comprises, by weight percentage: Mn 28-32%, C < 0.05%, Si < 0.01%, N < 0.01%, O ≤ 0.224%, and the balance is Fe.
[0017] It is worth noting that the present invention controls the Mn content within the range of 28-32, with the remainder being Fe, to ensure that the bone scaffold material has good mechanical strength and bone ingrowth after degradation; by controlling the trace elements C, Si and N within the range of <0.01%, the above elements are prevented from excessively affecting the mechanical properties of the iron-manganese alloy.
[0018] In the present invention, the mass percentage of Mn in the iron-manganese pre-alloy is 28-32%, for example, it can be 28.5%, 29%, 29.5%, 30%, 30.5%, 31% or 31.5%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0019] As a preferred technical solution of the present invention, the smelting power of the electrode induction smelting in step (1) is 15-25KW, for example, it can be 16KW, 17KW, 18KW, 19KW, 20KW, 21KW, 22KW, 23KW or 24KW, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0020] Preferably, the feed rate of the electrode induction melting in step (1) is 40-55 mm / min, for example, it can be 42 mm / min, 45 mm / min, 46 mm / min, 48 mm / min, 50 mm / min, 52 mm / min or 54 mm / min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0021] Preferably, the gas used in the electrode induction smelting in step (1) comprises an inert gas.
[0022] In the present invention, the inert gas includes argon.
[0023] Preferably, the gas pressure used in the electrode induction smelting in step (1) is 3-5 MPa, for example, 3.2 MPa, 3.5 MPa, 3.6 MPa, 3.8 MPa, 4 MPa, 4.2 MPa, 4.5 MPa, 4.6 MPa or 4.8 MPa, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0024] Preferably, the nozzle gap in the electrode induction melting in step (1) is 0.3-0.5 mm, for example, it can be 0.32 mm, 0.35 mm, 0.36 mm, 0.38 mm, 0.4 mm, 0.42 mm, 0.45 mm, 0.46 mm or 0.48 mm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0025] In the present invention, the nozzle structure consists of an upper and a lower part, and the distance between the centers of the two parts is the nozzle gap.
[0026] In the present invention, during the electrode induction smelting process, the parameters such as smelting power, feed rate, gas pressure and nozzle gap are controlled, so that the powder composition is more uniform, the impurity content is lower, and the fluidity is stronger, so that the particle size of the obtained iron-manganese pre-alloyed powder is within the range of 15-53μm and meets the process technology requirements of 3D printing.
[0027] Preferably, the average particle size of the iron-manganese pre-alloyed powder in step (1) is 15-53 μm, for example, it can be 18 μm, 20 μm, 22 μm, 25 μm, 28 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm or 52 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] As a preferred technical solution of the present invention, the pore size of the mesh structure in step (2) is 100-400 μm, for example, it can be 120 μm, 150 μm, 180 μm, 200 μm, 220 μm, 250 μm, 280 μm, 300 μm, 320 μm, 350 μm or 380 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] Preferably, the rod diameter of the mesh structure in step (2) is 300-500 μm, for example, it can be 320 μm, 350 μm, 380 μm, 400 μm, 420 μm, 450 μm, 460 μm or 480 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0030] In the present invention, the rod diameter refers to the diameter of the rods constituting the mesh structure.
[0031] It is worth noting that the present invention prepares a porous iron-manganese alloy bone scaffold by designing a mesh structure and then regulating the porosity, pore shape and rod diameter structure in the mesh structure, and the high porosity of the obtained iron-manganese alloy bone scaffold matches the mechanical properties.
[0032] As a preferred technical solution of the present invention, the power of the 3D printing in step (3) is 250-320 W, for example, it can be 255 W, 260 W, 265 W, 270 W, 275 W, 280 W, 285 W, 290 W, 295 W, 300 W, 305 W, 310 W or 315 W, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0033] Preferably, the scanning speed of the 3D printing in step (3) is 700-1000 mm / s, for example, it can be 750 mm / s, 800 mm / s, 850 mm / s, 900 mm / s or 950 mm / s, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0034] Preferably, the scanning pitch of the 3D printing in step (3) is 0.1-0.15 mm, for example, it can be 0.11 mm, 0.12 mm, 0.13 mm or 0.14 mm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0035] Preferably, the scanning layer thickness of the 3D printing in step (3) is 30-50 μm, for example, 30 μm, 40 μm or 50 μm, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0036] As a preferred technical solution of the present invention, the heat treatment in step (3) is carried out under vacuum conditions.
