Thick epitaxy alignment method
The thick epitaxial alignment method forms a protruding alignment mark using a hard mask layer with distinct etching properties, ensuring clear visibility and stability during thick epitaxial processes, addressing the obscuration issue in existing technologies.
Patent Information
- Application Number
- CN202410852757.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-12-03
AI Technical Summary
Existing methods fail to maintain clear alignment marks for thick epitaxial layers due to the marks being obscured by the increasing thickness of the epitaxial layer, leading to difficulties in layer alignment during subsequent processes.
A thick epitaxial alignment method involving the formation of a hard mask layer with a specific thickness, followed by etching to create an alignment mark that protrudes from the substrate, using materials with different etching rates to ensure the mark remains visible despite the thick epitaxial layer deposition.
The method ensures that alignment marks remain clearly identifiable even after thick epitaxial deposition, maintaining accurate layer alignment by compensating for the thickness of the epitaxial layer with a higher hard mask layer, thus enhancing process stability.
Smart Images

Figure CN119069407A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of integrated circuit design and manufacturing, and in particular to a thick epitaxial alignment method. Background Art
[0002] High-voltage devices usually need to produce buried layers or high-voltage wells of high-voltage devices before the logic process is formed, and then grow epitaxial EPI as a voltage-resistant layer, and then pattern the active area. Therefore, the epitaxial layer needs to be aligned with the layer before the epitaxial layer to ensure that the buried layer or high-voltage well layer and other pre-epitaxial structural layers are in the correct position in the subsequent process. Usually, in order to achieve alignment accuracy after the epitaxial process, an alignment mark with a certain step difference or material difference is generated before the epitaxial process. After the epitaxial growth, its outline is used as the alignment mark in processes such as lithography.
[0003] As the withstand voltage of high-voltage devices increases, the thickness of the epitaxial layer becomes thicker and thicker. When the epitaxial layer reaches a certain thickness, the alignment marks before the epitaxial process will disappear and cannot be identified, resulting in the inability to align the layers after the epitaxial process in subsequent processes. Figures 1 to 3 As shown, the grooves in the figure represent photolithography marks. Figures 1 to 3 The thickness of the epitaxial layers shown gradually increases. After the epitaxial layers are formed, the initial marks become significantly lighter and thinner, and the clarity is reduced during the alignment process, which increases the difficulty of alignment. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a thick epitaxial alignment method, which can also form clear alignment marks with high readability for thick epitaxial processes.
[0005] To solve the above problems, the present invention provides a thick epitaxial alignment method, comprising the following steps: First, a hard mask layer with a certain thickness is formed on the substrate where the epitaxial layer is to be deposited, and then zero-layer photolithography and etching are performed to define an etching window of an alignment mark on the hard mask layer, and the hard mask layer is etched and then the etching is continued downward into the substrate layer to form a filling window of the alignment mark; Depositing a filling layer, wherein the filling layer fills the filling window of the alignment mark; Etching and removing the hard mask layer, after which the alignment mark in the filling window protrudes from the surface of the substrate and has a protruding height not less than the thickness of the hard mask layer, thereby forming an alignment mark; An epitaxial layer is deposited to form an epitaxial layer of a desired thickness.
[0006] The thickness of the deposited hard mask layer is at least 1.5 times the thickness of the epitaxial layer to be deposited.
[0007] The thickness of the deposited hard mask layer is the thickness of the epitaxial layer to be deposited plus at least 1 μm.
[0008] Furthermore, the material of the hard mask layer is silicon oxide or silicon nitride.
[0009] Furthermore, the filling layer is made of silicon oxide, silicon nitride, epitaxial silicon, or polycrystalline silicon.
[0010] Furthermore, the hard mask layer and the filling layer are made of different materials and have different etching rates or selectivities in dry etching, wet etching or CMP processes.
[0011] The epitaxial layer can also be deposited in steps: Firstly, a first epitaxial deposition process is performed to deposit an epitaxial layer with a first thickness, wherein the thickness of the epitaxial layer with the first thickness can cover the alignment mark; Performing an etching process to etch back the epitaxial layer of the first thickness to expose the alignment mark; The second epitaxial deposition process is continued to deposit the epitaxial layer until a predetermined thickness is reached to form a final epitaxial layer.
