Negative pole piece, battery comprising negative pole piece and electric device comprising negative pole piece

By using water-based binders with relative dielectric constants greater than or equal to 2.5 and modified conductive carbon materials in sodium batteries, the problems of low energy density and poor circulation performance of sodium ion batteries are solved, and the high energy density and long energy density of sodium batteries are achieved Cycle life.

CN119069619AActive Publication Date: 2024-12-03CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310622552.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03
Estimated Expiration
2043-05-30

Smart Images

  • Figure CN119069619A_ABST
    Figure CN119069619A_ABST
Patent Text Reader

Abstract

The invention provides a negative pole piece for a sodium battery, a battery comprising the negative pole piece and an electric device, the negative pole piece comprises a negative current collector and a conductive coating, and the conductive coating is located on at least one side of the negative current collector. The conductive coating comprises a conductive agent and a water-based binder, and the water-based binder is selected from water-based binders with the relative dielectric constant larger than or equal to 2.5.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a negative electrode plate for a sodium battery, a battery comprising the negative electrode plate, and an electrical device. Background Art

[0002] Secondary batteries rely on active ions to be reciprocated between the positive and negative electrodes for charging and discharging. Secondary batteries represented by lithium-ion batteries have outstanding characteristics such as high energy density, long cycle life, no pollution, and no memory effect. Therefore, as a clean energy source, secondary batteries have gradually spread from electronic products to large-scale devices such as electric vehicles to adapt to the sustainable development strategy of the environment and energy. However, due to the scarcity of active material resources related to lithium-ion batteries, battery costs have always remained high, and at the same time they face severe problems such as the depletion of related resources, so it is necessary to develop other low-cost metal ion secondary battery systems.

[0003] Sodium-ion batteries have become a hot research topic in recent years due to their low cost, abundant resources, and similar manufacturing process to lithium-ion batteries. However, the low energy density of sodium-ion batteries is still a bottleneck limiting their application and promotion. Summary of the invention

[0004] In order to achieve the above-mentioned purpose, the present application provides a negative electrode plate for a sodium battery, which can enable the battery containing the negative electrode plate to have both high energy density and good cycle performance; the present application also provides a battery and an electrical device containing the negative electrode plate.

[0005] In a first aspect, an embodiment of the present application provides a negative electrode sheet for a sodium battery, comprising a negative electrode current collector and a conductive coating, wherein the conductive coating is located on at least one side of the negative electrode current collector. The conductive coating comprises a conductive agent and an aqueous binder, wherein the aqueous binder is selected from aqueous binders having a relative dielectric constant greater than or equal to 2.5.

[0006] Without intending to be bound by any theory or explanation, aqueous binders with a relative dielectric constant of 2.5 or greater can promote Na +Combining with electrons to form sodium metal is beneficial to the deposition of sodium metal at the negative electrode, and on the other hand, it can promote the interface flatness of the conductive coating. When the conductive coating has a high interface flatness, the orientation and trend of sodium metal deposition can be regulated so that the sodium metal is uniformly deposited on the surface of the negative electrode. Thus, not only can the formation of sodium dendrites be suppressed, thereby improving the reliability and long-term cycle performance of the battery; but also the difficulty of sodium metal detachment can be reduced, and the irreversible loss of active sodium ions can be reduced, thereby improving the energy density and cycle life of the battery. In addition, compared with other binders, the binder network formed by the aqueous binder with a relative dielectric constant greater than or equal to 2.5 in the conductive layer has a higher mechanical strength, which can provide certain supporting properties for the conductive coating. Thus, it is beneficial to improve the structural stability of the conductive coating and reduce the risk of changes in the collector structure caused by the detachment of sodium metal, thereby improving the cycle stability of the battery and extending the cycle life of the battery. Therefore, the negative electrode sheet of the embodiment of the present application is applied to the sodium battery, which can make the sodium battery have high energy density, high cycle stability and long cycle life.

[0007] In any embodiment of the present application, the aqueous binder includes at least one of carboxymethyl cellulose and its derivatives, polyacrylic acid and its derivatives, acrylonitrile multipolymers, sodium alginate and its derivatives, polyacrylate and its derivatives.

