Electroplated part, manufacturing method thereof, functional module and electronic equipment
By using metal nickel and rare earth metal in the plating layer of electroplating parts, combined with suitable electroplating process parameters, the problem of insufficient hardness and corrosion resistance of the existing electroplating black nickel plating layer is solved, and the good brightness and mechanical performance of the plating layer are improved. Improve the reliability of electroplating parts.
Patent Information
- Application Number
- CN202310633292.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
The existing electroplated black nickel coating has poor hardness and corrosion resistance, making it difficult to meet the needs for light absorption and appearance decoration of electronic equipment.
The plating components are metal nickel and rare earth metals. The rare earth metals include neodymium or samarium. The molar ratio of rare earth metal to metal nickel in the plating is 1:5.2-1:38.9. The plating base is copper or copper alloy, and it is formed by electroplating technology. The coating controls the pH value and component concentration of the electroplating solution to ensure uniformity and density of the coating.
It improves the brightness, hardness and corrosion resistance of the plating layer, enhances the reliability of the electroplating parts, and improves the mechanical reliability of functional modules and electronic equipment.
Smart Images

Figure CN119061445A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of electroplating technology, and in particular to an electroplated part and a manufacturing method thereof, a functional module, and an electronic device. Background Art
[0002] Black nickel plating can be used as a coating to cover the surface of some equipment, such as covering the surface of optical equipment or electronic equipment, which can absorb light or solar energy, or decorate the appearance of electronic equipment. At the same time, since black nickel plating has a certain hardness and corrosion resistance, black nickel plating can also provide good protection for the equipment.
[0003] At present, the main process of black nickel electroplating is to add organic or inorganic blackening agents to nickel salts. Common systems include: Ni-Cr type, Ni-Zn type, Ni-Mo type, Ni-Sn type and Ni-Cd type. However, the hardness and corrosion resistance of the black nickel coating produced are still poor. Summary of the invention
[0004] In order to overcome the problems existing in the related art, the present disclosure provides an electroplating part and a manufacturing method thereof, a functional module, and an electronic device.
[0005] According to a first aspect of the present disclosure, an electroplated part is provided, the electroplated part comprising a plated part substrate and a plating layer covering the plated part substrate, the plating layer comprising metal nickel and a rare earth metal.
[0006] In some embodiments of the present disclosure, the rare earth metal includes metal neodymium or samarium.
[0007] In some embodiments of the present disclosure, in the coating, the molar ratio of the rare earth metal to the metallic nickel is 1:5.2-1:38.9.
[0008] In some embodiments of the present disclosure, the plated substrate is a copper substrate or a copper alloy substrate.
[0009] According to a second aspect of the present disclosure, a method for manufacturing an electroplated part is provided. The method for manufacturing an electroplated part is used to manufacture the electroplated part provided in the first aspect of the present disclosure. The method for manufacturing an electroplated part comprises:
[0010] Provides plated substrate and nickel metal;
[0011] Placing an electroplating solution in an electroplating tank, wherein the electroplating solution contains nickel ions and rare earth metal ions;
[0012] The substrate of the plated component is placed in the electroplating solution, with the substrate of the plated component serving as a cathode, the nickel metal is in contact with the electroplating solution, and the nickel metal serves as an anode. The substrate of the plated component is electroplated in the electroplating solution to form a coating on the substrate of the plated component to form the electroplated component, wherein the coating includes metallic nickel and rare earth metals.
[0013] In some embodiments of the present disclosure, the method for manufacturing the electroplated part further includes:
[0014] adding a rare earth salt solution into an initial plating solution to obtain a mixed solution;
[0015] An ammonia solution is added to the mixed solution to adjust the pH value of the mixed solution to a first value range, thereby obtaining the electroplating solution.
[0016] In some embodiments of the present disclosure, the first pH value range of the mixed solution is 2.6-2.8.
[0017] In some embodiments of the present disclosure, the mass volume concentration of each component in the mixed solution is:
[0018] Aminosulfonic acid: 200g / L-350g / L;
[0019] Boric acid: 15g / L-20g / L;
[0020] Phosphorous acid: 10g / L-12g / L;
[0021] Neodymium oxide: 0.5g / L-2.5g / L;
[0022] Nickel compound: 10g / L-30g / L;
[0023] The balance was deionized water.
