Composite diffusion plate based on perovskite quantum dots and preparation method thereof
Through the preparation method of perovskite quantum dot diffusion plate coated with multilayer polymer matrix, the problem of poor stability of perovskite quantum dots at high concentrations is solved, and the improvement of high stability and optical performance is achieved, while reducing costs , avoiding the use of high-cost water and oxygen barrier films.
Patent Information
- Application Number
- CN202310629835.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-30
AI Technical Summary
Existing perovskite quantum dot diffusion plates have poor stability at high concentrations and require the use of high-cost water-oxygen barrier membranes, which limits their application and cost-effectiveness.
The preparation method of perovskite quantum dot optical diffusion plates is adopted to form perovskite quantum dot optical diffusion plate by in-situ extrusion based on perovskite precursor and auxiliary ligand, and coated with a variety of polymer matrix. The three-layer polymer matrix coated structure of ore quantum dots improves stability and optical properties.
The stability and optical performance of perovskite quantum dot diffusion plates are significantly improved without the need for the use of expensive water-oxygen barrier films, reducing production costs, and simplifying the process flow.
Smart Images

Figure CN119065038A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a composite diffusion plate based on perovskite quantum dots and a preparation method thereof, belonging to the technical field of optoelectronic display materials. Background Art
[0002] From the perspective of market information, it can be understood that in July 2022, a senior researcher at Nanocrystal Technology mentioned that quantum dot films and quantum dot diffusion plates have become key materials and solutions for upgrading mainstream LCD backlight products. Nanocrystal Technology is a leader in quantum dot display technology, with a relatively obvious bias towards transformation in the technical positioning and product design selection from Cd-containing to low-Cd / Cd-free quantum dots and from diffusion films to diffusion plates. In addition, Nanocrystal Technology also plans to launch a full-concentration diffusion plate for the PS system, abandoning expensive barrier films to significantly reduce costs and provide the necessary conditions for the sinking of quantum dot display terminals. Quantum dot materials have important application value in different new displays. Not only can they be used with Mini LED, OLED, Micro LED and other technologies to achieve color conversion, but they can also produce active matrix quantum dot light-emitting diodes (AM-QLED), which is called the next generation of display technology. With the increasing maturity of quantum dot technology and the continuous improvement of the industrial chain, there will be more abundant quantum dot applications that can be commercialized.
[0003] It is understood that the quantum dot optical diffuser jointly developed by Chuang Yida and Nanosys of the United States integrates the diffuser and quantum dot light-emitting layer. It is a key core component of high color gamut display devices, with wide color gamut, high color uniformity, low blue light, long life, automated assembly, low mass production cost and other advantages. It is a major innovation in LCD backlight technology. The diffuser jointly launched by the two parties has been supplied in batches by leading manufacturers in the industry such as TCL, Hisense, Skyworth, BOE, Huawei, Xiaomi, and Changhong, and won the annual SID Best Display Component Product Award in 2022.
[0004] Regarding the diffuser, it is generally known that when light passes through a medium with a different refractive index during propagation, physical processes such as refraction, reflection and scattering will occur. The optical diffuser is made by adding an inorganic or organic light diffuser to the polymer matrix, or designing an array microstructure on the surface of the polymer matrix, thereby adjusting the refraction, reflection and scattering of light to change the propagation path of the light, so that the angle of the light changes by about 170°, thereby achieving full dispersion of the incident light and producing an optical diffusion effect. The optical diffuser can fully scatter the incident light to achieve a softer and more uniform illumination effect, and is widely used in liquid crystal displays, LED lighting and imaging systems.
[0005] Regarding perovskite quantum dots, they are generally known as nano-sized luminescent particles. The system is mainly divided into two categories, one is organic / inorganic hybrid lead halide perovskite (MAPbX3, FAPbX3; X = Cl, Br, I, MA = CH3NH3, FA = (NH2)2CH); the other is all-inorganic perovskite (CsPbX3, X = Cl, Br, I). Perovskite quantum dots usually have the advantages of ultra-high quantum yield, narrow emission half-peak width, short fluorescence lifetime, high crystallinity, high electron-hole mobility, and low price. They are widely used in the field of light-emitting diodes and photovoltaic cells. However, the disadvantages of perovskite quantum dots are also obvious. Without good design control, the stability of quantum dot materials is poor, and they are particularly susceptible to environmental conditions such as temperature, humidity, oxygen, and light, which has a rapid decay effect on luminescence performance.
[0006] However, the quantum dot diffusion plates currently sold by Chuang Yida are based on the CdSe system, which contains Cd and is not environmentally friendly. At the same time, the concentration of quantum dots in the diffusion plates is low, and the product is positioned as a low-concentration diffusion plate. Nanocrystal Technology is promoting full-concentration diffusion plates, but it still needs to further solve the problems of agglomeration of adjacent quantum dots at high concentrations and growth control.
[0007] For Cd-free, high-concentration diffusers, poor stability is a key technical issue that has not been well resolved. Therefore, there is an urgent need to develop new perovskite quantum dot-based diffusers that can improve stability and optical performance without the use of costly water and oxygen barrier films and can be produced by relatively simple and easy methods. Summary of the invention
[0008] In view of the above, the present application provides a perovskite quantum dot optical diffuser with multilayer coating, and an in-situ extrusion preparation method for a perovskite quantum dot diffuser with full concentration, no Cd, and high stability. First, the perovskite precursor cations and anions, the in-situ auxiliary ligands, and the first matrix plastic particles are put into an extruder for melt extrusion granulation. The space limitation of the first matrix plastic particles and the growth limitation of the auxiliary ligands are utilized to obtain perovskite quantum dot seeds in the first matrix layer, which are modified by auxiliary ligands on the surface and coated with the first matrix polymer on the outer layer. Then, the seeds are evenly stirred with the second matrix polymer and then put into the extruder for melt extrusion to obtain colloid particles coated with the second matrix polymer, while helping the internal crystal structure of the quantum dots to anneal to eliminate defects, and the optical performance and stability are improved. Finally, the colloid particles are stirred and extruded with the third matrix polymer, the diffusion particles, and the additives to form an in-situ extruded perovskite quantum dot diffuser with excellent optical performance and high stability. The extruded diffuser plate obtained by the method of the present application combines the property advantages of multiple polymer matrices, while greatly reducing the cost without the need to use expensive water and oxygen barrier films, and significantly improving the stability and optical properties.
