Preparation method of galvanized strip steel, galvanized strip steel and automobile outer plate
By optimizing the preparation method of galvanized strip steel, including the control of cleaning, annealing and galvanizing process parameters, the problem of frequent furnace defects in the production of galvanized automobile outer plates is solved, the surface quality is improved, and high-level galvanized automobiles are achieved Stable production of outer plates.
Patent Information
- Application Number
- CN202411246883.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-06
AI Technical Summary
In the production of galvanized automobile outer plates, defects such as furnace roller scratches, sunken roller printing, zinc gray zinc slag in the annealing furnace frequently occur, resulting in unstable surface quality of high-level galvanized automobile outer plates.
By optimizing the cleaning process parameters of strip steel, controlling the atmosphere in the annealing furnace, stabilizing the vibration amplitude, liquid level and temperature of the zinc pot roller, ensuring the continuity and quality of the galvanizing process, including using alkaline washing and electrolytic cleaning during the cleaning process. , control the operating speed, furnace pressure and atmosphere composition of the strip steel during annealing, control the vibration and liquid level of the zinc pot roller during galvanizing, and adjust the corresponding parameters during flattening and oiling.
It effectively reduces the frequency of nodules in the furnace, avoids defects such as zinc ash, sunken roll printing, improves the surface quality of galvanized automobile outer plates, and meets high-level quality requirements.
Smart Images

Figure CN119061340A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of steel material preparation, and in particular to a method for preparing galvanized steel strip, galvanized steel strip and automobile outer panel. Background Art
[0002] Automotive sheet is the largest raw material in automobile production, with an average of 600-800kg of automotive sheet used in each passenger car. With the rapid development of my country's automobile industry, the demand for galvanized automotive outer panels has increased year by year, and the demand for high surface quality has continued to increase.
[0003] In order to obtain galvanized automobile outer panels with good surface quality, it is necessary to continuously explore and optimize the process control in the links of strip cleaning, annealing, galvanizing, skin finishing, quality inspection, etc. At present, the basic production process of galvanized automobile sheet production lines at home and abroad is generally the same. The main process includes uncoiling-welding-cleaning-annealing-galvanizing-skin finishing-edge trimming-coiling, which can meet the normal production of ordinary automobile inner panels. However, when producing high-level galvanized automobile outer panels, the current production process frequently causes defects such as furnace roller scratches in the annealing furnace, sinking roller marks in the zinc pot area, zinc ash and zinc slag, which restrict the stable production of high-level galvanized automobile outer panels. Therefore, how to improve the surface quality of galvanized automobile outer panels is a technical problem that needs to be solved urgently. Summary of the invention
[0004] The present application provides a method for preparing a galvanized steel strip, a galvanized steel strip and an automobile outer panel to solve the following technical problem: how to improve the surface quality of a galvanized automobile outer panel.
[0005] In a first aspect, the present application provides a method for preparing a galvanized steel strip, the method comprising:
[0006] Cleaning the steel strip under set parameters to obtain a clean steel strip;
[0007] The cleaned steel strip is annealed, and the following annealing parameters are controlled: the running speed of the steel strip, the furnace pressure in the heating section, the H 2 content, O content in the furnace, and obtain annealed strip steel;
[0008] The annealed steel strip is galvanized, and the following parameters of the galvanization are controlled: the vibration amplitude of the zinc pot roller, the zinc pot liquid level and the zinc pot temperature, to obtain a zinc layer steel strip;
[0009] The zinc layer steel strip is leveled and oiled to obtain a galvanized steel strip.
[0010] Optionally, the step of cleaning the steel strip under set parameters to obtain a clean steel strip includes:
[0011] The strip steel is subjected to alkali washing, electrolytic washing, rinsing and drying to obtain a clean strip steel; wherein the alkali solution concentration of the alkali washing is ≥35 g / L, the electrolyte concentration of the electrolytic washing is ≥45 g / L, and the brush roller currents of the alkali washing and rinsing satisfy the following relationship:
[0012] I 1 >I 2 +a,
[0013] In the formula, I 1 is the brush roller current, I 2 is the memory current, a is 0.5A~3A.
[0014] Optionally, the cleanliness of the clean steel strip meets the requirements of level 1 or above, or the reflectivity value of the clean steel strip is maintained above 93%.
