Experimental method for exploring influence of HPAM on heat exchange surface scaling problem

By preparing simulated production liquid and simulated geothermal fluid scaling process, calculating the average scaling rate and analyzing cloud point temperature, the problem of evaluating the impact of HPAM on heat exchange surface scaling in the prior art is solved, and the operation of the heat exchanger is realized Effective guidance on efficiency and safety.

CN119064404APending Publication Date: 2024-12-03CHINA PETROCHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310653590.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The prior art lacks experimental methods to accurately explore HPAM on the scaling problem of heat exchange surfaces, and it is difficult to effectively evaluate its impact on heat exchange efficiency.

Method used

An experimental method is adopted, including preparing simulated extracted liquid, simulating the scaling process of geothermal fluids, calculating the average scaling rate, repeating the test, intuitively processing the data, and determining the cloud point temperature of the test solution, analyzing the turbidification temperature of the simulated solution to the junction The effect of dirt.

Benefits of technology

This method can perfectly consider the combined effect of temperature and HPAM concentration on scale, explore the influence of heat exchange surface temperature, HPAM concentration, hydrolysis, surface roughness and material on scale rate, and provide guidance on application of polymer heat exchange tubes , improve the operating efficiency and safety of the heat exchanger.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119064404A_ABST
    Figure CN119064404A_ABST
Patent Text Reader

Abstract

The invention provides an experimental method for exploring the influence of HPAM on the scaling problem of a heat exchange surface. The experimental method for exploring the influence of HPAM on the scaling problem of the heat exchange surface comprises the steps that 1, simulated produced liquid is prepared; step 2, simulating a geothermal fluid scaling process; 3, the average scaling rate under a certain temperature condition is calculated; 4, repeatedly testing each temperature condition, namely repeatedly testing the step 3; step 5, performing visualized processing on test data; and 6, determining the cloud point temperature of the test solution, and analyzing the influence of the turbidity temperature of the simulation solution on scaling. The experimental method for exploring the influence of the HPAM on the scaling problem of the heat exchange surface relates to a process measure for corrosion prevention and structure prevention of oilfield sewage, can explore the scaling condition of a heat exchange tube within a certain condition temperature and polymer (HPAM) concentration range, and can provide application guidance for the polymer heat exchange tube on site.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oilfield waste heat utilization, and in particular to an experimental method for exploring the influence of HPAM on scaling of heat exchange surfaces. Background Art

[0002] Heat exchangers are devices for heat exchange and are also the core equipment for industrial thermal energy utilization. Their heat exchange efficiency directly determines the upper limit of industrial thermal energy utilization efficiency. The negative impact of fouling on heat transfer surfaces has attracted widespread attention from researchers. With the application of polymer enhanced oil recovery technology in the field of reservoir development, some scholars have found that the fouling deposited on the heat exchange surface under the influence of polymers is significantly different from mineral fouling, and is more stubborn and difficult to remove.

[0003] There are various experimental research methods for scaling problems, including DSL method, dynamic experimental method and static experimental method, but there is currently a lack of experimental methods to accurately explore the effects of various HPAM parameters on scaling.

[0004] In the Chinese patent application with application number: CN201911330702.5, a crude oil heat exchanger high-temperature fouling indoor experimental device is involved, which belongs to the field of oil and gas storage and transportation engineering technology. It includes a high-temperature medium circulation system, a fouling simulation system, a cooling system and a data measurement and processing system; the high-temperature medium in the high-temperature medium circulation system circulates inside the fouling pipe, the fouling pipe is immersed in crude oil, and the temperature of the crude oil is adjusted by the cooling system to simulate the actual environment; by setting a temperature measuring device at a predetermined position, the measured temperature data is sent to the processor for processing, and the change of the heat transfer properties of the high-temperature medium with the extension of the heating time is observed, and the fouling rate is measured, so as to judge the fouling trend, fouling speed and influencing factors of a crude oil under specific working conditions, provide a theoretical basis for research, and provide a reference for actual production operation. If necessary, corresponding measures can be taken in a targeted manner to reduce or prevent the fouling of the crude oil heat exchanger and ensure the safe and efficient operation of the heat exchanger.

[0005] In the Chinese patent application with application number: CN202210029974.7, an experimental device for studying scaling behavior is involved. The experimental device includes a water storage tank, a first loop, a second loop and a third loop. The first loop connects the inlet and outlet of the water storage tank, and the first loop includes a first back pressure valve and a first flow meter; the second loop includes a heat exchanger, a condenser, a second back pressure valve and a second flow meter. The condenser is connected to the heat exchanger. The second back pressure valve and the second flow meter are arranged in the pipeline between the condenser and the inlet of the water storage tank, and the heat exchanger is connected to the outlet of the water storage tank; the third loop includes an autoclave, a preheater and a circulation component. The outlet of the autoclave is connected to the heat exchanger, the inlet of the autoclave is connected to the preheater, and the preheater is connected to the heat exchanger; a sample is arranged in the circulation component, and the circulation component is arranged at the outlet of the autoclave. According to the change of flow rate in the first loop and the second loop, the change of the residual area of ​​the micropores of the sample can be inferred, and the relationship between the flow rate and the residual area of ​​the micropores can be obtained. The invention can be widely used in the field of high temperature and high pressure water experimental technology.