[0009] According to one aspect of the present application, a composite diffuser plate based on perovskite quantum dots is provided, comprising:
[0010] matrix; and
[0011] Perovskite quantum dots and diffused particles distributed in the matrix,
[0012] Wherein, the chemical formula of the perovskite quantum dot is ABX3, A and B represent cations, and X represents anions;
[0013] The surface of the perovskite quantum dots is modified by ligands, and is coated with a first polymer, a second polymer and a third polymer in sequence from the inside to the outside;
[0014] The matrix is melt-formed from the first polymer, the second polymer, and the third polymer.
[0015] Optionally, the first polymer is selected from at least one of PMMA, PS, PC, MS, PET, PP, PE, and PAN.
[0016] Optionally, the second polymer is selected from at least one of EVOH, PVA, and PVDC.
[0017] Optionally, the third polymer is selected from at least one of PVDF, PEG, PAM, POM, PVP, PES, SEBS, SMA, and PEEK.
[0018] Optionally, the cation A is selected from Cs + 、MA + , FA + At least one of the cations B is selected from Pb 2+ Sn 2+ At least one of the anions X is selected from Cl - Br - ,I - At least one of .
[0019] Preferably, the perovskite quantum dots are selected from at least one of CsPbCl3, MAPbCl3, FAPbCl3, CsPbBr3, MAPbBr3, FAPbBr3, CsPbI3, MAPbI3, FAPbI3, CsSnI3, MASnI3, and FASnI3.
[0020] Optionally, the diffusion particles are selected from at least one of nano-SiO2 particles, nano-TiO2 particles, nano-BaSO4 particles, nano-CaCO3 particles, and PMMA microspheres.
[0021] Optionally, the ligand is selected from at least one of DDAB, PEABr, TOPO, DMA, OPA, TBABr, TBACl, IDA, TPP, ODPA, BA, and CA.
[0022] Optionally, the coating layer of the first polymer has a thickness of 2-20 μm.
[0023] Optionally, the thickness of the coating layer of the first polymer is independently selected from any value among 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm or any range value between two of them.
[0024] Preferably, the thickness of the coating layer of the first polymer is 8-12 μm.
[0025] Optionally, the thickness of the coating layer of the second polymer is 5-30 μm.
[0026] Optionally, the thickness of the coating layer of the second polymer is independently selected from any value among 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, 21μm, 22μm, 23μm, 24μm, 25μm, 26μm, 27μm, 28μm, 29μm, 30μm, or any range value between two of them.
[0027] Preferably, the thickness of the coating layer of the second polymer is 12-18 μm.
[0028] Optionally, the coating layer of the third polymer has a thickness of 5-30 μm.
[0029] Optionally, the thickness of the coating layer of the third polymer is independently selected from any value among 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, 21μm, 22μm, 23μm, 24μm, 25μm, 26μm, 27μm, 28μm, 29μm, 30μm or any range value between two of them.
[0030] Preferably, the thickness of the coating layer of the third polymer is 12-18 μm.
[0031] According to another aspect of the present application, there is provided a method for preparing the composite diffuser plate as described above, comprising:
[0032] a) respectively mixing the salt corresponding to the cation A, the salt corresponding to the cation B, the salt corresponding to the anion X and the ligand with the first polymer to prepare an A-site cation precursor, a B-site cation precursor, an anion precursor and a ligand precursor;
[0033] b) mixing the A-site cation precursor, the B-site cation precursor, the anion precursor and the ligand precursor, and extruding to obtain seed crystals;
[0034] c) mixing the seed crystals with the second polymer and extruding to obtain a masterbatch;
[0035] d) mixing the master batch with the third polymer and the diffusion particles, extruding, and in-situ producing the composite diffusion plate after demoulding.
[0036] Optionally, in step a), the salt corresponding to the cation A is selected from at least one of stearate, tungstate, molybdate, carbonate, and bicarbonate, the salt corresponding to the cation B is selected from at least one of stearate, tungstate, molybdate, carbonate, and bicarbonate, and the salt corresponding to the anion X is selected from metal halides.
[0037] Optionally, the mass ratio of the salt corresponding to the cation A to the first polymer is 1:2000 to 50:2000.
[0038] Optionally, the mass ratio of the salt corresponding to the cation B to the first polymer is 1:2000 to 80:2000.
[0039] Optionally, the mass ratio of the salt corresponding to the anion X to the first polymer is 1:2000 to 40:2000.
[0040] Optionally, the mass ratio of the ligand to the first polymer is 1:2000 to 30:2000.
[0041] Optionally, in step b), the A-site cation precursor, the B-site cation precursor and the anion precursor are mixed so that the molar ratio of the salt corresponding to the cation B to the salt corresponding to the cation A is 1:1 to 2:1; and the molar ratio of the salt corresponding to the anion X to the salt corresponding to the cation A is 1:1 to 5:1;.
[0042] Optionally, the A-site cation precursor and the ligand precursor are mixed so that the molar ratio of the salt corresponding to the cation A to the ligand is 1:1 to 1:5.
[0043] Optionally, in step b), the extrusion temperature is 150-250°C.
[0044] Optionally, in step b), the extrusion temperature is independently selected from any value of 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C or any range therebetween.
[0045] Optionally, in step b), the extrusion rate is 100 r / min to 800 r / min.
[0046] Optionally, in step b), the extrusion rate is independently selected from any value of 100 r / min, 200 r / min, 300 r / min, 400 r / min, 500 r / min, 600 r / min, 700 r / min, 800 r / min or any range between two values.
[0047] Optionally, in step c), the mass ratio of the seed crystal to the second polymer is 10:2 to 10:5.
[0048] Optionally, in step c), the extrusion temperature is 150-250°C.
[0049] Optionally, in step c), the extrusion temperature is independently selected from any value of 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C or any range therebetween.
[0050] Optionally, in step c), the extrusion rate is 100 r / min to 800 r / min.
[0051] Optionally, in step c), the extrusion rate is independently selected from any value of 100 r / min, 200 r / min, 300 r / min, 400 r / min, 500 r / min, 600 r / min, 700 r / min, 800 r / min or any range between two values.
[0052] Optionally, in step d), the mass ratio of the masterbatch to the third polymer is 10:2 to 10:5.
[0053] The mass ratio of the masterbatch to the diffusion particles is 10:0.1 to 10:0.8.
[0054] Optionally, the extrusion temperature in step d) is 150-250°C.
[0055] Optionally, the extrusion temperature in step d) is independently selected from any value of 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C or any range therebetween.
[0056] Optionally, the extrusion rate in step d) is 100 r / min to 800 r / min.
[0057] Optionally, the extrusion rate in step d) is independently selected from any value of 100 r / min, 200 r / min, 300 r / min, 400 r / min, 500 r / min, 600 r / min, 700 r / min, 800 r / min or any range between two values.