[0015] Optionally, the strip running speed is 90mpm to 130mpm, the furnace pressure in the heating section is 2.0hPa to 4.0hPa, and the H 2 The content is 3.0% to 6.0%, calculated in parts per million, and the O content in the furnace is ≤20ppm.
[0016] Optionally, the vibration amplitude of the zinc pot roller is ≤3.0 mm / s, the zinc pot liquid level is -42 mm to -38 mm, and the zinc pot temperature is 450°C to 460°C.
[0017] Optionally, the galvanizing also includes the following parameters: the dew point of the furnace nose is -10°C to -30°C, the rotation speed of the zinc ash pump of the furnace nose is 110rpm to 190rpm, and the Al content in the zinc liquid of the zinc pot is 0.22% to 0.25% by mass fraction.
[0018] Optionally, the cleaning pressure of the finishing is 80 bar to 150 bar, and the roughness of the finishing roller is 1.6 μm to 2.5 μm.
[0019] Optionally, the oiling includes the following parameters: the heating temperature of the oiler body is 55°C to 75°C, the thermocouple detection temperature at the top of the oiler is >60°C, the heating temperature of the knife beam of the oiler is 65°C to 75°C, and the voltage of the upper and lower knife beams of the oiler is 70kV to 85kV.
[0020] In a second aspect, the present application provides a galvanized steel strip prepared by the method of any one of the embodiments of the first aspect, wherein the galvanized steel strip satisfies at least one of the following properties: the number of black spots on the edge is ≤ 20 / 100 cm 2 , the number of black spots in the middle is ≤15 / 100cm 2 , quality degradation rate ≤5%.
[0021] In a third aspect, the present application provides an automobile outer panel, wherein the automobile outer panel adopts the galvanized steel strip described in the embodiment of the second aspect.
[0022] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0023] The present application provides a method for preparing galvanized steel strip, comprising: cleaning the steel strip under set parameters to obtain clean steel strip; annealing the clean steel strip, and controlling the following parameters of the annealing: the running speed of the steel strip, the furnace pressure in the heating section, the H 2 content, O content in the furnace, to obtain annealed steel strip; galvanize the annealed steel strip, and control the following parameters of the galvanizing: the vibration amplitude of the zinc pot roller, the zinc pot liquid level and the zinc pot temperature, to obtain a zinc layer steel strip; flatten and oil the zinc layer steel strip to obtain a galvanized steel strip. By optimizing the cleaning process parameters, the cleaning quality of the steel strip before annealing is improved, and by strictly controlling the parameters such as the oxygen content and hydrogen content in the furnace, the frequency of nodules in the steel strip in the furnace is reduced; by stabilizing the vibration amplitude of the zinc pot roller, the zinc pot liquid level, temperature and other parameters, the quality effect of surface galvanizing is guaranteed. Thereby improving the surface quality of galvanized automobile outer panels. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0025] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0026] Figure 1 A schematic flow chart of a method for preparing galvanized steel strip provided in an embodiment of the present application. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0028] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0029] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.
[0030] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0031] Based on the existing technology, the present invention mainly improves the cleaning quality, accurately controls the atmosphere in the annealing furnace, and continuously explores new technologies for the galvanizing process. It effectively controls common defects in the galvanizing process, such as furnace roller scratches, sinking roller marks, zinc ash and zinc slag, to meet high-level quality requirements and create favorable conditions for continuous and stable production.
[0032] Figure 1 A schematic flow chart of a method for preparing galvanized steel strip provided in an embodiment of the present application.
[0033] See also Figure 1The present application provides a method for preparing galvanized steel strip, the method comprising:
[0034] S1. Cleaning the steel strip under set parameters to obtain a clean steel strip;
[0035] In some embodiments, the step of cleaning the steel strip under set parameters to obtain a clean steel strip includes:
[0036] The strip steel is subjected to alkali washing, electrolytic washing, rinsing and drying to obtain a clean strip steel; wherein the alkali solution concentration of the alkali washing is ≥35 g / L, the electrolyte concentration of the electrolytic washing is ≥45 g / L, and the brush roller currents of the alkali washing and rinsing satisfy the following relationship:
[0037] I 1 >I 2 +a,
[0038] In the formula, I 1 is the brush roller current, I 2 is the memory current, a is 0.5A~3A.