[0006] In the Chinese patent application with application number: CN201921870656.3, a fouling thermal resistance test system for a shell-and-tube heat exchanger is involved, comprising a shell-and-tube heat exchanger (1), wherein an electric heating rod (2) arranged along its length is inserted into the shell-and-tube heat exchanger (1), and the inlet of the shell-and-tube heat exchanger (1) is connected to a solution tank (6) for providing an aqueous solution containing scaling substances through a test water pipe (5) with a flow meter group (3) and a water supply pump (4); a plurality of thermocouples (7) for measuring temperature are distributed on the shell-and-tube heat exchanger (1), and the temperature measured in real time by the thermocouples (7) is collected by a data collector (8), and the data collector (8) is connected to a computer (9) through a line. The test system of the utility model uses a prepared aqueous solution containing scaling substances to form scale on the outer wall surface of the inner tube of the shell-and-tube heat exchanger, and can measure the wall temperature and water temperature after two-phase flow deposition with a scale concentration range of 200-1300 mg / L, so as to achieve the purpose of monitoring the thermal resistance value of the scale.

[0007] In the Chinese patent application with application number: CN201922103996.X, a laboratory simulation scaling device is involved; it includes a heater, a heat exchanger, and a cooler. A radiator and a buffer tube are provided between the heat exchanger and the cooler. The heater increases the temperature of the heating medium. The cooler contains a cooling medium responsible for lowering the temperature of the heating medium. The heating medium and the cooling medium exchange heat in the heat exchanger. The radiator is responsible for lowering the temperature of the heated cooling medium. The buffer tube is used to adjust the flow rate of the cooling medium entering the heat exchanger. Since the solubility of most substances decreases with increasing temperature, a large amount of scaling substances will be produced in the heat exchanger. The heat exchanger made of a curved transparent material makes it easy to judge the effect of chemical antiscalants and electronic descaling devices on the descaling and prevention of scaling of the system by changes in the transparency of the heat exchange surface. The whole set of equipment can judge the descaling and prevention effect simply, quickly and intuitively.

[0008] The above existing technologies are significantly different from the present invention and fail to solve the technical problem we want to solve. Therefore, we invented a new experimental method for exploring the effect of HPAM on scaling of heat exchange surfaces. Summary of the invention

[0009] The object of the present invention is to provide an experimental method for exploring the scaling of heat exchange tubes under certain temperature conditions and polymer (HPAM) concentration ranges, and for exploring the influence of HPAM on the scaling problem of heat exchange surfaces.

[0010] The purpose of the present invention can be achieved by the following technical measures: an experimental method for exploring the effect of HPAM on the scaling problem of heat exchange surfaces, the experimental method for exploring the effect of HPAM on the scaling problem of heat exchange surfaces comprises:

[0011] Step 1, preparing simulated produced fluid;

[0012] Step 2, simulating the scaling process of geothermal fluid;

[0013] Step 3, calculating the average scaling rate under certain temperature conditions;

[0014] Step 4, repeat the test for each temperature condition, i.e. repeat the test step 3;

[0015] Step 5, visualizing the test data;

[0016] Step 6, determine the turbidity point temperature of the test solution and analyze the effect of the turbidity temperature of the simulated solution on scaling.

[0017] The purpose of the present invention can also be achieved by the following technical measures:

[0018] Step 1 includes:

[0019] Step 11, taking a certain amount of deionized water, boiling it, and then cooling it to room temperature to remove dissolved gas in the deionized water, and ultrasonically cleaning it for 10 minutes to further degas;

[0020] Step 12, slowly adding HPAM particles to degassed deionized water and continuously stirring until the solution is clear and no lumps remain, to obtain an HPAM mother solution;

[0021] Step 13, prepare sodium chloride, calcium chloride and sodium bicarbonate solutions respectively, transfer them into the prepared HPAM mother solution in sequence, and adjust the volume to the target capacity.

[0022] In step 2, different test temperatures are set to simulate the scaling process of geothermal fluids, and the time required for heating under different conditions is recorded.

[0023] Step 2 includes:

[0024] Step 21, preheating the test environment, heating the simulated solution according to the test condition requirements, and recording the time required for heating;

[0025] Step 22, when the solution reaches the preset target temperature, stop timing and record the heating time t1;

[0026] Step 23, suspend the heating process and allow the dirt on the surface of the heating tube to dry naturally in the air;

[0027] Step 24, test different heating rates and record the time required for heating, repeat steps 22 and 23 to obtain t2, t3, t4, t5 and t6.

[0028] In step 3, the reaction is terminated, the mass difference before and after the simulated scaling test is weighed and recorded, and the average scaling rate under certain temperature conditions is calculated according to the scaling rate formula to describe the change in heating time caused by the scaling test pipe section to describe the increase in heat transfer thermal resistance caused by scaling.