[0037] In the present invention, the vacuum degree of the heat treatment is less than 10 -3 Pa.
[0038] Preferably, the temperature of the heat treatment in step (3) is 840-860°C, for example, it can be 842°C, 845°C, 848°C, 850°C, 852°C, 855°C or 858°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0039] Preferably, the holding time of the heat treatment in step (3) is 105-135 min, for example, it can be 107 min, 110 min, 112 min, 115 min, 118 min, 120 min, 122 min, 125 min, 128 min, 130 min or 132 min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0040] In the present invention, by controlling the temperature and holding time of the heat treatment, an iron-manganese alloy can be obtained whose mechanical properties perfectly match the mechanical properties of the bone in the intended repair area.
[0041] In the present invention, after the heat treatment and heat preservation are completed, the process further includes cooling the furnace to room temperature.
[0042] As a preferred technical solution of the present invention, after the heat treatment in step (3), wire cutting is also included before the cleaning treatment.
[0043] Preferably, the cleaning solution of the cleaning treatment in step (3) comprises hydrofluoric acid and water.
[0044] Preferably, the volume ratio of hydrofluoric acid to water is (3-6):(94-97), for example, 3:97, 3.5:96.5, 4:96, 4.5:95.5, 5:95, 5.5:94.5 or 6:94, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0045] In the present invention, hydrofluoric acid and water in a specific volume ratio are used as cleaning liquid, so that the surface of the sample can be cleaned and polished at the same time.
[0046] In the present invention, the total volume of the hydrofluoric acid and water is 100, and the mass concentration of the hydrofluoric acid is 25-35%, for example, it can be 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33% or 34%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0047] Preferably, the cleaning treatment time in step (3) is 30-40s, for example, it can be 31s, 32s, 33s, 34s, 35s, 36s, 37s, 38s or 39s, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0048] Preferably, the cleaning process in step (3) also includes drying, sterilization and packaging in sequence.
[0049] Preferably, the drying temperature is 60-80°C, for example, 62°C, 65°C, 68°C, 70°C, 72°C, 75°C or 78°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0050] Preferably, the drying time is 10-30 min, for example, it can be 12 min, 15 min, 18 min, 20 min, 22 min, 25 min, 26 min or 28 min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0051] As a preferred technical solution of the present invention, the preparation method comprises the following steps:
[0052] (1) subjecting the iron-manganese pre-alloy to electrode induction melting to obtain an iron-manganese pre-alloy powder having an average particle size of 15-53 μm;
[0053] The iron-manganese pre-alloy comprises, in terms of mass percentage, 28-32% Mn, C<0.05%, Si<0.01%, N<0.01%, O≤0.224%, and the balance is Fe;
[0054] The melting power of the electrode induction melting is 15-25KW, the feed rate is 40-55mm / min, the gas pressure used is 3-5MPa, and the nozzle gap is 0.3-0.5mm;
[0055] (2) designing a mesh structure of a 3D printing model of an iron-manganese alloy bone scaffold material, then performing layered slicing, and importing the layered slicing results into a 3D printing program;
[0056] The porosity of the mesh structure is 37.89-77.17%, the pore size is 100-400 μm, and the rod diameter is 300-500 μm;
[0057] (3) sequentially performing 3D printing, heat treatment, wire cutting and cleaning on the iron-manganese pre-alloyed powder obtained in step (1);
[0058] The power of the 3D printing is 250-320W, the scanning speed is 700-1000mm / s, the scanning spacing is 0.1-0.15mm, and the scanning layer thickness is 30-50μm;
[0059] The heat treatment is carried out under vacuum conditions; the heat treatment temperature is 840-860°C, and the insulation time is 105-135min;
[0060] The cleaning solution of the cleaning treatment comprises hydrofluoric acid and water in a volume ratio of (3-6): (94-97); the cleaning treatment time is 30-40s;
[0061] The cleaning process also includes drying, sterilization and packaging in sequence;
[0062] There is no particular order in which steps (1) and (2) are performed.