[0039] In the above embodiment, by controlling the cleaning parameters, it is possible to ensure that the residual oil and iron of the chilled coil steel are effectively removed, improve the cleaning quality, and ensure that the cleanliness meets the requirements of the outer plate. For example, the concentration of the alkali solution for alkali cleaning can be 35g / L, 36g / L, 37g / L, 40g / L, 45g / L, 50g / L, etc., and the concentration of the electrolyte for electrolytic cleaning can be 45g / L, 48g / L, 50g / L, 52g / L, 55g / L, 60g / L, etc.
[0040] In some embodiments, the alkali solution temperature is 65°C to 85°C, the conductivity of the rinse water is <30 μs / cm, the brush roller pressure is ≤100 mm, and the drying temperature of the drying machine is 90°C to 130°C.
[0041] In some embodiments, the cleanliness of the clean steel strip meets the requirements of level 1 or above, or the reflectivity value of the clean steel strip is maintained above 93%.
[0042] S2, annealing the cleaned steel strip, and controlling the following annealing parameters: steel strip running speed, heating section furnace pressure, furnace H 2 content, O content in the furnace, and obtain annealed strip steel;
[0043] In some embodiments, the strip running speed is 90mpm to 130mpm, the furnace pressure in the heating section is 2.0hPa to 4.0hPa, and the H 2 The content is 3.0% to 6.0%, calculated in parts per million, and the O content in the furnace is ≤20ppm.
[0044] In the above embodiment, the speed of the strip steel in the furnace zone is not allowed to be increased or decreased during the production of the outer plate, and the atmosphere in the furnace is kept in a stable control range to avoid quality defects such as nodules and color differences in the strip steel. Thus, the stability of the annealing surface is ensured. For example, the strip steel running speed can be 90mpm, 100mpm, 110mpm, 120mpm, 130mpm, etc., and the furnace pressure in the heating section can be 2.0hPa, 2.5hPa, 3.0hPa, 3.5hPa, 4.0hPa, etc., and the H in the furnace is calculated by mass fraction. 2 The content is 3.0%, 4.0%, 4.5%, 5.0%, 6.0%, etc. In parts per million, the O content in the furnace can be 5ppm, 8ppm, 10ppm, 12ppm, 15ppm, 18ppm, 20ppm, etc.
[0045] S3, galvanizing the annealed steel strip, and controlling the following parameters of the galvanizing: vibration amplitude of the zinc pot roller, zinc pot liquid level and zinc pot temperature, to obtain a zinc layer steel strip;
[0046] In some embodiments, the vibration amplitude of the zinc pot roller is ≤3.0 mm / s, the zinc pot liquid level is -42 mm to -38 mm, and the zinc pot temperature is 450°C to 460°C.
[0047] In the above implementation, the zinc pot needs to be tested for zinc pot roller vibration. The zinc pot three rollers are tested once per shift and completed within 2 hours after each shift. When the vibration value reaches 1.5-3.0 mm / s, the vibration measurement frequency is increased to once every 4 hours. When the vibration value is ≥3.0 mm / s, the outer plate production is stopped.
[0048] In some embodiments, the galvanizing further includes the following parameters: the furnace nose dew point is -10°C to -30°C, the furnace nose zinc ash pump speed is 110rpm to 190rpm, and the Al content in the zinc pot zinc liquid is 0.22% to 0.25% by mass fraction.
[0049] In some embodiments, the galvanizing slag removal requirements are: slag removal can only be performed at the slag removal roll, one slag removal roll is arranged for every five outer plates, and all floating slag on the upper and lower surfaces is cleaned during slag removal. Before slag removal, confirm whether there is an ingot on the DS side, ensure that there is an ingot on the DS side at any time during slag removal, and ensure the stability of the liquid level.
[0050] In some embodiments, the galvanizing slag stripping requirements are as follows: the weld must be stripped, and the stripping distance must be more than 50 cm from the middle of the strip and more than 15 cm from the edge. The stripping direction is to strip the slag towards the four corners of the zinc pot. During the production of the outer plate, the zinc slag on the lower surface is not allowed to be pushed from both sides to the upper surface. Clean the zinc liquid level next to the zinc ash pump and the zinc slag around the level gauge detection point.
