Gallium nitride p-channel enhanced device with self-aligned structure and preparation method of gallium nitride p-channel enhanced device

By regenerating heavily doped p-type material layer and etchless gate structure on GaN(cap)/Al(In,Ga)N/GaN heterostructure, the problem of performance limitation of GaN p-channel devices is solved, and the problem of achieving the realization of the following: High performance and monolithic integration effects.

CN119069350APending Publication Date: 2024-12-03INST OF MICROELECTRONICS CHINESE ACAD OF SCI LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411218103.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The performance of GaN p-channel devices in logic circuits and large-scale integration is limited by current capability and threshold voltage, especially because channel resistance and drift region resistance balance due to etching groove gate structures are difficult to achieve.

Method used

Using a self-aligning structure and a heavily doped layer, the p-type material layer is regenerated on the GaN(cap)/Al(In,Ga)N/GaN heterostructure, combined with the etch-free gate structure, and achieve high power. Functions of ohmic contact and low channel resistance, reducing on-resistance.

Benefits of technology

It realizes high-performance p-channel devices, has good threshold uniformity and output performance, and is compatible with n-channel device processes, realizing monolithic integration of n/p devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069350A_ABST
    Figure CN119069350A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a gallium nitride p channel enhanced device with a self-aligned structure, and the method comprises the steps: S1, preparing a heteroepitaxial substrate which comprises a substrate, a buffer layer, a barrier layer and a cap layer from bottom to top; s2, preparing a hard mask layer on the surface of the cap layer; s3, the hard mask layer in the middle area of the device is reserved to expose the cap layer, or the heteroepitaxial structures on the two sides of the device are etched at different depths to expose the buffer layer; s4, growing a heavily doped p-type material layer on the exposed cap layer or buffer layer to obtain a source-drain region, and removing the hard mask layer in the middle region to obtain a groove-shaped gate region; s5, preparing an ohmic contact electrode on the p-type material layer to obtain a source electrode and a drain electrode; and S6, depositing a gate dielectric layer on the surface of the groove-shaped gate region, and growing metal to obtain a gate, thereby completing the preparation of the gallium nitride p channel enhanced device with the self-aligned structure. Meanwhile, the invention also provides the gallium nitride p channel enhanced device with the self-aligned structure, which is prepared by the preparation method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of semiconductor technology, and in particular to a self-aligned structured gallium nitride p-channel enhancement type device and a preparation method thereof. Background Art

[0002] The wide bandgap characteristics of GaN make the devices and circuits made of it have application prospects in extreme environments, such as aerospace, deep-sea exploration, etc. The coexistence of 2DEG (2-D ElectronGas) and 2DHG (2-D Hole Gas) in the GaN (cap) / Al (In, Ga) N / GaN heterostructure makes the monolithic integration of n / p channel devices possible. Compared with the existing high-performance GaN n-channel devices, GaN's realization of logic circuits and large-scale integration are mainly faced with the constraints of p-channel device performance, including current capability, threshold voltage (enhancement mode) and other scientific issues. For the data on the proportion of resistance of each part of the p-channel device, the channel resistance and drift region resistance account for the vast majority. For the gate channel, it is difficult to obtain a good balance between the threshold voltage and the channel resistance due to the damage introduced by the etching groove gate structure. Summary of the invention

[0003] In view of this, the present disclosure provides a self-aligned structured gallium nitride p-channel enhancement mode device and a preparation method thereof, which achieves good ohmic contact by heavily doping layers and selecting metals with high work functions, while the non-etched gate structure ensures high channel mobility and low channel resistance, thereby realizing a high-performance p-channel device.