[0063] In a second aspect, the present invention provides a porous degradable iron-manganese alloy bone scaffold material, wherein the porous degradable iron-manganese alloy bone scaffold material is prepared by the preparation method described in the first aspect.
[0064] Preferably, the porosity of the porous degradable iron-manganese alloy bone scaffold material is 37.89-77.17%, for example, it can be 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, 62%, 65%, 68%, 70%, 72% or 75%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0065] Preferably, the average pore size of the porous degradable iron-manganese alloy bone scaffold material is 100-400 μm, for example, it can be 120 μm, 150 μm, 180 μm, 200 μm, 220 μm, 250 μm, 280 μm, 300 μm, 320 μm, 350 μm or 380 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0066] Preferably, the elastic modulus of the porous degradable iron-manganese alloy bone scaffold material is 10.4-14.88 Gpa, for example, it can be 10.5 Gpa, 11 Gpa, 11.5 Gpa, 12 Gpa, 12.5 Gpa, 13 Gpa, 13.5 Gpa, 14 Gpa or 14.5 Gpa, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0067] Preferably, the yield strength of the porous degradable iron-manganese alloy bone scaffold material is 160.70-243.3 MPa, for example, it can be 170 MPa, 180 MPa, 190 MPa, 200 MPa, 210 MPa, 220 MPa, 230 MPa or 240 MPa, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0068] The iron-manganese alloy bone scaffold material prepared by the invention is paramagnetic, has good biocompatibility both in vitro and in vivo, has good bone ingrowth in vivo, has quantitatively adjustable degradation rate and good mechanical properties after degradation, and is suitable for use in preparing artificial bones.
[0069] In a third aspect, the present invention provides an application of the porous degradable ferromanganese alloy bone scaffold material as described in the second aspect, wherein the application of the porous degradable ferromanganese alloy bone scaffold material in preparing artificial bones is preferably an application in preparing artificial bones in weight-bearing areas.
[0070] Compared with the prior art, the present invention has the following beneficial effects:
[0071] (1) The preparation method provided by the present invention adopts a one-step method of electrode induction melting gas atomization to prepare powder, and the obtained iron-manganese pre-alloy powder has less element burnout, better fluidity, more uniform composition and less impurities introduced; by designing a mesh structure and combining 3D printing and heat treatment, an iron-manganese alloy bone scaffold material matching the shape of the bone defect can be customized, and the porosity and pore structure can be quantitatively adjusted while ensuring that the mechanical properties of the iron-manganese alloy are perfectly matched with the mechanical properties of the bone in the intended repair area, thereby solving the problem of the high porosity and mechanical properties of the bone scaffold material being mutually restricted; finally, the obtained iron-manganese alloy is cleaned, and the surface of the iron-manganese alloy can be polished while cleaning;
[0072] (2) The iron-manganese alloy bone scaffold material obtained by the present invention is paramagnetic, has good biocompatibility both in vitro and in vivo, has good bone ingrowth in vivo, and has quantitatively adjustable degradation rate and good mechanical properties after degradation, and is suitable for use in the preparation of artificial bones. DETAILED DESCRIPTION
[0073] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0074] Example 1
[0075] This embodiment provides a method for preparing a porous degradable iron-manganese alloy bone scaffold material, the preparation method comprising the following steps:
[0076] (1) subjecting the iron-manganese pre-alloy to electrode induction melting to obtain an iron-manganese pre-alloy powder having an average particle size of 35 μm;
[0077] The iron-manganese pre-alloy comprises, in terms of mass percentage, 30% Mn, less than 0.05% C, less than 0.01% Si, less than 0.01% N, 0.2% O, and the balance Fe;
[0078] The melting power of the electrode induction melting is 20KW, the feed rate is 48mm / min, the argon pressure used is 4MPa, and the nozzle gap is 0.4mm;
[0079] (2) designing a mesh structure of a 3D printing model of an iron-manganese alloy bone scaffold material, then performing layered slicing, and importing the layered slicing results into a 3D printing program;
[0080] The porosity of the mesh structure is 48.00%, the pore size is 400 μm, and the rod diameter is 400 μm;
[0081] (3) sequentially performing 3D printing, heat treatment, wire cutting and cleaning on the iron-manganese pre-alloyed powder obtained in step (1);
[0082] The power of the 3D printing is 290W, the scanning speed is 850mm / s, the scanning spacing is 0.12mm, and the scanning layer thickness is 40μm;
[0083] The vacuum degree of the heat treatment is 10 -4 Pa, temperature is 850°C, and holding time is 120min; after the heat treatment, the furnace is cooled to room temperature;
[0084] The cleaning solution for the cleaning treatment includes hydrofluoric acid and water in a volume ratio of 5:95; the mass concentration of the hydrofluoric acid is 30%; and the cleaning treatment time is 35s;
[0085] The cleaning process also includes drying, sterilization and packaging in sequence; the drying temperature is 70°C and the time is 20 minutes;
[0086] There is no particular order in which steps (1) and (2) are performed.