[0029] In step 5, the scaling rate formula is:

[0030]

[0031] Where M 1 is the mass of the short heating tube before scaling test, M 2 is the mass of the heating tube with dirt attached after the test, t i It is the time required to reach the preset experimental temperature at different heating rates.

[0032] In step 5, the average heat absorption Q of the solution during the heating process is solved using the known heating range and the experimentally measured heating time, and the change of Q with the experimental rounds is used to characterize the effect of fouling on the surface heat transfer characteristics.

[0033] In step 5, the average heat absorption is calculated as:

[0034]

[0035] Where c p is the specific heat capacity of water at constant pressure, ρ is the density of water, V is the volume of water, ΔT is the temperature difference of deionized water before and after heating, and t is the reaction time.

[0036] In step 6, the change of the light transmittance of the solution under different conditions with the temperature is tested. Based on the light transmittance of the solution, the turbidity point temperature of the test solution can be determined, and the effect of the turbidity temperature of the simulated solution on scaling can be further analyzed.

[0037] Step 6 includes:

[0038] Step 61, turn on the spectrophotometer, adjust the wavelength of the light source to 500nm, adjust the spectrophotometer to percentage mode, and preheat for 30 minutes;

[0039] Step 62, take a cuvette, fill it with deionized water at room temperature, measure the light transmittance under the light source of this wavelength, and calibrate it as 100%;

[0040] Step 63, placing the simulated solutions at different temperature nodes in a cuvette to measure the variation characteristics of the spectral signal with temperature.

[0041] The experimental method used in the present invention to explore the effect of HPAM on the scaling problem of the heat exchange surface has relatively comprehensive considerations of the combined effect of temperature and HPAM polymer concentration on scaling and the effect of the solution turbidity temperature on scaling, and based on field applications, the actual operation is slow in scaling and the heat exchange is intermittent. Based on this experimental method, the effects of heat exchange surface temperature, HPAM concentration, HPAM hydrolysis degree, surface roughness, HPAM polymerization degree and heat exchange tube surface material on HPAM changing the scaling rate and the effect of fouling under HPAM changing the surface heat transfer efficiency can be explored.

[0042] The present invention relates to a process measure for preventing oilfield sewage from corrosion and structure, which can explore the scaling of heat exchange tubes within a certain temperature condition and polymer (HPAM) concentration range, and provide application guidance for polymer heat exchange tubes on site. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a diagram of the experimental system for the effect of temperature-concentration on scaling of the present invention;

[0044] Figure 2 This is a system diagram of the experiment on the effect of the solution turbidity temperature on scaling of the present invention;

[0045] Figure 3 A flowchart of a specific embodiment of an experimental method for exploring the effect of HPAM on scaling of heat exchange surfaces according to the present invention;

[0046] In the figure, 1. constant temperature oil bath; 2. closed cover plate; 3. heat exchange tube; 4. simulated liquid; 5. thermocouple A; 6. thermocouple B; 7. thermocouple C; 8. temperature recorder. DETAILED DESCRIPTION

[0047] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0048] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations and / or combinations thereof.

[0049] The experimental method for exploring the influence of HPAM on the scaling problem of heat exchange surface of the present invention prepares simulated produced fluid with characteristics similar to those of real produced fluid for simulation use, prepares heat exchange medium of different temperatures through a circulating heater, and connects a temperature recorder to the fixed thermocouple to the inlet and outlet of the simulated heat exchange pipe section and the simulated produced fluid. After fully testing the influence of different temperatures, simulated produced fluids of different concentrations are replaced to test the influence of concentration.

[0050] In the temperature-concentration experiment module, the problem that most people in the experiment choose to increase the inorganic salt ion concentration of the solution to accelerate scaling due to slow scaling, which deviates from the actual operation process, is taken into consideration. Multiple experiments and horizontal and vertical comparisons are conducted on each operating condition to obtain more valid data without deviating from the data of the actual production operation process.

[0051] Taking into account the intermittent problem in the actual operation of the heat exchanger, the heat exchange tubes were dried in different experimental rounds under the same operating conditions, and the scaled metal tubes in each round were supplemented with weighing analysis and heat transfer characteristics analysis. The inorganic salt scale deposition caused by the evaporation of high-temperature fluid on the heat exchange surface during shutdown was reproduced, thereby providing a more accurate description of the entire heat exchange tube scaling process and the change process of surface heat transfer efficiency.

[0052] HPAM heat exchange scaling experiment module uses a spectrometer to adjust the wavelength of the light source, irradiates the prepared simulated produced liquid, and measures and calibrates the transmittance through a cuvette. The simulated produced liquid with a solution and a thermocouple is sealed in a cuvette, placed in a blast drying oven and heated to different temperatures, taken out and placed in a spectrophotometer, and the characteristics of the produced liquid transmittance changing with temperature are recorded, and the produced liquid turbidity point temperature under different parameters is calibrated. The temperature-concentration influence experiment module is then used to determine the influence of the upper and lower ranges of the turbidity point temperature on the scaling of the heat exchange surface.