[0008] Optionally, the aqueous binder includes at least one of carboxymethyl cellulose and its derivatives.

[0009] The aqueous binder selected from the above types has a high polarity, and can not only have a high adhesion with the negative electrode current collector (such as copper foil, aluminum foil, etc.), thereby improving the interfacial adhesion between the conductive coating and the negative electrode current collector, but also can form hydrogen bonds with the polar functional groups on the surface of the conductive agent, thereby improving the cohesion of the conductive coating and inhibiting the structural changes of the conductive coating caused by the release of sodium. As a result, it is beneficial to further improve the interface flatness and structural stability of the conductive coating, and it is beneficial for sodium metal to be uniformly deposited on the surface of the negative electrode sheet and release, thereby helping to further improve the cycle performance of the battery. In particular, the viscosity of carboxymethyl cellulose and its derivatives are relatively stable, and have the properties of resistance to swelling and corrosion of electrolytes, which can provide stable viscosity and adhesion, thereby enabling the conductive coating and the negative electrode current collector to maintain a high interfacial adhesion during the battery charge and discharge cycle, thereby improving the structural stability of the negative electrode sheet and reducing the internal resistance of the battery. Therefore, the negative electrode sheet of the embodiment of the present application is applied to sodium batteries, which can significantly improve the cycle performance of the battery.

[0010] In any embodiment of the present application, the water-based binder includes a chemically blended modified water-based binder.

[0011] Optionally, the aqueous binder includes chemically blended modified carboxymethyl cellulose.

[0012] Chemical blending modification can flexibly regulate the structure of water-based binders, giving them good bonding properties, mechanical strength, suitable viscosity, etc. As a result, the interface flatness and structural stability of the conductive coating can be improved, and the sodium-philic nucleation sites of the conductive coating can be increased, thereby further improving the cycle performance of the battery.

[0013] In any embodiment of the present application, the aqueous binder includes carboxymethyl cellulose modified by graft copolymerization-blending of one or more of acrylic acid, o-hydroxyphenylethylamine, and polyvinyl alcohol.

[0014] The carboxymethyl cellulose modified by graft copolymerization and blending of one or more of acrylic acid, o-hydroxyphenylethylamine, and polyvinyl alcohol may contain more polar groups. In the conductive coating, this type of carboxymethyl cellulose can form hydrogen bonds between molecules in situ through polar groups, thereby further improving the mechanical properties of the binder network. This can further improve the collapse and change of the pole piece structure caused by the deposition of the metal layer. In addition, the polar group can further reduce the overpotential of sodium deposition. When the aqueous binder includes carboxymethyl cellulose graft copolymerized-modified by the above substances, this type of carboxymethyl cellulose is uniformly distributed in the conductive coating, so that sodium metal is uniformly deposited on the surface of the negative electrode. As a result, not only can the formation of sodium dendrites be suppressed, thereby improving the reliability and long-term cycle performance of the battery; but also the difficulty of sodium metal escaping can be reduced, and the irreversible loss of active sodium can be reduced, thereby improving the energy density and cycle life of the battery.

[0015] In any embodiment of the present application, the average degree of polymerization of the aqueous binder is 50-2500, and can be optionally 800-2000. When the average degree of polymerization of the aqueous binder is within this range, the aqueous binder can have a suitable viscosity and a higher resistance to electrolyte swelling and corrosion. As a result, the conductive coating and the negative electrode current collector can maintain a high interfacial adhesion during the battery charge and discharge cycle, thereby improving the structural stability of the negative electrode plate and reducing the internal resistance of the battery. Therefore, the negative electrode plate of the embodiment of the present application is applied to a sodium battery, which can significantly improve the cycle performance of the battery.

[0016] In any embodiment of the present application, the viscosity of the aqueous binder is 600mPa·s-2000mPa·s, and can be 600mPa·s-1200mPa·s. When the viscosity of the aqueous binder meets the given range, the aqueous binder can provide a stable bonding force during the battery charge and discharge cycle, so that the conductive coating and the negative electrode current collector maintain a high interfacial bonding force. This is conducive to improving the structural stability of the negative electrode sheet, reducing the internal resistance of the battery, and thus improving the cycle performance of the battery.