[0087] Example 2
[0088] This embodiment provides a method for preparing a porous degradable iron-manganese alloy bone scaffold material, the preparation method comprising the following steps:
[0089] (1) subjecting the iron-manganese pre-alloy to electrode induction melting to obtain an iron-manganese pre-alloy powder having an average particle size of 35 μm;
[0090] The iron-manganese pre-alloy comprises, in terms of mass percentage, 28% Mn, less than 0.05% C, less than 0.01% Si, less than 0.01% N, 0.15% O, and the balance Fe;
[0091] The melting power of the electrode induction melting is 15KW, the feed rate is 40mm / min, the argon pressure used is 5MPa, and the nozzle gap is 0.3mm;
[0092] (2) designing a mesh structure of a 3D printing model of an iron-manganese alloy bone scaffold material, then performing layered slicing, and importing the layered slicing results into a 3D printing program;
[0093] The porosity of the mesh structure is 44%, the pore size is 200 μm, and the rod diameter is 300 μm;
[0094] (3) sequentially performing 3D printing, heat treatment, wire cutting and cleaning on the iron-manganese pre-alloyed powder obtained in step (1);
[0095] The power of the 3D printing is 250W, the scanning speed is 700mm / s, the scanning spacing is 0.1mm, and the scanning layer thickness is 30μm;
[0096] The vacuum degree of the heat treatment is 5×10 -4 Pa, temperature is 840°C, and holding time is 135min; after the heat treatment, the furnace is cooled to room temperature;
[0097] The cleaning solution for the cleaning treatment comprises hydrofluoric acid and water in a volume ratio of 5:95; the mass concentration of the hydrofluoric acid is 30%; and the cleaning treatment time is 40s;
[0098] The cleaning process also includes drying, sterilization and packaging in sequence; the drying temperature is 70°C and the time is 20 minutes;
[0099] There is no particular order in which steps (1) and (2) are performed.
[0100] Example 3
[0101] This embodiment provides a method for preparing a porous degradable iron-manganese alloy bone scaffold material, the preparation method comprising the following steps:
[0102] (1) subjecting the iron-manganese pre-alloy to electrode induction melting to obtain an iron-manganese pre-alloy powder having an average particle size of 35 μm;
[0103] The iron-manganese pre-alloy comprises, in terms of mass percentage, 32% Mn, less than 0.05% C, less than 0.01% Si, less than 0.01% N, 0.1% O, and the balance Fe;
[0104] The melting power of the electrode induction melting is 25KW, the feed rate is 55mm / min, the argon pressure used is 3MPa, and the nozzle gap is 0.5mm;
[0105] (2) designing a mesh structure of a 3D printing model of an iron-manganese alloy bone scaffold material, then performing layered slicing, and importing the layered slicing results into a 3D printing program;
[0106] The porosity of the mesh structure is 40%, the pore size is 100 μm, and the rod diameter is 400 μm;
[0107] (3) sequentially performing 3D printing, heat treatment, wire cutting and cleaning on the iron-manganese pre-alloyed powder obtained in step (1);
[0108] The power of the 3D printing is 320W, the scanning speed is 1000mm / s, the scanning spacing is 0.15mm, and the scanning layer thickness is 50μm;
[0109] The vacuum degree of the heat treatment is 5×10 -4 Pa, temperature is 860°C, and holding time is 105min; after the heat treatment, the furnace is cooled to room temperature;
[0110] The cleaning solution for the cleaning treatment comprises hydrofluoric acid and water in a volume ratio of 5:95; the mass concentration of the hydrofluoric acid is 30%; and the cleaning treatment time is 30s;
[0111] The cleaning process also includes drying, sterilization and packaging in sequence; the drying temperature is 70°C and the time is 20 minutes;
[0112] There is no particular order in which steps (1) and (2) are performed.