[0051] In some embodiments, the galvanizing thickness is within the online fluctuation range of +5g / m 2 , to meet the order requirements, the distance between the upper and lower air knives is 12mm~30mm, and the air knife height is ≤200mm.
[0052] By controlling the process parameters of galvanizing, it is ensured that the zinc pot process is kept within the required range for a long time and stably, and defects such as zinc ash and roller marks of sinking rollers are avoided. For example, the vibration amplitude of the zinc pot roller can be 1.0mm / s, 1.5mm / s, 2.0mm / s, 2.5mm / s, 3.0mm / s, etc., the zinc pot liquid level can be -42mm, -41mm, -40mm, -39mm, -38mm, etc., and the zinc pot temperature can be 450℃, 452℃, 454℃, 456℃, 458℃, 460℃, etc. The dew point of the furnace nose can be -10℃, -15℃, -20℃, -25℃, -30℃, etc. The speed of the zinc ash pump at the furnace nose can be 110rpm, 120rpm, 130rpm, 140rpm, 160rpm, 180rpm, 190rpm, etc. In terms of mass fraction, the Al content in the zinc liquid in the zinc pot is 0.22%, 0.23%, 0.24%, 0.25%, etc.
[0053] S4, leveling and oiling the zinc layer steel strip to obtain galvanized steel strip.
[0054] In some embodiments, the cleaning pressure of the finishing is 80 bar to 150 bar, and the roughness of the finishing roller is 1.6 μm to 2.5 μm.
[0055] In some embodiments, the skin-passing elongation of the leveler is ±0.1% of the planned value. During the production of the outer plate, the maximum tension of the IF steel skin-passing entrance and exit does not exceed 10% of the secondary value, and the operator makes appropriate adjustments according to the plate shape. In case of peeling defects mixed with raw materials, the skin-passing machine should be opened to the middle position in advance, and high-pressure cleaning should be performed to ensure normal operation. When bright spot defects occur during skin-passing, it is forbidden to wash a fixed point or a fixed section of the roller surface for a long time to prevent color difference defects.
[0056] In the above embodiment, by controlling the parameters of flattening, the strip shape is ensured under the premise of meeting the required elongation. For example, the cleaning pressure of the skinning can be 80 bar, 90 bar, 100 bar, 110 bar, 120 bar, 130 bar, 140 bar, 150 bar, etc., and the roughness of the skinning roller can be 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, 2.1 μm, 2.4 μm, 2.5 μm, etc.
[0057] In some embodiments, the oiling includes the following parameters: the heating temperature of the oiler body is 55°C to 75°C, the thermocouple detection temperature at the top of the oiler is >60°C, the heating temperature of the knife beam of the oiler is 65°C to 75°C, and the voltage of the upper and lower knife beams of the oiler is 70kV to 85kV.
[0058] In some embodiments, the oiler is turned on and preheated 5 hours in advance.
[0059] In the above embodiment, the uniformity and adhesion of the oiling are ensured by controlling the process parameters of the oiling. For example, the heating temperature of the oiling machine body can be 55°C, 60°C, 65°C, 70°C, 75°C, etc., the thermocouple detection temperature of the top of the oiling machine can be 61°C, 65°C, 68°C, 70°C, 75°C, etc., the heating temperature of the knife beam of the oiling machine can be 65°C, 67°C, 69°C, 70°C, 72°C, 74°C, 75°C, etc., and the voltage of the upper and lower knife beams of the oiling machine can be 70kV, 72kV, 75kV, 78kV, 82kV, 85kV, etc.
[0060] In some embodiments, the method further comprises: performing quality inspection on the galvanized steel strip. Doing a good job of quality inspection is a guarantee of the quality of the outer plate.
[0061] In some embodiments, during the production of outer plates, the post must use a stroboscope to check the quality of each roll of outer plates in the intermediate quality inspection room, focusing on the defects of sinking roller marks, short-line scratches, and scratches in the furnace. Among them, the sinking roller marks visible by the side light of the lower tower strip are not allowed to exceed 100mm from the edge. If exceeded, the production process must be adjusted in time or the roll must be thrown up and the strip must be pulled up.