[0017] In any embodiment of the present application, the purity of the aqueous binder is above 95%, and can be selected to be above 95%-99%. This is beneficial to improve the bonding performance between the conductive coating and the negative electrode current collector, thereby improving the structural stability of the negative electrode sheet and further improving the cycle performance of the battery.

[0018] In any embodiment of the present application, the conductive agent includes a conductive carbon material.

[0019] Optionally, the conductive agent includes one or more of carbon nanotubes, graphene, and conductive carbon fibers.

[0020] More optionally, the conductive agent includes carbon nanotubes and / or reduced graphene oxide.

[0021] The conductive carbon material contains an appropriate amount of active oxygen-containing groups on its surface, which can interact with the aqueous binder to improve the mechanical properties of the conductive coating. This can inhibit the structural changes of the negative electrode sheet caused by the release of sodium during the charge and discharge process, thereby improving the cycle performance of the battery.

[0022] In any embodiment of the present application, the conductive agent includes a modified conductive carbon material.

[0023] Optionally, the conductive agent includes a conductive carbon material modified with one or more of -OH, -COOH, and -NH2.

[0024] More optionally, the conductive agent includes carbon nanotubes and / or reduced graphene oxide modified with one or more of -OH, -COOH, and -NH2.

[0025] The modified conductive carbon material can interact with the aqueous binder to form hydrogen bonds. As a result, the mechanical properties of the conductive coating can be further improved, and the structural changes of the conductive coating caused by the insertion and extraction of sodium can be suppressed. In addition, the presence of polar groups further reduces the overpotential of sodium metal deposition. When the conductive carbon material includes the modified groups, sodium metal can be deposited more evenly on the surface of the negative electrode. As a result, not only can the formation of sodium dendrites be suppressed, thereby improving the reliability and long-term cycle performance of the battery; but also the irreversible loss of active sodium can be reduced, thereby improving the energy density and cycle life of the battery.

[0026] In any embodiment of the present application, the sodium deposition potential of the conductive coating is 2.6 V-2.75 V. This is beneficial to the uniform deposition of sodium metal on the surface of the negative electrode, thereby improving the cycle performance of the battery.

[0027] In any embodiment of the present application, the thickness of the conductive coating is 1 μm-5 μm, and optionally 2 μm-3 μm. Thus, the thickness of the negative electrode plate can be reduced while the sodium metal is uniformly deposited on the surface of the negative electrode plate, thereby improving the energy density of the battery.

[0028] In any embodiment of the present application, based on the total mass of the conductive coating, the mass percentage of the aqueous binder is less than or equal to 5%, and can be optionally 2%-2.6%. The mass percentage of the aqueous binder satisfies the given range, which can improve the interface flatness and structural stability of the conductive coating while making the conductive coating have a suitable conductive agent content. As a result, the surface of the conductive coating can have an appropriate amount of sodium-philic nucleation sites, which is beneficial to improving the cycle performance of the battery.

[0029] In any embodiment of the present application, the Fourier transform infrared spectrum FTIR spectrum of the conductive coating has at least one of the characteristic peaks located at the following positions: 1300 cm -1 -1050cm -1 ; 3300cm -1 -2500cm -1 ; 3400cm -1 -3200cm -1 As a result, not only can the formation of sodium dendrites be suppressed, thereby improving the reliability and long-term cycle performance of the battery; it can also reduce the difficulty of sodium metal extraction and reduce the irreversible loss of active sodium ions, thereby improving the energy density and cycle life of the battery.

[0030] The second aspect of the embodiment of the present application provides a battery, comprising the negative electrode plate of the first aspect. Thus, the battery of the embodiment of the present application can have high energy density, high cycle stability and long cycle life.

[0031] A third aspect of an embodiment of the present application provides an electrical device, comprising the battery of the second aspect.

[0032] The electric device according to the embodiment of the present application comprises the battery according to the second aspect, and thus has at least the same advantages as the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of an implementation of a battery cell of the present application.