[0053] like Figure 3 As shown, Figure 3 The flowchart of the experimental method for exploring the effect of HPAM on the scaling problem of heat exchange surface of the present invention comprises:

[0054] (101) preparing simulated produced fluid;

[0055] (102) Setting different test temperatures to simulate the scaling process of geothermal fluids and recording the time required for temperature rise under different conditions;

[0056] (103) The reaction was terminated, and the mass difference before and after the simulated scaling test was weighed and recorded. The average scaling rate under different temperature conditions was calculated according to the scaling rate formula to describe the change in heating time caused by the scaling test pipe section to describe the increase in heat transfer resistance caused by scaling;

[0057] (104) Repeat the test for each temperature condition, i.e., repeat the test step (103);

[0058] (105) The experimental data are processed visually: the average heat absorption Q of the solution during the heating process is solved using the known heating range and the experimentally measured heating time. The change of Q with the experimental rounds is used to characterize the effect of fouling on the surface heat transfer characteristics.

[0059] (106) The changes in the transmittance of solutions under different conditions with temperature were tested. Based on the transmittance of the solution, the turbidity point temperature of the test solution can be determined, and the effect of the turbidity temperature of the simulated solution on scaling can be further analyzed.

[0060] Specifically, the step (101) includes:

[0061] (11) Take a certain amount of deionized water, boil it, and then cool it to room temperature to remove dissolved gas in the deionized water. Ultrasonic cleaning is then performed for 10 minutes to further degas the water.

[0062] (12) HPAM particles were slowly added to degassed deionized water with continuous stirring until the solution became clear and free of lumps to obtain HPAM mother solution.

[0063] (13) Sodium chloride, calcium chloride, and sodium bicarbonate solutions were prepared separately, and transferred into the prepared HPAM mother solution in sequence, and the volume was adjusted to the target capacity.

[0064] Specifically, the step (102) includes:

[0065] (21) Preheat the test environment, heat the simulated solution according to the test conditions, and record the heating time

[0066] (22) When the solution reaches the preset target temperature (45°C), stop timing and record the heating time t1.

[0067] (23) Pause the heating process and allow the dirt on the surface of the heating tube to dry naturally in the air.

[0068] (24) Experiment with different heating rates and record the time required for heating. Repeat steps (22) and (23) to obtain t2, t3, t4, t5 and t6.

[0069] Specifically, the step (106) includes:

[0070] (61) Turn on the spectrophotometer, adjust the wavelength of the light source to 500 nm, set the spectrophotometer to percentage mode, and preheat for 30 minutes.

[0071] (62) Take a cuvette, fill it with deionized water at room temperature, measure the transmittance under the light source of this wavelength, and calibrate it as 100%

[0072] (63) The simulated solutions at different temperature nodes were placed in a cuvette, and the variation characteristics of the spectral signal with temperature were measured.

[0073] The following are several specific embodiments of the present invention.

[0074] Example 1

[0075] In a specific embodiment 1 of the application of the present invention, the present invention is divided into a temperature-concentration influence experimental system: "temperature control system + simulation system + temperature recording system" and a solution turbidity intervention scaling experimental system: "light source system + temperature recording system + air drying system + camera system".

[0076] 1. Temperature-concentration effect experiment module

[0077] The temperature-concentration experimental system is mainly composed of a temperature control system, a simulation system and a temperature recording system. The main body of the temperature control system is a circulation heater. After the hot glycerin is heated to a predetermined temperature in the heater, it is pumped out by the heater. The pumped hot glycerin flows through the test pipe section through the insulated silicone tube and finally returns to the circulation heater. The simulation system consists of a fixture, a test pipe section and a solution container. The fixture enables the test tube to be fixed in a certain position, and the depth of immersion in the test liquid is maintained constant; the test pipe section heated to a certain temperature by hot glycerin is immersed in the test liquid to simulate the scaling process of the heat exchanger; the temperature recording system consists of a thermocouple and a temperature recorder. Three groups of thermocouples A, B and C monitor the solution temperature, the test tube inlet temperature and the test tube outlet temperature respectively. The temperature recorder records the readings of the three groups of thermocouples in real time with a time step of 1 second, thereby realizing the monitoring of the entire simulation process. The specific connection method is as follows: Figure 1 shown.

[0078] Experimental steps:

[0079] 1. Test tube preparation

[0080] a) Use tweezers to pick up cotton wool dipped in petroleum ether with a boiling range of 60-90°C and carefully clean the test tube to remove the oil stains on the surface of the test tube.

[0081] b) Immerse the test tube in a beaker filled with deionized water and clean the beaker in an ultrasonic cleaner for 10 minutes.

[0082] c) Take out the test tube, use anhydrous ethanol to remove moisture from the surface of the test tube, and transfer the test tube to a forced air drying oven for 30 minutes.