[0024] In some embodiments of the present disclosure, in a unit volume of the electroplating solution, the molar ratio of neodymium ions to nickel ions is 1:5.2-1:38.9.
[0025] In some embodiments of the present disclosure, the method for manufacturing the electroplated part further includes:
[0026] The aminosulfonic acid, the nickel compound, the boric acid, and the phosphorous acid are added into deionized water according to a preset mass volume concentration to form the initial plating solution.
[0027] In some embodiments of the present disclosure, the method for manufacturing the electroplated part further includes:
[0028] At a preset temperature, adding the neodymium oxide to an aminosulfonic acid solution having a pH value in a second value range to dissolve the neodymium oxide and obtain an initial solution;
[0029] The pH value of the initial dissolving solution is adjusted to a third value range to obtain the rare earth salt solution.
[0030] In some embodiments of the present disclosure, the second value range is 1.5-1.7; and / or,
[0031] The third value range is 2.6-2.8.
[0032] In some embodiments of the present disclosure, the nickel compound includes nickel chloride, nickel sulfate, or nickel sulfamate;
[0033] When the nickel compound is nickel chloride, the mass volume concentration of nickel chloride is 10g / L-15g / L;
[0034] When the nickel compound is nickel sulfate, the mass volume concentration of the nickel sulfate is 11.94 g / L-17.91 g / L;
[0035] When the nickel compound is nickel sulfamate, the mass volume concentration of the nickel sulfamate is 19.36 g / L-29.04 g / L.
[0036] In some embodiments of the present disclosure, the electroplating conditions satisfy at least one of the following:
[0037] The current density is 0.1A / dm 2 -0.9A / dm 2 and / or,
[0038] The plating time is 15 seconds to 180 seconds.
[0039] According to a third aspect of the present disclosure, a functional module is provided, comprising the electroplating part provided in the first aspect of the present disclosure.
[0040] According to a fourth aspect of the present disclosure, an electronic device is provided, comprising the electroplated part provided in the first aspect of the present disclosure.
[0041] The technical solution provided by the embodiments of the present disclosure may include the following beneficial effects: by setting the composition of the plating layer in the electroplated part to rare earth metals and metallic nickel, the plating layer has good brightness, good hardness and corrosion resistance, thereby improving the reliability of the electroplated part, so that the functional modules and electronic devices including the electroplated part have good mechanical reliability.
[0042] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0044] Figure 1 is a schematic cross-sectional view of an electroplated part according to an exemplary embodiment.
[0045] Figure 2 is a schematic diagram of an electroplating part according to an exemplary embodiment.
[0046] Figure 3 is a schematic diagram of an electroplating part according to another exemplary embodiment.
[0047] Figure 4 It is a schematic diagram of an electroplated part shown as a comparative example.
[0048] Figure 5 The present invention is a flow chart of a method for manufacturing an electroplated part according to an exemplary embodiment. DETAILED DESCRIPTION
[0049] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise indicated. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are merely examples of devices and methods consistent with some aspects of the present invention as detailed in the appended claims.
[0050] Black nickel plating can be used as a coating to cover the surface of some equipment, such as covering the surface of optical equipment or electronic equipment, which can absorb light or solar energy, or decorate the appearance of electronic equipment. At the same time, since black nickel plating has a certain hardness and corrosion resistance, black nickel plating can also provide good protection for the equipment.
[0051] At present, the main process of black nickel electroplating is to add organic or inorganic blackening agents to nickel salts. Common systems include: Ni-Cr type, Ni-Zn type, Ni-Mo type, Ni-Sn type and Ni-Cd type. However, the hardness and corrosion resistance of the black nickel coating produced are still poor.
[0052] In order to solve the above technical problems, the present disclosure provides an electroplated part, including a plated part substrate and a plating layer covering the plated part substrate, wherein the plating layer includes metal nickel and rare earth metal. The present disclosure sets the composition of the plating layer in the electroplated part to be rare earth metal and metal nickel, so that the plating layer has good brightness and good hardness and corrosion resistance, thereby improving the reliability of the electroplated part.