[0012] Furthermore, the etching process adopts an isotropic etching process to etch the epitaxial layer of the first thickness.
[0013] Furthermore, before the second epitaxial deposition process is performed, a heating repair process is also performed to repair the surface damage of the epitaxial layer caused by the epitaxial back etching process.
[0014] Furthermore, the repair process is to repair the epitaxial silicon surface in an oxygen atmosphere.
[0015] Furthermore, before the second epitaxial deposition process, a pre-cleaning step for removing the damaged layer after oxidation is also included, so that the single crystal silicon layer is exposed before the second epitaxial deposition process.
[0016] The thick epitaxial alignment method of the present invention first deposits a hard mask layer with a certain thickness, and compensates the influence of the thick epitaxial layer on the alignment mark by the thickness of the hard mask layer to form an alignment mark with a higher height, and then deposits a thick epitaxial layer to eliminate the influence of the thickness of the epitaxial layer on the alignment mark. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figures 1 to 3 This is a schematic diagram showing that in an epitaxial deposition process, as the thickness of the epitaxial layer increases, the alignment mark is gradually covered and the readability becomes poor.
[0018] Figures 4 to 11It is a schematic diagram of the steps of the method of the present invention. Description of Reference Numerals
[0019] 1 is the substrate, 2 is the hard mask layer, and 3 is the filling layer (alignment mark) DETAILED DESCRIPTION
[0020] The following is a specific implementation of the present invention in conjunction with the accompanying drawings, and the technical solutions in the present invention are clearly and completely described, but the present invention is not limited to the following implementations. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. According to the following description and claims, the advantages and features of the present invention will be clearer. It should be noted that the drawings are all in a very simplified form and use non-precise ratios, which are only used to conveniently and clearly assist in explaining the embodiments of the present invention. All other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0021] The present invention can be implemented in different forms and should not be interpreted as being limited to the embodiments proposed herein. On the contrary, providing these embodiments will make the disclosure thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. In the accompanying drawings, for clarity, the size and relative size of the layers and zones may be exaggerated, and the same reference numerals represent the same elements from beginning to end. In the description of the present application, it should be noted that the orientation or positional relationship indicated by the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside", etc. is based on the orientation or positional relationship shown in the accompanying drawings, only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation to the present application. In addition, the terms "first", "second", and "third" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.
[0022] The present invention discloses a thick epitaxial alignment method, which mainly forms an alignment mark on the substrate surface that is much higher than the original substrate surface before the thick epitaxial layer is deposited, so that after the epitaxial layer deposition process, the thick epitaxial layer formed still cannot cover the alignment mark, and a clear alignment mark can still be formed in the subsequent process. Figure 4 Compared with the prior art, in which the alignment mark is formed below the substrate or only exceeds the substrate by a small proportion of the EPI growth thickness (generally 1 / 10 to 1 / 100, such as growing an epitaxial layer with a thickness of 4 μm, the alignment mark layer SiN / SiO2 is only 500 to 2000 Å above the surface), the alignment mark formed in the present invention needs to be much higher than the original substrate, which is mainly adjusted by the thickness of the hard mask layer.
[0023] Specifically, first, a thick hard mask layer 2 is formed on the surface of the substrate where the epitaxial layer is to be deposited. Figure 5 As shown, the thickness Dh of the hard mask layer 2 is at least 1.5 times the thickness De of the epitaxial layer to be deposited, that is, Dh≥1.5De; or, according to specific process conditions, the thickness Dh of the hard mask layer is more than 1μm greater than the thickness of the epitaxial layer to be deposited, that is, Dh≥De+1μm.
[0024] The material of the hard mask layer may be silicon nitride, silicon oxide or the like.
[0025] Zero-layer photolithography and etching are performed to etch through the hard mask layer and into the substrate to form a pattern with a certain depth. Figure 6 shown.
[0026] Deposit a filling layer 3, such as silicon nitride or silicon oxide, epitaxial single crystal silicon, polycrystalline silicon, etc. Figure 7 The filling layer is filled into the space between the etched hard mask and the substrate.