[0083] d) Take out the test tube, cool it naturally to room temperature, and weigh it on an analytical balance for at least 5 consecutive times. After removing the bad spots, calculate the average value of the remaining data as the initial mass M1 of the test tube.

[0084] 2. Solution Preparation

[0085] a) Take a certain amount of deionized water, boil it, and then cool it to room temperature to remove dissolved gas in the deionized water. Put the deionized water and cool it into a beaker, and then place the beaker in an ultrasonic cleaner and perform ultrasonic cleaning for 10 minutes to further degas.

[0086] b) Place a beaker containing degassed deionized water on a magnetic stirrer, continue stirring and slowly add HPAM particles, then seal the beaker and stir for at least 12 hours until the solution is clear and no lumps remain.

[0087] c) Prepare sodium chloride, calcium chloride and sodium bicarbonate solutions in small beakers respectively, transfer the solutions into the prepared HPAM mother solution, rinse the beaker with degassed deionized water, and dilute to the target capacity.

[0088] d) Stir the solution until it is evenly mixed, take 300 mL of the solution and place it in a small beaker, seal the beaker mouth and heat it to the initial temperature (20°C). The experiment was carried out in a constant temperature (20°C) laboratory.

[0089] 3. Pre-treatment

[0090] a) Insert the test tube into the fixture, then connect it to the inlet and outlet pipes of the circulation heater and secure it with cable ties.

[0091] b) Start the circulation heater and repeatedly adjust the temperature of the hot fluid in the circulation heater until the reading of thermocouple B responsible for monitoring the temperature of the hot fluid at the inlet of the test tube is exactly the preset surface temperature. Preheat the test tube at this temperature for 10 minutes.

[0092] 4. Testing

[0093] a) Insert the thermocouple into the fixture, then cover the fixture on the small beaker containing the simulated produced liquid, turn on the temperature recorder, and collect the solution temperature change data at a certain time step.

[0094] b) When the thermocouple reading in the solution reaches the preset target temperature (45°C), stop timing and record the heating time t1.

[0095] c) Remove the fixture, suspend temperature recording, and allow the dirt on the surface of the heating tube to dry naturally in the air.

[0096] d) Replace a set of small beakers and simulated liquid, repeat steps 4-b and 4-c, and obtain t2, t3, t4, t5 and t6.

[0097] 5. Post-processing and data processing

[0098] a) Remove the heating tube from the fixture, pour out the residual hot glycerin in the tube, clean the surface dirt and rinse the residual glycerin in the tube with distilled water, and then put the test tube into a drying oven to dry.

[0099] b) Take out the dried heating tube, cool it to room temperature, and then place it on a precision analytical balance and weigh it continuously for at least 5 times. After removing the bad spots, take the average value as the final mass M2.

[0100] c) The average fouling rate of this experiment is calculated according to the formula. In addition, the heating time of each experiment is also collected to describe the impact of fouling on the heat transfer effect.

[0101] This experimental method strictly controls the heating temperature range under different working conditions, and describes the increase in heat transfer resistance caused by fouling by comparing the change in heating time of the scaled test pipe section under different working conditions. On this basis, some intuitive improvements are made to the display of data: the average heat absorption Q of the solution during the heating process is solved by using the known heating range and the heating time measured in the experiment, and the change of Q with the experimental rounds is used to characterize the effect of fouling on the surface heat transfer characteristics. The improved method can not only intuitively describe the effect of fouling on the surface heat transfer characteristics, but also meet the needs of heat exchangers in actual production.

[0102] The scaling simulation experiment usually faces the problem of too slow scaling rate. On the one hand, the slow scaling rate leads to a relatively small increase in thermal resistance caused by scaling and is difficult to be observed experimentally. On the other hand, it also greatly increases the difficulty of characterizing and analyzing the resulting scaling. To solve this problem, most people currently choose to artificially increase the concentration of inorganic salt ions in the solution to accelerate the scaling process, but this method is significantly different from actual production. Therefore, in this experimental method, six rounds of continuous experiments are carried out for each determined working condition, and a series of experimental working conditions are compared horizontally and vertically to obtain more effective data.

[0103] The actual operation of the heat exchanger is intermittent, that is, there are downtimes. During downtime, the high-temperature fluid evaporates on the heat exchange surface, and the inorganic salts will all condense on the heat exchange surface. If you want to reproduce the fouling deposition caused by this part of the evaporation in the experiment, you need to dry the simulated heat exchange tubes between different experimental rounds under the same working conditions. This operation method also lays a certain foundation for subsequent extended research - if experimental conditions permit, the metal tubes that are scaled in each round can be supplemented with weighing analysis and heat transfer characteristics analysis, thereby providing a more accurate description of the entire heat exchange tube scaling process and the surface heat transfer efficiency change process.

