Optical laminate and image display device using the same
By designing a retardation layer structure including a polarizer, a first liquid crystal orientation fixing layer and a second liquid crystal orientation fixing layer in the optical laminate, and adjusting the display uneven parameters by adjusting the refractive index and thickness of the adhesive layer, the liquid crystal orientation fixing is solved The display uneven problem caused by the layer enables a more uniform image display.
Patent Information
- Application Number
- CN202410695104.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
In an image display device using the optical laminate using the liquid crystal orientation fixing layer as the retardation layer, there may be a problem of uneven display, especially when a pink thin line is observed in the absorption axis direction of the polarizer.
By designing a retardation layer structure including a polarizer, a first liquid crystal orientation fixing layer and a second liquid crystal orientation fixing layer in the optical laminate, the display uneven parameters are adjusted by using the refractive index and thickness of the adhesive layer to ensure that the display is not The average parameter is less than or equal to 3.0. The specific implementation method includes using a pressure-sensitive adhesive or adhesive to optimize the refractive index and thickness of the liquid crystal orientation fixing layer.
The display uneven problem that occurs in the image display device is effectively suppressed, especially in reflection under the three-wavelength light source, which significantly reduces the pink thin line phenomenon in the absorption axis direction of the polarizer and improves the display uniformity.
Smart Images

Figure CN119065045A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical laminate and an image display device using the optical laminate. Background Art
[0002] In recent years, image display devices typified by liquid crystal display devices and electroluminescent (EL) display devices (e.g., organic EL display devices or inorganic EL display devices) have rapidly gained wider applications. In an image display device, an optical laminate including a retardation film (e.g., an antireflection film obtained by integrating a polarizing plate and a retardation film with each other) has been used in many cases. In recent years, with an increase in the demand for thinning of image display devices, the demand for thinning of optical laminates has also increased. In order to thin the optical laminate, progress has been made in thinning a retardation layer (retardation film) that contributes greatly to the thickness. A typical example of a thin retardation film is a film obtained by aligning a liquid crystal compound and fixing the alignment state (hereinafter referred to as “liquid crystal film”). The liquid crystal compound has a much larger birefringence (Δn) than a resin, and thus the thickness of the liquid crystal film used to obtain a desired in-plane retardation can be much smaller than the thickness of a stretched film of a resin film. However, in an image display device using an optical laminate including a liquid crystal film, display unevenness may occur depending on the observation environment (specifically, a phenomenon in which a thin pink line is particularly obvious when observed in the absorption axis direction of a polarizer). Summary of the Invention
[0003] The present invention has been made to solve the above-described conventional problems, and a main object thereof is to provide an optical laminate having a liquid crystal alignment fixing layer that can suppress specific display unevenness when applied to an image display device.
[0004] [1] According to at least one embodiment of the present invention, there is provided an optical laminate including: a polarizing plate including a polarizer; and a retardation layer. The retardation layer includes a first liquid crystal alignment fixing layer and a second liquid crystal alignment fixing layer laminated on the first liquid crystal alignment fixing layer via an adhesive layer in this order from the polarizer side. The retardation layer as a whole has one of a circular polarization function and an elliptical polarization function, and has a relationship of Re(450) < Re(550) < Re(650). The refractive index n LC1 of the first liquid crystal alignment fixing layer, the refractive index n LC2 of the second liquid crystal alignment fixing layer, the refractive index n AD of the adhesive layer, the thickness T AD of the adhesive layer, and the thickness change amount TV AD satisfy the following formula (1).
[0005] |{(n LC1 + n LC2 ) / 2 – n AD}| × (TV AD / T AD )×1,000≤3.0 (1)
[0006] [2] In the above item [1], the adhesive layer is formed of a pressure-sensitive adhesive.
[0007] [3] In the above clause [2], the thickness of the adhesive layer T AD 4μm or larger.
[0008] [4] In the above item [1], the adhesive layer is formed by an adhesive.
[0009] [5] In any of the above items [1] to [4], the refractive index n of the adhesive layer is AD 1.54 or greater.
[0010] [6] In any one of the above items [1] to [5], the thickness of the first liquid crystal alignment fixing layer is 1.7 μm or less.
[0011] [7] According to at least one embodiment of the present invention, there is provided an image display device comprising the optical laminate according to any one of the above items [1] to [6].
[0012] According to at least one embodiment of the present invention, an optical laminate including a liquid crystal alignment fixing layer and capable of suppressing specific display unevenness when applied to an image display device can be realized.
[0013] Instruction Manual
[0014] Figure 1 is a schematic cross-sectional view of an optical stack according to at least one embodiment of the present invention. DETAILED DESCRIPTION
[0015] Typical embodiments of the present invention are described below. However, the present invention is not limited to these embodiments.
[0016] (Definition of terms and symbols)
[0017] Definitions of terms and symbols used herein are as follows.
[0018] (1) Refractive index (nx, ny and nz)
[0019] “nx” represents the refractive index in the direction of maximum in-plane refractive index (i.e., slow axis direction), “ny” represents the refractive index in the direction perpendicular to the slow axis in the plane (i.e., fast axis direction), and “nz” represents the refractive index in the thickness direction.
[0020] (2) In-plane retardation (Re)
[0021] “Re(λ)” refers to the in-plane retardation of a film measured with light having a wavelength of λ nm at 23° C. For example, “Re(550)” refers to the in-plane retardation of a film measured with light having a wavelength of 550 nm at 23° C. When the thickness of the film is represented by d (nm), Re(λ) is determined by the equation “Re=(nx−ny)×d”.
[0022] (3) Thickness direction retardation (Rth)
[0023] “Rth(λ)” refers to the retardation in the thickness direction of the film measured at 23° C. with light having a wavelength of λ nm. For example, “Rth(550)” refers to the retardation in the thickness direction of the film measured at 23° C. with light having a wavelength of 550 nm. When the thickness of the film is represented by d (nm), Rth(λ) is determined by the equation “Rth=(nx−nz)×d”.
[0024] (4) Nz coefficient
[0025] The Nz coefficient is determined from the equation "Nz = Rth / Re".
[0026] (5) Angle
[0027] When an angle is mentioned herein, the angle encompasses angles in both the clockwise and counterclockwise directions unless otherwise specified.
[0028] A. Optical laminates
[0029] Figure 1 is a schematic cross-sectional view of an optical stack according to at least one embodiment of the present invention. The optical stack 100 of the example shown includes a polarizing plate 10 and a delay layer 20. The polarizing plate 10 and the delay layer 20 are stacked by any suitable adhesive layer (e.g., an adhesive layer or a pressure-sensitive adhesive layer: not shown). The polarizing plate 10 generally includes a polarizer 11 and protective layers 12 and 13 disposed on both sides of the polarizer 11. Depending on the purpose, at least one of the protective layers 12 and 13 may be omitted. Therefore, the polarizing plate may be a so-called double-sided protected polarizing plate or a so-called single-sided protected polarizing plate, or may be formed by a polarizer alone.
[0030] The retardation layer 20 includes, in order from the polarizing plate 10 side, a first liquid crystal alignment fixing layer 21 and a second liquid crystal alignment fixing layer 22 laminated on the first liquid crystal alignment fixing layer 21 via an adhesive layer 25. When a liquid crystal alignment fixing layer is used as a retardation layer, a desired in-plane retardation can be achieved with a thickness much smaller than that of a stretched film of a resin film. As a result, significant thinning of the optical laminate can be achieved. The retardation layer 20 as a whole has one of a circular polarization function or an elliptical polarization function, and has a relationship of Re(450) < Re(550) < Re(650) (as a laminate of the first liquid crystal alignment fixing layer 21 and the second liquid crystal alignment fixing layer 22). In at least one embodiment of the present invention, the retardation layer as a whole can have, for example, an Nz coefficient of from 0.30 to 0.70. As used herein, the term "liquid crystal alignment fixing layer" refers to a layer in which a liquid crystal compound is aligned in a predetermined direction and whose alignment state is fixed. The term "liquid crystal alignment fixing layer" is a concept that encompasses an alignment fixing layer obtained by curing a liquid crystal monomer.
[0031] In at least one embodiment of the present invention, the refractive index n of the first liquid crystal alignment fixing layer LC1 , the refractive index n of the second liquid crystal alignment fixing layer LC2 and the refractive index n of the adhesive layer AD and the thickness T of the adhesive layer AD and the thickness variation amount TV AD satisfy the following formula (1). The left side of formula (1) is sometimes referred to as the "display unevenness parameter". In addition, unless otherwise specified, the term "refractive index" of the liquid crystal alignment fixing layer as used herein refers to the refractive index in the transmission axis direction of the polarizer. The adhesive layer is substantially optically isotropic, and thus the refractive index n AD is also isotropic.
[0032] |{(n LC1 + n LC2 ) / 2 – n AD}| × (TV AD / T AD ) × 1,000 ≤ 3.0 (1)
[0033] The display unevenness parameter is preferably 2.5 or less, more preferably 2.0 or less, still more preferably 1.8 or less, particularly preferably 1.2 or less, and especially preferably 0.7 or less. The display unevenness parameter (absolute value) is preferably as small as possible and can be, for example, 0.0.
[0034] The inventors of the present invention have discovered the following new problem while studying the further thinning of an optical stack including a liquid crystal orientation fixing layer as a delay layer: Depending on the observation environment, specific display unevenness may occur in an image display device using an optical stack including a liquid crystal orientation fixing layer as a delay layer. Specifically, the inventors have found that in the reflection under a three-wavelength light source, a phenomenon in which particularly obvious thin lines of pink (sometimes referred to as "linear unevenness") are observed in the entire absorption axis direction of the polarizer may occur. In addition, the inventors of the present invention have conducted extensive research on the suppression of such linear unevenness, and found that linear unevenness can be suppressed by suppressing the interference of the optical stack. In addition, the inventors of the present invention have found that by setting the above-mentioned display unevenness parameters to a predetermined value or less, rather than separately adjusting, for example, the refractive index or thickness of the constituent layers of the optical stack to suppress the interference of the optical stack, the linear unevenness can be comprehensively suppressed in the specific structure of the optical stack according to, for example, the purpose and / or the constituent materials, thereby completing the present invention. That is, this effect according to the embodiment of the present invention solves the problem newly discovered in the study of further thinning of an optical stack including a liquid crystal orientation fixing layer as a delay layer, and is an unexpectedly excellent effect. It goes without saying that at least one embodiment of the present invention can suppress display unevenness that has been recognized so far.
[0035] As long as the effect according to the embodiment of the present invention is obtained (specifically, as long as the above-mentioned display unevenness parameter can be set to a predetermined value or less), any suitable configuration can be adopted as the adhesive layer 25. For example, the adhesive layer can be formed of a pressure-sensitive adhesive or can be formed of an adhesive. When the adhesive layer is formed of a pressure-sensitive adhesive, its thickness can be increased, so the display unevenness parameter can be easily adjusted to a desired value. In this case, the thickness T of the adhesive layer AD For example, it may be 4 μm or more, or, for example, it may be 5 μm or more. When the adhesive layer is formed of an adhesive, the display unevenness parameter can be adjusted to a desired value with an extremely small thickness. Regardless of whether the adhesive layer is an adhesive layer or a pressure-sensitive adhesive layer, the refractive index n of the adhesive layer AD When the refractive index of the adhesive layer falls within this range, it is easy to adjust the display unevenness parameter to a predetermined value or less.
[0036] In the optical stack, the total thickness of the first liquid crystal orientation fixing layer and the second liquid crystal orientation fixing layer is preferably 20 μm or less, more preferably from 3 μm to 10 μm. According to at least one embodiment of the present invention, the problem of newly discovered linear non-uniformity in an optical stack including an extremely thin liquid crystal orientation fixing layer can be solved. When the total thickness from the first liquid crystal orientation fixing layer to the second liquid crystal orientation fixing layer falls within the above range, the total thickness from the polarizing plate to the second liquid crystal orientation fixing layer (the basic total thickness of the optical stack, excluding the thickness of the pressure-sensitive adhesive used to bond to the image display panel) can be, for example, 100 μm or less, or, for example, can be 30 μm to 80 μm.
[0037] In actual use, the optical laminate includes a pressure-sensitive adhesive layer (not shown) as the outermost layer on the second liquid crystal orientation fixing layer side (image display panel side) so as to be bonded to the image display panel. In this case, it is preferred to temporarily bond a release liner to the surface of the pressure-sensitive adhesive layer until the optical laminate is used. When the release liner is temporarily bonded, the pressure-sensitive adhesive layer can be protected, and the optical laminate can be formed into a roll shape.
[0038] The constituent elements of the optical stack are described in detail below.
[0039] B. Polarizing plate
[0040] B-1. Polarizer
[0041] The polarizing plate 11 is generally formed of a polyvinyl alcohol (PVA)-based resin film containing a dichroic substance such as iodine. Examples of the PVA-based resin include polyvinyl alcohol, partially formalized polyvinyl alcohol, ethylene-vinyl alcohol copolymer, and partially saponified products based on ethylene-vinyl acetate copolymer.
[0042] The PVA-based resin preferably contains an acetoacetyl-modified PVA-based resin. Utilizing this structure, a polaroid with desired mechanical strength can be obtained. When the total amount of the PVA-based resin is defined as 100 wt %, the blending amount of the acetoacetyl-modified PVA-based resin is preferably 5 wt % to 20 wt %, more preferably 8 wt % to 12 wt %. When the blending amount falls within such a range, a polaroid with more excellent mechanical strength is obtained.
