Thin film cathode material, preparation method and flexible all-solid-state lithium ion battery
By depositing a protective film on the nickel-cobalt-manganese ternary cathode material of lithium-ion batteries, the problems of poor battery performance and safety are solved, high energy density and stability are achieved, and the risk of explosion is reduced.
Patent Information
- Application Number
- CN202411026928.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-12-03
AI Technical Summary
The electrochemical, thermal stability and safety performance of existing lithium-ion batteries are poor, especially the structural stability and circulation performance of nickel-cobalt-manganese ternary cathode materials under high nickel content, which poses a risk of explosion.
Prepare protective layer films (such as Li3PO4, LiPON or ZnO) on the LiNi1-x-yCoxMnyO2 cathode film, and deposit the protective layer through radio frequency magnetron sputtering technology to prevent direct contact between NCM and electrolyte, inhibit Mn dissolution side reactions, and improve conductivity rate and structural stability.
It significantly improves the discharge specific capacity, cycle stability and rate performance of lithium-ion batteries, enhances the safety of the battery, prevents explosion, and maintains battery stability in the bending state.
Smart Images

Figure CN119069616A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a thin film cathode material, a preparation method and a flexible all-solid-state lithium ion battery. Background Art
[0002] Lithium-ion batteries have the remarkable characteristics of high voltage, high capacity, long cycle life, good safety performance and no memory effect. They are a green and environmentally friendly new energy storage battery and have been widely used in new energy vehicles, energy storage, 3C consumer electronics, 5G data centers, smart terminals and other fields.
[0003] Materials such as lithium cobalt oxide, lithium nickel oxide and lithium iron phosphate are difficult to meet the needs of long-term battery life in the new energy field due to their low energy density, while nickel-cobalt-manganese ternary positive electrode materials (NCM, LiNi 1-x-y Co x Mn y O2) integrates the advantages of the three materials under the synergistic effect of Ni, Co and Mn elements, namely the high specific capacity of nickel-based materials, the good cycle performance of cobalt-based materials and the high safety of manganese-based materials. It is a lithium-ion electrode material with good development prospects at present, with the advantages of high specific capacity, good thermal stability, good cycle performance and low cost. However, its shortcomings still need to be improved, such as low electronic conductivity and poor high-rate stability. And current studies have shown that with the increase of Ni content, the structural stability, battery cycle performance, battery rate performance and thermal stability of high-nickel ternary materials in the charging and discharging process have decreased to varying degrees, resulting in poor electrochemical performance, thermal stability and safety performance of the battery. These shortcomings have hindered the development of lithium-ion batteries to a certain extent.
[0004] In addition, commonly used rechargeable lithium-ion batteries use liquid electrolytes. Due to the presence of these liquid electrolytes, when the battery is overcharged, has an internal short circuit or other abnormal conditions, there is a risk of fire or explosion, which greatly limits the scope of use of the battery. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a thin film cathode material, a preparation method and a flexible all-solid-state lithium-ion battery to solve the problems of poor electrochemical performance, thermal stability and safety performance of batteries in the prior art.
[0006] The technical solution of the present invention to solve the above technical problems is as follows:
[0007] The present invention provides a method for preparing a thin film cathode material, comprising preparing a cathode film on a substrate; preparing a protective layer film on the surface of the cathode film; and preparing a material of the cathode film being LiNi 1-x-y Co x Mn yFor O2, the value ranges of x and y are such that 0 < x < 1 and 0 < y < 1; the protective layer film is a Li3PO4 film, a LiPON film or a ZnO film.
[0008] Based on the above technical solution, the present invention can be further improved as follows.
[0009] Furthermore, the thickness of the protective layer film is 15 - 30 nm.
[0010] Furthermore, it further includes the following steps:
[0011] S1. Prepare a Pt buffer layer on a metal substrate to obtain the substrate;
[0012] S2. Prepare the cathode film on the substrate by radio frequency magnetron sputtering or coating;
[0013] S3. Sputter deposit a protective layer target on the cathode film by magnetron sputtering to obtain the protective layer film.
[0014] Furthermore, in step S2, the first working gas for the radio frequency magnetron sputtering is a mixed gas of argon and oxygen, the vacuum degree of the radio frequency magnetron sputtering is 0.1 - 0.7 Pa, the radio frequency power supply power is 50 - 100 W, the pre-sputtering time is 25 - 35 min, sputtering is carried out without bias voltage, the sputtering time is 2 - 8 h, annealing is carried out after sputtering, the temperature of the annealing is 500 - 800 °C, and the time is 3 h - 5 h.
[0015] Furthermore, in step S3, magnetron sputtering is carried out in an environment filled with a second working gas, the vacuum degree of the magnetron sputtering is 0.4 - 0.6 Pa, and the radio frequency power is 50 - 100 W.
[0016] Furthermore, when the protective layer film is a Li3PO4 film, the target of the protective layer is a Li3PO4 target, the second working gas is argon, and the sputtering time is 2 - 4 min;
[0017] When the protective layer film is a LiPON film, the target of the protective layer is a Li3PO4 target, the second working gas is nitrogen, and the sputtering time is 1 - 7 min;
[0018] When the protective layer film is a ZnO film, the target of the protective layer is a Zn target, the second working gas is a mixed gas of argon and oxygen, and the sputtering time is 1 - 3 min.
[0019] The present invention also provides a thin film cathode material, and the material is prepared by the method as described above.