[0053] In an exemplary embodiment of the present disclosure, an electroplating part is provided, Figures 1 to 3 As shown, Figure 1 is a schematic cross-sectional view of an electroplating part according to an exemplary embodiment. Figures 2 to 3 is a schematic diagram of an electroplated part according to an exemplary embodiment. The electroplated part 100 includes a plated part base 10 and a plating layer 20 covering the plated part base 10. The plated part base 10 may be a rod-shaped profile, a plate-shaped profile, or a profile of a certain shape pre-designed by a technician formed of a metal material. The plated part base 10 is a substrate covered and protected by the plating layer 20. In some embodiments, the plated part base 10 may be a housing of an electronic device, such as a mobile phone or tablet computer housing made of metal, or a mobile phone or tablet computer middle frame made of metal. In other embodiments, the plated part base 10 may be, for example, a charging terminal on a charging cable of an electronic device. Exemplarily, the metal material forming the plated part base 10 may include metal aluminum, metal copper, aluminum alloy, copper alloy, but is not limited thereto. In some embodiments, the plated part base 10 is a copper base or a copper alloy base.
[0054] The plating layer 20 can partially or completely cover the plated substrate 10, and the components of the plating layer 20 include metallic nickel and rare earth metals, with metallic nickel being the main component of the plating layer 20. When the plated substrate 10 is a copper substrate or a copper alloy substrate, the plating layer 20 can inhibit the diffusion of copper elements from the plated substrate 10 to the outer layer, and can also make the formed electroplated part 100 have a smoother surface, and the porosity of the surface of the electroplated part 100 is low, so as to protect the plated substrate 10. At the same time, the plating layer 20 can prevent the plated substrate 10 from being corroded by acid and reduce the wear on the surface of the plated substrate 10. The plating layer 20 includes rare earth metals, and the rare earth metals can include one or a mixture of two or more rare earths selected from lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, yttrium, and scandium. Reference Figure 2 and Figure 3 As shown in FIG. 1 , when rare earth metal is provided in the plating layer 20, the surface of the electroplated part 100 can have a bright metallic luster, thereby improving the aesthetic appearance of the electroplated part 100. In addition, when rare earth metal is provided in the plating layer 20, the surface of the plating layer 20 can be made uniform and dense, and the plating layer 20 has good hardness and corrosion resistance, which is beneficial to the Figure 2 and Figure 3 The hardness of the electroplated part shown in the figure is tested, and the hardness of the coating on the electroplated part exceeds 700HV. In some embodiments, the rare earth metal in the coating 20 is metal neodymium or samarium. After testing, when the coating 20 includes metal nickel and metal neodymium or metal samarium, the brightening effect, hardness and corrosion resistance of the coating 20 are greatly improved compared with the prior art.
[0055] It should be noted that the rare earth metal in the coating 20 may be not only neodymium or samarium, but also other metals such as lanthanum, cerium or praseodymium. The embodiments of the present disclosure are not limited to the case where the rare earth metal in the coating 20 is neodymium or samarium.
[0056] refer to Figure 4 As shown, Figure 4 A schematic diagram of a comparative electroplated part is shown in FIG. In the electroplated part shown in the comparative example, the substrate of the plated part may be a metal substrate, for example, the substrate of the plated part is a copper substrate, and the coating may include metal nickel and sulfide, wherein the sulfide may be zinc sulfide, wherein zinc sulfide is an inorganic compound with a chemical formula of ZnS and is a white or slightly yellow powder. Visual inspection of the electroplated part shown in the comparative example shows that the coating has poor compactness and uniformity, and the coating does not cover the substrate of the plated part well, and has poor brightness. The hardness of the electroplated part in the comparative example is tested, and the hardness of the coating thereon may be 523HV.
[0057] For example, in the electroplated part provided in the embodiment of the present disclosure, the molar ratio of the rare earth metal to the metal nickel in the plating layer is 1:5.2-1:38.9, that is, the molar ratio of the rare earth metal to the metal nickel in the plating layer can be any ratio from 1:5.2 to 1:38.9, for example, it can be 1:5.2, 1:6, 1:10, 1:18, 1:25, 1:38.9, etc., and the present disclosure does not make an exhaustive list of them. By controlling the molar ratio of the rare earth metal to the metal nickel in the plating layer, the plating layer can be controlled to have good compactness and uniformity, while ensuring that the plating layer has good hardness and corrosion resistance, and ensuring the reliability of the electroplated part.
[0058] It should be emphasized that the molar ratio of rare earth metal to metallic nickel in the coating can be any value in the range of 1:5.2-1:38.9 in addition to 1:5.2, 1:6, 1:10, 1:18, 1:25, 1:38.9, etc. The above description of the molar ratio of rare earth metal to metallic nickel in the coating is only an example and not a limitation. The present disclosure does not specifically limit the molar ratio of rare earth metal to metallic nickel in the coating.