[0043] The polarizer preferably contains iodide or sodium chloride (sometimes collectively referred to as "halide"). Examples of iodide include potassium iodide, sodium iodide and lithium iodide. The content of halide in the polarizer is preferably from 5 to 20 parts by weight, more preferably from 10 to 15 parts by weight, relative to 100 parts by weight of PVA-based resin. In the production method described later, the halide is blended into a coating liquid for forming a PVA-based resin layer used as a precursor of the polarizer, and can be finally introduced into the polarizer. When the halide is introduced into the polarizer, the orientation properties of the PVA molecules in the polarizer can be improved, so a polarizer with excellent optical properties (usually, high polarization degree and high single-layer transmittance are obtained at the same time) can be obtained.
[0044] The polarizer preferably exhibits absorption dichroism at any wavelength within the wavelength range of 380nm to 780nm. The single-layer transmittance of the polarizer is preferably from 41.0% to 46.0%, more preferably from 42.0% to 45.0%. The polarization degree of the polarizer is preferably 97.0% or greater, more preferably 99.0% or greater, and even more preferably 99.9% or greater. According to at least one embodiment of the present invention, even when the single-layer transmittance falls within the above range, the polarization degree can be maintained within such a range.
[0045] The thickness of the polarizer is, for example, 12 μm or less, preferably 10 μm or less, more preferably 1 μm to 8 μm, and even more preferably 3 μm to 7 μm. The combination of such a thin polarizer and a liquid crystal orientation fixing layer allows the optical laminate to be significantly thinned. In addition, when the thickness of the polarizer falls within the above range, its curling when heated can be satisfactorily suppressed, and its satisfactory appearance durability when heated can be obtained.
[0046] The polarizing plate may be manufactured by any appropriate method. For example, the resin film used to form the polarizing plate may be a single-layer resin film or may be a laminate of two or more layers.
[0047] Specific examples of polarizers formed from a single-layer resin film include hydrophilic polymer films, such as PVA-based films; partially formalized PVA-based films and partially saponified films based on ethylene-vinyl acetate copolymers, which have been dyed and stretched with a dichroic substance such as iodine or a dichroic dye; and polyene-based oriented films, such as a dehydrated product of PVA and a dehydrochlorinated product of polyvinyl chloride. It is preferred to use a polarizer obtained by dyeing and uniaxially stretching a PVA-based film with iodine because such a polarizer has excellent optical properties.
[0048] For example, iodine dyeing is carried out by immersing the film based on PVA in an aqueous solution of iodine. The stretching ratio of uniaxial stretching is preferably 3 times to 7 times. Stretching can be carried out after dyeing, or can be carried out while dyeing. In addition, dyeing can be carried out after stretching. As required, swelling treatment, cross-linking treatment, washing treatment, drying treatment, etc. are carried out to the film based on PVA. For example, when washing the film based on PVA with water by immersing it in water before dyeing, not only pollutants and anti-blocking agents on the film surface based on PVA can be washed off, but also the film based on PVA can be swollen to prevent uneven dyeing.
[0049] A specific example of a polarizer obtained by using a laminate is a laminate using a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate or a polarizer obtained by applying a resin substrate and a laminate based on a PVA-based resin layer formed on a resin substrate. The polarizer obtained by using a resin substrate and a laminate based on a PVA-based resin layer formed by coating on a resin substrate can be produced by, for example, the following methods: a PVA-based resin solution is applied to a resin substrate; a solution is dried to form a PVA-based resin layer on a resin substrate, thereby providing a resin substrate and a laminate based on a PVA-based resin layer; and a laminate is stretched and dyed to convert a PVA-based resin layer into a polarizer. In this embodiment, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is preferably formed on one side of the resin substrate. Stretching generally includes stretching the laminate in a state where the laminate is immersed in a boric acid aqueous solution. In addition, stretching may further include stretching the laminate in air at a high temperature (e.g., 95°C or higher) before stretching in a boric acid aqueous solution as required. In addition, in this embodiment, the laminate is preferably subjected to a drying shrinkage treatment, which includes heating the laminate while conveying the laminate in its length direction to shrink the laminate by 2% or more in its width direction. The production method of this embodiment generally includes subjecting the laminate to an auxiliary stretching treatment in air, a dyeing treatment, an underwater stretching treatment and a drying shrinkage treatment in the order described. When the auxiliary stretching is introduced, the crystallinity of the PVA can be improved even when the PVA is applied to the thermoplastic resin, and thus high optical properties can be achieved. In addition, when the orientation properties of the PVA are improved in advance while improving the crystallinity, when the laminate is immersed in water in a subsequent dyeing step or a stretching step, problems such as a decrease in the orientation properties of the PVA and its dissolution can be prevented, and thus high optical properties can be achieved. In addition, in the case where the PVA-based resin layer is immersed in a liquid, the interference with the orientation of the polyvinyl alcohol molecules and the decrease in their orientation properties can be suppressed compared to the case where the PVA-based resin does not contain any halide. Therefore, the optical properties of the obtained polarizer can be improved by a treatment step such as a dyeing treatment and an underwater stretching treatment in which the laminate is immersed in a liquid. In addition, shrinking the laminate in its width direction by drying and shrinking treatment can improve optical properties. The laminate of the obtained resin substrate and polarizer can be used as it is (that is, the resin substrate can be used as a protective layer of the polarizer), or can be laminated on the peeling surface of the resin substrate from the laminate of the resin substrate and polarizer, or laminated on the surface on the opposite side of the peeling surface according to the purpose. Details about this method of producing polarizers are described in, for example, Japanese Patent Application Publication No. 2012-73580 and Japanese Patent No. 6470455, and their descriptions are incorporated herein by reference in their entirety.
[0050] B-2. Protective layer
[0051] The protective layers 12 and 13 are each formed of any appropriate resin film. The material used to form the resin film is, for example, typically a cellulose-based resin (e.g., triacetyl cellulose (TAC)), a cycloolefin-based resin (e.g., polynorbornene), a (meth) acrylic resin, a polyester-based resin such as polyethylene terephthalate (PET) or polyethylene naphthalate (PEN), a polyolefin-based resin such as polyethylene, or a polycarbonate-based resin. A typical example of a (meth) acrylic resin is a (meth) acrylic resin having a lactone ring structure. The (meth) acrylic resin having a lactone ring structure is described in, for example, Japanese Patent Application Publication No. 2000-230016, Japanese Patent Application Publication No. 2001-151814, Japanese Patent Application Publication No. 2002-120326, Japanese Patent Application Publication No. 2002-254544, and Japanese Patent Application Publication No. 2005-146084, which are incorporated herein by reference. Among them, cellulose-based resins are preferred, and TAC is more preferred, from the viewpoint of, for example, easy processing into an irregular shape. Cycloolefin-based resins and (meth)acrylic resins are preferred from the viewpoint of obtaining a polarizing plate having low moisture permeability and excellent durability.
[0052] The optical stack is usually arranged on the observer side of the image display device, and the protective layer 12 is usually arranged on the observer side thereof. Therefore, the protective layer 12 can be surface-treated as needed. Examples of surface treatment include hard coating treatment, anti-reflection treatment, anti-sticking treatment, and anti-glare treatment. In addition / alternatively, when viewed through a pair of polarized sunglasses (usually imparting circular (elliptical) polarization function or imparting ultra-high delay), the protective layer 12 can be treated as needed to improve observability. When such treatment is performed, excellent observability can be achieved even when observing the display screen through a polarized lens such as a pair of polarized sunglasses. Therefore, the optical stack can even be suitably applied to image display devices that can be used outdoors.
[0053] In at least one embodiment of the present invention, the protective layer 13 is preferably optically isotropic. As used herein, the phrase "optically isotropic" means that the layer has an in-plane retardation Re(550) of 0nm to 10nm and a thickness direction retardation Rth(550) of -10nm to +10nm.
[0054] The thickness of each of the protective layers 12 and 13 is preferably 10 to 80 μm, more preferably 12 to 40 μm, and still more preferably 15 to 35 μm. When the protective layer 12 is subjected to surface treatment, the thickness of the protective layer 12 is a thickness including the thickness of its surface treatment layer.
[0055] C. Delay layer
[0056] As described above, the delay layer 20 includes a first liquid crystal alignment fixing layer 21 and a second liquid crystal alignment fixing layer 22 in this order starting from the polarizing plate side. Further, as described above, the delay layer 20 as a whole has one of a circular polarization function or an elliptical polarization function, and has a relationship of Re(450) < Re(550) < Re(650) (as a laminate of the first liquid crystal alignment fixing layer 21 and the second liquid crystal alignment fixing layer 22). Regarding the description of the delay layer in this section, when the delay layer is simply referred to as the "delay layer", the entire delay layer is described, and when the delay layer is simply referred to as the "liquid crystal alignment fixing layer", the first liquid crystal alignment fixing layer and the second liquid crystal alignment fixing layer are described together.
[0057] The Re(550) of the delay layer 20 is preferably from 100 nm to 200 nm, more preferably from 110 nm to 180 nm, still more preferably from 120 nm to 170 nm, and particularly preferably from 130 nm to 150 nm. When the Re(550) of the delay layer falls within such a range, the delay layer can exhibit a satisfactory circular polarization function or elliptical polarization function in combination with a polarizer.
[0058] The delay layer 20 has a relationship of Re(450) < Re(550) < Re(650). That is, the delay layer 20 preferably exhibits such a reverse wavelength dispersion dependence that its retardation value increases as the wavelength of the measurement light increases. With this structure, a satisfactory antireflection function can be achieved in an extremely wide wavelength band. The ratio "Re(450) / Re(550)" is, for example, greater than 0.5 and less than 1.0, preferably from 0.7 to 0.95, more preferably from 0.75 to 0.92, and still more preferably from 0.8 to 0.9. The ratio "Re(650) / Re(550)" is preferably 1.0 or greater and less than 1.15, more preferably from 1.03 to 1.1.
[0059] In at least one embodiment of the present invention, the delay layer 20 may have an Nz coefficient of, for example, 0.30 to 0.70 as described above. Therefore, the delay layer 20 exhibits a refractive index characteristic of nx > nz > ny. With this structure, reflection in the tilt direction can be satisfactorily prevented, and an antireflection function can be exhibited at a wide viewing angle. The Nz coefficient is preferably from 0.35 to 0.65, more preferably from 0.40 to 0.60, and still more preferably from 0.45 to 0.55.
[0060] Examples of liquid crystal compounds for liquid crystal orientation fixed layers include liquid crystal polymers and liquid crystal monomers. Liquid crystal compounds are preferably polymerizable (i.e., liquid crystal monomers). When liquid crystal compounds are polymerizable, the orientation state of the molecules of the liquid crystal compounds can be fixed by orienting the molecules of the liquid crystal compounds and then polymerizing the compounds. In this case, the polymer formed by polymerization is non-liquid crystal. Therefore, the formed liquid crystal orientation fixed layer does not experience, for example, a transition to a liquid crystal phase, a glass phase, or a crystalline phase caused by temperature changes, which is peculiar to liquid crystal compounds. As a result, the liquid crystal orientation fixed layer becomes a delay layer with excellent stability and is not affected by temperature changes.
[0061] In at least one embodiment of the present invention, the liquid crystal orientation fixing layer can be formed by using a composition containing a polymerizable liquid crystal compound (polymerizable liquid crystal compound, i.e., liquid crystal monomer). Herein, the "polymerizable liquid crystal compound" in the composition refers to a compound having a polymerizable group and having liquid crystal properties. A polymerizable group refers to a group that participates in a polymerization reaction, and is preferably a photopolymerizable group. Herein, a "photopolymerizable group" refers to a group that can participate in a polymerization reaction by, for example, an active free radical or acid generated by a photopolymerization initiator. For example, as described in Japanese Patent Translation Publication No. 2002-533742 (WO 00 / 37585A1), European Patent No. 358208 (US Patent No. 5,211,877), European Patent No. 66137 (US Patent No. 4,388,453), WO 93 / 22397A1, European Patent Application Publication No. 0261712, German Patent Application Publication No. 19504224, German Patent Application Publication No. 4408171, British Patent No. 2280445, etc., each can be used as a liquid crystal monomer. Specific examples of such polymerizable mesogen compounds include products available from BASF SE under the product name LC242, products available from Merck KGaA under the product name E7, and products available from Wacker Chemie AG under the product name LC-Sillicon-CC3767.
[0062] The mechanism of expression of the liquid crystal properties of the liquid crystal compound may be thermotropic or lyotropic. In addition, the structure of the liquid crystal phase may be nematic liquid crystal or smectic liquid crystal. From the viewpoint of easy production, nematic liquid crystal having thermotropic liquid crystal properties is preferred.
[0063] The temperature range in which the liquid crystal monomer exhibits liquid crystallinity varies depending on the type thereof. Specifically, the temperature range is preferably 40°C to 120°C, more preferably 50°C to 100°C, and most preferably 60°C to 90°C.
[0064] The birefringence Δn of the liquid crystal orientation fixing layer is preferably 0.06 or greater, more preferably 0.08 or greater, further preferably 0.09 or greater, and particularly preferably 0.10 or greater. The upper limit of Δn may be, for example, 0.13, or, for example, 0.12. When Δn falls within such a range, the desired in-plane delay can be achieved with an extremely small thickness. As a result, the thickness of each of the liquid crystal orientation fixing layer and the optical stack can be further reduced, and thus can ultimately contribute to the significant thinning of the image display device.
[0065] The liquid crystal orientation fixed layer may exhibit such a reverse wavelength dispersion characteristic, i.e., its retardation value increases with an increase in the wavelength of the measuring light, such a positive wavelength dispersion characteristic, i.e., the retardation value decreases with an increase in the wavelength of the measuring light, or such a flat wavelength dispersion characteristic, i.e., the retardation value remains substantially unchanged even when the wavelength of the measuring light changes.