[0020] The present invention also provides a flexible all-solid-state lithium-ion battery, comprising the thin film cathode material as described above, wherein a solid electrolyte film, an anode film and an anode current collector are sequentially arranged on the protective layer film of the thin film cathode material.
[0021] The present invention also provides a method for preparing the flexible all-solid-state lithium-ion battery as described above, comprising the following steps:
[0022] S4, preparing a solid electrolyte on the protective layer film by radio frequency magnetron sputtering;
[0023] S5, preparing an anode on the solid electrolyte film by radio frequency magnetron sputtering;
[0024] S6. Prepare the anode current collector on the anode by DC magnetron sputtering, and encapsulate and obtain the flexible all-solid-state lithium-ion battery.
[0025] Further, in step S4, the sputtering deposition time of the RF magnetron sputtering is 5 to 10 hours, and the sputtering power is 50 to 100 W; in step S5, the sputtering deposition time of the RF magnetron sputtering is 18 to 22 minutes, and the sputtering power is 50 to 100 W; in step S6, the sputtering deposition time of the DC magnetron sputtering is 4 to 6 minutes, and the sputtering power is 50 to 100 W.
[0026] The beneficial effects of the present invention are:
[0027] (1) The method for preparing the thin film cathode material of the present invention comprises: 1-x-y Co x Mn y A protective layer film is prepared on the cathode film of O2, so that the obtained film cathode material has a small and uniform microscopic particle size and has high electrical conductivity and capacitance;
[0028] (2) The method for preparing the thin film cathode material of the present invention can prevent direct contact between NCM and electrolyte and inhibit the side reaction of Mn dissolution by depositing a uniformly distributed nano-thick protective film on the surface of the cathode film;
[0029] (3) The method for preparing the thin film cathode material of the present invention adopts a magnetron sputtering method to prepare each layer separately, which has the advantages of simple preparation steps, mild conditions, easy operation and low cost;
[0030] (4) The thin film cathode material of the present invention has extremely excellent electrochemical stability and structural stability;
[0031] (5) The flexible all-solid-state lithium-ion battery of the present invention has good discharge specific capacity, cycle stability and rate performance;
[0032] (6) The flexible all-solid-state lithium-ion battery of the present invention has a solid electrolyte that can isolate the positive and negative electrodes, thereby preventing the battery from exploding and improving safety;
[0033] (7) The flexible all-solid-state lithium-ion battery of the present invention has a certain flexibility, and the battery will not short-circuit or cause damage to the solid electrolyte when in a bent state. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 For the thin film cathode material of the present invention, in Example 1, the original LiNi 0.5 Co 0.2 Mn 0.3 Scanning electron microscope image of O2 / Ti, Figure 1 The image a in the middle is a scanning electron microscope image with a scale bar of 100 nm. Figure 1 b is a scanning electron microscope image with a scale bar of 10 μm;
[0035] Figure 2 The SEM image of the thin film cathode material of the present invention is as follows: Figure 2 The image a in the middle is a scanning electron microscope image with a scale bar of 100 nm. Figure 2 b is a scanning electron microscope image with a scale bar of 10 μm;
[0036] Figure 3 The film cathode material of the present invention, in Example 1, after depositing Li3PO4 for 4 min, LiNi 0.5 Co 0.2 Mn 0.3 Cross-sectional SEM image of O2 film;
[0037] Figure 4 The film cathode material of the present invention, in Example 2, is the SEM image of the NCM@5minLiPON film electrode; Figure 4 The image a in the middle is a scanning electron microscope image with a scale bar of 100 nm. Figure 4 b is a scanning electron microscope image with a scale bar of 10 μm;
[0038] Figure 5 The thin film cathode material of the present invention, in Example 2, is a cross-sectional SEM image of the NCM@5minLiPON thin film electrode;
[0039] Figure 6 The film cathode material of the present invention is a SEM image of a ZnO film sputtered on the NCM film in Example 3; Figure 6 The image a in the middle is a scanning electron microscope image with a scale bar of 100 nm. Figure 6 b is a scanning electron microscope image with a scale bar of 10 μm;
[0040] Figure 7For the thin-film cathode material of the present invention, in Example 1, the XRD pattern of the LiPON thin-film electrode deposited for 4 minutes;
[0041] Figure 8 For the thin-film cathode material of the present invention, in Example 2, the XRD pattern of the LiPON thin-film electrode deposited for 5 minutes;
[0042] Fig. 9 For the thin-film cathode material of the present invention, in Example 3, NCM after depositing ZnO thin film for 2 minutes;
[0043] Fig.10 For the thin-film cathode material of the present invention, the EIS spectrum of Example 1;
[0044] Fig.11 For the thin-film cathode material of the present invention, the EIS spectrum of Example 2;
[0045] Fig.12 For the thin-film cathode material of the present invention, the EIS spectrum of Example 3;
[0046] Fig.13 For the thin-film cathode material of the present invention, the rate performance graph of the thin-film cathode material of Example 1;
[0047] Fig.14 For the thin-film cathode material of the present invention, the cycling performance graph of the thin-film cathode material of Example 1 at 1C;
[0048] Fig.15 Schematic diagram of the layer structure of the flexible all-solid-state lithium-ion battery of the present invention.
[0049] In the drawings, the list of components represented by each reference numeral is as follows:
[0050] 1. Substrate; 2. Cathode thin film; 3. Protective layer thin film; 4. Solid electrolyte thin film; 5. Anode thin film; 6. Anode current collector. Detailed implementation manners
[0051] The principles and features of the present invention will be described below with reference to the accompanying drawings. The examples given are only for explaining the present invention and are not intended to limit the scope of the present invention.