[0104] 2. Solution turbidity effect experimental module

[0105] The composition of the produced fluid system of polymer flooding is relatively complex. In addition to a certain concentration of HPAM components, there are also relatively rich Na+, Ca 2 +,HCO 3 - and other inorganic salt ions, and when polymers such as HPAM and some metal cations are present in the solution at the same time, the solution system will become turbid as the temperature rises, causing the solution to appear turbid. For a certain solution system, this transition is a transient process controlled by the solution temperature, and the critical temperature at which this "turbidity" process occurs is defined as the "cloud point temperature". This experimental system can accurately explore the effect of turbidity temperature on scaling during the turbidity process of the solution, and provide valuable guidance for the temperature range of heat exchanger operation.

[0106] The experimental system is mainly composed of a spectrophotometer, a cuvette, an electronic balance, a thermocouple, a temperature display, a camera and a blast drying oven.

[0107] Experimental steps:

[0108] (1) Take a certain amount of deionized water, boil it and cool it to room temperature to reduce the dissolved gas in the deionized water.

[0109] (2) Take a certain amount of boiled and cooled deionized water in a beaker, determine the mass of calcium chloride and sodium chloride required according to the mass fraction of the cloud point temperature test solution, and then use a precision analytical balance to weigh the required inorganic salts and dissolve them in deionized water.

[0110] (3) Take a certain amount of boiled and cooled deionized water in a beaker, stir continuously, and slowly disperse the required mass of polymer into the beaker, and continue stirring until the solution is completely transparent and no large pieces of polymer are present.

[0111] (4) Inject the inorganic salt solution into the polymer solution, rinse the beaker and dilute the mixed solution to the required volume.

[0112] (5) Continue stirring until the mixed solution is uniform.

[0113] (6) Turn on the spectrophotometer, adjust the wavelength of the light source to 500 nm, set the spectrophotometer to percentage mode, and preheat for 30 minutes.

[0114] (7) Take a cuvette and fill it with deionized water at room temperature. Measure the transmittance under the light source of this wavelength and calibrate it as 100%.

[0115] (8) Fix the thermocouple contacts in another cuvette and transfer part of the solution to this cuvette.

[0116] (9) Seal the cuvette containing the solution and place it in a forced air drying oven at 105°C until the thermometer reads 93°C.

[0117] (10) The cuvette containing the solution is taken out from the air drying oven and quickly placed in a spectrophotometer. A camera is used to record the change in the transmittance of the liquid in the cuvette with temperature.

[0118] (11) Repeat steps (7) to (10) at least three times for any working condition to ensure the reliability of the experiment, and calculate the average value and record it.

[0119] According to the above steps, the characteristics of the change of the light transmittance of multiple test solutions with temperature can be measured. Based on the light transmittance of the solution, the turbidity point temperature of the test solution can be determined. The scaling experiment of the HPAM solution (i.e., module 1) is carried out in the range above and below the turbidity point temperature, and the intervention effect of the turbidity point temperature on scaling is determined from the difference in the scaling rate.

[0120] Example 2

[0121] like Figure 1 and Figure 2 As shown, Figure 1 This is a diagram of the experimental system for the effect of temperature-concentration on scaling of the present invention. Figure 2 This is a diagram of the experimental system for the effect of solution turbidity temperature on scaling according to the present invention.

[0122] The temperature-concentration effect on scaling experimental module of the present invention includes 1-circulation heater; 2-fixer; 3-heat exchange pipe section; 4-simulated produced fluid; 5-hot fluid thermocouple; 6-cold fluid thermocouple; 7-simulated produced fluid thermocouple; 8-temperature recorder; a total of nine parts or components. The specific implementation method is as follows:

[0123] Start the 1-circulation heater, repeatedly adjust the temperature of the hot fluid in the circulation heater until the reading of the 5-thermocouple B responsible for monitoring the temperature of the hot fluid at the inlet of the test tube is exactly the preset surface temperature, and preheat the test tube at this temperature for 10 minutes. Insert the thermocouple into the fixture, then cover the 2-fixture on the small beaker containing the 4-simulated produced liquid, turn on the 8-temperature recorder, and collect the solution temperature change data at a certain time step. When the reading of the 7-simulated produced liquid thermocouple reaches the preset target temperature, stop the timing and record the heating time t1.

[0124] Take out the 2-fixture device, suspend temperature recording, and let the dirt on the surface of the heating tube dry naturally in the air. Replace a set of small beakers and 4-simulation liquid, and repeat the above steps. The entire experimental process is completed until sufficient analysis data is obtained, and the experimental simulation of the influence of HPAM on the scaling problem of the heat exchange surface is realized.