[0066] The first liquid crystal orientation fixing layer 21 can generally be used as a λ / 2 plate, and the second liquid crystal orientation fixing layer 22 can generally be used as a λ / 4 plate. Specifically, the first liquid crystal orientation fixing layer has a Re (550) preferably from 150nm to 300nm, more preferably from 200nm to 270nm, and more preferably from 220nm to 260nm, and the second liquid crystal orientation fixing layer has a Re (550) preferably from 100nm to 200nm, more preferably from 110nm to 160nm, and more preferably from 120nm to 140nm. The thickness of the first liquid crystal orientation fixing layer can be adjusted so that the in-plane delay of the desired λ / 2 plate can be obtained. In at least one embodiment of the present invention, the thickness of the first liquid crystal orientation fixing layer can be, for example, from 2.0μm to 4.0μm. In at least one embodiment of the present invention, the thickness of the first liquid crystal orientation fixing layer is preferably 1.7μm or less, more preferably 1.6μm or less, and more preferably 1.5μm or less. In this case, the thickness of the first liquid crystal orientation fixing layer can be, for example, 1.3μm or more. As described above, according to at least one embodiment of the present invention, linear unevenness can be suppressed while making the thickness of the first liquid crystal orientation fixing layer thinner than that of the prior art. The thickness of the second liquid crystal orientation fixing layer can be adjusted so that the desired in-plane delay of the λ / 4 plate can be obtained. Specifically, the thickness of the layer can be, for example, from 0.8 μm to 2.5 μm. The angle formed by the slow axis of the first liquid crystal orientation fixing layer and the transmission axis of the polarizer is preferably from 10° to 20°, more preferably from 12° to 18°, and more preferably from 14° to 16°, and the angle formed by the slow axis of the second liquid crystal orientation fixing layer and the transmission axis of the polarizer is preferably from 70° to 80°, more preferably from 72° to 78°, and more preferably from 74° to 76°. The arrangement order of the first liquid crystal orientation fixing layer and the second liquid crystal orientation fixing layer can be reversed, and the angle formed by the slow axis of the first liquid crystal orientation fixing layer and the transmission axis of the polarizer and the angle formed by the slow axis of the second liquid crystal orientation fixing layer and the transmission axis of the polarizer can be reversed.
[0067] The refractive index of the liquid crystal alignment fixing layer may vary depending on the composition used to form the liquid crystal alignment fixing layer (basically, the type of liquid crystal compound, and the type, amount, combination, blending amount, etc. of additives). LC1 and the refractive index n of the second liquid crystal alignment fixing layer LC2 can be the same or different from each other (the refractive index n of the first liquid crystal alignment fixing layer LC1 It can be larger, or the refractive index n of the second liquid crystal alignment fixing layer LC2 The refractive index n of the first liquid crystal alignment fixing layer may be larger. LC1 It is preferably from 1.55 to 1.75, and more preferably from 1.60 to 1.70. The refractive index n of the second liquid crystal alignment fixing layerLC2 It is preferably from 1.45 to 1.65, and more preferably from 1.50 to 1.60. The refractive index n of the first liquid crystal alignment fixing layer LC1 and the refractive index n of the second liquid crystal alignment fixing layer LC2 The refractive index n of the first liquid crystal alignment fixing layer is LC1 The refractive index n of the second liquid crystal alignment fixing layer LC2 The absolute value of the difference can be, for example, from 0.00 to 0.20. The refractive index of the liquid crystal alignment fixing layer is generally consistent with the configuration of the composition used to form the liquid crystal alignment fixing layer to obtain the desired optical properties. As a result, linear unevenness may occur, but according to at least one embodiment of the present invention, linear unevenness can be suppressed by setting the display unevenness parameter to a predetermined value or less.
[0068] A side chain type thermotropic liquid crystal polymer can be introduced into the first liquid crystal orientation fixing layer and / or the second liquid crystal orientation fixing layer (basically, the liquid crystal composition used to form those layers). When a side chain type thermotropic liquid crystal polymer is introduced, a vertical orientation (vertical orientation) effect on the liquid crystal monomer may occur. As a result, the nz of the first liquid crystal orientation fixing layer and / or the second liquid crystal orientation fixing layer can be made larger, and as a result, the Nz coefficient of the first liquid crystal orientation fixing layer and / or the second liquid crystal orientation fixing layer can be set to fall within the above-mentioned desired range. Finally, the Nz coefficient of the delay layer can be set to fall within the above-mentioned desired range without the arrangement of the positive C plate described later.
[0069] A copolymer containing a monomer unit having a thermotropic liquid crystal segment side chain and a monomer unit having a non-liquid crystal segment side chain is generally used as a side chain type thermotropic liquid crystal polymer. When the side chain type liquid crystal polymer contains a thermotropic liquid crystal segment on its side chain, the polymer can be oriented when the liquid crystal composition is heated to a predetermined temperature. In addition, when the side chain type liquid crystal polymer contains a non-liquid crystal segment on its side chain, the non-liquid crystal segment interacts with the photopolymerizable liquid crystal monomer, and thus a vertical orientation effect on the photopolymerizable liquid crystal monomer can occur.
[0070] A copolymer containing a liquid crystalline monomer unit represented by the general formula (I) and a non-liquid crystalline monomer unit represented by the general formula (II) is preferably used as the side chain type thermotropic liquid crystalline polymer.
[0071]
[0072] In formula (I), R 1 represents a hydrogen atom or a methyl group, R 2 represents a cyano group, a fluoro group, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, and X 1 Indicates –CO 2– or –OCO–. “a” represents an integer from 1 to 6, and “b” and “c” each independently represent 1 or 2.
[0073] In formula (II), R 3 represents a hydrogen atom or a methyl group, and R 4 represents an alkyl group having 7 to 22 carbon atoms, a fluoroalkyl group having 1 to 22 carbon atoms, or a group represented by the following general formula (III).
[0074]
[0075] In formula (III), R 5 represents an alkyl group having 1 to 5 carbon atoms, and "d" represents an integer from 1 to 6.
[0076] The ratio between the liquid crystal monomer unit and the non-liquid crystal monomer unit in the side chain type liquid crystal polymer can be appropriately set according to the purpose. The (molar ratio) of the non-liquid crystal monomer to the liquid crystal monomer unit and the non-liquid crystal monomer unit is preferably from 0.05 to 0.8, more preferably from 0.1 to 0.6, and even more preferably from 0.15 to 0.5. By this configuration, a liquid crystal orientation fixing layer showing a desired refractive index characteristic (Nz coefficient) can be obtained.
[0077] The ratio between liquid crystal monomer and side chain type liquid crystal polymer in liquid crystal composition can be appropriately set according to purpose. When the content of side chain type liquid crystal polymer is large, Nz coefficient tends to increase, and when the content of liquid crystal monomer is large, Nz coefficient tends to decrease. Relative to the content of side chain type liquid crystal polymer, the content of liquid crystal monomer is preferably from 1.2 times to 20 times, more preferably from 1.3 times to 10 times, still more preferably from 1.4 times to 9 times, particularly preferably from 1.5 times to 8 times. Through this configuration, it is possible to obtain a liquid crystal orientation fixing layer showing a desired refractive index characteristic (Nz coefficient).
[0078] Details of the side chain type liquid crystal polymer and a method of forming a liquid crystal alignment fixing layer having an Nz coefficient of less than 1.0 are described in Japanese Patent No. 6769921, the specification of which is incorporated herein by reference.
[0079] The retardation layer 20 may further include a positive C plate. The positive C plate has a refractive index characteristic showing a relationship of nz>nx=ny. The thickness direction retardation Rth(550) of the positive C plate is preferably from -20nm to -300nm, more preferably -30nm to -250nm, still more preferably -40nm to -200nm, and particularly preferably -50nm to -150nm. Here, "nx=ny" covers not only the case where nx and ny are exactly equal to each other, but also the case where nx and ny are substantially equal to each other. That is, the in-plane retardation Re(550) of the positive C plate can be less than 10nm.
[0080] The positive C plate can be formed by using, for example, a composition containing the above-mentioned side chain type liquid crystal polymer. A specific example of the method for forming the positive C plate is the method described in
[0020] to
[0028] of Japanese Patent Application Publication No. 2002-333642. In this case, the thickness of the positive C plate is preferably from 0.5 μm to 10 μm, more preferably from 0.5 μm to 8 μm, and even more preferably from 0.5 μm to 5 μm.
[0081] D. Adhesive layer
[0082] D-1. Overview
[0083] As long as the display unevenness parameter can be set to a predetermined value or less, any suitable configuration can be adopted as the adhesive layer 25. Specifically, as described above, the adhesive layer can be formed of a pressure-sensitive adhesive, or can be formed of an adhesive. Regardless of whether the adhesive layer is an adhesive layer or a pressure-sensitive adhesive layer, the refractive index n of the adhesive layer is AD For example, it may be 1.45 or more, for example, it may be 1.50 or more, or for example, it may be 1.52 or more. The refractive index n of the adhesive layer is AD It is preferably 1.54 or more, more preferably 1.55 or more, still more preferably 1.57 or more, and particularly preferably 1.60 or more. Meanwhile, the refractive index n of the adhesive layer is AD For example, it may be 1.63 or less.
[0084] When the adhesive layer is a pressure-sensitive adhesive layer, the thickness T of the adhesive layer AD For example, it is 3 μm or more, preferably 4 μm or more, more preferably 5 μm or more, still more preferably 10 μm or more, and particularly preferably 15 μm or more. AD For example, it may be 30 μm or less. When the adhesive layer is an adhesive layer, the thickness T of the adhesive layer AD It is preferably 0.5 μm to 2.0 μm, and more preferably 0.8 μm to 1.2 μm. The thickness variation TV of the adhesive layer AD It is preferably 0.20 μm or less, more preferably 0.18 μm or less, and still more preferably 0.16 μm or less. Meanwhile, the thickness variation TV of the adhesive layer AD For example, it can be 0.03 μm or greater. When the refractive index and thickness of the adhesive layer are combined to adjust, the display unevenness parameter can be adjusted to any suitable range according to the configuration of the liquid crystal orientation fixing layer. Considering the relationship between thickness and thickness variation, the adhesive layer can be preferably a pressure-sensitive adhesive layer. This is because the thickness can be increased to reduce the influence of the thickness variation.
[0085] The pressure-sensitive adhesive and the adhesive for forming the adhesive layer are described below respectively.
[0086] D-2. Pressure-sensitive adhesive
[0087] As long as the above characteristics are met, any suitable configuration can be adopted as pressure-sensitive adhesive.The specific example of pressure-sensitive adhesive includes acrylic pressure-sensitive adhesive, rubber-based pressure-sensitive adhesive, silicone-based pressure-sensitive adhesive, polyester-based pressure-sensitive adhesive, carbamate-based pressure-sensitive adhesive, epoxy-based pressure-sensitive adhesive and polyether-based pressure-sensitive adhesive.Pressure-sensitive adhesive with desired characteristics according to purpose can be prepared by adjusting the type, quantity, combination and blending ratio of the monomer of the base polymer for forming pressure-sensitive adhesive and the blending amount, reaction temperature, reaction time etc. of the cross-linking agent.The base polymer of pressure-sensitive adhesive can be used alone or in combination.Wherein, from the viewpoint of for example transparency, processability and durability, preferred acrylic pressure-sensitive adhesive (acrylic pressure-sensitive adhesive composition).Acrylic pressure-sensitive adhesive composition usually contains (methyl) acrylic polymer as main component as base polymer.(methyl) acrylic polymer can be incorporated into pressure-sensitive adhesive composition with 50 % by weight or more, preferably 70 % by weight or more, more preferably 90 % by weight or more of the solid content of pressure-sensitive adhesive composition. (Meth)acrylate refers to acrylate and / or methacrylate.
[0088] The (meth)acrylic polymer preferably includes a monomer (m1) containing an aromatic ring as a monomer component. A compound containing at least one aromatic ring and at least one ethylenically unsaturated group in its molecule can be used as the monomer (m1). As the monomer (m1), such compounds can be used alone or in combination.
[0089] Examples of ethylenically unsaturated groups include (meth)acryloyl, vinyl and (meth)allyl. Among them, from the viewpoint of polymerization reactivity, (meth)acryloyl is preferred, and from the viewpoint of flexibility and pressure-sensitive adhesive performance, acryl is more preferred. From the viewpoint of suppressing the decrease in the flexibility of the pressure-sensitive adhesive, a compound having an ethylenically unsaturated group in its molecule (i.e., a monofunctional monomer) is preferably used as monomer (m1).
[0090] The number of aromatic rings in the molecule of the compound used as the monomer (m1) may be 1, or may be 2 or more. The upper limit of the number of aromatic rings in the monomer (m1) is not particularly limited, and may be, for example, 16 or less. In some embodiments, from the viewpoint of the ease of preparing the (meth) acrylic polymer and the transparency of the pressure-sensitive adhesive, the number of aromatic rings may be, for example, 12 or less, preferably 8 or less, more preferably 6 or less, 5 or less, 4 or less, 3 or less, or 2 or less.