[0058] Optionally, the mixing further comprises adding an auxiliary agent, wherein the auxiliary agent is selected from at least one of nano-SiO2 particles, nano-TiO2 particles, nano-BaSO4 particles, nano-CaCO3 particles, and PMMA microspheres.
[0059] Optionally, the mass ratio of the auxiliary agent to the masterbatch is 0.01 to 0.08: 1. The auxiliary agent has the functions of changing the light diffusion path, changing the light path, and having an incremental effect.
[0060] According to the present application, when determining the extrusion temperature of each of the above steps, in addition to the melting temperature of the polymer used, it is also necessary to consider the comprehensive influence and optimization of various other factors. For example, the extrusion temperature used in step b) is adjusted based on the window of the melting temperature of the first polymer, taking into account the growth temperature of the quantum dots; the extrusion temperature used in steps c) and d) is determined based on the window of the melting temperature of the second polymer or the third polymer, taking into account the ripening temperature of the quantum dots.
[0061] In the composite diffusion plate according to the present application, the surface of the perovskite quantum dot is modified by a ligand, and the first polymer, the second polymer and the third polymer are sequentially coated from the inside to the outside. Here, on the basis of limiting the extrusion temperature of each of the above steps, by limiting the coating thickness of the first polymer, the spatial growth of the quantum dot seed can be limited, thereby obtaining quantum dots with high luminescence performance at the nanometer level; by limiting the coating thickness of the second polymer and the third polymer, it not only plays the role of oxygen and water blocking respectively, but also helps to reduce defects and control defects, and the polymer layer interacts and couples with the surface anions and cations of the ionic crystal through the lone pairs of electrons in the characteristic chemical groups of the polymer; in addition, by introducing ligands, the surface defects of the quantum dots can also be effectively modified and regulated, and the ligand chemical substances also interact with QD through the lone pairs of electrons on special groups.
[0062] According to the present application, the thickness of the polymer coating layer can be adjusted by, for example, changing the feed amount and / or limiting the extrusion rate or time.
[0063] Optionally, the raw materials used in steps a) to d) are in powder form, and the powder can be obtained, for example, by pulverizing master batches.
[0064] Optionally, the mixing in steps a) to d) is independently performed under stirring.
[0065] Optionally, the stirring speed is 80-150 rpm and the time is 1-5 h.
[0066] Optionally, the extrusion in steps b) to d) is independently carried out in an extruder.
[0067] Optionally, in steps b) to d), before the extrusion, the screw of the extruder is cleaned using corresponding polymer masterbatch.
[0068] In a specific embodiment, the method comprises the following steps:
[0069] 1) Preparation of cationic precursor: Weighing cationic A stearate powder and first polymer powder (obtained by crushing masterbatch), mixing at room temperature, stirring at 120 rpm for 3 h using a stirrer to obtain A-site cationic precursor powder; Weighing cationic B stearate powder and first polymer powder, mixing at room temperature, stirring at 120 rpm for 3 h using a stirrer to obtain B-site cationic precursor powder.
[0070] 2) Preparing an anion precursor: weighing anion X metal halide powder and first polymer powder, mixing them at room temperature, and stirring them at 120 rpm for 3 hours using a stirrer to obtain X-position anion precursor powder.
[0071] 3) Preparation of ligand precursor: weigh the ligand powder and the first polymer powder, mix them at room temperature, and stir them at 120 rpm for 3 hours using a stirrer to obtain a ligand precursor powder.
[0072] 4) Preparation of seed crystals (perovskite quantum dots ABX3@first polymer matrix): set the extruder temperature to 80°C, 100°C, 120°C, 150°C, 150°C, and 110°C for six temperature control programs for preheating for 1 hour, and then use pure first polymer masterbatch to clean the machine screw for 1 hour; adjust the pump body parameters, set the pump body displacement to 10ml / rev, 1.51rpm / Hz, and frequency to 16Hz; weigh the A-site cation precursor powder, B-site cation precursor powder, X-site anion precursor powder, and ligand precursor powder, mix them at room temperature, and use a stirrer to stir at 120rpm for 3h to obtain a mixture K; feed the mixture K into the extruder feed port and extrude it at a temperature of 150°C and a rate of 250r / min to obtain ABX3@matrix 1 seed crystals.
[0073] 5) Preparation of masterbatch (perovskite quantum dot ABX3@first polymer matrix@second polymer matrix): weigh the ABX3@matrix 1 seed crystals obtained in 4) and the second polymer powder, mix them at room temperature, use a stirrer at 120 rpm for 3 hours to obtain a mixture M; set the extruder temperature to 80°C, 100°C, 130°C, 170°C, 170°C, and 120°C for six temperature control programs, preheat for 1 hour, and then use pure second polymer masterbatch to clean the machine screw for 1 hour; adjust the pump body parameters, set the pump body displacement to 15 ml / rev, 1.37 rpm / Hz, and frequency to 20 Hz; put the mixture M into the extruder feed port, extrude it at a temperature of 170°C and a rate of 370 r / min to obtain ABX3@matrix 1@matrix 2 masterbatch.
[0074] 6) Preparation of a composite diffusion plate (perovskite quantum dot ABX3@first polymer matrix@second polymer matrix@third polymer matrix): weigh the ABX3@matrix 1@matrix 2 masterbatch, the third polymer powder and the diffusion particles and the additives obtained in 5), mix them at room temperature, and use a stirrer to stir at a speed of 120 rpm for 3 hours to obtain a mixture P; set the extruder temperature to 80°C, 100°C, 150°C, 150°C, 150°C, and 90°C for six temperature control programs for preheating for 1 hour, and then use pure third polymer powder to clean the machine screw for 1 hour; adjust the pump body parameters, set the pump body displacement to 13 ml / rev, 1.51 rpm / Hz, and frequency to 18 Hz; put the mixture P into the extruder feeding port, install a mold at the extrusion port, and extrude at a temperature of 150°C and a rate of 400 r / min to obtain an ABX3@matrix 1@matrix 2@matrix 3 diffusion plate.
[0075] The beneficial effects that this application can produce include:
[0076] 1) The composite diffuser plate of the present application has quantum dots with three layers of polymer matrix covering the core-shell layer. The first layer of polymer matrix is used to achieve spatial growth restriction of quantum dots, thereby obtaining quantum dot materials with high luminescence performance at the nanometer level; the second layer of polymer matrix can achieve high oxygen barrier effect; the third layer of polymer matrix can achieve high water barrier effect, while protecting the high oxygen barrier properties of the second layer of polymer matrix under low humidity, thereby achieving high luminescence performance and high stability.