[0052] As Fig.15 shown, for the preparation method of the thin-film cathode material of the present invention, a cathode thin film 2 is prepared on a substrate 1; a protective layer thin film 3 is prepared on the surface of the cathode thin film 2; the material of the cathode thin film 2 is LiNi 1-x-y Co x Mn y O2 material (NCM), where the value ranges of x and y are 0 < x < 1 and 0 < y < 1; the protective layer thin film 3 is a Li3PO4 thin film, a LiPON thin film or a ZnO thin film.
[0053] The preparation method of the present invention prepares LiNi on a substrate 1 1-x-y Co x Mn y The cathode film 2 of O2 makes the obtained film cathode material have small and uniform microscopic particle size, high conductivity and capacitance. At the same time, by depositing a uniformly distributed nano-thick protective film, i.e., protective layer film 3, on the surface of the cathode film 2, it can prevent direct contact between NCM and electrolyte, inhibit the side reaction of Mn dissolution, and maintain the high capacity of the electrode, so that the film cathode material has extremely excellent electrochemical stability and structural stability, thereby significantly improving the discharge specific capacity, cycle stability performance and rate performance of lithium-ion batteries.
[0054] Preferably, the thickness of the protective layer film 3 is 25 nm.
[0055] Preferably, the substrate 1 is a titanium substrate, LiNi 1-x-y Co x Mn y O2 material is LiNi 0.5 Co 0.2 Mn 0.3 O2.
[0056] Preferably, the present invention further comprises the following steps:
[0057] S1. Prepare a Pt buffer layer on a metal substrate to obtain a substrate 1; sputtering the Pt buffer layer is mainly to prevent oxidation of the titanium substrate.
[0058] S2, preparing a cathode film 2 on the substrate 1 by radio frequency magnetron sputtering or coating;
[0059] Preferably, the first working gas of RF magnetron sputtering is a mixture of argon and oxygen, the vacuum degree of RF magnetron sputtering is 0.1-0.7 Pa, the RF power supply power is 50-100 W, the pre-sputtering time is 25-35 min, sputtering is carried out without bias, the sputtering time is 2-8 h, and annealing is performed after sputtering is completed. The annealing temperature is 500-800 ° C and the annealing time is 3-5 h.
[0060] The higher the annealing temperature, the more complete the structure, and the better the electrochemical performance. When the annealing temperature reaches 750°C, the NCM film crystal orientation is better, which is conducive to the release and insertion of lithium ions during the charge and discharge process.
[0061] Preferably, in the first working gas, the volume percentage of argon is 50% to 100%.
[0062] S3, using magnetron sputtering to deposit the target material of the protective layer film 3 on the cathode film 2 to obtain the protective layer film 3.
[0063] Preferably, magnetron sputtering is performed in an environment filled with the second working gas, the vacuum degree of magnetron sputtering is 0.4-0.6 Pa, and the radio frequency power is 50-100W.
[0064] Preferably, when the protective layer film 3 is a Li3PO4 film, the target material of the protective layer film 3 is a Li3PO4 target material, the second working gas is argon, and the sputtering time is 2 to 4 minutes;
[0065] When the protective layer film 3 is a LiPON film, the target material of the protective layer film 3 is a Li3PO4 target material, the second working gas is nitrogen, and the sputtering time is 1 to 7 minutes;
[0066] When the protective layer film 3 is a ZnO film, the target material of the protective layer film 3 is a Zn target material, the second working gas is a mixed gas of argon and oxygen, and the sputtering time is 1 to 3 minutes.
[0067] Preferably, the volume percentage of argon is 40%, and the volume percentage of oxygen is 60%.
[0068] It should be noted that in the above-mentioned preparation process of the present invention, some specific operations and parameters (such as working gas pressure, etc.) are conventional methods, or limited adjustments based on conventional methods.
[0069] In one embodiment of the present invention, the specific preparation operation process and related parameters are as follows:
[0070] 1) The metal foil is placed in deionized water and ethanol solution in turn and ultrasonically cleaned repeatedly for multiple times, each time for 5 to 15 minutes. After the cleaning is completed, the metal foil is placed in a magnetron sputtering device to sputter to prepare a Pt buffer layer, thereby obtaining a substrate 1.
[0071] 2) Place the substrate 1 obtained in step 1) on the coating sample stage of the magnetron sputtering instrument, and then place the commercial LiNi 0.5 C o0.2 Mn 0.3 The O2 target was placed in the magnetron target position, with a distance of 40 to 100 mm from the substrate 1. The coating chamber and the sample chamber were then evacuated to a vacuum level of 5 × 10 -4 Pa, then open the stop valve, adjust the flowmeter, introduce argon and oxygen into the coating chamber, adjust the air flow rate, control the vacuum degree of the coating chamber to maintain at 0.1-0.7Pa, and start sputtering LiNi 0.5 Co 0.2 Mn 0.3 O2 target.
[0072] The RF power is controlled to be 50-100W, the heating temperature of the substrate 1 is 600-800°C, and pre-sputtering is performed for 25-35 minutes to clean the impurities on the surface of the target material; then the LiNi 0.5 C o0.2 Mn 0.3 The O2 target and the baffle of the substrate 1 begin to sputter coating the surface of the substrate 1, and the sputtering time is 2 to 8 hours to obtain the cathode film 2.