[0091] The aromatic ring in the compound used as monomer (m1) can be, for example, a carbon ring including a benzene ring (which can be a benzene ring for forming a part of a biphenyl structure or a fluorene structure), or a condensed ring, such as a naphthalene ring, an indene ring, an azulene ring, an anthracene ring, or a phenanthrene ring, or the aromatic ring can be a heterocycle, such as a pyridine ring, a pyrimidine ring, a pyridazine ring, a pyrazine ring, a triazine ring, a pyrrole ring, a pyrazole ring, an imidazole ring, a triazole ring, an oxazole ring, an isoxazole ring, a thiazole ring or a thiophene ring. The heteroatom incorporated into the heterocycle as a ring-forming atom can be, for example, one or two or more selected from the following: nitrogen; sulfur; and oxygen. In some embodiments, the heteroatom for forming a heterocycle can be one or both of nitrogen and sulfur. Monomer (m1) can have a structure in which one or two or more carbon rings and one or two or more heterocycles are fused to each other, such as a dinaphthothiophene structure.
[0092] The aromatic ring (preferably carbocyclic ring) may have one or two or more substituents on its ring-forming atoms, or may not contain substituents thereon. When the aromatic ring has substituents, examples of substituents include alkyl, alkoxy, aryloxy, hydroxyl, halogen atoms (e.g., fluorine atoms, chlorine atoms or bromine atoms), hydroxyalkyl, hydroxyalkoxy and glycidyloxy. In the substituents with carbon atoms, the number of carbon atoms in the substituent is preferably from 1 to 4, more preferably from 1 to 3, and may be, for example, 1 or 2. In some embodiments, the aromatic ring may not contain substituents on the ring-forming atoms, or may be an aromatic ring with one or two or more substituents selected from the group consisting of: alkyl; alkoxy; and halogen atoms (e.g., bromine atoms) thereon. The phrase "the aromatic ring in the monomer (m1) has substituents on its ring-forming atoms" means that the aromatic ring has substituents other than substituents with ethylenically unsaturated groups.
[0093] The aromatic ring and the ethylenically unsaturated group may be directly bonded to each other, or may be bonded to each other through a connecting group. The connecting group may be, for example, a group having one or two or more structures selected from the following: alkylene, oxyalkylene, poly(oxyalkylene), phenyl, alkylphenyl, alkoxyphenyl, a group having a structure in which one or two or more hydrogen atoms in each of these groups are replaced by hydroxyl (e.g., hydroxyalkylene), oxy (-O-group) and sulfoxy (-S-group). In some embodiments, the monomer containing the aromatic ring has the following structure: wherein the aromatic ring and the ethylenically unsaturated group are directly bonded to each other, or bonded to each other via a connecting group selected from the following: alkylene; oxyalkylene; and preferably a poly(oxyalkylene) group may be used. The number of carbon atoms in each of the alkylene and oxyalkylene groups is preferably from 1 to 4, more preferably from 1 to 3, and may be, for example, 1 or 2. The number of repetitions of the oxyalkylene unit in the poly(oxyalkylene) group may be, for example, 2 or 3.
[0094] Examples of compounds that can be preferably used as monomer (m1) include (meth)acrylates containing aromatic rings and vinyl compounds containing aromatic rings. (Meth)acrylates containing aromatic rings and vinyl compounds containing aromatic rings can be used alone or in combination. One or two or more (meth)acrylates containing aromatic rings and one or two or more vinyl compounds containing aromatic rings can be used in combination.
[0095] The content of the monomer (m1) in the monomer component for forming the (meth) acrylic polymer can be set so that it is possible to achieve, for example, a pressure-sensitive adhesive layer that realizes a desired refractive index and desired pressure-sensitive adhesive properties (for example, peel strength and flexibility) and / or desired optical properties (for example, total light transmittance and haze value) at the same time. In some embodiments, the content of the monomer (m1) in the monomer component can be, for example, 30 wt % or more, preferably 50 wt % or more, can be 60 wt % or more, or can be 70 wt % or more. In some embodiments, from the viewpoint of making it easier to obtain a higher refractive index, the content of the monomer (m1) can be, for example, greater than 70 wt %, can be 75 wt % or more, can be 80 wt % or more, can be 85 wt % or more, can be 90 wt % or more, or can be 95 wt % or more. The upper limit of the content of the monomer (m1) in the monomer component is 100 wt %. From the viewpoint of realizing both high refractive index and pressure-sensitive adhesive properties and / or optical properties in a balanced manner, it is advantageous that the content of the above-mentioned monomer (m1) is set to be less than 100 wt %, and the content is, for example, preferably about 99 wt % or less, more preferably 98 wt % or less, and can be 97 wt % or less, or can be 96 wt % or less. In some embodiments, the content of monomer (m1) may be 93 wt % or less, may be 90 wt % or less, may be 80 wt % or less, or may be 75 wt % or less. In some embodiments in which pressure-sensitive adhesive properties and / or optical properties are more emphasized, the content of monomer (m1) in the monomer component may be 70 wt % or less, may be 60 wt % or less, or may be 45 wt % or less.
[0096] In some embodiments, it is preferred to use a monomer having two or more aromatic rings (preferably a carbon ring) in its molecule as a monomer (m1) because it is easy to obtain a high increase effect on the refractive index. Examples of monomers having two or more aromatic rings in their molecules (hereinafter also referred to as "monomers having multiple aromatic rings") include: monomers having a structure in which two or more non-condensed aromatic rings are bonded to each other via a connecting group, monomers having a structure in which two or more non-condensed aromatic rings are directly (i.e., not via any other atom) chemically bonded to each other, monomers having a condensed aromatic ring structure, monomers having a fluorene structure, monomers having a dinaphthothiophene structure, and monomers having a dibenzothiophene structure. Monomers each having multiple aromatic rings can be used alone or in combination.
[0097] The linking group may be, for example, an oxy group (-O-), a thiol group (-S-), an oxyalkylene group (e.g., -O-(CH 2 ) n -group, wherein "n" represents from 1 to 3, preferably 1), thioloxyalkylene (e.g., -S-(CH 2 ) n -group, wherein "n" represents from 1 to 3, preferably 1), a straight chain alkylene group (i.e., -(CH 2 ) n - group, wherein "n" represents from 1 to 6, preferably
[0098] 1 to 3), and the group obtained by halogenating the alkylene moiety in each oxyalkylene group or completely halogenating, thiooxyalkylene, and linear alkylene. From the viewpoint of the flexibility of, for example, a pressure-sensitive adhesive, the suitable example of a linking group includes an oxy group, a thioxy group, an oxyalkylene group, and a straight-chain alkylene group. The specific example of a monomer having a structure in which two or more non-condensed aromatic rings are bonded to each other via a linking group includes (methyl) phenoxybenzyl acrylate (for example, (methyl) phenoxybenzyl acrylate), (methyl) thiophenoxybenzyl acrylate, and (methyl) benzylbenzyl acrylate.
[0099] The monomer having a structure in which two or more non-condensed aromatic rings are directly chemically bonded to each other may be, for example, a (meth)acrylate containing a biphenyl structure, a (meth)acrylate containing a triphenyl structure, or a biphenyl containing a vinyl group. Specific examples thereof include o-phenylphenol (meth)acrylate and biphenylmethyl (meth)acrylate.
[0100] Examples of the monomer having a condensed aromatic ring structure include (meth)acrylates containing a naphthalene ring, (meth)acrylates containing an anthracene ring, naphthalene containing a vinyl group, and anthracene containing a vinyl group. Specific examples thereof include 1-naphthylmethyl (meth)acrylate (another name: 1-naphthylmethyl (meth)acrylate), hydroxyethylated β-naphthol acrylate, 2-naphthylethyl (meth)acrylate, 2-naphthylethyl acrylate, and 2-(4-methoxy-1-naphthyloxy)ethyl (meth)acrylate.
[0101] Specific examples of the monomer having a fluorene structure include 9,9-bis(4-hydroxyphenyl)fluorene(meth)acrylate and 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene(meth)acrylate. The monomer having a fluorene structure has a structural portion in which two benzene rings are directly chemically bonded to each other, and is therefore encompassed in the concept of a monomer having a structure in which two or more non-condensed aromatic rings are directly chemically bonded to each other.
[0102] Examples of monomers having a dinaphthothiophene structure include dinaphthothiophene containing a (meth)acryloyl group, dinaphthothiophene containing a vinyl group, and dinaphthothiophene containing a (meth)allyl group. Specific examples thereof include: (meth)acryloyloxymethyl dinaphthothiophene (e.g., having CH 2 CH(R 1 )C(O)OCH 2 – is bonded to the 5-position or 6-position of the dinaphthothiophene ring, wherein R 1 represents a hydrogen atom or a methyl group), (meth)acryloyloxyethyl dinaphthothiophene (for example, having CH 2 CH(R 1 )C(O)OCH(CH 3 )– or CH 2 CH(R 1 )C(O)OCH 2 CH 2 – is bonded to the 5-position or 6-position of the dinaphthothiophene ring, wherein R 1 represents a hydrogen atom or a methyl group), vinyl dinaphthothiophene (for example, a compound having a structure in which a vinyl group is bonded to the 5-position or 6-position of the naphthothiophene ring), and (methyl)allyloxy dinaphthothiophene. The monomer having a dinaphthothiophene structure has a naphthalene structure and also has a structure in which a thiophene ring and two naphthalene structures are fused to each other, and is therefore encompassed in the concept of a monomer having a fused aromatic ring structure.
[0103] Examples of monomers having a dibenzothiophene structure include dibenzothiophene containing a (meth)acryloyl group and dibenzothiophene containing a vinyl group. The monomer having a dibenzothiophene structure has a structure in which a thiophene ring and two benzene rings are fused to each other, and is therefore included in the concept of a monomer having a fused aromatic ring structure. Neither the dinaphthothiophene structure nor the dibenzothiophene structure corresponds to a structure in which two or more non-fused aromatic rings are directly chemically bonded to each other.
[0104] A monomer having an aromatic ring (preferably a carbocyclic ring) in its molecule can be used as monomer (m1). A monomer having an aromatic ring in its molecule can be used, for example, to improve the flexibility of a pressure-sensitive adhesive, to adjust pressure-sensitive adhesive properties, and to improve transparency. In some embodiments, from the viewpoint of improving the refractive index of a pressure-sensitive adhesive, a monomer having an aromatic ring in its molecule is preferably used in combination with a monomer having multiple aromatic rings.
[0105] Examples of the monomer having one aromatic ring in its molecule include: (meth)acrylates containing a carbon aromatic ring, such as benzyl (meth)acrylate, methoxybenzyl (meth)acrylate, phenyl (meth)acrylate, ethoxylated phenol (meth)acrylate, phenoxypropyl (meth)acrylate, phenoxybutyl (meth)acrylate, toluene (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, and benzyl (meth)acrylate chloride; (meth)acrylates containing a bromine-substituted aromatic ring, such as 2-(4,6-dibromo-2-isobutylphenoxy)ethyl (meth)acrylate, 2-(4,6-dibromo-2 6-(4,6-dibromo-2-isobutylphenoxy)ethyl (meth)acrylate, 6-(4,6-dibromo-2-isopropylphenoxy)hexyl (meth)acrylate, 2,6-dibromo-4-nonylphenyl acrylate, and 2,6-dibromo-4-dodecylphenyl acrylate; vinyl compounds containing a carboaromatic ring, such as styrene, α-methylstyrene, vinyltoluene, and tert-butylstyrene; and compounds each having a vinyl substituent on a heteroaromatic ring, such as N-vinylpyridine, N-vinylpyrimidine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, and N-vinyloxazole.
[0106] A monomer having a structure in which an oxyethylene chain is inserted between the ethylenically unsaturated group and the aromatic ring in each of the various aromatic ring-containing monomers described above can be used as the monomer (m1). The monomer having an oxyethylene chain inserted between the ethylenically unsaturated group and the aromatic ring as described above can be considered to be an ethoxylated product of the original monomer. The oxyethylene unit (–CH 2 CH 2The repetition number of (O-) is usually from 1 to 4, preferably from 1 to 3, more preferably from 1 or 2, and for example is 1. Specific examples of the ethoxylated aromatic ring-containing monomers include ethoxylated o-phenylphenol (meth) acrylate, ethoxylated nonylphenol (meth) acrylate, ethoxylated cresol (meth) acrylate, phenoxyethyl (meth) acrylate, and phenoxydiglycol di(meth) acrylate.
[0107] The content of monomers with multiple aromatic rings in monomer (m1) is not particularly limited, and for example, can be 5 wt % or more, can be 25 wt % or more, or can be 40 wt % or more. In some embodiments, from the viewpoint of easily realizing a pressure-sensitive adhesive with a higher refractive index, the content of monomers with multiple aromatic rings in monomer (m1) can be, for example, 50 wt % or more, preferably 70 wt % or more, can be 85 wt % or more, can be 90 wt % or more, or can be 95 wt % or more. Substantially 100 wt % of monomers (m1) can be monomers with multiple aromatic rings. That is, one or more monomers each having multiple aromatic rings can be used alone as monomers (m1). In addition, in some embodiments, for example, considering the balance between high refractive index and pressure-sensitive adhesive properties and / or optical properties, the content of monomers with multiple aromatic rings in monomer (m1) can be less than 100 wt %, can be 98 wt % or less, can be 90 wt % or less, can be 80 wt % or less, or can be 65 wt % or less. In some embodiments, considering the pressure-sensitive adhesive properties and / or optical properties, the content of the monomer having multiple aromatic rings in the monomer (m1) may be 70 wt % or less, 50 wt % or less, 25 wt % or less, or 10 wt % or less. Even when the content of the monomer having multiple aromatic rings in the monomer (m1) is less than 5 wt %, the embodiments of the present invention may be performed separately. The monomer having multiple aromatic rings may not be used.