[0113] Example 4
[0114] This embodiment provides a method for preparing a porous degradable iron-manganese alloy bone scaffold material. Except that the mass content of Mn in the iron-manganese pre-alloy in step (1) is 22%, other conditions are the same as those in Example 1.
[0115] Example 5
[0116] This embodiment provides a method for preparing a porous degradable iron-manganese alloy bone scaffold material. Except that the mass content of Mn in the iron-manganese pre-alloy in step (1) is 36%, other conditions are the same as those in Example 1.
[0117] Example 6
[0118] This embodiment provides a method for preparing a porous degradable iron-manganese alloy bone scaffold material. Except that the pore size of the mesh structure in step (2) is 20 μm, other conditions are the same as those in Example 1.
[0119] Example 7
[0120] This embodiment provides a method for preparing a porous degradable iron-manganese alloy bone scaffold material. Except that the pore size of the mesh structure in step (2) is 500 μm, other conditions are the same as those in Example 1.
[0121] Example 8
[0122] This embodiment provides a method for preparing a porous degradable iron-manganese alloy bone scaffold material. Except that the diameter of the rods of the mesh structure in step (2) is 200 μm, other conditions are the same as those in Example 1.
[0123] Example 9
[0124] This embodiment provides a method for preparing a porous degradable iron-manganese alloy bone scaffold material. Except that the rod diameter of the mesh structure in step (2) is 600 μm, other conditions are the same as those in Example 1.
[0125] Example 10
[0126] This embodiment provides a method for preparing a porous degradable iron-manganese alloy bone scaffold material. Except that the power of the 3D printing in step (3) is 200 W, other conditions are the same as those in Example 1.
[0127] Embodiment 11
[0128] This embodiment provides a method for preparing a porous degradable iron-manganese alloy bone scaffold material. Except that the power of the 3D printing in step (3) is 380 W, other conditions are the same as those in Example 1.
[0129] Example 12
[0130] This embodiment provides a method for preparing a porous degradable iron-manganese alloy bone scaffold material. Except that the heat treatment temperature in step (3) is 650° C., other conditions are the same as those in Example 1.
[0131] Embodiment 13
[0132] This embodiment provides a method for preparing a porous degradable iron-manganese alloy bone scaffold material. Except that the heat treatment temperature in step (3) is 1000° C., other conditions are the same as those in Example 1.
[0133] Embodiment 14
[0134] This embodiment provides a method for preparing a porous degradable iron-manganese alloy bone scaffold material. Except that the cleaning solution in step (3) is pure water, other conditions are the same as those in embodiment 1.
[0135] Comparative Example 1
[0136] This comparative example provides a method for preparing a porous degradable iron-manganese alloy bone scaffold material. Except that step (3) is not subjected to heat treatment, other conditions are the same as those in Example 1.
[0137] The mechanical properties of the iron-manganese alloy bone scaffold materials obtained in the above examples and comparative examples were tested; the elastic modulus and yield strength were measured by tensile tests. The test results are shown in Table 1.