[0059] In an exemplary embodiment, the present disclosure further provides a method for manufacturing an electroplated part, which is used to manufacture the electroplated part provided in the above embodiment of the present disclosure, referring to Figure 5 As shown, Figure 5 1 is a flow chart of a method for manufacturing an electroplated part according to an exemplary embodiment. The method for manufacturing an electroplated part comprises the following steps:
[0060] Step S100, providing a plated substrate and nickel metal;
[0061] Step S200, placing an electroplating solution in an electroplating tank, wherein the electroplating solution contains nickel ions and rare earth metal ions;
[0062] Step S300, placing the substrate of the plated component in the electroplating solution, with the substrate of the plated component as the cathode, the nickel metal in contact with the electroplating solution, the nickel metal as the anode, electroplating the substrate of the plated component in the electroplating solution, forming a coating on the substrate of the plated component to form an electroplated component, wherein the coating includes metallic nickel and rare earth metals.
[0063] In step S100, the nickel metal may be a nickel rod, a nickel block or a nickel plate, and the nickel metal serves as an electroplating anode during electroplating. The plated substrate may be a rod-shaped profile, a plate-shaped profile or a profile of a certain shape pre-designed by a technician formed of a metal material. The plated substrate serves as an electroplating cathode during electroplating, and the plated substrate is a substrate covered and protected by a subsequently formed coating. Exemplarily, the plated substrate may be pre-treated by sandpaper polishing, tap water rinsing, deionized water rinsing, ultrasonic degreasing, hot water cleaning, tap water rinsing, deionized water rinsing, pickling, etc., so as to ensure that the subsequently formed coating can be well deposited on the plated substrate.
[0064] In step S200, the electroplating tank is used to contain the electroplating solution for electroplating. Since the plating layer of the electroplated part includes metal nickel and rare earth metal, the electroplating solution is set to include nickel ions and rare earth metal ions so that the nickel ions and rare earth metal ions are reduced during electroplating to form a plating layer including metal nickel and rare earth metal.
[0065] In step S300, the substrate and nickel metal are placed in the electroplating solution respectively, and the substrate and nickel metal are connected to the two ends of the same wire respectively. The substrate is used as the cathode and the nickel metal is used as the anode. A direct current is passed through the wire to the electroplating solution. At this time, the migration of positive and negative ions occurs in the electroplating solution, and the negative ions move to the anode, that is, the nickel metal, and the positive ions, including hydrogen ions, nickel ions and rare earth metal ions, move to the cathode, that is, the substrate. The negative ions undergo oxidation reaction on the anode, and the positive ions undergo reduction reaction on the cathode. That is to say, the nickel ions and rare earth metal ions are reduced to metal nickel and rare earth metal on the substrate, and are deposited on the substrate to form a uniform, dense coating covering the substrate. The coating includes metal nickel and rare earth metal, and the coating and the substrate form an electroplated part.
[0066] For example, during the electroplating process, the electroplating conditions can be controlled to control the properties of the formed coating, and the electroplating conditions are controlled to satisfy at least one of the following: the current density is 0.1 A / dm 2 -0.9A / dm 2 ; and / or, the electroplating time is 15 seconds to 180 seconds. In some embodiments, the current density of the DC current used in the electroplating is controlled to be 0.1A / dm 2 -0.9A / dm 2 , the current density can be, for example, 0.1A / dm2 , 0.3A / dm 2 , 0.5A / dm 2 , 0.9A / dm 2 In some embodiments, the duration of electroplating is controlled to be 15-180 seconds, and the electroplating time can be, for example, 15 seconds, 30 seconds, 70 seconds, 180 seconds, etc. In some embodiments, by simultaneously controlling the current density and the electroplating time, the plated layer formed on the plated substrate has good uniformity and density.
[0067] In an exemplary embodiment, the method for manufacturing an electroplated part further includes configuring an electroplating solution, and the method for manufacturing the electroplating solution includes:
[0068] Step S101, adding a rare earth salt solution into an initial plating solution to obtain a mixed solution;
[0069] Step S102: adding an ammonia solution to the mixed solution to adjust the pH value of the mixed solution to a first value range to obtain an electroplating solution.