[0073] Preferably, the vacuum degree of the cavity is 2 to 3×10 -4 Pa.
[0074] 3) The target material of the protective layer film 3 and the cathode film 2 prepared in step 2) are placed in the cavity, and the vacuum degree of the cavity is pumped to 3×10 -4 Pa, then open the stop valve, introduce argon, adjust the argon flow rate to keep the vacuum degree at 0.1-0.7 Pa, and the RF power is 50-100 W. The deposition sputtering time is 2-5 min to obtain a nickel-cobalt-manganese ternary positive electrode thin film material coated with a protective layer film 3, that is, a modified nickel-cobalt-manganese ternary positive electrode material.
[0075] The thin film cathode material of the present invention is prepared by the above method. The thin film cathode material has high energy density, can effectively improve the electrochemical performance and safety performance of the battery, and has extremely important practical significance for the development and application of new energy power batteries.
[0076] like Fig.15 As shown, the flexible all-solid-state lithium-ion battery of the present invention comprises the above-mentioned thin film cathode material, and a solid electrolyte film 4, an anode film 5 and an anode current collector 6 are sequentially arranged on the protective layer film 3 of the thin film cathode material. The flexible all-solid-state lithium-ion battery has good electrochemical performance and safety performance of the battery.
[0077] The above-mentioned method for preparing a flexible all-solid-state lithium-ion battery comprises the following steps:
[0078] S4. Prepare a solid electrolyte film 4 on the protective layer film 3 by radio frequency magnetron sputtering.
[0079] Preferably, the process of this step is as follows: in an argon atmosphere of 0.7-1.0 Pa, after setting the sputtering power and sputtering mode, sputter deposition is performed at room temperature. The sputtering power of the solid electrolyte target is set to 50-100 W, the target-substrate distance is 40-100 mm, and the sputtering time is 5-10 h.
[0080] S5. Prepare an anode film 5 on the solid electrolyte film 4 by radio frequency magnetron sputtering.
[0081] Preferably, the process of this step is as follows: in an argon atmosphere of 0.4-0.6 Pa, Si is used as a target material, and after setting the sputtering power and sputtering mode of the target material, sputtering deposition is performed at room temperature. The sputtering power is set to 50-100 W, the target-substrate distance is 40-100 mm, and the sputtering time is 25-35 min.
[0082] S6. Prepare an anode current collector 6 on the anode by DC magnetron sputtering, encapsulate and obtain a flexible all-solid-state lithium-ion battery.
[0083] Preferably, the process of this step is as follows: in an argon atmosphere, Ti is used as a target material for sputtering deposition at room temperature for 5 minutes, the sputtering power is 50-100 W, and the target-substrate distance is 40-100 mm.
[0084] The present invention is specifically described below by way of examples.
[0085] Example 1
[0086] This embodiment adopts the method of the present invention to prepare the thin film cathode material, wherein the protective layer film 3 is a Li3PO4 thin film, and the sputtering time of the Li3PO4 target material is 4 minutes. The specific steps are as follows:
[0087] 1) First, the titanium foil was placed in deionized water and ethanol solution for ultrasonic cleaning three times, each time for 15 minutes, and the prepared titanium foil substrate was placed in a magnetron sputtering instrument and a Pt buffer layer was sputtered for 3 minutes to obtain a titanium substrate, namely a Ti substrate.
[0088] 2) The Ti substrate obtained in step 1) and the commercial LiNi 0.5 Co 0.2 Mn 0.3 The O2 target was placed in the magnetron sputtering chamber, and the vacuum degree of the chamber was pumped to 5×10 -4 pa, then open the stop valve, adjust the flowmeter, introduce argon and oxygen, adjust the vacuum degree of the chamber to 0.5 pa, adjust the power setting value of the RF power supply, and start sputtering LiNi 0.5 Co 0.2 Mn 0.3 O2 material, the sputtering time is 4h, and after sputtering, in-situ annealing treatment is carried out at a temperature of 750℃ to obtain NCM / Ti film.
[0089] 3) Load the Li3PO4 target and the prepared NCM / Ti film into the chamber, and pump the vacuum of the chamber to 3×10 -4Pa, then open the stop valve, introduce argon, adjust the argon flow rate to keep the vacuum degree at 0.5 Pa, and the RF power is 50 W. Deposition and sputtering for 4 minutes to obtain a nickel-cobalt-manganese ternary positive electrode thin film material coated with a Li3PO4 film, namely, NCM@Li3PO4 / Ti film.
[0090] In this embodiment, the original LiNi 0.5 Co 0.2 Mn 0.3 The scanning electron microscope image of O2 / Ti is as follows Figure 1 As shown, the SEM image of the Li3PO4 film after deposition for 4 min is as follows Figure 2 As shown, it can be clearly observed that both the original and NCM@4min Li3PO4 are composed of large rod-shaped particles made up of fine particles, and the surface of the NCM@4min Li3PO4 enlarged image is more uniform compared to the original material.
[0091] Figure 3 After depositing Li3PO4 film for 4 min, LiNi 0.5 Co 0.2 Mn 0.3 Cross-sectional SEM image of O2 thin film material. Figure 3 It can be seen that LiNi 0.5 Co 0.2 Mn 0.3 A 25nm Li3PO4 film is deposited on the surface of the O2 thin film material. Each film layer has a uniform thickness and a flat interface at the nanoscale level. This figure shows that the LiNi 0.5 Co 0.2 Mn 0.3 Surface reactions at the interface of the O2 film and the organic electrolyte, such as decomposition of the organic electrolyte and dissolution of manganese.