[0138] Table 1
[0139]
[0140]
[0141] From Table 1, we can see that:
[0142] (1) The preparation method provided in Examples 1-3 of the present invention provides an iron-manganese alloy bone scaffold material having a porous structure, good biocompatibility, and a mechanical property that matches the mechanical property of the bone in the intended repair area;
[0143] (2) From the comparison between Example 1 and Examples 4-5, it can be seen that when the Mn content in the raw material is low, the original structure of the printed state in the alloy is γ+ε dual phase, rather than γ austenite, so that the grain size is relatively small, and the yield strength and elastic modulus of the obtained iron-manganese alloy bone scaffold material are relatively high; when the Mn content in the raw material is high, because the original structure of the printed state in the alloy is γ single phase structure and the grain size is large, the yield strength and elastic modulus of the obtained iron-manganese alloy bone scaffold material are relatively low;
[0144] (3) Comprehensively comparing Example 1 with Examples 6-9, it can be seen that when the aperture of the designed mesh structure is smaller or the rod diameter is larger, the porosity of the obtained iron-manganese alloy bone scaffold material is smaller, the ability to resist stress concentration during deformation is higher, the yield strength and elastic modulus are higher, but the elastic modulus is not completely matched with the mechanical properties of the bone in the intended repair area; when the aperture of the designed mesh structure is larger or the rod diameter is smaller, the porosity of the obtained iron-manganese alloy bone scaffold material is larger, the test structure is more prone to stress concentration, the material is more prone to crack propagation during deformation, and the yield strength and elastic modulus are relatively lower;
[0145] (4) By comparing Example 1 with Examples 10-11, it can be seen that when the laser power of 3D printing is low, the powder cannot be completely melted by the laser during the printing process, thereby generating some irregularly shaped unfused defects, resulting in the low yield strength and elastic modulus of the obtained iron-manganese alloy bone scaffold material during the tensile process; when the laser power of 3D printing is high, warping deformation and regular keyhole-type defects are prone to occur during the printing process, resulting in the low yield strength and elastic modulus of the obtained iron-manganese alloy bone scaffold material during the tensile process;
[0146] (5) Comprehensive Example 1 and Example 12-13, Comparative Example 1 show that, since the microstructure of the iron-manganese alloy bone scaffold material under the design composition is mainly γ austenite, no obvious phase change will occur with the increase of the heat treatment temperature, and a small amount of γ→ε transformation will occur, which is mainly the growth of austenite grains and lath martensite. The increase of the heat treatment temperature leads to a decrease in the yield strength and elastic modulus of the material; when the heat treatment temperature is too low, the growth of austenite grains and lath martensite is insufficient, resulting in a high yield strength and elastic modulus of the obtained material, and the elastic modulus is not completely matched with the mechanical properties of the bone in the intended repair area; when no heat treatment is performed, because the microstructure of the material is mainly γ austenite and the grain size is relatively small, the yield strength and elastic modulus of the obtained material are high, and the elastic modulus is not completely matched with the mechanical properties of the bone in the intended repair area;
[0147] (6) A comparison between Example 1 and Example 14 shows that when pure water is used for cleaning, although the yield strength and elastic modulus match the mechanical properties of the bone in the area to be repaired, the surface of the metal bone scaffold is relatively rough and is not suitable for preparing artificial bones.
[0148] The degradation rate test of the iron-manganese alloy bone scaffold material obtained in Examples 1-3 was carried out, specifically: the test solution was prepared by a modified Hanks solution, and its ion composition and concentration were very similar to human plasma. Samples were taken out after 1 week, 1 month and 3 months of degradation, and then characterized. The temperature of the test solution was maintained at 37°C, and its pH value was recorded every 24 hours; wherein, the degradation rates of the iron-manganese alloy bone scaffold materials obtained in Examples 1-3 were 0.24 mm / year, 0.21 mm / year, and 0.20 mm / year, respectively; it can be seen that the preparation method of the iron-manganese alloy bone scaffold material provided by the present invention, by adjusting the porosity and pore structure of the bone scaffold material, combined with the regulation of the preparation process parameters, realizes quantitative control of the degradation rate.
[0149] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a porous degradable iron-manganese alloy bone scaffold material, characterized in that: The preparation method comprises the following steps: (1) subjecting the iron-manganese pre-alloy to electrode induction melting to obtain an iron-manganese pre-alloy powder; (2) designing a mesh structure of a 3D printing model of an iron-manganese alloy bone scaffold material, then performing layered slicing, and importing the layered slicing results into a 3D printing program; The porosity of the mesh structure is 37.89-77.17%; (3) sequentially performing 3D printing, heat treatment and cleaning on the iron-manganese pre-alloyed powder obtained in step (1); There is no particular order in which steps (1) and (2) are performed.
2. The preparation method according to claim 1, characterized in that: In terms of mass percentage, the iron-manganese pre-alloy in step (1) comprises: Mn 28-32%, C<0.05%, Si<0.01%, N<0.01%, O≤0.224%, and the balance is Fe.