[0070] In step S101, the rare earth salt solution mainly includes rare earth metal ions, and the initial plating solution mainly includes nickel ions and other components that form the plating solution. In order to introduce rare earth metal ions into the subsequently formed plating solution without bringing in other negative ions to form impurities, rare earth oxides are dissolved in acid to form a rare earth salt solution, and the rare earth oxides can be one or a mixture of two or more of lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, yttrium and scandium rare earth oxides. Exemplarily, the rare earth metal ions in the rare earth salt solution can be neodymium ions, and the rare earth oxides that configure the rare earth salt solution can be neodymium oxide. The rare earth salt solution is added to the initial plating solution to obtain a mixed solution including nickel ions and rare earth metal ions.
[0071] In some possible embodiments, the mass volume concentration of each component in the mixed solution is: aminosulfonic acid: 200g / L-350g / L; boric acid: 15g / L-20g / L; phosphorous acid: 10g / L-12g / L; neodymium oxide: 0.5g / L-2.5g / L; nickel compound: 10g / L-30g / L; the balance is deionized water. In the mixed solution, the nickel compound can be a nickel salt, for example, it can be one or a mixture of two or more of nickel aminosulfonate, nickel chloride, and nickel sulfate. The nickel compound is used as the main salt of the subsequently formed electroplating solution to provide the subsequently formed electroplating solution with nickel metal ions required for nickel plating; and it can be used as a conductive salt to move the positive ions and negative ions in the subsequently formed electroplating solution, thereby enhancing the conductivity of the subsequently formed electroplating solution during electroplating; it can also be used as an anode activator to promote the dissolution of the anode, i.e., nickel metal, during the electroplating process to prevent anode passivation.
[0072] It should be noted that the mass volume concentration ratio of each component in the mixed solution can be adjusted according to the type of substrate material and rare earth metal. The above description is based on the substrate material being copper or copper alloy as an example. The mass volume concentration ratio of each component in the mixed solution described above can also be applied to other substrate materials. The disclosed embodiments do not specifically limit the mass volume concentration ratio of each component in the mixed solution, the components in the mixed solution, etc.
[0073] Aminosulfonic acid is used to make the subsequently formed electroplating solution have a lower pH value. When the pH value of the electroplating solution is high, the electroplating ability of the electroplating solution is better and the current efficiency of the cathode is higher. However, if the pH value is too high, the pH value of the electroplating solution near the cathode will rise rapidly due to the continuous precipitation of hydrogen on the cathode, which will easily lead to the precipitation of halogen nickel salts and nickel hydroxide colloid near the cathode, so that the formed coating may be mixed with halogen nickel salts and nickel hydroxide, which will increase the brittleness of the coating; and due to the adsorption of nickel hydroxide colloid, hydrogen bubbles are easily retained on the cathode surface, making the crystals of the coating rough and pinholes appear, thereby affecting the mechanical properties of the coating.
[0074] Boric acid is used as a pH buffer to adjust the pH value of the subsequent electroplating solution, slow down the rise of the pH value of the electroplating solution in the cathode area, and allow the use of a higher current density during electroplating without causing nickel hydroxide colloid to form near the cathode. Boric acid can also increase the degree of cathode polarization, thereby improving the performance of the electroplating solution and reducing the "burning" phenomenon of the electroplating solution at high current density. Boric acid can also improve the mechanical properties of the coating.
[0075] Phosphorous acid can improve the deposition efficiency of the reduced nickel and rare earth metals during electroplating, so that the coating has good uniformity and density. Neodymium oxide mainly provides neodymium metal ions, so that the neodymium metal ions undergo a reduction reaction on the substrate during electroplating, so that the reduced nickel and rare earth metals form a coating.
[0076] In step S102, when the pH value of the electroplating solution is too high, it is easy for the formed coating to be mixed with halogen nickel salts and nickel hydroxide, so that the brittleness of the coating is increased, and the porosity of the formed coating is high; and when the pH value of the electroplating solution is too low, it is easy to reduce the cathode current efficiency during electroplating, affecting the reliability of the formed coating. Therefore, it is necessary to control the pH value of the electroplating solution to be maintained in a suitable range. By adding an appropriate amount of ammonia water to the mixed solution formed in step S101, the pH value of the mixed solution is maintained within a first value range, thereby forming an electroplating solution with a suitable pH value. The first value range can be the target pH value of the electroplating solution pre-set by the technician, for example, it can be between 2.6-2.8. For example, the pH value of the electroplating solution can be 2.6, 2.65, 2.7, 2.74, 2.8 and other values. In some embodiments, the pH value of the electroplating solution can be 2.7. It should be noted that the embodiment of the present disclosure does not specifically limit the value range of the pH of the electroplating solution.