[0092] Figure 7 This is the XRD pattern of the Li3PO4 thin film electrode, NCM@Li3PO4 / Ti film, which was deposited for 4 minutes. The XRD diffraction pattern shows the peaks (002, 101 and 102) of the titanium substrate and the peaks (003 and 104) of the NCM material. The ratio of the peak intensities of (003) and (004) in the figure, I003 / I004, is 1.08, which is less than 1.2, indicating that the material has a certain amount of cation mixing. The peak of Li3PO4 is not seen in the GIXRD pattern at grazing incidence of 0.3°, indicating that the deposited Li3PO4 film is an amorphous structure.
[0093] To better understand LiNi for lithium energy storage 0.5 Co 0.2 Mn 0.3The excellent electrochemical performance of O2 materials is revealed by electrochemical impedance spectroscopy (EIS) in the frequency domain from 0.01Hz to 100kHz. The results of the Nyquist curve are as follows: Fig.10 As shown in Figure 1. The Nyquist plot consists of a semicircle in the high frequency range and a steeper straight line in the low frequency range. The electrolyte / electrode interface charge transfer resistance (Rct) is associated with the semicircle, and the Li diffusion-related Warburg impedance (W) is associated with the inclined line. Fig.10 It can be seen that the Rct of NCM@4min Li3PO4 is significantly smaller than that of the original NCM. It can be considered that the byproducts such as LiF, LixPFy and LixPFyO2 produced by the side reactions during the full charge process are deposited on the surface of the active material, further hindering the Li + diffusion, and Li3PO4 film can effectively inhibit the side reactions.
[0094] Fig.13 This is a rate performance diagram of the thin film cathode material prepared in this embodiment. Fig.13 It can be seen that the discharge capacity of NCM@4minLi3PO4 samples at various rates is higher than that of the original LiNi 0.5 Co 0.2 Mn 0.3 O2, the enhancement in rate capability, especially the high-rate performance, is mainly attributed to the Li3PO4 protective layer.
[0095] Fig.14 The figure is a cycle performance diagram of the thin film cathode material prepared in this embodiment at 1C. Fig.14 It can be seen that without any coating, the capacity retention rate of the NCM film after 50 cycles is 86.32%. The capacity retention rate of the ternary thin film cathode material prepared by sputtering for 4 min is 91.15%, and the specific capacity is higher than that of the original NCM thin film cathode (the initial specific capacities of the original NCM and NCM@4min Li3PO4 are 101.3 and 125.6 mAh·g, respectively). -1 ).
[0096] The test results of the above scanning electron microscopy, X-ray diffraction, and electrochemical performance EIS tests show that after setting up the Li3PO4 film, the NCM@Li3PO4 / Ti thin film electrode has better performance and more research prospects.
[0097] Example 2
[0098] This embodiment adopts the method of the present invention to prepare the thin film cathode material, wherein the protective layer film 3 is a LiPON film, and the sputtering time of the Li3PO4 target material is 5 minutes. The specific steps are as follows:
[0099] 1) First, the titanium foil was placed in deionized water and ethanol solution for ultrasonic cleaning three times, each time for 15 minutes, and the prepared titanium foil substrate was placed in a magnetron sputtering instrument and a Pt buffer layer was sputtered for 3 minutes to obtain a titanium substrate, namely a Ti substrate.
[0100] 2) The Ti substrate obtained in step 1) and the commercial LiNi 0.5 Co 0.2 Mn 0.3 The O2 target was placed in the magnetron sputtering chamber, and the vacuum degree of the chamber was pumped to 5×10 -4 Pa, then open the stop valve, adjust the flowmeter, introduce argon and oxygen, adjust the vacuum degree of the chamber to 0.5Pa, adjust the power setting value of the RF power supply, and start sputtering LiNi 0.5 Co 0.2 Mn 0.3 O2 material, sputtering time is 4h, after sputtering, in-situ annealing treatment is performed at 750℃ to obtain NCM / Ti film.
[0101] 3) Load the Li3PO4 target and the prepared NCM / Ti film into the chamber, and evacuate the chamber to a vacuum of 3×10 -4 Pa, then open the stop valve, introduce nitrogen, adjust the argon flow rate to keep the vacuum degree at 0.5 Pa, and the RF power is 50 W. Sputter deposition is performed for 5 minutes to obtain a thin film cathode material with a LiPON thin film, namely, NCM@LiPON / Ti thin film. This embodiment is specifically recorded as NCM@5minLiPON according to its sputter deposition time.
[0102] SEM image of NCM@5minLiPON Figure 4 As shown, according to Figure 4 It can be seen that the sputtered NCM film is composed of fine particles, and the enlarged image shows that the film surface is very dense. Such a microstructure can not only ensure the 0.5 Co 0.2 Mn 0.3 The O2 cathode film has stable electrochemical stability and can avoid the side reaction between some active substances and the electrolyte caused by uneven protective layer.
[0103] Figure 5 This is a cross-sectional SEM image of the NCM@5minLiPON thin film electrode, where a layer of LiPON thin film can be seen. LiPON is obtained by sputtering in a nitrogen atmosphere, where a small amount of nitrogen replaces the oxygen in the compound, which has a profound effect on ionic conductivity and electrochemical stability.