[0062] In some embodiments, black spot inspection must be carried out during the production of the outer panel, once for each large roll. Before counting the black spots, the outer panel must be wiped clean with a special wipe cloth. The black spots on both the upper and lower surfaces need to be counted. The number of black spots on the edge is ≤ 20 / 100cm. 2 ; The number of black spots in the middle is ≤ 15 / 100cm 2 .
[0063] In some embodiments, the stamping inspection must be carried out during the production of the outer plate, normally once for every three rolls, and the first roll after the furnace speed increases or decreases and the first roll after the specification of the slag roll changes must be punched. The punching depth is set to 80mm. Judgment criteria: After punching, the convex surface is ground (the concave surface is not ground), and no more than two convex high points caused by zinc slag or zinc ash on the concave surface are allowed (not caused by mold problems).
[0064] In some embodiments, the outer plate must be inspected vertically during production: vertical grinding is performed once every three large rolls. Defects that cannot be confirmed by vertical grinding must be confirmed again by offline grinding of the export sample plate. The first roll after the roll change must be vertically ground, perpendicular to the rolling direction, and the grinding length must be 2m.
[0065] In some embodiments, during the production of the outer plate, it is necessary to arrange to re-roll and produce one roll of random inspection roll, and grind the 50m range at the head of the strip and the middle of the strip at least once to check whether there are periodic defects.
[0066] Based on a general inventive concept, the present application provides a galvanized steel strip prepared by the method of any one of the embodiments of the first aspect, wherein the galvanized steel strip satisfies at least one of the following properties: the number of black spots on the edge is ≤ 20 / 100 cm 2 , the number of black spots in the middle is ≤15 / 100cm 2 , quality degradation rate ≤5%.
[0067] The galvanized steel strip is realized based on the preparation method of the galvanized steel strip mentioned above. The specific steps of the preparation method of the galvanized steel strip can refer to the above embodiment. Since the galvanized steel strip adopts part or all of the technical solutions of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment, which will not be described one by one here.
[0068] Based on a general inventive concept, the present application provides an automobile outer panel, which adopts the galvanized steel strip described in the embodiment of the second aspect.
[0069] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.
[0070] This embodiment provides a method for preparing a galvanized steel strip, the method comprising:
[0071] S11, cleaning the steel strip under set parameters to obtain a clean steel strip;
[0072] S21, annealing the cleaned steel strip, and controlling the following annealing parameters: steel strip running speed, heating section furnace pressure, furnace H 2 content, O content in the furnace, and obtain annealed strip steel;
[0073] S31, galvanizing the annealed steel strip, and controlling the following parameters of the galvanizing: vibration amplitude of the zinc pot roller, zinc pot liquid level and zinc pot temperature, to obtain a zinc layer steel strip;
[0074] S41. Smooth and oil the zinc layer steel strip to obtain galvanized steel strip. Please refer to Tables 1 to 3 for the parameters of the preparation method of the galvanized steel strip.
[0075] Table 1 Parameters of cleaning and annealing processes in the preparation of galvanized steel strip
[0076]
[0077]
[0078] Table 2 Parameters of galvanizing and skin-passing processes in the preparation of galvanized steel strip
[0079]
[0080] Table 3 Parameters of the oiling process in the preparation of galvanized steel strip
[0081]
[0082] It should be noted that in the actual production process, the furnace pressure and H 2 The content, O content in the furnace, zinc pot level, zinc liquid temperature, and zinc pot roller vibration fluctuate within a certain range, rather than specific values. Therefore, the range values in Tables 1 to 3 are the corresponding fluctuation ranges.
[0083] The quality degradation rate of about 1,000 tons of products produced by the processes of the above-mentioned embodiments 1 to 5 and comparative examples 1 to 3 was statistically compared and analyzed. The above-mentioned reasonable method of controlling the process reduced the defect rate, thereby improving the surface quality of the strip steel. The quality degradation rate of comparative examples 1 to 3 was about 10%, and the quality degradation rate was reduced to less than 5% after the method of the present application was applied. The results are shown in Table 4.