[0077] For example, in a unit volume of the electroplating solution, the molar ratio of neodymium ions to nickel ions is 1:5.2-1:38.9, that is, the molar ratio of neodymium ions to nickel ions in the electroplating solution can be any ratio between 1:5.2 and 1:38.9, for example, it can be 1:5.2, 1:6, 1:10, 1:18, 1:25, 1:38.9, etc., which are not exhaustively listed in the present disclosure. In this way, the molar ratio of rare earth metal to metallic nickel in the coating formed during electroplating is 1:5.2-1:38.9, so that the formed coating has good compactness and uniformity, and improves the hardness and corrosion resistance of the coating.
[0078] In an exemplary embodiment, the method for manufacturing an electroplated part further includes configuring an initial plating solution, and the method for manufacturing the initial plating solution includes:
[0079] Add amino compounds, nickel compounds, and acidic substances into deionized water to form an initial plating solution. For example, the amino compounds may be aminosulfonic acid, and the acidic substances may be boric acid and / or phosphorous acid, etc., that is, aminosulfonic acid, nickel compounds, boric acid, and phosphorous acid are added into deionized water according to a preset mass volume concentration to form an initial plating solution. It should be noted that the content of each component in the initial plating solution can be adjusted according to the substrate material or the type of rare earth metal in the coating, for example, the preset mass volume concentration of each component in the initial plating solution may be aminosulfonic acid: 200g / L-300g / L, boric acid: 15g / L-20g / L, phosphorous acid: 10g / L-12g / L, and nickel compounds: 10g / L-30g / L. In the initial plating solution, the effects of aminosulfonic acid, boric acid, phosphorous acid, and nickel compounds have been fully described in the above embodiments, and will not be repeated here.
[0080] In some possible embodiments, the nickel compound may include one or a mixture of two or more of nickel chloride, nickel sulfate or nickel sulfamate. In some embodiments, when the nickel compound is nickel chloride, the mass volume concentration of nickel chloride may be 10g / L-15g / L, and nickel chloride may simultaneously act as a main salt, a conductive salt and an anode active agent, providing the electroplating solution with nickel metal ions required for nickel plating, and allowing the positive ions and negative ions in the electroplating solution to move, thereby enhancing the conductivity of the electroplating solution during electroplating, and further promoting the dissolution of the anode, i.e., nickel metal, to prevent anode passivation. In other embodiments, when the nickel compound is nickel sulfate, the mass volume concentration of nickel sulfate may be 11.94g / L-17.91g / L, and nickel sulfate, as the main salt and conductive salt of the electroplating solution, provides the electroplating solution with nickel metal ions required for nickel plating, and allows the positive ions and negative ions in the electroplating solution to move, thereby enhancing the conductivity of the electroplating solution during electroplating. In other embodiments, when the nickel compound is nickel sulfamate, the mass volume concentration of nickel sulfamate can be 19.36g / L-29.04g / L. Nickel sulfamate serves as the main salt and conductive salt of the electroplating solution, provides the electroplating solution with nickel metal ions required for nickel plating, and allows the positive ions and negative ions in the electroplating solution to move, thereby enhancing the conductivity of the electroplating solution during electroplating. In addition, the electroplating solution using nickel sulfamate as the main salt has a coating with low internal stress, fast deposition rate, good coverage, high hardness, good gloss, and extremely superior ductility. It should be noted that when the nickel compounds in different embodiments use different nickel salts, the nickel elements in different embodiments have the same amount of substance.
[0081] It should be noted that the type and mass volume concentration of the amino compound can be adjusted according to the substrate material and rare earth metal, etc. The above description of the type and mass volume concentration of the amino compound is only an example and not a limitation.
[0082] In an exemplary embodiment, the method for manufacturing the electroplated part further includes preparing a rare earth solution, and the method for manufacturing the rare earth solution includes:
[0083] Step S1, adding neodymium oxide to an aminosulfonic acid solution having a pH value in a second value range at a preset temperature to dissolve the neodymium oxide and obtain an initial solution;
[0084] Step S2, adjusting the pH value of the initial dissolved solution to a third value range to obtain a rare earth salt solution.