[0108] The content of the monomer with multiple aromatic rings in the monomer component for forming the (meth) acrylic polymer is not particularly limited, and can be set to make it possible to achieve a pressure-sensitive adhesive layer that realizes the desired refractive index and desired pressure-sensitive adhesive properties (e.g., peel strength and flexibility) and / or desired optical properties (e.g., total light transmittance and haze value) simultaneously. The content of the monomer with multiple aromatic rings in the monomer component can be, for example, 3 wt % or more, can be 10 wt % or more, or can be 25 wt % or more. In some embodiments, from the viewpoint of easily realizing a pressure-sensitive adhesive with a higher refractive index, the content of the monomer with multiple aromatic rings in the monomer component can be, for example, greater than 35 wt %, preferably greater than 50 wt %, can be greater than 70 wt %, can be 75 wt % or more, can be 85 wt % or more, can be 90 wt % or more, or can be 95 wt % or more. The content of the monomer with multiple aromatic rings in the monomer component can be 100 wt %. However, from the viewpoint of realizing both high refractive index and pressure-sensitive adhesive properties and / or optical properties in a balanced manner, it is advantageous to set the content to be less than 100 wt %, and the content is preferably about 99 wt % or less, more preferably 98 wt % or less, and can be 96 wt % or less, can be 93 wt % or less, can be 90 wt % or less, can be 85 wt % or less, can be 80 wt % or less, or can be 75 wt % or less. In some embodiments, considering pressure-sensitive adhesive properties and / or optical properties, the content of the monomer with multiple aromatic rings in the monomer component can be 70 wt % or less, can be 50 wt % or less, can be 25 wt % or less, can be 15 wt % or less, or can be 5 wt % or less. Even when the content of the monomer with multiple aromatic rings in the monomer component is less than 3 wt %, embodiments of the present invention can be carried out separately.
[0109] It is preferred to use a high refractive index monomer as at least a portion of the monomer (m1). The term "high refractive index monomer" used herein refers to a monomer having a refractive index of, for example, about 1.510 or greater, preferably about 1.530 or greater, more preferably about 1.550 or greater. From the viewpoint of the ease of preparing a pressure-sensitive adhesive composition and the ease of realizing both a high refractive index and flexibility suitable as a pressure-sensitive adhesive, the upper limit of the refractive index of the high refractive index monomer is not particularly limited, and for example, is 3.000 or less, and can be 2.500 or less, can be 2.000 or less, can be 1.900 or less, can be 1.800 or less, or can be 1.700 or less. The high refractive index monomer can be used alone or in combination.
[0110] The refractive index of the monomer can be measured with, for example, an Abbe refractometer under the conditions of a measurement wavelength of 589 nm and a measurement temperature of 25° C. Model “DR-M4” manufactured by Atago Co., Ltd. or its equivalent can be used as the Abbe refractometer. When a nominal value of the refractive index at 25° C. is provided by a manufacturer or the like, the nominal value can be adopted.
[0111] Compounds having a corresponding refractive index among the compounds included in the concept of the aromatic ring-containing monomer (m1) (e.g., the plurality of compounds and one compound given as examples above) can be appropriately used as the high refractive index monomer. Specific examples thereof include: m-phenoxybenzyl acrylate (refractive index: 1.566, Tg of its homopolymer: -35°C), 1-naphthylmethyl acrylate (refractive index: 1.595, Tg of its homopolymer: 31°C), ethoxylated o-phenylphenol acrylate (number of repetitions of its ethylene oxide unit: 1, refractive index: 1.578), benzyl acrylate (refractive index (nD20): 1.519, Tg of its homopolymer: 6°C), phenoxyethyl acrylate (refractive index (nD20): 1.517, Tg of its homopolymer: 2°C), phenoxydiglycol acrylate (refractive index: 1.510 , Tg of its homopolymer: –35°C), 6-acryloxymethyl dinaphthothiophene (6MDNTA, refractive index: 1.75), 6-methacryloxymethyl dinaphthothiophene (6MDNTMA, refractive index: 1.726), 5-acryloxyethyl dinaphthothiophene (5EDNTA, refractive index: 1.786), 6-acryloxyethyl dinaphthothiophene (6EDNTA, refractive index: 1.722), 6-vinyl dinaphthothiophene (6VDNT, refractive index: 1.802), and 5-vinyl dinaphthothiophene (abbreviation: 5VDNT, refractive index: 1.793).
[0112] The content of the high refractive index monomer (i.e., a monomer containing an aromatic ring having a refractive index of about 1.510 or more, preferably about 1.530 or more, more preferably about 1.550 or more) in the monomer (m1) is not particularly limited, and can be, for example, 5% by weight or more, 25% by weight or more, 35% by weight or more, or 40% by weight or more. In some embodiments, from the viewpoint of easily obtaining a higher refractive index, the content of the high refractive index monomer in the monomer (m1) can be, for example, 50% by weight or more, preferably 70% by weight or more, 85% by weight or more, 90% by weight or more, or 95% by weight or more. Substantially 100% by weight of the monomer (m1) can be a high refractive index monomer. In addition, in some embodiments, for example, from the viewpoint of realizing both high refractive index and pressure-sensitive adhesive properties and / or optical properties in a balanced manner, the content of the high refractive index monomer in the monomer (m1) may be less than 100 wt %, may be 98 wt % or less, may be 90 wt % or less, may be 80 wt % or less, or may be 65 wt % or less. In some embodiments, considering the pressure-sensitive adhesive properties and / or optical properties, the content of the high refractive index monomer in the monomer (m1) may be 70 wt % or less, may be 50 wt % or less, may be 25 wt % or less, may be 15 wt % or less, or may be 10 wt % or less. Even when the content of the high refractive index monomer in the monomer (m1) is less than 5 wt %, embodiments of the present invention may be performed separately. High refractive index monomers may not be used.
[0113] The (meth) acrylic polymer may contain a monomer that can be copolymerized with the monomer (m1) containing an aromatic ring as a monomer component (copolymerizable monomer). Examples of copolymerizable monomers include aliphatic (meth) alkyl acrylates, alicyclic (meth) alkyl acrylates, carboxyl-containing monomers, hydroxyl-containing monomers, and amide-containing monomers. The type, amount, combination, content of the monomer component, etc. of the copolymerizable monomers can be appropriately set according to the purpose.
[0114] According to the purpose, acrylic pressure-sensitive adhesive (acrylic pressure-sensitive adhesive composition) may contain a refractive index modifier. As used herein, the term "refractive index modifier" refers to a material that can be used to improve the refractive index of the pressure-sensitive adhesive layer. It is preferred to use a material with a refractive index higher than the refractive index of the pressure-sensitive adhesive layer containing a refractive index modifier as the refractive index modifier. In addition, it is preferred to use a material with a refractive index higher than the refractive index of the base polymer (e.g., acrylic polymer) of the pressure-sensitive adhesive layer containing a refractive index modifier as the refractive index modifier. By appropriately using a refractive index modifier, a higher refractive index and actual pressure-sensitive adhesive performance can be appropriately achieved. In some embodiments, the refractive index modifier is preferably an organic material. The organic material used as the refractive index modifier can be a polymer or a non-polymer. In addition, the organic material may or may not have a polymerizable functional group. The refractive index modifier may be used alone or in combination.
[0115] Refractive index improver (for example, additives described later (H RO )) can be set to any suitable range in a relative relationship with the refractive index of the base polymer, and is therefore not limited to a specific range. The refractive index of the refractive index improver can be selected from, for example, a scope greater than 1.55, greater than 1.56 or greater than 1.57, which is higher than the refractive index of the base polymer. In some embodiments, from the viewpoint of improving the refractive index of the pressure-sensitive adhesive, it is advantageous that the refractive index of the refractive index improver is 1.58 or greater, and the refractive index is preferably 1.60 or greater, more preferably 1.63 or greater, and can be 1.65 or greater, can be 1.70 or greater, or can be 1.75 or greater. Use a refractive index improver with a higher refractive index, even by using a smaller amount of refractive index improver can also achieve the target refractive index. From the viewpoint of suppressing the reduction of pressure-sensitive adhesive properties and optical properties, this situation is preferred. The upper limit of the refractive index of the refractive index modifier is not particularly limited, and is, for example, 3.000 or less, and may be 2.500 or less, may be 2.000 or less, may be 1.950 or less, may be 1.900 or less, or may be 1.850 or less, from the viewpoint of, for example, compatibility in pressure-sensitive adhesives and the ease of achieving both an increase in the refractive index and flexibility suitable as a pressure-sensitive adhesive.
[0116] In some embodiments, a refractive index modifier (e.g., an additive (H RO)) is set to be greater than 0. In some embodiments, ΔnA is, for example, 0.02 or greater, and may be 0.05 or greater, may be 0.07 or greater, may be 0.10 or greater, may be 0.15 or greater, or may be 0.20 or greater, or 0.25 or greater. The refractive index improvement effect by using a refractive index modifier tends to increase by selecting a base polymer and a refractive index modifier, so that ΔnA can become larger. In addition, in some aspects, from the perspective of, for example, compatibility in a pressure-sensitive adhesive layer and transparency of the pressure-sensitive adhesive layer, ΔnA may be, for example, 0.70 or less, may be 0.60 or less, may be 0.50 or less, or may be 0.40 or less or 0.35 or less.
[0117] In some embodiments, a refractive index modifier (e.g., an additive (H RO )) and the difference between the refractive index nb of the pressure-sensitive adhesive layer containing the refractive index modifier and the refractive index nT, i.e., nb-nT (hereinafter also referred to as "ΔnB") is set to be greater than 0. In some embodiments, ΔnB is, for example, 0.02 or greater, and may be 0.05 or greater, may be 0.07 or greater, may be 0.10 or greater, may be 0.15 or greater, or may be 0.20 or greater, or 0.25 or greater. The refractive index improvement effect by using a refractive index modifier tends to increase by selecting the composition of the pressure-sensitive adhesive layer and the refractive index modifier, so that ΔnB can become larger. In addition, in some embodiments, from the viewpoint of, for example, compatibility in the pressure-sensitive adhesive layer and the transparency of the pressure-sensitive adhesive layer, ΔnB may be, for example, 0.70 or less, may be 0.60 or less, may be 0.50 or less, or may be 0.40 or less or 0.35 or less.
[0118] Refractive index improver can be suitably set according to purpose relative to the usage amount (when using multiple refractive index improver) of 100 weight parts of base polymers.From the viewpoint of the refractive index improving pressure-sensitive adhesive, relative to the base polymer of 100 weight parts, the usage amount of refractive index improver can be set to such as 1 weight part or more, advantageously set to 3 weight parts or more, and preferably set to 5 weight parts or more, can be 7 weight parts or more, can be 10 weight parts or more, can be 15 weight parts or more, or can be 20 weight parts or more.In addition, in some embodiments, relative to the base polymer of 100 weight parts, the usage amount of refractive index improver can be set to such as 80 weight parts or less, and usage amount is advantageously set to 60 weight parts or less, and from the viewpoint of realizing the increase of the refractive index of pressure-sensitive adhesive in a balanced manner and suppressing the reduction of pressure-sensitive adhesive characteristics and optical characteristics, preferably set to 45 weight parts or less. In some embodiments where each of them emphasizes pressure-sensitive adhesive properties and optical properties, the amount of the refractive index modifier used, for example, can be 30 parts by weight or less, 20 parts by weight or less, 15 parts by weight or less, 10 parts by weight or less, 5 parts by weight or less, or 3 parts by weight or less relative to 100 parts by weight of the base polymer. Even when the amount of the refractive index modifier used is less than 1 part by weight relative to 100 parts by weight of the base polymer in the pressure-sensitive adhesive layer, or when the refractive index modifier is not used substantially, the embodiments of the present invention can be implemented separately. In this case, the phrase "substantially not using a refractive index modifier" means that at least the intentional use of the refractive index modifier is prevented.
[0119] (Additives (H RO ))
[0120] In some embodiments, it may be preferred to use an organic material having a higher refractive index than the base polymer as a refractive index modifier. Such organic materials are sometimes referred to as "additives" hereinafter. RO )". In this case, "H RO " indicates an organic material having a high refractive index. When a base polymer (eg, an acrylic polymer, preferably an acrylic polymer (A)) and an additive (H RO ) can be used in combination to achieve a pressure-sensitive adhesive that more suitably achieves both refractive index and pressure-sensitive adhesive properties (e.g., peel strength and flexibility) and / or optical properties (e.g., total light transmittance and haze value). RO ) may be a polymer or a non-polymer. In addition, the organic material may or may not have a polymerizable functional group. RO ) can be used alone or in combination.
[0121] Similar to the refractive index of the monomer, the additive (H RO ) can be measured with, for example, an Abbe refractometer under the conditions of a measurement wavelength of 589 nm and a measurement temperature of 25° C. When a nominal value of the refractive index at 25° C. is provided by a manufacturer or the like, the nominal value can be adopted.
[0122] Used as additive (H RO The molecular weight of the organic material of the additive (H) can be appropriately selected according to the purpose. RO The molecular weight of the additive (H) may be selected from, for example, a range of 30,000 or less. RO ) is preferably a polymer or non-polymer having a molecular weight lower than that of the base polymer. In some embodiments, the additive (H) is preferably a polymer or non-polymer having a molecular weight lower than that of the base polymer. From the viewpoint of achieving an increasing effect on the refractive index and other properties (e.g., flexibility suitable for pressure-sensitive adhesives and optical properties such as haze) in a balanced manner, RO ) is suitably less than about 10,000, preferably less than 5,000, more preferably less than 3,000 (e.g., less than 1,000), and may be less than 800, may be less than 600, may be less than 500, or may be less than 400. From the viewpoint of improving compatibility in the pressure-sensitive adhesive layer, the additive (H RO ) may be advantageous if the molecular weight of the additive (H) is not too large. RO ) can be, for example, 130 or more, or 150 or more. In some embodiments, the molecular weight of the additive (H RO ) from the perspective of the refractive index of the additive (H RO ) preferably has a molecular weight of 170 or greater, more preferably 200 or greater, and may be 230 or greater, may be 250 or greater, may be 270 or greater, may be 500 or greater, may be 1,000 or greater, or may be 2,000 or greater. In some embodiments, polymers having a molecular weight of about 1,000 to about 10,000 (e.g., 1,000 or greater and less than 5,000) may be used as additives (H RO ).