[0004] In order to achieve the above purpose, the technical solution of the present invention is as follows:

[0005] According to an embodiment of one aspect of the present disclosure, a method for preparing a self-aligned structured gallium nitride p-channel enhancement-mode device is provided, comprising: operation S1: preparing a heteroepitaxial substrate, including, from bottom to top, a substrate, a buffer layer, a barrier layer, and a cap layer; operation S2: preparing a hard mask layer on the surface of the cap layer; operation S3: retaining the hard mask layer in the middle region of the device to expose the cap layer, or etching the heteroepitaxial structure on both sides of the device to different depths so as to expose the buffer layer; operation S4: regrowing a heavily doped p-type material layer on the exposed cap layer or buffer layer to obtain a source and drain region, and removing the hard mask layer in the middle region to obtain a groove-shaped gate region; operation S5: preparing an ohmic contact electrode on the p-type material layer to obtain a source and a drain; operation S6: depositing a gate dielectric layer on the surface of the groove-shaped gate region, and growing a metal to obtain a gate, thereby completing the preparation of the self-aligned structured gallium nitride p-channel enhancement-mode device.

[0006] According to the embodiment of the present disclosure, the buffer layer is a GaN buffer layer; the barrier layer is an Al(In, Ga)N barrier layer; and the cap layer is a GaN cap layer.

[0007] According to the embodiment of the present disclosure, the thickness of the barrier layer is in the range of 3-25 nm; the barrier layer may be Al x Ga (1-x) N ternary alloy barrier layer, wherein the Al composition is between 0 and 100%.

[0008] According to the embodiment of the present disclosure, the thickness of the barrier layer is in the range of 3-25 nm; the barrier layer may be Al x In (1-x) N ternary alloy barrier layer, wherein the Al component is between 75% and 90%.

[0009] According to an embodiment of the present disclosure, the thickness of the barrier layer is in the range of 3-25 nm; the barrier layer may be an AlxInyGa(1-xy)N quaternary alloy barrier layer, wherein the Al and In components are between 0 and 100%.

[0010] According to the embodiment of the present disclosure, the cap layer is undoped or p-type doped, and the doping concentration is between 0 and 1×10 21 cm -3 The thickness is between 3 and 200 nm.

[0011] According to the embodiment of the present disclosure, the p-type material layer is grown by MBE or MOCVD process, and the p-type material layer is heavily doped with p + -InGaN or p + -AlGaN, where the Al and In components are between 0 and 100%; the thickness of the p-type material layer is between 5 and 200 nm, and the doping concentration is between 1×10 17 ~1×10 21 cm -3 between.

[0012] According to the embodiment of the present disclosure, the thickness of the gate dielectric layer is between 5 and 40 nm, and the preparation material is selected from Al2O3, SiN x , SiO 2, NiO,Ga x O 1-x N, Al x Si 1-x O or Al x Si 1-x N.

[0013] According to the embodiment of the present disclosure, the gate is a single-layer gate structure or a composite gate structure, the composite gate structure includes a dielectric insertion layer recessed into the groove and a high-insulation gate dielectric layer, wherein the thickness of the dielectric insertion layer is between 0 and 5 nm, and is used to reduce the interface state density between the high-insulation gate dielectric and the III-group nitride hierarchical structure, the dielectric insertion layer is a single crystal or a nearly single crystal dielectric, and the preparation material is selected from AlN, SiN x or GaO x .

[0014] Another aspect of the present disclosure provides a self-aligned gallium nitride p-channel enhancement mode device prepared by any of the preparation methods described above. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] The above and other objects, features and advantages of the present disclosure will become more apparent through the following description of the embodiments of the present disclosure with reference to the accompanying drawings, in which:

[0016] Figure 1 A flow chart of a method for preparing a self-aligned GaN p-channel enhancement mode device according to an embodiment of the present disclosure is shown;

[0017] Figure 2 The process flow chart of preparing a self-aligned gallium nitride p-channel enhancement mode device according to an embodiment of the present disclosure is shown.