[0077] 2) The preparation method of the present application is implemented through multi-step melt coating extrusion. By considering the primary growth temperature of quantum dots, the secondary ripening defect elimination temperature and the different melting temperature requirements of the three layers of polymers, the growth and coating process of quantum dots are rationally controlled; and by controlling the feed amount and reaction time, the density and coating thickness of the three coating layers are regulated, thereby achieving the optimal design of optical performance and stability.
[0078] 3) The preparation method of the present application is implemented by in-situ extrusion, which has a simple process and low condition requirements; compared with the liquid phase high-temperature hot injection synthesis of quantum dot mother liquor, this method has more environmental advantages and lower costs, and can avoid the tedious steps of purifying quantum dots, preparing quantum dot films and assembling quantum dot diffusion plates, especially realizing an effective solution for full-concentration diffusion plates. BRIEF DESCRIPTION OF THE DRAWINGS
[0079] Figure 1 It is a schematic diagram of the structure and preparation process of the composite diffuser plate according to the present application.
[0080] Figure 2 This is a schematic diagram of the structure of the green diffuser plate prepared in Example 1 of the present application.
[0081] Figure 3 This is a schematic diagram of the structure of the red diffuser prepared in Example 2 of the present application.
[0082] Figure 4 This is a schematic diagram of the structure of the green diffuser plate prepared in Example 3 of the present application.
[0083] Figure 5 This is a schematic diagram of the structure of the red diffuser prepared in Example 4 of the present application.
[0084] Figure 6 This is a schematic diagram of the structure of the green diffuser plate prepared in Example 5 of the present application.
[0085] Figure 7 This is a schematic diagram of the structure of the red diffuser prepared in Example 6 of the present application. DETAILED DESCRIPTION
[0086] As mentioned above, the present application provides a multi-coated in-situ extruded diffuser plate, the structure and preparation process of which are as follows: Figure 1 As shown. According to the present application, the integral part of the in-situ extruded diffusion plate is formed by extruding three polymer matrices after melting, and the space is distributed with luminescent nanoparticles and diffusion particles coated with three layers of polymers (not shown in the figure). The core crystal structure of the nanoparticle can be represented by ABX3, and its surface is modified by ligand molecules to passivate surface defects; the first polymer matrix is further outward, which is used to spatially restrict the growth of quantum dots, and the thickness of the polymer matrix is generally about 10μm; the next outer circle is the second polymer matrix, which is used to prevent the rapid penetration of oxygen, and the thickness of the polymer matrix is generally about 15μm; the outermost circle is the third polymer matrix, which is used to prevent the rapid penetration of water vapor, protect the quantum dots from being damaged by water vapor, and ensure the oxygen barrier properties of the second polymer matrix layer, and the thickness of the polymer matrix is generally about 15μm.
[0087] The present application also provides a method for preparing an in-situ extruded perovskite quantum dot diffusion plate with high stability through multiple coatings, comprising: A1) using a first matrix plastic particle to prepare a cation precursor, an anion precursor and a ligand precursor; A2) adding the cation precursor, anion precursor and ligand precursor to an extruder, mixing them evenly and extruding them to form a first mixture; A3) adding a second matrix plastic particle to the first mixture, stirring them evenly and extruding them through the extruder to form a second mixture; A4) adding a third matrix plastic particle, a diffusing agent and an auxiliary agent to the second mixture, stirring them evenly and extruding them to form a quantum dot light-emitting functional plate. The preparation method provided in the present application forms a multi-layer core-shell structure of core quantum dots by multiple coatings of polymer matrices with different functions, thereby enhancing the quantum dots' resistance to external water, oxygen, light, and heat damage, and improving the stability of the quantum dots; on the other hand, through the melting process of cationic precursors and anionic precursors with plastic particles, the plastic particles play an auxiliary growth role in the process, thereby achieving more efficient growth of quantum dots. At the same time, multiple coating and heating also further promote the regrowth of quantum dots, thereby achieving uniform fusion of quantum dots and various plastic matrices in the plate body, thereby improving the color gamut and luminous efficiency.
[0088] According to the present application, multiple coatings of polymer matrices with different functionalities are combined with perovskite quantum dots of different systems, thereby achieving an improvement in the performance of the diffuser plate and an improvement in its preparation method. On this basis, the present application can also be extended to the product development direction of the diffuser plate prepared using high molecular polymers and quantum dot materials different from those described in the present application in related fields. Furthermore, the present application can be applied to various solutions for preparing products different from the diffuser plate using coating layers different from high molecular polymers and systems different from perovskite quantum dots.
[0089] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0090] The experimental methods in the following examples without specifying specific conditions are usually carried out according to conventional conditions or conditions recommended by the manufacturer.
[0091] Unless otherwise specified, the raw materials and reagents used in the examples of this application were purchased through commercial channels.
[0092] The analytical measuring instruments used in the examples of this application are as follows:
[0093] Measuring instrument name: Admesy spectrometer from the Netherlands;
[0094] Measuring instrument model: hera01-FO23L20.
[0095] Example 1: CsPbBr3@PMMA@EVOH@PVDF green diffuser
[0096] 1) Preparation of cationic precursor: 41.6 g of cesium stearate powder and 20 kg of PMMA powder (obtained by crushing masterbatch) were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain A-site cationic precursor powder; 77.4 g of lead stearate powder and 20 kg of PMMA powder were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain B-site cationic precursor powder.
[0097] 2) Preparation of anion precursor: Weigh 22.5 g zinc bromide (ZnBr2) powder and 20 kg PMMA powder and mix them at room temperature, and stir them at 120 rpm for 3 h using a stirrer to obtain X-site anion precursor powder.
[0098] 3) Preparation of ligand precursor: 40.6 g of didecyl dimethyl ammonium bromide (DDAB) powder and 20 kg of PMMA powder were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain a ligand precursor powder.
[0099] 4) Preparation of seed crystals (perovskite quantum dots ABX3@first polymer matrix): set the extruder temperature to 80°C, 100°C, 120°C, 150°C, 150°C, and 110°C for six temperature control programs for preheating for 1 hour, and then use pure PMMA masterbatch to clean the machine screw for 1 hour; adjust the pump body parameters, set the pump body displacement to 10ml / rev, 1.51rpm / Hz, and frequency to 16Hz; weigh 5kg of A-site cation precursor powder, 5kg of B-site cation precursor powder, 10kg of X-site anion precursor powder, and 20kg of ligand precursor powder, mix them at room temperature, and use a stirrer to stir at 120rpm for 3h to obtain a mixture K; put the mixture K into the extruder feed port, extrude it at a rate of 250r / min at a high temperature platform of 150 to obtain CsPbBr3@PMMA seed crystals.