[0104] Figure 8This is the XRD diagram of the deposited 5min LiPON thin film electrode, namely NCM@5minLiPON / Ti thin film. During the chemical synthesis and process control of NCM materials, due to the Ni 2+ Radius and Li + The radii are relatively close, and the two can easily occupy each other's positions. This is the lithium-nickel mixing phenomenon.
[0105] I(003) / I(104) is usually used to determine the lithium-nickel mixing in the material. When I(003) / I(104)>1.2, the lithium-nickel mixing of the ternary material is small and the layered structure of the material is well developed. In this embodiment, the ratio of I(003) / I(104) is 1.63, which is greater than 1.2. No peaks of the LiPON film were observed from the XRD diagram, only peaks from the Ti substrate were observed, indicating that the LiPON film is an amorphous structure.
[0106] In order to characterize the change of interfacial resistance of LiPON film, EIS analysis was performed. Fig.11 As shown, a main semicircle is observed for both pristine NCM and NCM@5minLiPON. This is due to the overlap between the contribution of the solid electrolyte interface (SEI) layer at high frequencies and the charge transfer resistance of the surface film and active materials at medium and high frequencies. The inclined line at low frequencies represents the bulk diffusion of lithium ions.
[0107] When EIS data were collected while charging to 4.3 V, it was clear that NCM@5minLiPON showed a significantly smaller diameter compared to the original NCM. EIS studies of LiPON films showed that lower charge transfer resistance was equivalent to lower electrode polarization. The reduction in charge transfer resistance explains the improved rate performance of NCM@5minLiPON.
[0108] Scanning electron microscopy, X-ray diffraction, and electrochemical performance EIS tests show that after setting up the LiPON film, the NCM@LiPON / Ti thin film electrode has better performance and more research prospects.
[0109] Example 3
[0110] This embodiment adopts the method of the present invention to prepare a thin film cathode material, wherein the protective layer film 3 is a ZnO thin film, and the sputtering time of the metal Zn target is 2 minutes. The specific steps are as follows:
[0111] 1) First, the titanium foil was placed in deionized water and ethanol solution for ultrasonic cleaning three times, each time for 15 minutes, and the prepared titanium foil substrate was placed in a magnetron sputtering instrument and a Pt buffer layer was sputtered for 3 minutes to obtain a titanium substrate, namely a Ti substrate.
[0112] 2) The Ti substrate obtained in step 1) and the commercial LiNi0.5 Co 0.2 Mn 0.3 The O2 target was placed in the magnetron sputtering chamber, and the vacuum degree of the chamber was pumped to 5×10 -4 pa, then open the stop valve, adjust the flowmeter, introduce argon and oxygen, adjust the vacuum degree of the chamber to 0.5 pa, adjust the power setting value of the RF power supply, and start sputtering LiNi 0.5 Co 0.2 Mn 0.3 O2 material, sputtering time is 4h, after sputtering, in-situ annealing treatment is performed at 750℃ to obtain NCM / Ti film.
[0113] 3) Place the NCM / Ti film and the metal Zn target obtained in step 2) into the chamber of a magnetron sputtering coating machine, and use high-purity oxygen and argon as sputtering gas and reaction gas. Before deposition, the vacuum degree of the chamber is pumped to 3×10 -4 Pa, and sputtering was carried out in a mixed atmosphere of argon (40%) and oxygen (60%) at a vacuum degree of 0.5 Pa for 2 min to obtain NCM@ZnO / Ti thin film.
[0114] Figure 6 This is a SEM picture of a ZnO film sputtered on the NCM film in this embodiment. It can be seen from the figure that the surface of the sputtered NCM film is composed of a layer of fine particles. The enlarged image shows that the surface of the film is very dense. The uniform and dense film is prepared by magnetron sputtering.
[0115] Fig. 9 The XRD spectrum of NCM after depositing ZnO film for 2 minutes, namely NCM@2minZnO / Ti, shows that the characteristic peaks of the film sample are the characteristic peaks of NCM and the peaks of the titanium substrate, and no characteristic peaks belonging to ZnO are found. Compared with the peaks of the titanium substrate, the peaks of the NCM film are not obvious. The reason for this phenomenon is that the thickness of the NCM film prepared by sputtering is relatively thin, and the peak of the titanium substrate is too strong to greatly cover the diffraction peak of the film.
[0116] To better understand the factors leading to the enhanced electrochemical performance of these coated electrodes, EIS was also introduced to study their electrochemical kinetics, which were performed after an initial charge to 4.3 V, as shown in Fig.12 As shown. It can be seen that all Nyquist plots show two arcs in the high to medium frequency region. The first semicircle contributes to the diffusion of lithium ions through the surface layer, and the second semicircle is assigned to the charge transfer reaction. It is obvious that NCM@2minZnO has the smallest charge transfer resistance. This indicates that the charge transfer of the electrode deposited with 2min ZnO film is greatly reduced to improve the electrochemical performance.
[0117] The above-mentioned scanning electron microscopy, X-ray diffraction, and electrochemical performance EIS tests show that the NCM@ZnO / Ti thin film electrode with ZnO thin film has better performance and more research prospects.
[0118] Example 4
[0119] This embodiment adopts the method of the present invention to prepare a flexible all-solid-state lithium-ion battery, wherein the protective layer film 3 is a LiPON film, and the sputtering time of the Li3PO4 target material is 4 minutes. In addition, in this embodiment, the heating temperature of the substrate 1 is 750°C.