[0125] The experimental module for the effect of solution turbidity temperature on scaling of the present invention includes seven components: an electronic balance, a spectrophotometer, a cuvette, an air drying oven, a thermocouple, a temperature recorder, and a camera. The specific implementation method is as follows:

[0126] Take a certain amount of deionized water, boil it and cool it to room temperature to reduce the dissolved gas in the deionized water. Take a certain amount of boiled and cooled deionized water in a beaker, determine the mass of calcium chloride and sodium chloride required according to the mass fraction of the turbidity temperature test solution, and then use a precision analytical balance to weigh the required inorganic salt and dissolve it in deionized water. Take another amount of boiled and cooled deionized water in a beaker, stir continuously, and slowly disperse the required mass of polymer into the beaker, and continue stirring until the solution is completely transparent and no large pieces of polymer exist. Inject the inorganic salt solution into the polymer solution, rinse the beaker and dilute the mixed solution to the required volume. Continue stirring until the mixed solution is uniform. Turn on the spectrophotometer, adjust the wavelength of the light source to 500nm, adjust the spectrophotometer to the percentage mode, and preheat for 30 minutes. Take a cuvette, fill it with deionized water at room temperature, measure the transmittance under the light source of this wavelength, and calibrate it as 100%. Fix the thermocouple contacts in another cuvette, and transfer part of the solution to this cuvette. Seal the cuvette containing the solution and place it in a blast drying oven at 105°C to raise the temperature until the thermometer reading reaches 93°C. Take the cuvette containing the solution out of the blast drying oven and quickly put it into the spectrophotometer to use a camera to record the change in the transmittance of the liquid in the cuvette with temperature. Repeat the steps at least 3 times for any working condition to ensure the reliability of the experiment, and calculate the average value for record.

[0127] According to the above steps, the characteristics of the change of the light transmittance of multiple test solutions with temperature can be measured. Based on the light transmittance of the solution, the turbidity point temperature of the test solution can be determined. The scaling experiment of the HPAM solution (i.e., module 1) is carried out in the range above and below the turbidity point temperature, and the intervention effect of the turbidity point temperature on scaling is determined from the difference in the scaling rate.

[0128] Example 3

[0129] In order to determine the criticality of cloud point temperature in the HPAM intervention scaling process, the scaling characteristics of two solution systems in polymer-containing and polymer-free solutions were experimentally analyzed.

[0130] To verify whether the solution cloud point temperature is the critical temperature in the HPAM intervention calcium carbonate scaling problem, it is only necessary to compare whether there is a significant difference in the scaling amount of the solution containing HPAM and the solution without HPAM at a temperature ΔT above the cloud point temperature. The selected solution system (NaHCO 3 The concentration is 1260mg / L, CaCl 2 The concentration is 832.5 mg / L, Ca 2+ The turbidity point temperature of the test solution with a concentration of 300 mg / L is about 75°C. In order to avoid the influence of the temperature control error of the circulating heater on the experimental results, ΔT=10°C and the surface temperature of the heat exchange tube are taken as 85°C. The influence of the test solution without polymer and the test solution with polymer on the scaling characteristics are analyzed at this time. The difference in scaling rate between the solution system containing polymer and the solution system without polymer at 110°C can be compared.

[0131] The experimental equipment and experimental steps are as described in Example 1. The experimental scheme for determining the criticality of cloud point temperature is as follows:

[0132] Scheme 1: polymer concentration is 0 mg / L, CaCl 2 The concentration is 832.5 mg / L, NaHCO 3 The concentration is 1260 mg / L, the NaCl concentration is 0 mg / L, and the surface temperature is 85°C.

[0133] Scheme 2: polymer concentration is 800 mg / L, CaCl 2 The concentration is 832.5 mg / L, NaHCO 3 The concentration is 1260 mg / L, the NaCl concentration is 0 mg / L, and the surface temperature is 85°C.

[0134] Scheme 3: polymer concentration is 0 mg / L, CaCl 2 The concentration is 1888.94 mg / L, NaHCO 3 The concentration is 868.78 mg / L, the NaCl concentration is 12905.91 mg / L, and the surface temperature is 110℃.

[0135] Scheme 4: polymer concentration is 800 mg / L, CaCl 2 The concentration is 1888.94 mg / L, NaHCO 3 The concentration is 868.78 mg / L, the NaCl concentration is 12905.91 mg / L, and the surface temperature is 110℃.

[0136] In the two simulated working fluids with significantly different compositions, even when the surface temperature of the heat exchange tubes reached above the "cloud point temperature", HPAM did not show a significant promoting effect on the scaling rate. For the simulated working fluid with a composition close to reality, high-concentration HPAM did not show a significant effect on the scaling rate after the surface temperature exceeded the cloud point temperature; while for the simulated working fluid with a relatively simple composition, high-concentration HPAM could even reduce the scaling rate to a certain extent after the surface temperature exceeded the cloud point temperature.

[0137] Compared with high-concentration HPAM, low-concentration HPAM has a significantly stronger inhibitory effect on the scaling rate than a promoting effect; therefore, since it has been confirmed here that high-concentration HPAM will not significantly increase the scaling rate at surface temperatures above the cloud point temperature, then at least at the concentrations involved in this experiment, the effect of HPAM on the scaling rate is not strictly critical to the cloud point temperature.