[0018] Figure 3 The process flow chart of preparing another self-aligned structure gallium nitride p-channel enhancement mode device according to an embodiment of the present disclosure is shown. DETAILED DESCRIPTION

[0019] The present invention provides a self-aligned GaN p-channel enhancement device and a preparation method thereof, and prepares a p-channel device with Al(In,Ga)N barrier based on GaN(cap) / Al(In,Ga)N / GaN heterostructure. + -InGaN or p + -AlGaN method, reducing ohmic contact resistance, non-etched gate structure ensures high channel mobility and low channel resistance, effectively reducing the on-resistance of the device and achieving a larger current capacity of the device. The GaN-based enhanced p-channel device prepared by this technology has good threshold uniformity and output performance, and is compatible with the process preparation of n-channel devices, and can achieve monolithic integration of n / p devices.

[0020] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.

[0021] In an embodiment of the present disclosure, a method for preparing a self-aligned GaN p-channel enhancement mode device is provided. Figures 1 to 3 As shown, the preparation method comprises:

[0022] Operation S1: preparing a heteroepitaxial substrate, including a substrate, a buffer layer, a barrier layer, and a cap layer from bottom to top;

[0023] Operation S2: preparing a hard mask layer on the surface of the cap layer;

[0024] Operation S3: retaining the hard mask layer in the middle region of the device to expose the cap layer, or etching the heteroepitaxial structure on both sides of the device to expose the buffer layer;

[0025] Operation S4: regrowing a heavily doped p-type material layer on the exposed cap layer or buffer layer to obtain a source / drain region, and removing the hard mask layer in the middle region to obtain a groove-shaped gate region;

[0026] Operation S5: preparing an ohmic contact electrode on the p-type material layer to obtain a source electrode and a drain electrode;

[0027] Operation S6: preparing a gate dielectric layer on the surface of the grooved gate region, and preparing an ohmic contact electrode to obtain a gate, thereby completing the preparation of a self-aligned structured gallium nitride p-channel enhancement mode device.

[0028] It should be noted that in operation S3, when the heteroepitaxial structure on both sides of the device is etched, different degrees of etching can be performed according to actual conditions. For example, the etching process can automatically stop on the surface of the barrier layer (Al(In,Ga)N layer), or the Al(In,Ga)N barrier layer can be completely etched and removed (over-etched) to the surface of the buffer layer, or a portion of the buffer layer can be etched to obtain the source and drain regions on both sides.

[0029] In operation S3 , retaining the hard mask layer in the middle region of the device involves processes such as marking or patterning, and unnecessary hard mask layers can be removed.

[0030] According to the embodiment of the present disclosure, the thickness of the barrier layer can be in the range of 3-25 nm, and it is characterized in that the barrier layer can be Al x Ga (1-x) N ternary alloy barrier layer, wherein the Al component is between 0 and 100%; the Al(In,Ga)N barrier layer can also be Al x In (1-x) N ternary alloy barrier layer, wherein the Al component is between 75% and 90%; the Al(In,Ga)N barrier layer can also be Al x In y Ga (1-x-y) N quaternary alloy barrier layer, wherein Al and In compositions are between 0 and 100%;

[0031] According to the embodiment of the present disclosure, the cap layer (cap layer) is undoped or p-type doped, and the doping concentration is between 0 and 1×10 21 cm -3 Between, the thickness is between 3nm~200nm;

[0032] In the above preparation process, the hard mask and regrowth are used to form the source and drain regions (p + -InGaN or p + -AlGaN) can be SiO2 or SiNx, etc.

[0033] Use MBE (molecular beam epitaxy) or MOCVD (metal organic chemical vapor deposition) and other growth methods to grow heavily doped p + -InGaN or p + -AlGaN, obtain a p-type material layer to reduce the ohmic contact resistance; wherein the Al and In components are between 0 and 100%; heavily doped p + -InGaN or p + -AlGaN layer thickness is between 5nm~200nm, and doping concentration is between 1×10 17 cm -3 ~1×10 21 cm -3 between.