[0034] Figure 2 yes Figure 1 An exploded view of an embodiment of a battery cell of the present application is shown.

[0035] Figure 3 It is a schematic diagram of an embodiment of a battery module of the present application.

[0036] Figure 4 It is a schematic diagram of an embodiment of the battery pack of the present application.

[0037] Figure 5 yes Figure 4 An exploded view of an embodiment of a battery pack of the present application is shown.

[0038] Figure 6 It is a schematic diagram of an implementation of an electrical device of the present application, and the electrical device may include a battery pack or a battery module according to an embodiment of the present application as a power source.

[0039] 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 battery cell; 51 shell; 52 electrode assembly; 53 cover plate. DETAILED DESCRIPTION

[0040] Below, the embodiments of the negative electrode plate, the battery containing the negative electrode plate and the electric device of the present application are described in detail with appropriate reference to the drawings. However, there are cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0041] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0042] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0043] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0044] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0045] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0046] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0047] In the present application, the terms "plurality", "multiplicity" and the like refer to two or more.

[0048] Unless otherwise specified, the terms used in this application have the commonly understood meanings that are commonly understood by those skilled in the art.

[0049] Unless otherwise specified, the values ​​of the parameters mentioned in this application can be measured by various test methods commonly used in the art, for example, they can be measured according to the test methods given in the examples of this application. Unless otherwise specified, the test temperature of each parameter is 25°C.

[0050] Sodium-ion batteries have become a hot research topic in recent years due to their low cost, abundant resources, and similar manufacturing process to lithium-ion batteries. However, the low energy density of sodium-ion batteries is still a bottleneck limiting their application and promotion.

[0051] The sodium metal negative electrode has an ultra-high theoretical specific capacity and a low reduction potential. The sodium metal negative electrode usually includes a primer layer. During the charging process, the active sodium ions released from the positive electrode can be deposited at the sodium-philic nucleation sites of the primer layer to form a sodium metal layer. However, the sodium deposition interface of the primer layer involved in the related art is poor, and sodium dendrites are easily formed when sodium metal is deposited, thereby causing the risk of puncturing the isolation membrane, thereby reducing the reliability of the battery. In addition, after the sodium metal is embedded in the primer layer, when it is released again, holes will be formed in the primer layer. On the one hand, these holes will have a negative impact on the mechanical properties of the primer layer and increase the probability of collapse of the primer layer structure; on the other hand, part of the sodium metal in the holes is difficult to release, which may form "dead sodium", exacerbating the irreversible capacity loss of the battery. As a result, the long-term cycle performance of the battery is deteriorated.

[0052] In view of this, an embodiment of the present application provides a negative electrode plate for a sodium battery, which can enable the battery containing the negative electrode plate to have both high energy density and good cycle performance; the present application also provides a battery and an electrical device containing the composite conductive agent.

[0053] Negative electrode

[0054] In a first aspect of an embodiment of the present application, a negative electrode plate for a sodium battery is proposed, which includes a negative electrode current collector and a conductive coating, and the conductive coating is located on at least one side of the negative electrode current collector. The conductive coating includes a conductive agent and an aqueous binder, and the aqueous binder is selected from an aqueous binder with a relative dielectric constant greater than or equal to 2.5. For example, the aqueous binder can be selected from an aqueous binder with a relative dielectric constant of 2.5, 2.8, 3.0, 3.2, 3.5, 3.9, 4.1, 4.4, 4.8, 5.3, 5.7, 6.0, or a range consisting of any two of the above values.