[0120] The specific steps are as follows:
[0121] 1) First, the substrate for sputtering the thin film is processed: titanium foil is used as substrate 1. First, the titanium foil is cleaned, and then the titanium foil substrate to be dried is placed in a magnetron sputtering instrument to sputter a Pt buffer layer for 3 minutes. The Pt buffer layer of appropriate thickness sputtered on the titanium foil can serve as a current collector and can also prevent impurities in the titanium foil substrate from diffusing into the NCM film during the annealing process.
[0122] 2) Place the titanium substrate and LiNi 0.5 Co 0.2 Mn 0.3 O2 target: Place the treated titanium substrate on the coating sample stage of the magnetron sputtering instrument, and then place the positive electrode target, which is commercial LiNi 0.5 Co 0.2 Mn 0.3 The O2 target was placed in the magnetron target position, so that the distance between the positive target and the titanium substrate was 40-100 mm. Then the coating chamber and the sample chamber were evacuated to control the vacuum degree at 3×10 -4 Pa, then open the stop valve, adjust the flowmeter, introduce argon and oxygen into the coating chamber, adjust the air intake flow rate, and control the vacuum degree of the coating chamber to maintain at 0.5Pa.
[0123] 3) Using high temperature in-situ annealing technology, thin film materials were prepared on titanium substrates: RF sputtering power was applied, the RF power was controlled to 50W, the titanium substrate was heated to 750°C, and pre-sputtering was performed for 30 minutes to clean impurities on the target surface; then the LiNi 0.5 Co 0.2 Mn 0.3 O2 target and baffle of titanium substrate, start sputtering coating on the surface of titanium substrate, the sputtering time is 4h, and cathode film 2 is obtained.
[0124] 4) Depositing LiPON film on the surface of cathode film 2: Place the prepared NCM thin film titanium substrate on the coating sample stage of the magnetron sputtering instrument, and then place the Li3PO4 target material on the magnetron target position, with a distance of 40 to 100 mm between the two, and then evacuate the coating chamber and the sample chamber to control the vacuum degree at 3×10 -4 Pa, open the stop valve, adjust the flowmeter, and then introduce nitrogen into the coating chamber, adjust the air intake flow rate, control the vacuum degree of the coating chamber to maintain at 0.5Pa, the RF power is 50W, and the sputtering time is 4min.
[0125] 5) Preparation of Li 1.5 Al 0.5 Ge 1.5 (PO4)3 solid electrolyte: In an argon atmosphere, the working pressure is 0.8pa, and the gas flow rate is 10sccm. 1.5 Al 0.5 Ge 1.5 (PO4)3 was used as the target material for sputtering deposition for 5 h with a sputtering power of 100 W.
[0126] 6) Preparation of Si anode: In an argon atmosphere, the working pressure is 0.6 Pa, the gas flow rate is 12 sccm, and Si is used as the target material for sputtering deposition for 22 minutes with a sputtering power of 50 W.
[0127] 7) Preparation of Ti anode current collector: In an argon atmosphere, a working pressure of 0.5 Pa, a gas flow rate of 8 sccm, Ti was used as a target material for sputtering deposition for 4 min with a sputtering power of 100 W to finally obtain a Ti anode current collector, which was encapsulated to obtain a flexible all-solid-state lithium-ion battery.
[0128] Example 5
[0129] In this embodiment, the method of the present invention is used to prepare a flexible all-solid-state lithium-ion battery, wherein the protective layer film 3 is a LiPON film, and the sputtering time of the Li3PO4 target material is 4 minutes. In addition, in this embodiment, LiNi 0.5 Co 0.2 Mn 0.3 The sputtering time of O2 target is 6h.
[0130] The specific steps are:
[0131] 1) First, the titanium substrate for sputtering the thin film is processed: titanium foil is used as the substrate, the titanium foil is first cleaned, and then the titanium foil substrate to be dried is placed in a magnetron sputtering device to sputter the Pt buffer layer for 3 minutes.
[0132] 2) Place the titanium substrate and LiNi 0.5 Co 0.2 Mn 0.3O2 target: Place the treated titanium substrate on the coating sample stage of the magnetron sputtering instrument, and then 0.5 Co 0.2 Mn 0.3 The O2 target was placed in the magnetron target position, and the distance between the positive target and the titanium substrate was 40-100 mm. Then the coating chamber and the sample chamber were evacuated to control the vacuum degree at 3×10 -4 Pa, then open the stop valve, adjust the flowmeter, introduce argon and oxygen into the coating chamber, adjust the air intake flow rate, and control the vacuum degree of the coating chamber to maintain at 0.5Pa.
[0133] 3) Using high temperature in-situ annealing technology, thin film materials were prepared on the positive electrode current collector titanium substrate: RF sputtering power was applied, the RF power was controlled to 50W, the substrate heating temperature was 750℃, pre-sputtering was performed for 30min, and then the LiNi 0.5 Co 0.2 Mn 0.3 The O2 target and the baffle of the titanium substrate began to sputter coating the surface of the titanium substrate. The sputtering time was 6 hours to obtain a thin film.
[0134] 4) Deposition of LiPON thin film on the surface of thin film material: Place the prepared NCM thin film titanium substrate on the coating sample stage of the magnetron sputtering instrument, and then place the Li3PO4 target material on the magnetron target position, with a distance of 40 to 100 mm between the two, and then evacuate the coating chamber and the sample chamber, and control the vacuum degree to 3×10 -4 Pa, open the stop valve, adjust the flowmeter, and then introduce nitrogen into the coating chamber, adjust the inlet flow, control the vacuum degree of the coating chamber to maintain at 0.5Pa, and the RF power is 50W. The sputtering time is 4min.