[0034] When preparing the gate, the gate structure can adopt a single-layer gate structure, deposit a single layer of high-insulation gate dielectric to reduce gate leakage, and the thickness of the high-insulation gate dielectric layer is between 5 nm and 40 nm, such as Al2O3, SiN x , SiO 2, NiO,Ga x O 1-x N, Al x Si 1-x O or Al x Si 1-x N; The gate structure can also adopt a composite gate structure, which includes a dielectric insertion layer recessed into the recessed gate groove and a high-insulation gate dielectric layer, wherein the thickness of the dielectric insertion layer is between 0 and 5 nm, which is used to reduce the interface state density between the high-insulation gate dielectric and the III-nitride hierarchical structure, and the dielectric insertion layer is made of a single crystal or a nearly single crystal dielectric, such as AlN, SiN x or GaO x。

[0035] The present invention adopts a self-aligned process to prepare an enhanced GaN p-channel device, which specifically includes the following process steps: GaN(cap) / Al(In,Ga)N / GaN heteroepitaxial substrate; marking; etching of GaN(cap) / Al(In,Ga)N / GaN in the source and drain regions; + -InGaN or p + -AlGaN regrowth; Ohmic contact; Device isolation process; Gate dielectric deposition; Gate metal deposition. Figure 2 The p-channel enhancement mode transistor is realized by using the unetched GaN(cap) / Al(In,Ga)N heterojunction and the regrowth heavily doped p + -InGaN or p + -AlGaN and self-aligned process methods reduce the ohmic contact resistance of GaN p-channel devices, reduce process complexity, achieve a larger current level, and ensure good conduction capability of the device while realizing an enhanced p-channel device.

[0036] In the embodiment of the present disclosure, Figure 2 and Figure 3 As shown, the present disclosure also provides two self-aligned gallium nitride p-channel enhancement mode devices with different structures prepared by the above-mentioned preparation method.

[0037] So far, the embodiments of the present disclosure have been described in detail in conjunction with the accompanying drawings. It should be noted that the implementation methods not shown or described in the drawings or the body of the specification are all forms known to ordinary technicians in the relevant technical field and are not described in detail. In addition, the above definitions of each element and method are not limited to the various specific structures, shapes or methods mentioned in the embodiments, and ordinary technicians in the field can simply change or replace them.

[0038] Based on the above description, those skilled in the art should have a clear understanding of the self-aligned structured gallium nitride p-channel enhancement mode device and the preparation method disclosed in the present invention.

[0039] In summary, the present disclosure provides a self-aligned structured gallium nitride p-channel enhancement mode device and a preparation method thereof. The preparation method is based on a self-aligned process and achieves good ohmic contact through regrowth. At the same time, the non-etched gate structure ensures high channel mobility and low channel resistance, effectively reduces the on-resistance of the device, realizes high-performance p-channel devices, and is compatible with the process preparation of n-channel devices, and can realize monolithic integration of n / p devices.

[0040] It should be noted that, in this document, unless otherwise specified, “a” element is not limited to a single element, but may include one or more elements.

[0041] In addition, in this document, unless otherwise specified, ordinal numbers such as "first" and "second" are only used to distinguish multiple components with the same name, and do not indicate that there is a hierarchy, level, execution order, or process order between them. A "first" component and a "second" component may appear together in the same component, or appear in different components. The presence of a component with a larger ordinal number does not necessarily indicate the presence of another component with a smaller ordinal number.

[0042] In this document, unless otherwise specified, the so-called feature A "or" or "and / or" (and / or) feature B means that A exists alone, B exists alone, or A and B exist at the same time; the so-called feature A "and" (and) or "and" (and) or "and" (and) feature B means that A and B exist at the same time; the so-called "include", "comprise", "have" and "contain" mean including but not limited to these.

[0043] In addition, in this document, the terms "upper", "lower", "left", "right", "front", "back", or "between" are only used to describe the relative positions between multiple elements, and can be extended to include translation, rotation, or mirroring. In addition, in this document, unless otherwise specified, "an element is on another element" or similar descriptions do not necessarily mean that the element contacts the other element.