[0100] 5) Preparation of masterbatch (perovskite quantum dot ABX3@first polymer matrix@second polymer matrix): weigh 10 kg of the CsPbBr3@PMMA seed crystals obtained in the above step 4) and 2 kg of EVOH powder, mix them at room temperature, use a stirrer at 120 rpm for 3 hours to obtain a mixture M; set the extruder temperature to 80°C, 100°C, 130°C, 170°C, 170°C, and 120°C for six temperature control programs and preheat for 1 hour, then clean the machine screw with pure EVOH masterbatch for 1 hour; adjust the pump body parameters, set the pump body displacement to 15 ml / rev, 1.37 rpm / Hz, and frequency to 20 Hz; put the mixture M into the extruder feed port, extrude it at 170°C and 370 r / min to obtain CsPbBr3@PMMA@EVOH masterbatch.
[0101] 6) Preparation of a composite diffusion plate (perovskite quantum dot ABX3@first polymer matrix@second polymer matrix@third polymer matrix): weigh 10 kg of the CsPbBr3@PMMA@EVOH masterbatch prepared in the above step 5), 4 kg of PVDF and 0.5 kg of diffusion particles SiO2, mix them at room temperature, use a stirrer at 120 rpm for 3 hours to obtain a mixture P; set the extruder temperature to 80°C, 100°C, 150°C, 150°C, 150°C, 90°C for six temperature control programs for preheating for 1 hour, and then use pure PVDF powder to clean the machine screw for 1 hour; adjust the pump body parameters, set the pump body displacement to 13 ml / rev, 1.51 rpm / Hz, and frequency to 18 Hz; put the mixture P into the extruder feed port, and install a mold at the extrusion port, extrude at a temperature of 150 and a rate of 400 r / min to obtain a CsPbBr3@PMMA@EVOH@PVDF green diffusion plate. The coating structure of the green diffuser plate prepared in Example 1 is as follows Figure 2 shown.
[0102] Example 2: CsPbI3@PMMA@EVOH@PVDF red diffuser
[0103] 1) Preparation of cationic precursor: 41.6 g of cesium stearate powder and 20 kg of PMMA powder (obtained by crushing masterbatch) were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain A-site cationic precursor powder; 77.4 g of lead stearate powder and 20 kg of PMMA powder were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain B-site cationic precursor powder.
[0104] 2) Preparation of anion precursor: 31.9 g zinc iodide (ZnI2) powder and 20 kg PMMA powder were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain X-site anion precursor powder.
[0105] 3) Preparation of ligand precursor: 40.6 g of didecyl dimethyl ammonium bromide (DDAB) powder and 20 kg of PMMA powder were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain a ligand precursor powder.
[0106] 4) Preparation of seed crystals (perovskite quantum dots ABX3@first polymer matrix): set the extruder temperature to 80°C, 100°C, 120°C, 150°C, 150°C, and 110°C for six temperature control programs for preheating for 1 hour, and then use pure PMMA masterbatch to clean the machine screw for 1 hour; adjust the pump body parameters, set the pump body displacement to 10ml / rev, 1.51rpm / Hz, and frequency to 16Hz; weigh 5kg of A-site cation precursor powder, 5kg of B-site cation precursor powder, 10kg of X-site anion precursor powder, and 20kg of ligand precursor powder, mix them at room temperature, and use a stirrer to stir at 120rpm for 3h to obtain a mixture K; put the mixture K into the extruder feeding port, extrude it at a rate of 250r / min at a high temperature platform of 150 to obtain CsPbI3@PMMA seed crystals.
[0107] 5) Preparation of masterbatch (perovskite quantum dot ABX3@first polymer matrix@second polymer matrix): weigh 10 kg of the CsPbI3@PMMA seed crystals obtained in the above step 4) and 2 kg of EVOH powder, mix them at room temperature, use a stirrer at 120 rpm for 3 hours to obtain a mixture M; set the extruder temperature to 80°C, 100°C, 130°C, 170°C, 170°C, and 120°C for six temperature control programs and preheat for 1 hour, then clean the machine screw with pure EVOH masterbatch for 1 hour; adjust the pump body parameters, set the pump body displacement to 15 ml / rev, 1.37 rpm / Hz, and frequency to 20 Hz; put the mixture M into the extruder feed port, extrude it at 170°C and 370 r / min to obtain CsPbI3@PMMA@EVOH masterbatch.
[0108] 6) Preparation of a composite diffusion plate (perovskite quantum dot ABX3@first polymer matrix@second polymer matrix@third polymer matrix): weigh 10 kg of the CsPbI3@PMMA@EVOH masterbatch prepared in the above step 5), 4 kg of PVDF and 0.5 kg of diffusion particles SiO2, mix them at room temperature, use a stirrer at 120 rpm for 3 hours to obtain a mixture P; set the extruder temperature to 80°C, 100°C, 150°C, 150°C, 150°C, and 90°C for six temperature control programs, preheat for 1 hour, and then use pure PVDF powder to clean the machine screw for 1 hour; adjust the pump body parameters, set the pump body displacement to 13 ml / rev, 1.51 rpm / Hz, and frequency to 18 Hz; put the mixture P into the extruder feed port, and install a mold at the extrusion port, extrude at a temperature of 150 and a rate of 400 r / min to obtain a CsPbI3@PMMA@EVOH@PVDF red diffusion plate. The coating structure of the red diffuser plate prepared in Example 2 is as follows Figure 3 shown.
[0109] Example 3: CsPbBr3@PMMA@PVA@PVDF green diffusion plate
[0110] 1) Preparation of cationic precursor: 41.6 g of cesium stearate powder and 20 kg of PMMA powder (obtained by crushing masterbatch) were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain A-site cationic precursor powder; 77.4 g of lead stearate powder and 20 kg of PMMA powder were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain B-site cationic precursor powder.
[0111] 2) Preparation of anion precursor: Weigh 22.5 g zinc bromide (ZnBr2) powder and 20 kg PMMA powder and mix them at room temperature, and stir them at 120 rpm for 3 h using a stirrer to obtain X-site anion precursor powder.
[0112] 3) Preparation of ligand precursor: 40.6 g of didecyl dimethyl ammonium bromide (DDAB) powder and 20 kg of PMMA powder were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain a ligand precursor powder.