[0085] Since rare earth oxides are easily soluble in acid, and in order to avoid the rare earth salt solution from introducing other acid components into the electroplating solution after mixing with the initial plating solution, a sulfamic acid solution is used to dissolve the rare earth oxides so that the rare earth oxides react with sulfamic acid to generate an initial solution having rare earth metal ions. The pH value of the sulfamic acid solution is controlled within the second value range so that the rare earth oxides are more easily dissolved at a preset temperature. The preset temperature can be room temperature, for example, any temperature between 20-30°C, for example, 25°C. The second value range can be a pH value at which the rare earth oxide is easily dissolved at a preset temperature, which can be between 1.5-1.7, for example, pH values such as 1.5, 1.56, 1.62, 1.7, etc. At a preset temperature, a rare earth oxide such as neodymium oxide is added to a sulfamic acid solution with a pH value of 1.5-1.7, and stirred to dissolve the neodymium oxide to obtain an initial solution.
[0086] For example, since the pH value of the electroplating solution needs to be controlled within the first value range, i.e., 2.6-2.8, by adjusting the pH value of the initial dissolving solution to the third value range, the third value range can be close to the first value range or equal to the first value range, so that the obtained rare earth salt solution reaches or approaches the pH value required by the electroplating solution in advance, thereby improving the accuracy of the subsequent adjustment of the pH value of the mixed solution formed by mixing the rare earth salt solution and the initial plating solution. In some embodiments, the third value range is equal to the first value range, i.e., the third value range is between 2.6-2.8.
[0087] In the electroplated parts and the manufacturing method thereof provided by the present disclosure, by setting the composition of the coating in the plated electroplated parts to rare earth metals and metallic nickel, and by controlling the manufacturing process of the electroplated parts, such as the selection of each component in the electroplating solution, the concentration ratio of each component, the current density, the electroplating time and other parameters, the coating obtained by electroplating has good brightness, good hardness and good corrosion resistance, thereby improving the reliability of the electroplated parts.
[0088] In an exemplary embodiment, the present disclosure further provides a functional module, which may be, for example, a connector, a battery or other electrical components, etc. The functional module includes the electroplated parts provided in the above embodiments of the present disclosure, and the electroplated parts may be used as terminals in the connector, or one or more parts of the functional module may be electroplated so that the functional module includes the electroplated parts. Exemplarily, the connector is a coupling device that connects electrical terminals to form a circuit, and the connector may include, for example, but is not limited to, PCB (printed circuit board) connectors, plug-in I / O connectors, circuit connectors, and other types. Since the functional module includes the electroplated parts, the functional module has good mechanical reliability.
[0089] It should be noted that the above functional modules can be understood as modules including the electroplated parts as described above. The functional modules can be connectors, batteries or circuit board modules, etc. The present disclosure does not specifically limit the types of functional modules.
[0090] In an exemplary embodiment, the present disclosure further provides an electronic device, which may be a mobile phone, a computer, a tablet computer, a smart watch, and other devices. The electronic device may include the electroplated parts provided by the above-mentioned embodiments of the present disclosure. For example, the electroplated parts may be a metal back shell or a metal middle frame of the electronic device. The metal back shell or the metal middle frame has good hardness and corrosion resistance, so that the housing of the electronic device has good mechanical properties and improves the service life of the electronic device. For another example, the electroplated parts may be electrical connectors such as wiring terminals for internal circuits of electronic devices. The wiring terminals have good corrosion resistance and reliability, so that the electronic device has good electrical connectivity. The present disclosure does not limit the types of electroplated parts in electronic devices.
[0091] It can be understood that the electronic device described above may include the electroplated parts described above, which may be electrical connectors, metal decorative parts, metal back shells or metal middle frames, etc. In addition, it may also include the functional modules described above, such as: battery modules, connectors, etc.
[0092] Those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and practicing the invention disclosed herein. This application is intended to cover any variations, uses or adaptations of the present invention that follow the general principles of the present invention and include common knowledge or customary techniques in the art that are not disclosed in this disclosure. The specification and examples are to be considered exemplary only, and the true scope and spirit of the present invention are indicated by the following claims.