[0123] Regarding non-polymers or polymers having a low degree of polymerization (e.g., about dimer to pentamer), a molecular weight calculated based on a chemical structure or a measured value obtained by using matrix-assisted laser desorption / ionization time-of-flight mass spectrometry (MALDI-TOF-MS) can be used as an additive (H RO ) molecular weight. When the additive (H RO ) is a polymer having a relatively high degree of polymerization, the weight average molecular weight (Mw) based on GPC performed under appropriate conditions can be used. When the nominal value of the molecular weight is provided by a manufacturer, etc., the nominal value can be adopted.
[0124] Can be used as an additive (H RO Examples of the selected organic material include organic compounds having an aromatic ring and organic compounds having a heterocyclic ring (which may be an aromatic or non-aromatic heterocyclic ring).
[0125] Used as additive (H RO The aromatic ring of the organic compound having an aromatic ring (hereinafter also referred to as "a compound containing an aromatic ring") can be selected from the same aromatic rings as those in the compound used as the monomer (m1).
[0126] The aromatic ring may have one or two or more substituents on its ring-forming atoms, or may not have a substituent thereon. When the aromatic ring has a substituent, examples of the substituent include alkyl, alkoxy, aryloxy, hydroxyl, halogen atoms (e.g., fluorine atoms, chlorine atoms or bromine atoms), hydroxyalkyl, hydroxyalkoxy and glycidyloxy. In the substituent with carbon atoms, the number of carbon atoms in the substituent is, for example, from 1 to 10, advantageously from 1 to 6, preferably from 1 to 4, more preferably from 1 to 3, and for example, may be 1 or 2. In some embodiments, the aromatic ring may be free of substituents on the ring-forming atoms, or may be an aromatic ring with one or two or more substituents selected from the group consisting of: alkyl; alkoxy; and halogen atoms (e.g., bromine atoms).
[0127] Can be used as additive (H RO Examples of the aromatic ring-containing compound of the present invention include: a compound usable as the monomer (m1); an oligomer containing the compound usable as the monomer (m1) as a monomer unit; and a compound having a structure obtained by removing a group having an ethylenically unsaturated group (which may be a substituent bonded to a ring-forming atom) or a portion forming an ethylenically unsaturated group from the compound usable as the monomer (m1) and replacing it with a hydrogen atom or a group not containing an ethylenically unsaturated group (e.g., a hydroxyl group, an amino group, a halogen atom, an alkyl group, an alkoxy group, a hydroxyalkyl group, a hydroxyalkoxy group, or a glycidyloxy group). RO) include: monomers containing an aromatic ring, such as benzyl acrylate, m-phenoxybenzyl acrylate, 2-(o-phenylphenoxy)ethyl acrylate, phenoxyethyl acrylate, phenoxydiglycol acrylate, phenoxypolyethylene glycol acrylate, 2-hydroxy-3-phenoxypropyl acrylate, and monomers having a fluorene structure, monomers having a dinaphthothiophene structure, and monomers having the above-mentioned dibenzothiophene structure; and aromatic ring-containing compounds each free of an ethylenically unsaturated group, such as 3-phenoxybenzyl alcohol and dinaphthothiophene and derivatives thereof (for example, compounds having a structure in which one or two or more substituents selected from, for example, a hydroxyl group, a methanol group, a diethanol group, and a glycidyl group are bonded to the dinaphthothiophene ring). In addition, the compound containing an aromatic ring may be an oligomer containing such an aromatic ring-containing monomer as a monomer unit (preferably an oligomer having a molecular weight of about 5,000 or less, more preferably about 1,000 or less, for example, an oligomerization product of about a dimer to a pentamer). The oligomer may be, for example: a homopolymer of an aromatic ring-containing monomer; a copolymer of one or two or more aromatic ring-containing monomers; or a copolymer of one or two or more aromatic ring-containing monomers and any other monomers. One or two or more monomers each not containing an aromatic ring may each be used as the other monomer.
[0128] In some embodiments, an organic compound having two or more aromatic rings in its molecule (hereinafter also referred to as a "compound having multiple aromatic rings") may be preferably used as an additive (H RO ), because it is easy to obtain a high increase effect on the refractive index. The compound with multiple aromatic rings may or may not have a polymerizable functional group, such as an ethylenically unsaturated group. In addition, the compound with multiple aromatic rings may be a polymer or a non-polymer. In addition, the polymer may be an oligomer (preferably an oligomer with a molecular weight of about 5,000 or less, more preferably about 1,000 or less, for example, an oligomer product of about dimers to pentamers) containing a monomer with multiple aromatic rings as a monomer unit. The oligomer is, for example: a homopolymer of a monomer with multiple aromatic rings; a copolymer of one or two or more monomers, each of which has multiple aromatic rings; or a copolymer of one or two or more monomers each having multiple aromatic rings and any other monomer. Other monomers may be monomers containing aromatic rings that do not correspond to monomers with multiple aromatic rings, may be monomers that do not contain aromatic rings, or may be combinations thereof.
[0129] Non-limiting examples of compounds with multiple aromatic rings include compounds with a structure in which two or more non-condensed aromatic rings are bonded to each other via a connecting group, compounds with a structure in which two or more non-condensed aromatic rings are directly (i.e., not via any other atom) chemically bonded to each other, compounds with condensed aromatic ring structures, compounds with fluorene structures, compounds with dinaphthothiophene structures, and compounds with dibenzothiophene structures. Compounds each having multiple aromatic rings can be used alone or in combination.
[0130] In addition to the above-mentioned monomer having a fluorene structure and an oligomer which is a homopolymer or a copolymer of the monomer, specific examples of the compound having a fluorene structure include 9,9-bisphenylfluorene and derivatives thereof, such as 9,9-bis(4-hydroxyphenyl)fluorene (refractive index: 1.68), 9,9-bis(4-aminophenyl)fluorene (refractive index: 1.73), 9,9-bis(4-hydroxy-3-methylbenzene)fluorene (refractive index: 1.68) and 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (refractive index: 1.65).
[0131] In addition to the above-mentioned monomer having a dinaphthothiophene structure and an oligomer which is a homopolymer or a copolymer of the monomer, specific examples of the compound having a dinaphthothiophene structure include dinaphthothiophene and its derivatives, including: dinaphthothiophene (refractive index: 1.808); hydroxyalkyl dinaphthothiophenes, such as 6-hydroxymethyl dinaphthothiophene (refractive index: 1.766); dihydroxy dinaphthothiophenes, such as 2,12-dihydroxy dinaphthothiophene (refractive index: 1.750); Dihydroxyalkoxy dinaphthothiophenes such as 2,12-dihydroxyethoxy dinaphthothiophene (refractive index: 1.677); diglycidyloxy dinaphthothiophenes such as 2,12-diglycidyloxy dinaphthothiophene (refractive index: 1.723); and dinaphthothiophenes each having two or more ethylenically unsaturated groups such as 2,12-diallyloxy dinaphthothiophene (abbreviation: 2,12-DAODNT, refractive index: 1.729).
[0132] In addition to the above-mentioned monomer having a dibenzothiophene structure and an oligomer which is a homopolymer or a copolymer of the monomer, specific examples of the compound having a dibenzothiophene structure include dibenzothiophene (refractive index: 1.607), 4-dimethyldibenzothiophene (refractive index: 1.617) and 4,6-dimethyldibenzothiophene (refractive index: 1.617).
[0133] Can be used as an additive (H ROExamples of the selected organic compound having a heterocyclic ring (hereinafter also referred to as "organic compound containing a heterocyclic ring") include thioepoxide compounds and compounds containing a triazine ring. Examples of thioepoxide compounds include bis(2,3-epithiopropyl)disulfide and its polymerization product (refractive index: 1.74) described in Japanese Patent No. 3712653. An example of a compound having a triazine ring is a compound having at least one triazine ring (for example, 3 to 40 triazine rings, preferably 5 to 20 triazine rings) in its molecule. The triazine ring has aromaticity, so the compound having a triazine ring is also included in the concept of the compound containing an aromatic ring. In addition, a compound having multiple triazine rings is also included in the concept of a compound having multiple aromatic rings.
[0134] In some embodiments, it may be preferred to use a compound that does not contain an ethylenically unsaturated group as an additive (H RO ). By this configuration, the alternation of heat or light (reduction in leveling or increase in viscosity due to the progress of gelation) of the pressure-sensitive adhesive composition is suppressed, and thus the storage stability can be improved. RO From the viewpoint of preventing the occurrence of dimensional change, deformation (e.g., warping or wrinkling) or optical strain caused by the reaction of the ethylenically unsaturated groups in a pressure-sensitive adhesive sheet or a laminate including the pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer having a plurality of ethylenically unsaturated groups, it is also preferred to use an additive (H RO ).
[0135] The acrylic pressure-sensitive adhesive composition may preferably contain a silane coupling agent and / or a crosslinking agent. An example of a silane coupling agent is an epoxy-containing silane coupling agent. Examples of crosslinking agents include isocyanate-based crosslinking agents and peroxide-based crosslinking agents. In addition, the acrylic pressure-sensitive adhesive composition may contain additives. Specific examples of additives include antioxidants, conductive agents, colorants, powders such as pigments, dyes, surfactants, plasticizers, tackifiers, surface lubricants, leveling agents, softeners, antioxidants, light stabilizers, UV absorbers, polymerization inhibitors, inorganic fillers or organic fillers, metal powders, particles and foil. In addition, a redox system obtained by adding a reducing agent can be used to achieve a controlled composition. The type, quantity, combination, content, etc. of silane coupling agents, crosslinking agents and / or additives can be appropriately set according to the purpose.
[0136] D-3. Adhesive
[0137] As long as the above characteristics are met, any suitable configuration can also be adopted as adhesive. Adhesive (adhesive composition) can contain (methyl) acrylate and metal oxide particles with aromatic ring skeleton usually. Each material can be briefly described hereinafter. For other components (for example, curing component or pressure-sensitive adhesive) that can be incorporated into the adhesive, known configuration can be adopted, so its specific description is omitted.
[0138] When the adhesive composition contains a (meth)acrylate having an aromatic ring skeleton, an adhesive layer having a desired refractive index can be formed in at least one embodiment of the present invention. At least one is selected from the group consisting of: a (meth)acrylate having a polycyclic aromatic ring skeleton; and a (meth)acrylate having two or more aromatic rings is preferably used as a (meth)acrylate having an aromatic ring skeleton. Examples of such (meth)acrylates include benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxydiethylene glycol acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 1-naphthyl (meth)acrylate, phenoxybenzyl (meth)acrylate, ethylene oxide-modified o-phenylphenol (meth)acrylate, and the reaction product of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene and (meth)acrylic acid. Among them, phenoxybenzyl (meth)acrylate and phenoxyethyl (meth)acrylate are more preferably used, and phenoxybenzyl (meth)acrylate is particularly preferably used. When the total amount of the adhesive composition is defined as 100 wt %, the blending amount of the (meth)acrylate having an aromatic ring skeleton is preferably 20 wt % to 90 wt %, more preferably 30 wt % to 80 wt %.
[0139] Examples of metal oxide particles include silicon oxide, zirconium oxide, titanium oxide, zinc oxide, antimony pentoxide, tin oxide, aluminum oxide, indium oxide, indium tin oxide, iron oxide, cerium oxide, yttrium oxide, manganese oxide, holmium oxide, copper oxide, bismuth oxide, cobalt oxide, cobalt trioxide, iron trioxide, magnesium oxide, lanthanum oxide, praseodymium oxide, neodymium oxide, samarium oxide, europium oxide, gadolinium oxide, terbium oxide, dysprosium oxide, erbium oxide, thulium oxide, ytterbium oxide, ruthenium oxide, scandium oxide, tantalum pentoxide, niobium pentoxide, iridium oxide, rhodium oxide, ruthenium oxide, and composite oxides obtained by combining these oxides. Among them, zirconium oxide and titanium oxide are preferred, and zirconium oxide is particularly preferred. The metal oxide particles may be formed only by the above-mentioned metal oxides, or may contain any other components, but preferably the metal oxide has the maximum weight as a component in the particles. The shape of each metal oxide particle may be any suitable shape, such as spherical, elliptical, cubic, cuboid or pyramidal. Metal oxide particles surface-treated by any appropriate method may be used as the metal oxide particles.
[0140] From the viewpoint of improving the stability of the metal oxide particles in the adhesive composition and improving the refractive index of the adhesive layer, the average particle size of the metal oxide particles is preferably from 1 nm to 150 nm, more preferably from 1 nm to 50 nm. The average particle size of the metal oxide particles can be obtained, for example, by the following method: the average particle size can be calculated by observing the particles in an enlarged manner using, for example, a transmission electron microscope (TEM), a field emission transmission electron microscope (FE-TEM), or a field emission scanning electron microscope (FE-SEM), randomly selecting, for example, 1,000 particles thereof, measuring their maximum length, and determining their arithmetic mean.
[0141] From the perspective of improving the stability of the metal oxide particles in the adhesive composition and improving the refractive index of the adhesive layer, when the total amount of the adhesive composition is defined as 100 wt %, the blending amount of the metal oxide particles is preferably from 10 wt % to 50 wt %, more preferably from 15 wt % to 40 wt %.