[0113] 4) Preparation of seed crystals (perovskite quantum dots ABX3@first polymer matrix): set the extruder temperature to 80°C, 100°C, 120°C, 150°C, 150°C, and 110°C for six temperature control programs for preheating for 1 hour, and then use pure PMMA masterbatch to clean the machine screw for 1 hour; adjust the pump body parameters, set the pump body displacement to 10ml / rev, 1.51rpm / Hz, and frequency to 16Hz; weigh 5kg of A-site cation precursor powder, 5kg of B-site cation precursor powder, 10kg of X-site anion precursor powder, and 20kg of ligand precursor powder, mix them at room temperature, and use a stirrer to stir at 120rpm for 3h to obtain a mixture K; put the mixture K into the extruder feed port, extrude it at a rate of 250r / min at a high temperature platform of 150 to obtain CsPbBr3@PMMA seed crystals.
[0114] 5) Preparation of masterbatch (perovskite quantum dot ABX3@first polymer matrix@second polymer matrix): weigh 10 kg of the CsPbBr3@PMMA seed crystals obtained in the above step 4) and 2 kg of PVA powder and mix them at room temperature, use a stirrer to stir at 120 rpm for 3 hours to obtain a mixture M; set the extruder temperature to 80°C, 100°C, 130°C, 170°C, 170°C, and 120°C for six temperature control programs and preheat for 1 hour, then clean the machine screw with pure PVA masterbatch for 1 hour; adjust the pump body parameters, set the pump body displacement to 15 ml / rev, 1.37 rpm / Hz, and frequency to 20 Hz; put the mixture M into the extruder feed port, extrude it at 170°C and 370 r / min to obtain CsPbBr3@PMMA@PVA masterbatch.
[0115] 6) Preparation of a composite diffusion plate (perovskite quantum dot ABX3@first polymer matrix@second polymer matrix@third polymer matrix): weigh 10 kg of the CsPbBr3@PMMA@PVA masterbatch prepared in the above step 5), 4 kg of PVDF and 0.5 kg of diffusion particles SiO2, mix them at room temperature, and use a stirrer to stir at 120 rpm for 3 hours to obtain a mixture P; set the extruder temperature to 80°C, 100°C, 150°C, 150°C, 150°C, and 90°C for six temperature control programs for preheating for 1 hour, and then use pure PVDF powder to clean the machine screw for 1 hour; adjust the pump body parameters, set the pump body displacement to 13 ml / rev, 1.51 rpm / Hz, and frequency to 18 Hz; put the mixture P into the extruder feed port, and install a mold at the extrusion port, extrude at a temperature of 150 and a rate of 400 r / min to obtain a CsPbBr3@PMMA@PVA@PVDF green diffusion plate. The coating structure of the green diffuser plate prepared in Example 3 is as follows Figure 4 shown.
[0116] Example 4: CsPbI3@PMMA@PVA@PVDF red diffuser
[0117] 1) Preparation of cationic precursor: 41.6 g of cesium stearate powder and 20 kg of PMMA powder (obtained by crushing masterbatch) were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain A-site cationic precursor powder; 77.4 g of lead stearate powder and 20 kg of PMMA powder were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain B-site cationic precursor powder.
[0118] 2) Preparation of anion precursor: 31.9 g zinc iodide (ZnI2) powder and 20 kg PMMA powder were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain X-site anion precursor powder.
[0119] 3) Preparation of ligand precursor: 40.6 g of didecyl dimethyl ammonium bromide (DDAB) powder and 20 kg of PMMA powder were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain a ligand precursor powder.
[0120] 4) Preparation of seed crystals (perovskite quantum dots ABX3@first polymer matrix): set the extruder temperature to 80°C, 100°C, 120°C, 150°C, 150°C, and 110°C for six temperature control programs for preheating for 1 hour, and then use pure PMMA masterbatch to clean the machine screw for 1 hour; adjust the pump body parameters, set the pump body displacement to 10ml / rev, 1.51rpm / Hz, and frequency to 16Hz; weigh 5kg of A-site cation precursor powder, 5kg of B-site cation precursor powder, 10kg of X-site anion precursor powder, and 20kg of ligand precursor powder, mix them at room temperature, and use a stirrer to stir at 120rpm for 3h to obtain a mixture K; put the mixture K into the extruder feeding port, extrude it at a rate of 250r / min at a high temperature platform of 150 to obtain CsPbI3@PMMA seed crystals.
[0121] 5) Preparation of masterbatch (perovskite quantum dot ABX3@first polymer matrix@second polymer matrix): weigh 10 kg of the CsPbI3@PMMA seed crystals obtained in the above step 4) and 2 kg of PVA powder and mix them at room temperature, use a stirrer to stir at 120 rpm for 3 hours to obtain a mixture M; set the extruder temperature to 80°C, 100°C, 130°C, 170°C, 170°C, and 120°C for six temperature control programs and preheat for 1 hour, then clean the machine screw with pure PVA masterbatch for 1 hour; adjust the pump body parameters, set the pump body displacement to 15 ml / rev, 1.37 rpm / Hz, and frequency to 20 Hz; put the mixture M into the extruder feed port, extrude it at 170°C and 370 r / min to obtain CsPbI3@PMMA@PVA masterbatch.
[0122] 6) Preparation of a composite diffusion plate (perovskite quantum dot ABX3@first polymer matrix@second polymer matrix@third polymer matrix): weigh 10 kg of the CsPbI3@PMMA@PVA masterbatch prepared in the above step 5), 4 kg of PVDF and 0.5 kg of diffusion particles SiO2, mix them at room temperature, use a stirrer at a speed of 120 rpm for 3 hours to obtain a mixture P; set the extruder temperature to 80°C, 100°C, 150°C, 150°C, 150°C, 90°C for six temperature control programs for preheating for 1 hour, and then use pure PVDF powder to clean the machine screw for 1 hour; adjust the pump body parameters, set the pump body displacement to 13 ml / rev, 1.51 rpm / Hz, and frequency to 18 Hz; put the mixture P into the extruder feed port, and install a mold at the extrusion port, extrude at a temperature of 150 and a rate of 400 r / min to obtain a CsPbI3@PMMA@PVA@PVDF red diffusion plate. The coating structure of the red diffuser plate prepared in Example 4 is as follows Figure 5 shown.