[0027] The entire hard mask layer is removed by etching to expose the substrate surface. Figure 8 The materials of the aforementioned hard mask layer and the filling layer are the several materials mentioned above, but they need to be different materials, because in the subsequent dry, wet etching or CMP processes, the hard mask layer needs to be selectively removed while the filling layer material needs to be retained. Therefore, the two materials need to have different etching rates or grinding rates in the removal process to ensure the selection ratio, so as to remove only the hard mask layer.
[0028] The filling layer filled in the space formed by the original etching is retained to form an alignment mark protruding from the surface of the substrate. Figure 8 As shown in , unlike the alignment marks formed by the prior art, the alignment marks formed by the present invention are rooted in a certain depth of the underlying substrate layer. Since the height of the alignment marks formed by the present invention is much greater than the alignment marks formed by the traditional process, the alignment marks inserted into the substrate to a certain depth have better stability in the subsequent process and are not easy to fall over. Since the alignment marks of the present invention are much higher than the substrate, it is impossible to use traditional technology to deposit other film layers (such as SiO2, SiN, etc.) on the substrate, and then form alignment marks on the film layer or film layer + substrate by photolithography and etching. Using traditional methods, it is easy for the alignment marks formed by the excessively large aspect ratio to overturn and become unusable. Therefore, the present invention requires that a part of the alignment mark enter a certain depth into the silicon substrate to ensure that it will not overturn in subsequent process steps.
[0029] The epitaxial layer deposition process is then performed. The present invention provides two epitaxial layer deposition schemes: First, a one-time deposition is used to complete the epitaxial layer of required thickness, that is, the thickness of De, and the process is completed directly.
[0030] Second, the epitaxial layer of the thickness is deposited by a step-by-step deposition method, that is, the epitaxial layer of the thickness De is deposited twice. It should be noted that when the epitaxial layer of the thickness De is deposited by the distributed deposition method, the thickness of the hard mask layer in the previous process needs to be adjusted. It is no longer at least 1.5 times the thickness De of the epitaxial layer or more than 1 μm greater than the thickness of the epitaxial layer to be deposited, but is adjusted to 1 / 3 to 1 / 2 of the thickness De of the epitaxial layer. The other parameters are the same as above. The alignment mark formed after the hard mask is removed is still far higher than the substrate and inserted into the substrate to a certain depth, and has a certain stability.
[0031] The epitaxial layer is deposited twice to form an epitaxial layer with a thickness of De: The first epitaxial layer is grown to form an epitaxial layer with a first thickness D1 on the surface of the substrate, wherein the first thickness D1 is less than De. Fig. 9 shown.
[0032] An isotropic etching is performed to etch back a portion of the epitaxial layer of the first thickness D1 to expose the alignment mark, such as Fig.10 shown.
[0033] After etching, a thermal process can be selectively performed to repair the damage to the epitaxial surface caused by the etching process. Oxygen or other necessary gases can be introduced to oxidize and repair the epitaxial silicon surface, and then the damaged layer can be removed.
[0034] After removing the damaged layer, a pre-clean step may be selectively performed to clean the etching residues on the surface of the wafer.
[0035] Continue to grow the second epitaxial layer, and continue to grow the epitaxial layer on the surface of the substrate until the thickness of the epitaxial layer reaches De. Fig.11 shown.
[0036] After forming a thick epitaxial layer in this way, although the alignment mark may still be covered by an epitaxial layer of a certain thickness, the thickness of the epitaxial layer that blocks the alignment mark is much smaller than the original thickness of the epitaxial layer. The alignment mark can still maintain good clarity. Even if the deposited epitaxial layer is thicker, since a thicker hard mask layer is originally formed and then etched to form the alignment mark, the influence of the epitaxial layer thickness can be offset after epitaxial deposition, and the alignment mark can still be clearly identified.