[0055] Without intending to be bound by any theory or explanation, aqueous binders with a relative dielectric constant of 2.5 or greater can promote Na +Combining with electrons to form sodium metal is beneficial to the deposition of sodium metal at the negative electrode, and on the other hand, it can promote the interfacial flatness of the conductive coating. When the conductive coating has a high interfacial flatness, the orientation and trend of sodium metal deposition can be regulated so that the sodium metal is uniformly deposited on the surface of the negative electrode. As a result, not only can the formation of sodium dendrites be suppressed, thereby improving the reliability and long-term cycle performance of the battery; but also the difficulty of sodium metal detachment can be reduced, and the irreversible loss of active sodium ions can be reduced, thereby improving the energy density and cycle life of the battery. In addition, compared with other binders, the binder network formed by the aqueous binder with a relative dielectric constant greater than or equal to 2.5 in the conductive layer has higher mechanical strength, which can provide certain supporting properties for the conductive coating. As a result, it is beneficial to improve the structural stability of the conductive coating and reduce the risk of changes in the collector structure caused by the detachment of sodium metal, thereby improving the cycle stability of the battery and extending the cycle life of the battery.

[0056] Therefore, the negative electrode plate of the embodiment of the present application is applied to a sodium battery, which can enable the sodium battery to have high energy density, high cycle stability and long cycle life.

[0057] Examples of negative electrode current collectors may include one or more negative electrode current collectors known in the art that can be used for sodium batteries. In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as a metal foil, a copper foil or an aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0058] Examples of the conductive agent may include one or more conductive materials known in the art.

[0059] A water-based binder generally refers to a binder that can use water as a dispersant or solvent. Examples of water-based binders may include one or more water-based binders known in the art. Those skilled in the art may select a suitable water-based binder according to the needs of practical applications, provided that the relative dielectric constant is greater than or equal to 2.5, and this is not limited here.

[0060] In this article, relative dielectric constant has a meaning known in the art and can be measured by equipment and methods known in the art. For example, it can be measured with reference to the test standard GB / T 1409-88. The specific test method is as follows: The relative dielectric constant εr can be measured in an electrostatic field in the following way: First, the capacitance C0 of the capacitor is tested when there is a vacuum between the two capacitor plates. Then, for the same capacitor plates, the distance between the plates is kept unchanged, and after adding a dielectric between the plates, the capacitance Cx of the capacitor is measured. The relative dielectric constant of the dielectric can be calculated using the following formula.

[0061] εr=Cx / C0

[0062] At standard atmospheric pressure, the relative permittivity of dry air without carbon dioxide is 1.00053. Therefore, when the capacitance Ca of this electrode configuration in air is used instead of C0 to measure the relative permittivity εr, there is also sufficient accuracy.

[0063] In some embodiments, the aqueous binder may include at least one of carboxymethyl cellulose (CMC) and its derivatives, polyacrylic acid (PAA) and its derivatives, acrylonitrile multipolymers, sodium alginate and its derivatives, polyacrylate and its derivatives.

[0064] Alternatively, in some embodiments, the aqueous binder may include at least one of carboxymethyl cellulose and a derivative thereof.

[0065] Derivatives usually refer to products derived from the replacement of hydrogen atoms or atomic groups in a polymer by other atoms or atomic groups.

[0066] It is not intended to be limited to any theory or explanation. The aqueous binder selected from the above types has a high polarity, and can not only have a high adhesion with the negative electrode current collector (such as copper foil, aluminum foil, etc.), thereby improving the interfacial adhesion between the conductive coating and the negative electrode current collector, but also can form hydrogen bonds with the polar functional groups on the surface of the conductive agent, thereby improving the cohesion of the conductive coating and inhibiting the structural changes of the conductive coating caused by the sodium release. Thus, it is beneficial to further improve the interface flatness and structural stability of the conductive coating, and it is beneficial for sodium metal to be uniformly deposited on the surface of the negative electrode sheet and release, thereby helping to further improve the cycle performance of the battery. In particular, the viscosity of carboxymethyl cellulose and its derivatives are relatively stable, and have the properties of resistance to swelling and corrosion of the electrolyte, which can provide stable viscosity and adhesion, thereby enabling the conductive coating and the negative electrode current collector to maintain a high interfacial adhesion during the battery charge and discharge cycle, thereby improving the structural stability of the negative electrode sheet and reducing the internal resistance of the battery. Therefore, the negative electrode sheet of the embodiment of the present application is applied to sodium batteries, which can significantly improve the cycle performance of the battery.

[0067] In some embodiments, the water-based binder may include a chemically blended modified water-based binder.