[0142] Adhesive composition can further include (meth) acrylate containing hydroxyl.Through this structure, the bonding strength of adhesive layer can be further improved.When the total amount of adhesive composition is defined as 100 wt %, the blending amount of (meth) acrylate containing hydroxyl is preferably from 1 wt % to 30 wt %, more preferably 3 wt % to 20 wt %.
[0143] E. Image display device
[0144] The optical stack described in parts A to D can be applied to an image display device. Therefore, at least one embodiment of the present invention also covers an image display device using such an optical stack. Typical examples of image display devices include liquid crystal display devices and organic EL display devices. An image display device according to at least one embodiment of the present invention generally includes the optical stack described in parts A to D on its observer side.
[0145] Example
[0146] The present invention is specifically described below by examples. However, the present invention is not limited to these examples. The measuring methods and evaluation methods in the examples are as follows. The terms "parts" and "%" in the examples and comparative examples are based on weight unless otherwise specified.
[0147] (1) Refractive index (1-1) Pressure-sensitive adhesive layer
[0148] The refractive index of the pressure-sensitive adhesive layer formed in Examples and Comparative Examples was measured with an Abbe refractometer (manufactured by Atago Co., Ltd., product name: "DR-M2 / 1550"). The measurement wavelength was 589 nm, and the measurement temperature was 25°C.
[0149] (1-2) Adhesive layer and liquid crystal alignment fixing layer
[0150] The adhesive used in each of the examples and comparative examples was applied to a cycloolefin-based polymer film (COP film) (thickness: 100 μm), and the same kind of COP film was bonded to the applied surface, followed by irradiation with visible light by using an active energy line application device. Thus, a cured product layer (single-layer film) was obtained. The in-plane refractive index and the thickness-direction refractive index of the obtained cured product layer were each measured with a prism coupler (manufactured by Sairon Technology, product name: "SPA-4000") and the average value of the refractive index was defined as the average refractive index of the adhesive layer. The measurement wavelength was 594 nm and the measurement temperature was 23 ° C.
[0151] In addition, the refractive index of the transmission axis direction of the liquid crystal alignment fixing layer was determined as follows: In-plane retardation Re(550) and thickness retardation Rth(550) were measured using AxoScan (manufactured by Axometrics). nx, ny and nz were calculated from the following simultaneous equations.
[0152] Re(550)=(nx–ny)×d
[0153] Nz=Rth(550) / Re(550)=(nx–nz) / (nx–ny)
[0154] Furthermore, in the equation of an ellipse: (x 2 / a 2 )+(y 2 / b 2 )=1, "a" and "b" are set to nx and ny, respectively, and "x" and "y" are set to the refractive index in the "x" direction and the "y" direction in the angle θ direction on the ellipse, respectively. Solve the simultaneous equations from y=tanθ and the above nx and ny. Thus, calculate the refractive index in the transmission axis direction.
[0155] (2) Thickness
[0156] The thickness was measured with an interferometer thickness meter (manufactured by Otsuka Electronics Co., Ltd., "MCPD-9800").
[0157] (3) Thickness change
[0158] The thickness of the optical laminates obtained in the examples and comparative examples having the structure of "first liquid crystal orientation fixing layer / adhesive layer / second liquid crystal orientation fixing layer" was measured by using "USB4H09646" manufactured by Ocean Optics in a range of 10 cm × 10 cm at a pitch of 1 mm. The thickness difference at the location with the largest thickness difference between three adjacent points was defined as the thickness variation.
[0159] (4) Linear unevenness
[0160] A typical acrylic pressure-sensitive adhesive was arranged on the second liquid crystal orientation fixing layer side of the optical laminate obtained in each of Examples and Comparative Examples, and the resultant was bonded to a V3 reflective plate (NEODIS Corporation) via an acrylic pressure-sensitive adhesive to provide a test sample. The obtained test sample was visually observed under a three-band fluorescent lamp and evaluated by the following criteria.
[0161] 1: No linear unevenness was observed.
[0162] 2: Linear unevenness is slightly observed.
[0163] 3: Linear unevenness is observed, although its degree is actually acceptable.
[0164] 4: Nonlinearity is observed to a practically unacceptable degree.
[0165] 5: Significant linear inhomogeneity.
[0166] [Production Example 1: Preparation of Adhesive 1 for Laminating Polarizing Plate and Retardation Layer]
[0167] 10 parts of hydroxyethyl acrylamide (product name: "HEAA", manufactured by KJ Chemicals Co., Ltd.), 4 parts of 2-acetoacetoxyethyl methacrylate (product name: "AAEM", manufactured by Mitsubishi Chemical Co., Ltd.), 60 parts of acryloylmorpholine (product name: "ACMO", manufactured by KJ Chemicals Co., Ltd.), 11 parts of tripropylene glycol diacrylate (product name: "ARONIXM-220", manufactured by Toagosei Co., Ltd.), 1 part of 4-vinylphenylboronic acid (manufactured by FUJIFILM Wako Pure Chemical Co., Ltd.), 10 parts of acrylic oligomer (product name: "ARUFONUP-1190", manufactured by Toagosei Co., Ltd.), 1 part of bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (product name: "Omnirad 819", manufactured by IGM Resins Co., Ltd.), 2 parts of 1-hydroxycyclohexylphenyl ketone (product name: "Omnirad184", manufactured by IGM Resins Co., Ltd.), and 1 part of diethylthioxanthone (product name: "KAYACURE DETX-S", manufactured by Nippon Kayaku Co., Ltd.) were stirred at 50° C. for 1 hour to prepare an adhesive 1.
[0168] [Production Example 2: Preparation of Pressure-Sensitive Adhesive A1 for Laminating the First Liquid Crystal Alignment Fixing Layer and the Second Liquid Crystal Alignment Fixing Layer]
[0169] A monomer mixture containing 91 parts of butyl acrylate, 6 parts of acryloylmorpholine, 2.7 parts of acrylic acid, and 0.3 parts of 4-hydroxybutyl acrylate was charged into a four-necked flask with a stirring blade, a thermometer, a nitrogen inlet tube, and a condenser. In addition, 0.1 parts of 2,2′-azobisisobutyronitrile used as a polymerization initiator was loaded with 100 parts of ethyl acetate relative to 100 parts of the monomer mixture. While gently stirring the mixture, nitrogen purging was performed by introducing nitrogen. After that, the polymerization reaction was carried out for 8 hours while the liquid temperature in the flask was maintained at about 55°C. Thus, a solution of acrylic polymer A1 having a weight average molecular weight (Mw) of 2,700,000 was prepared.
[0170] 0.1 parts of an isocyanate-based crosslinking agent (toluene diisocyanate adduct of trimethylolpropane: manufactured by Tosoh Corporation, product name: "CORONATEL"), 0.3 parts of a peroxide crosslinking agent (benzoyl peroxide: manufactured by Nippon Oil & Fats Co., Ltd., product name: "NYPER BMT"), and 0.2 parts of an epoxy-containing silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name: "KBM-403") were blended into 100 parts of a solid content acrylic polymer A1 solution to provide a pressure-sensitive adhesive A1. The polymer concentration of the pressure-sensitive adhesive A1 was adjusted to 5%.
[0171] [Production Example 3: Preparation of Pressure-Sensitive Adhesive A2 for Laminating the First Liquid Crystal Alignment Fixing Layer and the Second Liquid Crystal Alignment Fixing Layer]
[0172] A pressure-sensitive adhesive A2 was obtained in the same manner as in Production Example 2 except that the polymer concentration was adjusted to 6%.
[0173] [Production Example 4: Preparation of Pressure-Sensitive Adhesive A3 for Laminating the First Liquid Crystal Alignment Fixing Layer and the Second Liquid Crystal Alignment Fixing Layer]
[0174] A pressure-sensitive adhesive A3 was obtained in the same manner as in Production Example 2 except that the polymer concentration was adjusted to 7%.
[0175] [Production Example 5: Preparation of Pressure-Sensitive Adhesive A4 for Laminating the First Liquid Crystal Alignment Fixing Layer and the Second Liquid Crystal Alignment Fixing Layer]
[0176] A pressure-sensitive adhesive A4 was obtained in the same manner as in Production Example 2 except that the polymer concentration was adjusted to 8%.
[0177] [Production Example 6: Preparation of Pressure-Sensitive Adhesive B for Laminating the First Liquid Crystal Alignment Fixing Layer and the Second Liquid Crystal Alignment Fixing Layer]
[0178] A monomer mixture containing 94.9 parts of butyl acrylate, 5 parts of acrylic acid and 0.1 parts of 2-hydroxyethyl acrylate was charged into a four-necked flask with a stirring blade, a thermometer, a nitrogen inlet tube and a condenser. In addition, 0.1 parts of 2,2′-azobisisobutyronitrile used as a polymerization initiator was loaded with 100 parts of ethyl acetate relative to 100 parts of the monomer mixture. While gently stirring the mixture, nitrogen purging was performed by introducing nitrogen. Thereafter, a polymerization reaction was performed for 8 hours while the liquid temperature in the flask was maintained at about 55°C. Thus, an acrylic polymer B solution having a weight average molecular weight (Mw) of 2,200,000 was prepared.
[0179] 0.6 parts of an isocyanate-based crosslinking agent (toluene diisocyanate adduct of trimethylolpropane: manufactured by Tosoh Corporation, product name: "CORONATEL"), 0.2 parts of a peroxide crosslinking agent (benzoyl peroxide: manufactured by Nippon Oil & Fats Co., Ltd., product name: "NYPER BMT") and 0.2 parts of an epoxy-containing silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name: "KBM-403") are blended into 100 parts of a solid content of an acrylic polymer B solution to provide a pressure-sensitive adhesive B.
[0180] [Production Example 7: Preparation of Pressure-Sensitive Adhesive C1 for Laminating the First Liquid Crystal Alignment Fixing Layer and the Second Liquid Crystal Alignment Fixing Layer]
[0181] A monomer mixture containing 19 parts of butyl acrylate, 80 parts of benzyl acrylate and 1 part of 4-hydroxybutyl acrylate was charged into a four-necked flask with a stirring blade, a thermometer, a nitrogen inlet tube and a condenser. In addition, 0.1 parts of 2,2′-azobisisobutyronitrile used as a polymerization initiator was loaded with 100 parts of ethyl acetate relative to 100 parts of the monomer mixture. While gently stirring the mixture, nitrogen purging was performed by introducing nitrogen. Thereafter, a polymerization reaction was performed for 6 hours while maintaining the liquid temperature in the flask at about 60°C. Thus, a solution of acrylic polymer C1 having a weight average molecular weight (Mw) of 1,900,000 was prepared.
[0182] 0.1 parts of an isocyanate-based crosslinking agent (toluene diisocyanate adduct of trimethylolpropane: manufactured by Mitsui Chemicals, product name: “D101E”) and 0.3 parts of a peroxide crosslinking agent (benzoyl peroxide: manufactured by Nippon Oil & Fats Co., Ltd., product name: “NYPER BMT”) were blended into 100 parts of the solid content of the acrylic polymer C1 solution to provide a pressure-sensitive adhesive C1.
[0183] [Production Example 8: Preparation of a pressure-sensitive adhesive C2 for laminating a first liquid crystal alignment fixing layer and a second liquid crystal alignment fixing layer]
[0184] A solution of acrylic polymer C2 having a weight average molecular weight (Mw) of 650,000 was prepared in the same manner as in Production Example 7, except that a monomer mixture containing 30 parts of butyl acrylate, 69 parts of m-phenoxybenzyl acrylate, and 1 part of 4-hydroxybutyl acrylate was used. A pressure-sensitive adhesive C2 was obtained in the same manner as in Production Example 7, except that acrylic polymer C2 was used.
[0185] [Production Example 9: Preparation of a pressure-sensitive adhesive C3 for laminating a first liquid crystal alignment fixing layer and a second liquid crystal alignment fixing layer]
[0186] A solution of acrylic polymer C3 having a weight average molecular weight (Mw) of 650,000 was prepared in the same manner as in Production Example 7, except that a monomer mixture containing 19 parts of butyl acrylate, 80 parts of m-phenoxybenzyl acrylate, and 1 part of 4-hydroxybutyl acrylate was used. A pressure-sensitive adhesive C3 was obtained in the same manner as in Production Example 7, except that acrylic polymer C3 was used.
[0187] [Production Example 10: Preparation of Pressure-Sensitive Adhesive C4 for Laminating the First Liquid Crystal Alignment Fixing Layer and the Second Liquid Crystal Alignment Fixing Layer]
[0188] A solution of acrylic polymer C4 having a weight average molecular weight (Mw) of 650,000 was prepared in the same manner as in Production Example 7, except that a monomer mixture containing 6 parts of butyl acrylate, 93 parts of m-phenoxybenzyl acrylate, and 1 part of 4-hydroxybutyl acrylate was used. A pressure-sensitive adhesive C4 was obtained in the same manner as in Production Example 7, except that acrylic polymer C4 was used.
[0189] [Production Example 11: Preparation of a pressure-sensitive adhesive C5 for laminating a first liquid crystal alignment fixing layer and a second liquid crystal alignment fixing layer]
[0190] 0.1 parts of an isocyanate-based crosslinking agent (toluene diisocyanate adduct of trimethylolpropane: manufactured by Mitsui Chemicals, product name: “D101E”), 0.3 parts of a peroxide crosslinking agent (benzoyl peroxide: manufactured by Nippon Oil & Fats Co., Ltd., product name: “NYPER BMT”) and 10 parts of a refractive index improver (6-acryloyloxymethyl dinaphthothiophene: manufactured by Sugai Chemical Industry Co., Ltd., product name: “6MDNTA”) were blended into 100 parts of the solid content of the acrylic polymer C4 of Production Example 10 to provide a pressure-sensitive adhesive C5.