[0123] Example 5: CsPbBr3@PS@EVOH@PVDF green diffusion plate
[0124] 1) Preparation of cationic precursor: Weigh 41.6 g of cesium stearate powder and 20 kg of PS powder (obtained by crushing masterbatch), mix them at room temperature, and stir them at 120 rpm for 3 h using a stirrer to obtain A-site cationic precursor powder; weigh 77.4 g of lead stearate powder and 20 kg of PS powder, mix them at room temperature, and stir them at 120 rpm for 3 h using a stirrer to obtain B-site cationic precursor powder.
[0125] 2) Preparation of anion precursor: Weigh 22.5 g zinc bromide (ZnBr2) powder and 20 kg PS powder and mix them at room temperature, and use a stirrer to stir at 120 rpm for 3 h to obtain X-site anion precursor powder.
[0126] 3) Preparation of ligand precursor: 40.6 g of didecyl dimethyl ammonium bromide (DDAB) powder and 20 kg of PS powder were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain a ligand precursor powder.
[0127] 4) Preparation of seed crystals (perovskite quantum dots ABX3@first polymer matrix): set the extruder temperature to 80°C, 100°C, 120°C, 150°C, 150°C, and 110°C for six temperature control programs for preheating for 1 hour, and then use pure PS masterbatch to clean the machine screw for 1 hour; adjust the pump body parameters, set the pump body displacement to 10ml / rev, 1.51rpm / Hz, and frequency to 16Hz; weigh 5kg of A-site cation precursor powder, 5kg of B-site cation precursor powder, 10kg of X-site anion precursor powder, and 20kg of ligand precursor powder, mix them at room temperature, and use a stirrer to stir at 120rpm for 3h to obtain a mixture K; put the mixture K into the extruder feeding port, extrude it at a rate of 250r / min at a high temperature platform of 150 to obtain CsPbBr3@PS seed crystals.
[0128] 5) Preparation of masterbatch (perovskite quantum dot ABX3@first polymer matrix@second polymer matrix): weigh 10 kg of the CsPbBr3@PS seed crystals obtained in the above step 4) and 2 kg of EVOH powder and mix them at room temperature, use a stirrer to stir at 120 rpm for 3 hours to obtain a mixture M; set the extruder temperature to 80°C, 100°C, 130°C, 170°C, 170°C, and 120°C for six temperature control programs and preheat for 1 hour, then clean the machine screw with pure EVOH masterbatch for 1 hour; adjust the pump body parameters, set the pump body displacement to 15 ml / rev, 1.37 rpm / Hz, and frequency to 20 Hz; put the mixture M into the extruder feed port, extrude it at 170°C and 370 r / min to obtain CsPbBr3@PS@EVOH masterbatch.
[0129] 6) Preparation of a composite diffusion plate (perovskite quantum dot ABX3@first polymer matrix@second polymer matrix@third polymer matrix): weigh 10 kg of the CsPbBr3@PS@EVOH masterbatch prepared in the above step 5), 4 kg of PVDF and 0.5 kg of diffusion particles SiO2, mix them at room temperature, use a stirrer at 120 rpm for 3 hours to obtain a mixture P; set the extruder temperature to 80°C, 100°C, 150°C, 150°C, 150°C, 90°C for six temperature control programs and preheat for 1 hour, then use pure PVDF powder to clean the machine screw for 1 hour; adjust the pump body parameters, set the pump body displacement to 13 ml / rev, 1.51 rpm / Hz, and frequency to 18 Hz; put the mixture P into the extruder feed port, and install a mold at the extrusion port, extrude at a temperature of 150 and a rate of 400 r / min to obtain a CsPbBr3@PS@EVOH@PVDF green diffusion plate. The coating structure of the green diffuser plate prepared in Example 5 is as follows Figure 6 shown.
[0130] Example 6: CsPbI3@PS@EVOH@PVDF red diffusion plate
[0131] 1) Preparation of cationic precursor: Weigh 41.6 g of cesium stearate powder and 20 kg of PS powder (obtained by crushing masterbatch), mix them at room temperature, and stir them at 120 rpm for 3 h using a stirrer to obtain A-site cationic precursor powder; weigh 77.4 g of lead stearate powder and 20 kg of PS powder, mix them at room temperature, and stir them at 120 rpm for 3 h using a stirrer to obtain B-site cationic precursor powder.
[0132] 2) Preparation of anion precursor: 31.9 g zinc iodide (ZnI2) powder and 20 kg PS powder were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain X-site anion precursor powder.
[0133] 3) Preparation of ligand precursor: 40.6 g of didecyl dimethyl ammonium bromide (DDAB) powder and 20 kg of PS powder were weighed and mixed at room temperature, and stirred at 120 rpm for 3 h using a stirrer to obtain a ligand precursor powder.
[0134] 4) Preparation of seed crystals (perovskite quantum dots ABX3@first polymer matrix): set the extruder temperature to 80°C, 100°C, 120°C, 150°C, 150°C, and 110°C for six temperature control programs for preheating for 1h, and then use pure PS masterbatch to clean the machine screw for 1h; adjust the pump body parameters, set the pump body displacement to 10ml / rev, 1.51rpm / Hz, and frequency to 16Hz; weigh 5kg of A-site cation precursor powder, 5kg of B-site cation precursor powder, 10kg of X-site anion precursor powder, and 20kg of ligand precursor powder, mix them at room temperature, and use a stirrer to stir at 120rpm for 3h to obtain a mixture K; put the mixture K into the extruder feed port, extrude it at a rate of 250r / min at a high temperature platform of 150 to obtain CsPbI3@PS seed crystals.
[0135] 5) Preparation of masterbatch (perovskite quantum dot ABX3@first polymer matrix@second polymer matrix): weigh 10 kg of the CsPbI3@PS seed crystals obtained in the above step 4) and 2 kg of EVOH powder, mix them at room temperature, use a stirrer at 120 rpm for 3 hours to obtain a mixture M; set the extruder temperature to 80°C, 100°C, 130°C, 170°C, 170°C, and 120°C for six temperature control programs and preheat for 1 hour, then clean the machine screw with pure EVOH masterbatch for 1 hour; adjust the pump body parameters, set the pump body displacement to 15 ml / rev, 1.37 rpm / Hz, and frequency to 20 Hz; put the mixture M into the extruder feed port, extrude it at 170°C and 370 r / min to obtain CsPbI3@PS@EVOH masterbatch.