[0068] Alternatively, in some embodiments, the aqueous binder may include chemically blended modified carboxymethyl cellulose.

[0069] Chemical blending modification has a well-known meaning in the art, which can refer to a macroscopically uniform and continuous material formed by mixing two or more polymers by chemical methods. Examples of chemical blending modification can include copolymerization-blending modification (e.g., graft copolymerization-blending modification, block copolymerization-blending modification, etc.), interpenetrating polymer network (PIN) method modification, etc. Those skilled in the art can select appropriate chemical blending modification methods and raw materials according to the needs of practical applications, which are not limited here.

[0070] Without intending to be limited by any theory or explanation, chemical blending modification can flexibly regulate the structure of the water-based binder, giving the water-based binder good bonding properties, mechanical strength, suitable viscosity and other properties. As a result, the interface flatness and structural stability of the conductive coating can be improved, and the sodium-philic nucleation sites of the conductive coating can be increased, thereby further improving the cycle performance of the battery.

[0071] In some embodiments, the aqueous binder may include carboxymethyl cellulose modified by graft copolymerization-blending of one or more of acrylic acid, o-hydroxyphenylethylamine, and polyvinyl alcohol.

[0072] Without intending to be limited by any theory or explanation, carboxymethyl cellulose modified by graft copolymerization-blending of one or more of acrylic acid, o-hydroxyphenylethylamine, and polyvinyl alcohol may contain more polar groups. In the conductive coating, this type of carboxymethyl cellulose can form hydrogen bonds between molecules in situ through polar groups, thereby further improving the mechanical properties of the binder network. This can further improve the collapse and change of the pole piece structure caused by the deposition of the metal layer. In addition, the polar group can further reduce the overpotential of sodium deposition. When the aqueous binder includes carboxymethyl cellulose grafted copolymerized-modified by the above substances, this type of carboxymethyl cellulose is uniformly distributed in the conductive coating, so that sodium metal is uniformly deposited on the surface of the negative electrode. As a result, not only can the formation of sodium dendrites be suppressed, thereby improving the reliability and long-term cycle performance of the battery; but also the difficulty of sodium metal detachment can be reduced, and the irreversible loss of active sodium can be reduced, thereby improving the energy density and cycle life of the battery.

[0073] The carboxymethyl cellulose modified by graft copolymerization-blending of one or more of the acrylic acid, o-hydroxyphenylethylamine and polyvinyl alcohol can be obtained commercially or prepared by methods known in the art, which are not limited here.

[0074] As an example, the carboxymethyl cellulose modified by acrylic acid graft copolymerization-blending can be obtained by an emulsion polymerization method. Specifically, carboxymethyl cellulose and acrylic acid can be copolymerized by an emulsion polymerization method so that the carboxyl group on the polyacrylic acid main chain and the hydroxyl group on the carboxymethyl cellulose main chain undergo a condensation reaction, thereby obtaining the carboxymethyl cellulose modified by acrylic acid graft copolymerization-blending. The reaction conditions and other necessary raw materials of emulsion polymerization are well known in the art, and those skilled in the art can adjust according to actual needs, and are not limited here. As an example, the carboxymethyl cellulose modified by o-hydroxyphenylethylamine graft copolymerization-blending can be obtained by the amidation reaction of o-hydroxyphenylethylamine and carboxymethyl cellulose. The reaction conditions and other necessary raw materials of the amidation reaction are well known in the art, and those skilled in the art can adjust according to actual needs, and are not limited here. As an example, the carboxymethyl cellulose modified by polyvinyl alcohol graft copolymerization-blending can be obtained by a solution polymerization method. Specifically, carboxymethyl cellulose and polyvinyl alcohol can be subjected to a condensation reaction by a solution polymerization method, thereby obtaining the carboxymethyl cellulose modified by polyvinyl alcohol graft copolymerization-blending. The reaction conditions and other necessary raw materials for solution polymerization are well known in the art, and those skilled in the art may adjust them according to actual needs, and are not limited here.