[0191] [Production Example 12: Preparation of Adhesive D1 for Laminating the First Liquid Crystal Alignment Fixing Layer and the Second Liquid Crystal Alignment Fixing Layer]
[0192] (Preparation of dispersant)
[0193] 415 grams (1 mol) of tristyrenated phenol and 1 g (0.018 mol) of potassium hydroxide were loaded into an autoclave, and the materials were uniformly mixed. Under the condition of a reaction system at 130°C, 352 g (8 mol) of ethylene oxide (EO) was added dropwise to the reaction system. After the dropwise addition of ethylene oxide was completed, aging was then performed at 130°C for 1 hour while the pressure of the system was maintained at 0.1 MPa. Thus, 8 mol of the EO adduct of tristyrenated phenol was obtained. 767 grams (1 mol) of the resulting 8 mol of EO adduct of tristyrenated phenol and 152 g (1.3 mol) of sodium monochloroacetate were loaded into a reactor, and the materials were uniformly stirred. Next, under the condition of a reaction system at 60°C, 52 g of sodium hydroxide was added thereto. Afterwards, the temperature of the system was raised to 80°C and aged for 3 hours. After aging, the product was cooled to 50°C, and 117 g (1.2 mol) of 98% sulfuric acid was added dropwise thereto at the same temperature. Thus, a white suspension was obtained. The white suspension was washed with distilled water, and the solvent was evaporated under reduced pressure. Thus, a dispersion was obtained.
[0194] (Preparation of Zirconia Dispersion)
[0195] 1.5 parts of the dispersant obtained above and 28.5 parts of m-phenoxybenzyl acrylate (manufactured by Kyoeisha Chemical Co., Ltd., product name: "Light Acrylate POB-A"; hereinafter referred to as "POB-A") were added to 100 parts of a dispersion of zirconium oxide in methanol (manufactured by Sakai Chemical Industry Co., Ltd., grade name: "SZR-CM", average particle size (D50) based on dynamic light scattering method: 8 nm, solid content concentration of zirconium oxide: 30%), and the materials were mixed. Next, the solvent was removed under reduced pressure using a rotary evaporator. Thus, a zirconium oxide dispersion as a monomer dispersion of zirconium oxide was obtained. The zirconium oxide dispersion contained zirconium oxide, the dispersant and POB-A in a weight ratio of 50 / 2.5 / 47.5.
[0196] (Preparation of Adhesive D1)
[0197] 35 parts of zirconium oxide dispersion, 40 parts of "POB-A", 10 parts of 4-hydroxybutyl acrylate, 10 parts of tripropylene glycol diacrylate (product name: "ARONIX M-220", manufactured by Toagosei Co., Ltd.), 1 part of bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (product name: "Omnirad 819", manufactured by IGM Resins Co., Ltd.), 2 parts of 1-hydroxycyclohexylphenyl ketone (product name: "Omnirad184", manufactured by IGM Resins Co., Ltd.), and 2 parts of diethylthioxanthone (product name "KAYACUREDETX-S" (manufactured by Nippon Kayaku Co., Ltd.) were stirred at 50° C. for 1 hour to prepare an adhesive D1.
[0198] [Production Example 13: Preparation of Adhesive D2 for Laminating the First Liquid Crystal Alignment Fixing Layer and the Second Liquid Crystal Alignment Fixing Layer]
[0199] 55 parts of zirconium oxide dispersion, 25 parts of "POB-A", 10 parts of 4-hydroxybutyl acrylate, 10 parts of "ARONIX M-220", 1 part of "Omnirad 819", 2 parts of "Omnirad 184" and 2 parts of "KAYACURE DETX-S" were stirred at 50°C for 1 hour to prepare adhesive D2.
[0200] [Production Example 14: Preparation of Adhesive E for Laminating the First Liquid Crystal Alignment Fixing Layer and the Second Liquid Crystal Alignment Fixing Layer]
[0201] 60 parts of OGSOL EA-F5710 (manufactured by Osaka Gas Chemicals Co., Ltd.), 10 parts of PLACCELFA1DDM (manufactured by Daicel Corporation), 20 parts of acryloylmorpholine (product name: "ACMO", manufactured by KJ Chemicals Co., Ltd.), 5 parts of ARUFON UP-1190 (manufactured by Toagosei Co., Ltd.), 1 part of bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (product name: "Omnirad 819", manufactured by IGM Resins Co., Ltd.), 2 parts of 1-hydroxycyclohexylphenyl ketone (product name: "Omnirad 184", manufactured by IGM Resins Co., Ltd.), and 2 parts of diethylthioxanthone (product name: "KAYACUREDETX-S" (manufactured by Nippon Kayaku Co., Ltd.) were stirred at 50° C. for 1 hour to prepare Adhesive E.
[0202] Embodiment 1:
[0203] 1. Production of polarizing plates
[0204] 1-1. Production of polarizers
[0205] An amorphous isophthalic acid copolymerized polyethylene terephthalate film (thickness: 100 μm) having an elongated shape and a Tg of about 75° C. was used as a thermoplastic resin substrate, and one surface of the resin substrate was subjected to a corona treatment.
[0206] 13 parts by weight of potassium iodide was added to 100 parts by weight of a PVA-based resin obtained by mixing polyvinyl alcohol (polymerization degree: 4,200, saponification degree: 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name: "Gohsefimer") and dissolving them in water at a ratio of 9:1 to prepare a PVA aqueous solution (application liquid).
[0207] The PVA aqueous solution was applied to the corona-treated surface of the resin substrate and dried at 60° C. to form a PVA-based resin layer having a thickness of 13 μm. Thus, a laminated material was produced.
[0208] The obtained laminate was uniaxially stretched at a ratio of 2.4 times in its longitudinal direction (length direction) in an oven at 130°C (auxiliary stretching treatment in air).
[0209] Next, the laminate was immersed in an insolubilization bath (boric acid aqueous solution obtained by mixing 100 parts by weight of water with 4 parts by weight of boric acid) having a liquid temperature of 40° C. for 30 seconds (insolubilization treatment).
[0210] Next, the laminate is immersed in a dyeing bath (an aqueous solution of iodine obtained by blending 100 parts by weight of water with iodine and potassium iodide in a weight ratio of 1:7) having a liquid temperature of 30°C for 60 seconds, while adjusting the concentration of the aqueous solution so that the single-layer transmittance (Ts) of the polarizer finally obtained becomes the desired value (dyeing treatment).
[0211] Next, the laminate was immersed in a crosslinking bath (boric acid aqueous solution obtained by blending 100 parts by weight of water with 3 parts by weight of potassium iodide and 5 parts by weight of boric acid) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment).
[0212] Thereafter, while the laminate is immersed in an aqueous boric acid solution (boric acid concentration: 4 wt %, potassium iodide concentration: 5 wt %) at a liquid temperature of 70°C, the laminate is uniaxially stretched in the longitudinal direction (length direction) between rollers having different circumferential speeds so that the total stretching ratio becomes 5.5 times (underwater stretching treatment).
[0213] Thereafter, the laminate was immersed in a washing bath (an aqueous solution obtained by blending 100 parts by weight of water with 4 parts by weight of potassium iodide) having a liquid temperature of 20° C. (washing treatment).
[0214] Thereafter, the laminate was brought into contact with a heating roller made of SUS whose surface temperature was maintained at approximately 75° C., while being dried in an oven maintained at approximately 90° C. (drying shrinkage treatment).
[0215] Thus, a polarizing plate having a thickness of about 5 μm was formed on the resin substrate to provide a polarizing plate having a configuration of “resin substrate / polarizing plate.” The single-layer transmittance Ts of the polarizing plate was 43.3%.
[0216] 1-2. Production of polarizing plates
[0217] The HC-COP film is bonded to the surface of the resulting polarizer (its surface is on the side opposite to the resin substrate) via a UV-curable adhesive. The HC-COP film is a film obtained by forming an HC layer (thickness: 4 μm) on a cycloolefin-based resin (COP) film (thickness: 25 μm), and is bonded so that the COP film is on the polarizer side. The COP film has a Re (550) of 135 nm. Next, the resin substrate is peeled off, and a triacetyl cellulose (TAC) film (thickness: 25 μm) is bonded to the peeled surface via a UV-curable adhesive. Therefore, a polarizing plate with a "HC layer / COP film (protective layer) / polarizer / TAC film (protective layer)" configuration is obtained.
[0218] 2. Production of delay layer
[0219] A polymerizable liquid crystal compound showing a nematic liquid crystal phase (manufactured by BASF SE, "Paliocolor LC242", the chemical formula is indicated below) was dissolved in cyclopentanone to prepare a solution having a solid content concentration of 30% by weight. A surfactant (manufactured by BYK-Chemie, "BYK-360") and a photopolymerization initiator (manufactured by IGM Resins, "Omnirad907") were added to the solution to prepare a liquid crystal composition solution. The amounts of the surfactant and the polymerization initiator added were set to 0.01 parts by weight and 3 parts by weight, respectively, relative to 100 parts by weight of the photopolymerizable liquid crystal compound. A biaxially stretched norbornene-based film (manufactured by Zeon, "ZEONOR film", thickness: 33 μm, Re (550) = 135 nm) was prepared as a substrate. The above liquid crystal composition was applied to the substrate with a rod coater so that Re (550) became 240 nm, and heated at 100° C. for 3 minutes to orient the liquid crystal. After the resultant was cooled to room temperature, it was irradiated under a nitrogen atmosphere with an integrated radiation dose of 400 mJ / cm 2The resultant was photocured by irradiation with UV light. Thus, a laminate having a "substrate / first liquid crystal orientation fixing layer" configuration was obtained. The first liquid crystal orientation fixing layer was uniformly oriented, and the thickness of the layer was 1.7 μm. In addition to changing the coating thickness, a laminate having a "substrate / second liquid crystal orientation fixing layer" configuration (uniform orientation, thickness: 0.92 μm, Re (550) = 130 nm) was obtained in the same manner as above.
[0220]
[0221] 3. Production of optical laminates
[0222] The first liquid crystal orientation fixing layer is bonded to the TAC film surface of the polarizing plate by the adhesive 1 (thickness: 1 μm) of production example 1, and then the substrate is peeled off. Next, the second liquid crystal orientation fixing layer is bonded to the surface of the first liquid crystal orientation fixing layer by the pressure-sensitive adhesive A3 (thickness: 5 μm) of production example 4, and the substrate is peeled off. Thus, an optical laminate having a configuration of "polarizing plate / first liquid crystal orientation fixing layer / adhesive layer / second liquid crystal orientation fixing layer" is obtained. In the optical laminate, the angle formed by the transmission axis of the polarizer of the polarizing plate and the slow axis of the first liquid crystal orientation fixing layer is 15°, and the angle formed by the transmission axis of the polarizer of the polarizing plate and the slow axis of the second liquid crystal orientation fixing layer is 75°. The average refractive index of the first liquid crystal orientation fixing layer and the second liquid crystal orientation fixing layer is 1.59, and the refractive index of the first liquid crystal orientation fixing layer n LC1 and the refractive index n of the second liquid crystal alignment fixing layer LC2 In the transmission axis direction of the polarizer, the refractive index n is 1.66 and 1.56 respectively. AD and thickness variation TV AD The results are shown in Table 1. The term "refractive index difference from the LC layer" in Table 1 refers to the refractive index n of the first liquid crystal alignment fixing layer. LC1 and the refractive index n of the second liquid crystal alignment fixing layer LC2 The average value in the transmission axis direction of the polarizer is equal to the refractive index n of the adhesive layer. AD The difference between.
[0223] [Examples 2 to 11 and Comparative Examples 1 to 3]
[0224] Optical laminates were respectively obtained in the same manner as in Example 1, except that the configuration of the adhesive layer was changed as in Table 1. The obtained optical laminates were subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0225] Table 1
[0226]
[0227] The optical laminate according to at least one embodiment of the present invention can be applied to image display devices (typically liquid crystal display devices or organic EL display devices).
Claims
1. An optical laminate comprising: A polarizing plate including a polarizer; and a retardation layer, wherein the retardation layer includes, in order from the polarizer side: a first liquid crystal alignment fixing layer, and a second liquid crystal alignment fixing layer laminated on the first liquid crystal alignment fixing layer via an adhesive layer, wherein the retardation layer as a whole has one of a circular polarization function or an elliptical polarization function, and has a relationship of Re(450) < Re(550) < Re(650), and The refractive index of the first liquid crystal alignment fixing layer is n LC1 , the refractive index n of the second liquid crystal alignment fixing layer LC2 and the refractive index n of the adhesive layer AD and the thickness T of the adhesive layer AD and thickness variation TV AD Satisfies the following formula (1): |{(n LC1 + n LC2 ) / 2 – n AD }| × (TV AD / T AD ) × 1,000 ≤ 3.0 (1)。 2 . The optical stack according to claim 1 , wherein the adhesive layer is formed of a pressure-sensitive adhesive.
3. The optical stack according to claim 2, wherein the thickness T of the adhesive layer is AD 4μm or larger. The optical stack according to claim 1 , wherein the adhesive layer is formed of an adhesive.
5. The optical stack according to any one of claims 1 to 4, wherein the refractive index n of the adhesive layer is AD 1.54 or greater. 6 . The optical stack according to claim 1 , wherein the thickness of the first liquid crystal alignment fixing layer is 1.7 μm or less.
7. An image display device comprising the optical stack according to any one of claims 1 to 4.