[0044] In addition, unless the steps are specifically described or must occur in sequence, the order of the above steps is not limited to the above list, and can be changed or rearranged according to the required design. And the above embodiments can be mixed and matched with each other or with other embodiments based on design and reliability considerations, that is, the technical features in different embodiments can be freely combined to form more embodiments.

[0045] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above description is only a specific embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the protection scope of the present disclosure.

Claims

1. A method for preparing a self-aligned GaN p-channel enhancement mode device, comprising: Operation S1: preparing a heteroepitaxial substrate, including a substrate, a buffer layer, a barrier layer, and a cap layer from bottom to top; Operation S2: preparing a hard mask layer on the surface of the cap layer; Operation S3: retaining the hard mask layer in the middle region of the device to expose the cap layer, or etching the heteroepitaxial structure on both sides of the device to different depths to expose the buffer layer; Operation S4: regrowing a heavily doped p-type material layer on the exposed cap layer or buffer layer to obtain a source / drain region, and removing the hard mask layer in the middle region to obtain a groove-shaped gate region; Operation S5: preparing an ohmic contact electrode on the p-type material layer to obtain a source electrode and a drain electrode; Operation S6: depositing a gate dielectric layer on the surface of the grooved gate region, and growing a metal to obtain a gate, thereby completing the preparation of a self-aligned structured gallium nitride p-channel enhancement mode device. 2 . The preparation method according to claim 1 , wherein the buffer layer is a GaN buffer layer; the barrier layer is an Al(In, Ga)N barrier layer; and the cap layer is a GaN cap layer.

3. The preparation method according to claim 1 or 2, wherein the thickness of the barrier layer is in the range of 3-25 nm; the barrier layer may be Al x Ga (1-x) N ternary alloy barrier layer, wherein the Al composition is between 0 and 100%.

4. The preparation method according to claim 1 or 2, wherein the thickness of the barrier layer is in the range of 3-25 nm; the barrier layer may be Al x In (1-x) N ternary alloy barrier layer, wherein the Al component is between 75% and 90%.

5. The preparation method according to claim 1 or 2, wherein the thickness of the barrier layer is in the range of 3-25 nm; the barrier layer may be Al x In y Ga (1-x-y) N quaternary alloy barrier layer, wherein the Al and In compositions are between 0 and 100%.

6. The preparation method according to claim 1 or 2, wherein the cap layer is undoped or p-type doped, and the doping concentration is between 0 and 1×10 21 cm -3 The thickness is between 3 and 200 nm.

7. The preparation method according to claim 1 or 2, wherein the p-type material layer is grown by MBE or MOCVD process, and the p-type material layer is heavily doped with p + -InGaN or p + -AlGaN, where the Al and In compositions are between 0 and 100%; The thickness of the p-type material layer is between 5 and 200 nm, and the doping concentration is between 1×10 17 ~1×10 21 cm -3 between.

8. The preparation method according to claim 1 or 2, wherein the thickness of the gate dielectric layer is between 5 and 40 nm, and the preparation material is selected from Al2O3, SiN x , SiO 2, NiO,Ga x O 1-x N, Al x Si 1-x O or Al x Si 1-x N.

9. The preparation method according to claim 8, wherein the gate is a single-layer gate structure or a composite gate structure, the composite gate structure comprises a dielectric insertion layer recessed into the groove and a high-insulation gate dielectric layer, wherein the thickness of the dielectric insertion layer is between 0 and 5 nm, and is used to reduce the interface state density between the high-insulation gate dielectric and the III-nitride hierarchical structure, the dielectric insertion layer is a single crystal or a nearly single crystal dielectric, and the preparation material is selected from AlN, SiN x or GaO x .

10. A self-aligned gallium nitride p-channel enhancement mode device prepared according to the preparation method according to any one of claims 1 to 9.