[0093] It should be understood that the present invention is not limited to the exact construction that has been described above and shown in the drawings and that various modifications and changes may be made without departing from the scope thereof. The scope of the present invention is limited only by the appended claims.
Claims
1. An electroplated part, characterized in that: The electroplating part comprises a plating part base and a plating layer covering the plating part base, wherein the plating layer comprises metal nickel and rare earth metal.
2. The electroplated part according to claim 1, characterized in that: The rare earth metal includes metal neodymium or samarium.
3. The electroplated part according to claim 1 or 2, characterized in that: In the coating, the molar ratio of the rare earth metal to the metal nickel is 1:5.2-1:38.
9.
4. The electroplated part according to claim 1, characterized in that: The plated substrate is a copper substrate or a copper alloy substrate.
5. A method for manufacturing an electroplated part, characterized in that: The method for manufacturing the electroplated part is used to manufacture the electroplated part according to any one of claims 1 to 4, and the method for manufacturing the electroplated part comprises: Provides plated substrate and nickel metal; Placing an electroplating solution in an electroplating tank, wherein the electroplating solution contains nickel ions and rare earth metal ions; The substrate of the plated component is placed in the electroplating solution, with the substrate of the plated component serving as a cathode, the nickel metal is in contact with the electroplating solution, and the nickel metal serves as an anode. The substrate of the plated component is electroplated in the electroplating solution to form a coating on the substrate of the plated component to form the electroplated component, wherein the coating includes metallic nickel and rare earth metals.
6. The method for manufacturing an electroplated part according to claim 5, characterized in that: The method for manufacturing the electroplated part further includes: adding a rare earth salt solution into an initial plating solution to obtain a mixed solution; An ammonia solution is added to the mixed solution to adjust the pH value of the mixed solution to a first value range, thereby obtaining the electroplating solution.
7. The method for manufacturing an electroplated part according to claim 6, characterized in that: The first pH value range of the mixed solution is 2.6-2.
8.
8. The method for manufacturing an electroplated part according to claim 6, characterized in that: The mass volume concentration of each component in the mixed solution is: Aminosulfonic acid: 200g / L-350g / L; Boric acid: 15g / L-20g / L; Phosphorous acid: 10g / L-12g / L; Neodymium oxide: 0.5g / L-2.5g / L; Nickel compound: 10g / L-30g / L; The balance was deionized water.
9. The method for manufacturing an electroplated part according to claim 5, characterized in that: In a unit volume of the electroplating solution, the molar ratio of neodymium ions to nickel ions is 1:5.2-1:38.
9.
10. The method for manufacturing an electroplated part according to claim 8, characterized in that: The method for manufacturing the electroplated part further includes: The aminosulfonic acid, the nickel compound, the boric acid, and the phosphorous acid are added into deionized water according to a preset mass volume concentration to form the initial plating solution.
11. The method for manufacturing an electroplated part according to claim 8, characterized in that: The method for manufacturing the electroplated part further includes: At a preset temperature, adding the neodymium oxide to an aminosulfonic acid solution having a pH value in a second value range to dissolve the neodymium oxide and obtain an initial solution; The pH value of the initial dissolving solution is adjusted to a third value range to obtain the rare earth salt solution.
12. The method for manufacturing an electroplated part according to claim 11, characterized in that: The second value range is 1.5-1.7; and / or, The third value range is 2.6-2.
8.
13. The method for manufacturing an electroplated part according to any one of claims 8 to 12, characterized in that: The nickel compound includes nickel chloride, nickel sulfate or nickel sulfamate; When the nickel compound is nickel chloride, the mass volume concentration of nickel chloride is 10g / L-15g / L; When the nickel compound is nickel sulfate, the mass volume concentration of the nickel sulfate is 11.94 g / L-17.91 g / L; When the nickel compound is nickel sulfamate, the mass volume concentration of the nickel sulfamate is 19.36 g / L-29.04 g / L.
14. The method for manufacturing an electroplated part according to claim 5, characterized in that: The electroplating conditions satisfy at least one of the following: The current density is 0.1A / dm 2 -0.9A / dm 2 and / or, The plating time is 15 seconds to 180 seconds.
15. A functional module, characterized in that: Comprising the electroplated part according to any one of claims 1 to 4.
16. An electronic device, characterized in that: Comprising the electroplated part according to any one of claims 1 to 4.