3. The preparation method according to claim 1 or 2, characterized in that: The smelting power of the electrode induction smelting in step (1) is 15-25KW; Preferably, the feed rate of the electrode induction melting in step (1) is 40-55 mm / min; Preferably, the gas used in the electrode induction melting in step (1) comprises an inert gas; Preferably, the gas pressure used in the electrode induction smelting in step (1) is 3-5 MPa; Preferably, the nozzle gap in the electrode induction melting in step (1) is 0.3-0.5 mm; Preferably, the average particle size of the iron-manganese pre-alloyed powder in step (1) is 15-53 μm.
4. The preparation method according to any one of claims 1 to 3, characterized in that The pore size of the mesh structure in step (2) is 100-400 μm; Preferably, the rod diameter of the mesh structure in step (2) is 300-500 μm.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The power of the 3D printing in step (3) is 250-320W; Preferably, the scanning speed of the 3D printing in step (3) is 700-1000 mm / s; Preferably, the scanning spacing of the 3D printing in step (3) is 0.1-0.15 mm; Preferably, the scanning layer thickness of the 3D printing in step (3) is 30-50 μm.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The heat treatment in step (3) is carried out under vacuum conditions; Preferably, the temperature of the heat treatment in step (3) is 840-860°C; Preferably, the holding time of the heat treatment in step (3) is 105-135 min.
7. The preparation method according to any one of claims 1 to 6, characterized in that: After the heat treatment in step (3), wire cutting is also included before the cleaning treatment; Preferably, the cleaning solution of the cleaning treatment in step (3) comprises hydrofluoric acid and water; Preferably, the volume ratio of hydrofluoric acid to water is (3-6):(94-97); Preferably, the cleaning time in step (3) is 30-40 seconds; Preferably, the cleaning process in step (3) further includes drying, sterilizing and packaging in sequence; Preferably, the drying temperature is 60-80°C; Preferably, the drying time is 10-30 minutes.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: (1) subjecting the iron-manganese pre-alloy to electrode induction melting to obtain an iron-manganese pre-alloy powder having an average particle size of 15-53 μm; The iron-manganese pre-alloy comprises, in terms of mass percentage, 28-32% Mn, C<0.05%, Si<0.01%, N<0.01%, O≤0.224%, and the balance is Fe; The melting power of the electrode induction melting is 15-25KW, the feed rate is 40-55mm / min, the gas pressure used is 3-5MPa, and the nozzle gap is 0.3-0.5mm; (2) designing a mesh structure of a 3D printing model of an iron-manganese alloy bone scaffold material, then performing layered slicing, and importing the layered slicing results into a 3D printing program; The porosity of the mesh structure is 37.89-77.17%, the pore size is 100-400 μm, and the rod diameter is 300-500 μm; (3) sequentially performing 3D printing, heat treatment, wire cutting and cleaning on the iron-manganese pre-alloyed powder obtained in step (1); The power of the 3D printing is 250-320W, the scanning speed is 700-1000mm / s, the scanning spacing is 0.1-0.15mm, and the scanning layer thickness is 30-50μm; The heat treatment is carried out under vacuum conditions; the heat treatment temperature is 840-860°C, and the insulation time is 105-135min; The cleaning solution of the cleaning treatment comprises hydrofluoric acid and water in a volume ratio of (3-6): (94-97); the cleaning treatment time is 30-40s; The cleaning process also includes drying, sterilization and packaging in sequence; There is no particular order in which steps (1) and (2) are performed.
9. A porous degradable iron-manganese alloy bone scaffold material, characterized in that: The porous degradable iron-manganese alloy bone scaffold material is prepared by the preparation method according to any one of claims 1 to 8; Preferably, the porosity of the porous degradable iron-manganese alloy bone scaffold material is 37.89-77.17%; Preferably, the pore size of the porous degradable iron-manganese alloy bone scaffold material is 100-400 μm; Preferably, the elastic modulus of the porous degradable iron-manganese alloy bone scaffold material is 10.4-14.9 GPa; Preferably, the yield strength of the porous degradable iron-manganese alloy bone scaffold material is 160.7-243.3 MPa.
10. An application of the porous degradable iron-manganese alloy bone scaffold material as claimed in claim 9, characterized in that: The use of the porous degradable iron-manganese alloy bone scaffold material in preparing artificial bones is preferably used in preparing artificial bones in weight-bearing areas.