[0138] It is inferred that there may be a critical temperature that needs to be determined: the turbidity of the solution above the cloud point temperature is traced back to the precipitation of the HPAM component, and the decrease in the transmittance of the polymer-inorganic salt solution with increasing temperature is a gradual rather than instantaneous process. Then, as the local temperature continues to rise, there should be a higher temperature that causes all or nearly all of the HPAM near the heat exchange surface to precipitate, thereby completely losing its effect on the scaling process. Below this higher temperature, there should be an equilibrium point that allows the promotion and inhibition of the scaling process by HPAM to be in equilibrium.

[0139] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions recorded in the aforementioned embodiments or replace some of the technical features therein with equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

[0140] Except for the technical features described in the specification, all other technical features are known technologies to those skilled in the art.

Claims

1. An experimental method for exploring the effect of HPAM on scaling of heat exchange surfaces, characterized in that: The experimental method used to investigate the effect of HPAM on heat exchange surface fouling includes: Step 1, preparing simulated produced fluid; Step 2, simulating the scaling process of geothermal fluid; Step 3, calculating the average scaling rate under certain temperature conditions; Step 4, repeat the test for each temperature condition, i.e. repeat the test step 3; Step 5, visualizing the test data; Step 6, determine the turbidity point temperature of the test solution and analyze the effect of the turbidity temperature of the simulated solution on scaling.

2. The experimental method for exploring the effect of HPAM on scaling of heat exchange surfaces according to claim 1, characterized in that: Step 1 includes: Step 11, taking a certain amount of deionized water, boiling it, and then cooling it to room temperature to remove dissolved gas in the deionized water, and ultrasonically cleaning it for 10 minutes to further degas; Step 12, slowly adding HPAM particles to degassed deionized water and continuously stirring until the solution is clear and no lumps remain, to obtain an HPAM mother solution; Step 13, prepare sodium chloride, calcium chloride and sodium bicarbonate solutions respectively, transfer them into the prepared HPAM mother solution in sequence, and adjust the volume to the target capacity.

3. The experimental method for exploring the effect of HPAM on scaling of heat exchange surfaces according to claim 1, characterized in that: In step 2, different test temperatures are set to simulate the scaling process of geothermal fluids, and the time required for heating under different conditions is recorded.

4. The experimental method for exploring the effect of HPAM on scaling of heat exchange surfaces according to claim 3, characterized in that: Step 2 includes: Step 21, preheating the test environment, heating the simulated solution according to the test condition requirements, and recording the time required for heating; Step 22, when the solution reaches the preset target temperature, stop timing and record the heating time t1; Step 23, suspend the heating process and allow the dirt on the surface of the heating tube to dry naturally in the air; Step 24, test different heating rates and record the time required for heating, repeat steps 22 and 23 to obtain t2, t3, t4, t5 and t6.

5. The experimental method for exploring the effect of HPAM on scaling of heat exchange surfaces according to claim 1, characterized in that: In step 3, the reaction is terminated, the mass difference before and after the simulated scaling test is weighed and recorded, and the average scaling rate under certain temperature conditions is calculated according to the scaling rate formula to describe the change in heating time caused by the scaling test pipe section to describe the increase in heat transfer thermal resistance caused by scaling.

6. The experimental method for exploring the effect of HPAM on scaling of heat exchange surfaces according to claim 5, characterized in that: In step 5, the scaling rate formula is: Where, M1 is the mass of the short heating tube before the scaling test, M2 is the mass of the heating tube with scale attached after the test, t i It is the time required to reach the preset experimental temperature at different heating rates.

7. The experimental method for exploring the effect of HPAM on scaling of heat exchange surfaces according to claim 1, characterized in that: In step 5, the average heat absorption Q of the solution during the heating process is solved using the known heating range and the experimentally measured heating time, and the change of Q with the experimental rounds is used to characterize the effect of fouling on the surface heat transfer characteristics.

8. The experimental method for exploring the effect of HPAM on scaling of heat exchange surfaces according to claim 7, characterized in that: In step 5, the average heat absorption is calculated as: Where c p is the specific heat capacity of water at constant pressure, ρ is the density of water, V is the volume of water, ΔT is the temperature difference of deionized water before and after heating, and t is the reaction time.

9. The experimental method for exploring the effect of HPAM on scaling of heat exchange surfaces according to claim 1, characterized in that: In step 6, the change of the light transmittance of the solution under different conditions with the temperature is tested. Based on the light transmittance of the solution, the turbidity point temperature of the test solution can be determined, and the effect of the turbidity temperature of the simulated solution on scaling can be further analyzed.

10. The experimental method for exploring the effect of HPAM on scaling of heat exchange surfaces according to claim 9, characterized in that: Step 6 includes: Step 61, turn on the spectrophotometer, adjust the wavelength of the light source to 500nm, adjust the spectrophotometer to percentage mode, and preheat for 30 minutes; Step 62, take a cuvette, fill it with deionized water at room temperature, measure the light transmittance under the light source of this wavelength, and calibrate it as 100%; Step 63, placing the simulated solutions at different temperature nodes in a cuvette to measure the variation characteristics of the spectral signal with temperature.