[0084] Table 4 Quality degradation rate and number of black spots in high-grade automotive sheet galvanizing production line
[0085]
[0086] In addition, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0087] In the embodiment of the present invention, the cleaning quality of the steel strip before annealing is improved by optimizing the cleaning process parameters, and the frequency of steel strip nodules in the furnace is reduced by strictly controlling the parameters such as the oxygen content and hydrogen content in the furnace; the quality effect of the surface galvanizing is guaranteed by stabilizing the vibration amplitude of the zinc pot roller, the zinc pot liquid level, temperature and other parameters, so as to achieve the ideal surface quality requirements of the automobile outer panel. The number of black spots on the edge of the galvanized steel strip is ≤20 / 100cm 2 , the number of black spots in the middle is ≤15 / 100cm 2 , quality degradation rate ≤5%.
[0088] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for preparing galvanized steel strip, It is characterized in that The method comprises: Cleaning the steel strip under set parameters to obtain a clean steel strip; The cleaned steel strip is annealed, and the following annealing parameters are controlled: the running speed of the steel strip, the furnace pressure in the heating section, the H 2 content, O content in the furnace, and obtain annealed strip steel; The annealed steel strip is galvanized, and the following parameters of the galvanization are controlled: the vibration amplitude of the zinc pot roller, the zinc pot liquid level and the zinc pot temperature, to obtain a zinc layer steel strip; The zinc layer steel strip is leveled and oiled to obtain a galvanized steel strip.
2. The method according to claim 1, It is characterized in that The strip steel is cleaned under set parameters to obtain a clean strip steel, comprising: The strip steel is subjected to alkali washing, electrolytic washing, rinsing and drying to obtain a clean strip steel; wherein the alkali solution concentration of the alkali washing is ≥35 g / L, the electrolyte concentration of the electrolytic washing is ≥45 g / L, and the brush roller currents of the alkali washing and rinsing satisfy the following relationship: I 1 >I 2 +a, In the formula, I 1 is the brush roller current, I 2 is the memory current, a is 0.5A~3A.
3. The method according to claim 2, It is characterized in that The cleanliness of the clean steel strip meets the requirements of level 1 or above, or the reflectivity value of the clean steel strip is maintained above 93%.
4. The method according to claim 1, It is characterized in that The running speed of the strip steel is 90mpm-130mpm, the furnace pressure of the heating section is 2.0hPa-4.0hPa, and the H 2 The content is 3.0% to 6.0%, calculated in parts per million, and the O content in the furnace is ≤20ppm.
5. The method according to claim 1, It is characterized in that The vibration amplitude of the zinc pot roller is ≤3.0mm / s, the zinc pot liquid level is -42mm~﹣38mm, and the zinc pot temperature is 450℃~460℃.
6. The method according to claim 1, It is characterized in that The galvanizing also includes the following parameters: the dew point of the furnace nose is -10°C to -30°C, the rotation speed of the zinc ash pump in the furnace nose is 110rpm to 190rpm, and the Al content in the zinc liquid in the zinc pot is 0.22% to 0.25% by mass fraction.
7. The method according to claim 1, It is characterized in that The cleaning pressure of the finishing is 80 bar to 150 bar, and the roughness of the finishing roller is 1.6 μm to 2.5 μm.
8. The method according to claim 1, It is characterized in that The oiling includes the following parameters: the heating temperature of the oiling machine body is 55℃~75℃, the thermocouple detection temperature of the top of the oiling machine is greater than 60℃, the heating temperature of the knife beam of the oiling machine is 65℃~75℃, and the voltage of the upper and lower knife beams of the oiling machine is 70kV~85kV.
9. A galvanized steel strip prepared by the method according to any one of claims 1 to 8, It is characterized in that The galvanized steel strip meets at least one of the following properties: the number of black spots on the edge is ≤ 20 / 100cm 2 , the number of black spots in the middle is ≤15 / 100cm 2 , quality degradation rate ≤5%.
10. An automobile outer panel, It is characterized in that The automobile outer panel adopts the galvanized steel strip described in claim 9.
Citation Information
Patent Citations
Production method of extra-deep drawing hot-dip galvanized steel for automobile roofs
CN110592492A
High-yield-ratio high-strength galvanized steel sheet and method for manufacturing the same
US20190032187A1
Cited By
Galvanized automobile sheet black spot detection method and related equipment
CN120598886A
A method and related equipment for detecting black spots on galvanized automotive steel sheets