[0037] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A thick epitaxial alignment method, characterized in that: The following steps are included: First, a hard mask layer with a certain thickness is formed on the substrate where the epitaxial layer is to be deposited, and then zero-layer photolithography and etching are performed to define an etching window of an alignment mark on the hard mask layer, and the hard mask layer is etched and then the etching is continued downward into the substrate layer to form a filling window of the alignment mark; Depositing a filling layer, wherein the filling layer fills the filling window of the alignment mark; The hard mask layer is removed by etching, and after the hard mask layer is removed, the alignment mark in the filling window protrudes from the surface of the substrate, has a protruding height not less than the thickness of the hard mask layer, and the alignment mark is embedded in the lower substrate to a certain depth, forming an alignment mark with a stable structure; An epitaxial layer is deposited to form an epitaxial layer of a desired thickness.
2. The thick epitaxial alignment method according to claim 1, characterized in that: The thickness of the deposited hard mask layer is at least 1.5 times the thickness of the epitaxial layer to be deposited.
3. The thick epitaxial alignment method according to claim 1, characterized in that: The thickness of the deposited hard mask layer is the thickness of the epitaxial layer to be deposited plus at least 1 μm.
4. The thick epitaxial alignment method according to claim 1, characterized in that: The material of the hard mask layer is silicon oxide or silicon nitride.
5. The thick epitaxial alignment method according to claim 1, characterized in that: The filling layer is made of silicon oxide, silicon nitride, epitaxial silicon, or polycrystalline silicon.
6. The thick epitaxial alignment method according to claim 1, characterized in that: The hard mask layer and the filling layer are made of different materials and have different etching rates or selectivity ratios in dry etching, wet etching or CMP processes.
7. A thick epitaxial alignment method, characterized in that: The following steps are included: First, a hard mask layer with a certain thickness is formed on the substrate where the epitaxial layer is to be deposited, and then zero-layer photolithography and etching are performed to define an etching window of an alignment mark on the hard mask layer, and the hard mask layer is etched and then the etching is continued downward into the substrate layer to form a filling window of the alignment mark; Depositing a filling layer, wherein the filling layer fills the filling window of the alignment mark; The hard mask layer is removed by etching, and after the hard mask layer is removed, the alignment mark in the filling window protrudes from the surface of the substrate, has a protruding height not less than the thickness of the hard mask layer, and the alignment mark is embedded in the lower substrate to a certain depth, forming an alignment mark with a stable structure; Firstly, a first epitaxial deposition process is performed to deposit an epitaxial layer with a first thickness, wherein the thickness of the epitaxial layer with the first thickness can cover the alignment mark; Performing an etching process to etch back the epitaxial layer of the first thickness to expose the alignment mark; The second epitaxial deposition process is continued to deposit the epitaxial layer until a predetermined thickness is reached to form a final epitaxial layer.
8. The thick epitaxial alignment method according to claim 7, characterized in that: The thickness of the hard mask layer is 1 / 3 to 1 / 2 of the total thickness of the thick epitaxial layer to be deposited.
9. The thick epitaxial alignment method according to claim 7, characterized in that: The material of the hard mask layer is silicon oxide or silicon nitride.
10. The thick epitaxial alignment method according to claim 7, characterized in that: The filling layer is made of silicon oxide, silicon nitride, epitaxial silicon, or polycrystalline silicon.
11. The thick epitaxial alignment method according to claim 7, characterized in that: The hard mask layer and the filling layer are made of different materials and have different etching rates or selectivity ratios in dry etching, wet etching or CMP processes.
12. The thick epitaxial alignment method according to claim 7, characterized in that: The etching process uses an isotropic etching process to etch the epitaxial layer of the first thickness.
13. The thick epitaxial alignment method according to claim 7, characterized in that: Before the second epitaxial deposition process is performed, a heating repair process is also performed to repair the surface damage of the epitaxial layer caused by the epitaxial back etching process.
14. The thick epitaxial alignment method according to claim 7, characterized in that: The repair process is to repair the epitaxial silicon surface in an oxygen atmosphere.
15. The thick epitaxial alignment method according to claim 7, characterized in that: Before the second epitaxial deposition process, a pre-cleaning step for removing the damaged layer after oxidation is also included, and before the second epitaxial deposition process, the single crystal silicon layer is exposed.