[0136] 6) Prepare a composite diffusion plate (perovskite quantum dot ABX3@first polymer matrix@second polymer matrix@third polymer matrix): weigh 10kg of the CsPbI3@PS@EVOH masterbatch prepared in the above step 5), 4kg of PVDF and 0.5kg of diffusion particles SiO2, mix them at room temperature, use a stirrer at a speed of 120rpm for 3h to obtain a mixture P; set the extruder temperature to 80℃, 100℃, 150℃, 150℃, 150℃, 90℃ for six temperature control programs to preheat for 1h, and then clean the machine screw with pure PVDF powder for 1h; adjust the pump body parameters, set the pump body displacement to 13ml / rev, 1.51rpm / Hz, and frequency to 18Hz; put the mixture P into the extruder feed port, install the mold at the extrusion port, extrude at a temperature of 150 and a rate of 400r / min to obtain a CsPbI3@PS@EVOH@PVDF red diffusion plate. The coating structure of the red diffusion plate prepared in Example 6 is as follows: Figure 7 shown.
[0137] The luminous performance of the diffuser plate prepared in the above embodiment was tested, as shown in the following table.
[0138]
[0139]
[0140] a The test conditions are: temperature 65 degrees, humidity 95%, 1000h;
[0141] b The test conditions are: temperature 45 degrees, humidity 95%, light intensity 38W / m 2 (450nm), 1000h.
[0142] The above are only several embodiments of the present application, and do not limit the present application in any form. Although the present application discloses the preferred embodiments as above, these embodiments are not used to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases, and all belong to the scope of the technical solution of the present application.
Claims
1. A composite diffuser based on perovskite quantum dots, characterized in that: include: matrix and Perovskite quantum dots and diffused particles distributed in the matrix, Wherein, the chemical formula of the perovskite quantum dot is ABX3, A and B represent cations, and X represents anions; The surface of the perovskite quantum dots is modified by ligands, and is coated with a first polymer, a second polymer and a third polymer in sequence from the inside to the outside; The matrix is melt-formed from the first polymer, the second polymer, and the third polymer.
2. The composite diffuser plate according to claim 1, characterized in that: The first polymer is selected from at least one of PMMA, PS, PC, MS, PET, PP, PE, and PAN; Preferably, the second polymer is selected from at least one of EVOH, PVA, and PVDC; Preferably, the third polymer is selected from at least one of PVDF, PEG, PAM, POM, PVP, PES, SEBS, SMA, and PEEK.
3. The composite diffuser plate according to claim 1, characterized in that: The cation A is selected from Cs + 、MA + , FA + At least one of the cations B is selected from Pb 2+ Sn 2+ At least one of the anions X is selected from Cl - Br - ,I - At least one of; Preferably, the perovskite quantum dots are selected from at least one of CsPbCl3, MAPbCl3, FAPbCl3, CsPbBr3, MAPbBr3, FAPbBr3, CsPbI3, MAPbI3, FAPbI3, CsSnI3, MASnI3, and FASnI3.
4. The composite diffuser plate according to claim 1, characterized in that: The diffusion particles are selected from at least one of nano-SiO2 particles, nano-TiO2 particles, nano-BaSO4 particles, nano-CaCO3 particles, and PMMA microspheres; Preferably, the ligand is selected from at least one of DDAB, PEABr, TOPO, DMA, OPA, TBABr, TBACl, IDA, TPP, ODPA, BA, and CA.
5. The composite diffuser plate according to claim 1, characterized in that: The thickness of the coating layer of the first polymer is 2-20 μm; Preferably, the thickness of the coating layer of the second polymer is 5-30 μm; Preferably, the coating layer of the third polymer has a thickness of 5-30 μm.
6. A method for preparing a composite diffuser plate according to any one of claims 1 to 5, characterized in that: include: a) respectively mixing the salt corresponding to the cation A, the salt corresponding to the cation B, the salt corresponding to the anion X and the ligand with the first polymer to prepare an A-site cation precursor, a B-site cation precursor, an anion precursor and a ligand precursor; b) mixing the A-site cation precursor, the B-site cation precursor, the anion precursor and the ligand precursor, and extruding to obtain seed crystals; c) mixing the seed crystals with the second polymer and extruding to obtain a masterbatch; d) mixing the master batch with the third polymer and the diffusion particles, extruding, and in-situ producing the composite diffusion plate after demoulding.
7. The method according to claim 6, characterized in that In step a), the salt corresponding to the cation A is selected from at least one of stearate, tungstate, molybdate, carbonate, and bicarbonate, the salt corresponding to the cation B is selected from at least one of stearate, tungstate, molybdate, carbonate, and bicarbonate, and the salt corresponding to the anion X is selected from metal halides; Preferably, the mass ratio of the salt corresponding to the cation A to the first polymer is 1:2000 to 50:2000; Preferably, the mass ratio of the salt corresponding to the cation B to the first polymer is 1:2000 to 80:2000; Preferably, the mass ratio of the salt corresponding to the anion X to the first polymer is 1:2000 to 40:2000; Preferably, the mass ratio of the ligand to the first polymer is 1:2000 to 30:2000.
8. The method according to claim 6, characterized in that In step b), the A-site cation precursor, the B-site cation precursor, and the anion precursor are mixed so that the molar ratio of the salt corresponding to the cation B to the salt corresponding to the cation A is 1:1 to 2:1; and the molar ratio of the salt corresponding to the anion X to the salt corresponding to the cation A is 1:1 to 5:1; Preferably, the A-site cation precursor is mixed with the ligand precursor so that the molar ratio of the salt corresponding to the cation A to the ligand is 1:1 to 1:5; Preferably, the extrusion temperature is 150-250°C; Preferably, the extrusion rate is 100 r / min to 800 r / min.
9. The method according to claim 6, characterized in that In step c), the mass ratio of the seed crystal to the second polymer is 10:2 to 10:5; Preferably, the extrusion temperature is 150-250°C; Preferably, the extrusion rate is 100 r / min to 800 r / min.
10. The method according to claim 6, characterized in that In step d), the mass ratio of the masterbatch to the third polymer is 10:2 to 10:5; The mass ratio of the masterbatch to the diffusion particles is 10:0.1 to 10:0.8; Preferably, the extrusion temperature is 150-250°C; Preferably, the extrusion rate is 100r / min to 800r / min; Preferably, the mixing further comprises adding an auxiliary agent, and the auxiliary agent is selected from at least one of nano-SiO2 particles, nano-TiO2 particles, nano-BaSO4 particles, nano-CaCO3 particles, and PMMA microspheres.
Citation Information
Patent Citations
Perovskite quantum dot composite film and preparation method thereof
CN110804233A
Perovskite quantum dot composite light diffusant and preparation method and application thereof
CN115197517A
Perovskite quantum dot diffusion plate and preparation method thereof
CN115637149A
Perovskite quantum dot-based light emitting structure and backlight module
CN211826818U
Method for preparing quantum dot composite material
WO2023024379A1