[0135] 5) Preparation of Li 1.5 Al 0.5 Ge 1.5 (PO4)3 solid electrolyte: In an argon atmosphere, the working pressure is 0.8pa, and the gas flow rate is 10sccm. 1.5 Al 0.5 Ge 1.5 (PO4)3 was used as the target material for sputtering deposition for 5 h with a sputtering power of 100 W.
[0136] 6) Preparation of Si anode: In an argon atmosphere, the working pressure is 0.6 Pa, the gas flow rate is 8 sccm, and Si is used as the target material for sputtering deposition for 18 minutes with a sputtering power of 100 W.
[0137] 7) Preparation of Ti anode current collector: In an argon atmosphere, a working pressure of 0.5 Pa, a gas flow rate of 12 sccm, Ti was used as a target material for sputtering deposition for 6 min with a sputtering power of 50 W to finally obtain a Ti anode current collector, which was encapsulated to obtain a flexible all-solid-state lithium-ion battery.
[0138] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a thin film cathode material, characterized in that: Prepare a cathode thin film (2) on a substrate (1); prepare a protective layer thin film (3) on the surface of the cathode thin film (2); the cathode thin film (2) is LiNi 1-x-y Co x Mn y O2, where the value ranges of x and y are 0 < x < 1 and 0 < y < 1 respectively; the protective layer thin film (3) is a Li3PO4 thin film, a LiPON thin film or a ZnO thin film.
2. The method for preparing a thin film cathode material according to claim 1, characterized in that: The thickness of the protective layer film (3) is 15 to 30 nm.
3. The method for preparing a thin film cathode material according to claim 1, characterized in that: The following steps are also included: S1. Preparing a Pt buffer layer on a metal substrate to obtain the substrate (1); S2, preparing the cathode film (2) on the substrate (1) by radio frequency magnetron sputtering or coating; S3, using a magnetron sputtering method to sputter and deposit the target material of the protective layer film (3) on the cathode film (2), so as to obtain the protective layer film (3).
4. The method for preparing a thin film cathode material according to claim 3, characterized in that: In step S2, the first working gas of the RF magnetron sputtering is a mixture of argon and oxygen, the vacuum degree is 0.1-0.7 Pa, the RF power supply power is 50-100 W, and the pre-sputtering time is 25-35 min; the RF magnetron sputtering is performed without bias, and the sputtering time is 2-8 h; annealing is performed after sputtering is completed, the annealing temperature is 500-800 ° C, and the annealing time is 3h-5h.
5. The method for preparing a thin film cathode material according to claim 3, characterized in that: In step S3, magnetron sputtering is performed in an environment filled with the second working gas, the vacuum degree of the magnetron sputtering is 0.4-0.6 Pa, and the radio frequency power is 50-100W.
6. The method for preparing a thin film cathode material according to claim 5, characterized in that: When the protective layer film (3) is the Li3PO4 film, the target material of the protective layer film (3) is the Li3PO4 target material, the second working gas is argon, and the sputtering time is 2 to 4 minutes; When the protective layer film (3) is the LiPON film, the target material of the protective layer film (3) is a Li3PO4 target material, the second working gas is nitrogen, and the sputtering time is 1 to 7 minutes; When the protective layer film (3) is the ZnO film, the target material of the protective layer film (3) is a Zn target material, the second working gas is a mixed gas of argon and oxygen, and the sputtering time is 1 to 3 minutes.
7. A thin film cathode material, characterized in that: The material is prepared by the method according to any one of claims 1 to 6.
8. A flexible all-solid-state lithium-ion battery, characterized in that: It comprises the thin film cathode material as claimed in claim 7, wherein a solid electrolyte film (4), an anode film (5) and an anode current collector (6) are sequentially arranged on the protective layer film (3) of the thin film cathode material.
9. A method for preparing a flexible all-solid-state lithium-ion battery as claimed in claim 8, characterized in that: The following steps are involved: S4, preparing the solid electrolyte film (4) on the protective layer film (3) by radio frequency magnetron sputtering; S5, preparing the anode film (5) on the solid electrolyte film (4) by radio frequency magnetron sputtering; S6. Prepare the anode current collector (6) on the anode film (5) by direct current magnetron sputtering, and encapsulate and obtain the flexible all-solid-state lithium-ion battery.
10. The method for preparing a flexible all-solid-state lithium-ion battery according to claim 9, characterized in that: In step S4, the sputtering deposition time of the RF magnetron sputtering is 5 to 10 hours, and the sputtering power is 50 to 100 W; in step S5, the sputtering deposition time of the RF magnetron sputtering is 18 to 22 minutes, and the sputtering power is 50 to 100 W; in step S6, the sputtering deposition time of the DC magnetron sputtering is 4 to 6 minutes, and the sputtering power is 50 to 100 W.
Citation Information
Patent Citations
Cathode material used for lithium battery and production method thereof
CN108039479A
All-solid-state thin film lithium ion battery and preparation method thereof
CN115275363A
SnSb / ZnO passive film composite electrode and preparation method thereof
CN115579459A
Device and method for preparing solid thin-membrane lithium battery by in-situ deposition
CN1747217A
Manganese-based sodium ion battery positive electrode material for suppressing jahn-teller effect and method for manufacturing the same