[0075] In some embodiments, the average polymer of the aqueous binder may be 50-2500, for example, 50, 100, 200, 500, 800, 1000, 1200, 1500, 1800, 2000, 2200, 2500, or a range consisting of any two of the above values.

[0076] Alternatively, in some embodiments, the average polymer of the carboxymethyl cellulose may also be 800-2000, for example, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800, 1900, 2000, or a range consisting of any two of the above values.

[0077] Without intending to be limited by any theory or explanation, when the average degree of polymerization of the aqueous binder is within the above-mentioned suitable range, the aqueous binder can have a suitable viscosity and a higher resistance to electrolyte swelling and corrosion. As a result, the conductive coating and the negative electrode current collector can maintain a high interfacial adhesion during the battery charge and discharge cycle, thereby improving the structural stability of the negative electrode plate and reducing the internal resistance of the battery. Therefore, the negative electrode plate of the embodiment of the present application is applied to a sodium battery, which can significantly improve the cycle performance of the battery.

[0078] The average degree of polymerization has a meaning well known in the art, and the average molecular weight can be measured by equipment and methods known in the art, and the degree of polymerization (total molecular weight / molecular weight of a single repeating unit) can be calculated by the average molecular weight. For example, the average molecular weight can be measured using one of end group analysis, boiling point elevation, freezing point depression, membrane osmotic pressure, light scattering, low-angle laser scattering, viscosity, gel permeation chromatography, etc.

[0079] In some embodiments, the viscosity of the aqueous adhesive can be 600mPa·s-2000mPa·s, for example, 600mPa·s, 900mPa·s, 1000mPa·s, 1100mPa·s, 1200mPa·s, 1300mPa·s, 1400mPa·s, 1500mPa·s, 1600mPa·s, 1700mPa·s, 1800mPa·s, 1900mPa·s, 2000mPa·s, or a range consisting of any two of the above values.

[0080] Optionally, in some embodiments, the viscosity of the aqueous adhesive can also be 600mPa·s-1200mPa·s, for example, it can be 600mPa·s, 700mPa·s, 800mPa·s, 900mPa·s, 1000mPa·s, 1100mPa·s, 1200mPa·s, or a range consisting of any two of the above values.

[0081] Without intending to be limited by any theory or explanation, when the viscosity of the aqueous binder meets the given range, the aqueous binder can provide stable bonding force during the battery charge and discharge cycle, so that the conductive coating and the negative electrode current collector maintain a high interfacial bonding force. This is conducive to improving the structural stability of the negative electrode sheet, reducing the internal resistance of the battery, and thus improving the battery cycle performance.

[0082] The viscosity of the aqueous binder has a well-known meaning in the art and can be measured by equipment and methods known in the art. For example, it can be measured by a capillary viscosity method according to GB / T 10247-2008.

[0083] In some embodiments, the purity of the aqueous binder may be above 95%. Alternatively, the purity of the aqueous binder may be between 95% and 99%.

[0084] When the purity of the aqueous binder meets the given range, it is beneficial to improve the bonding performance between the conductive coating and the negative electrode current collector, thereby improving the structural stability of the negative electrode sheet and thus improving the cycle performance of the battery.

[0085] The purity of the aqueous binder has a well-known meaning in the art and can be measured by equipment and methods known in the art, for example, by gas chromatography.

[0086] In some embodiments, the conductive agent may include a conductive carbon material.

[0087] Alternatively, in some embodiments, the conductive agent may include one or more of carbon nanotubes, graphene, and conductive carbon fibers.

[0088] Alternatively, in some embodiments, the conductive agent may include carbon nanotubes and / or reduced graphene oxide.

[0089] Without intending to be bound by any theory or explanation, the conductive carbon material contains an appropriate amount of active oxygen-containing groups on its surface, which can interact with the aqueous binder to improve the mechanical properties of the conductive coating. As a result, the structural changes of the negative electrode sheet caused by the release of sodium during the charge and discharge process can be suppressed, thereby improving the cycle performance of the battery.

[0090] In some embodiments, the conductive agent may include a modified conductive carbon material.

[0091] Alternatively, in some embodiments, the conductive agent may include a conductive carbon material modified by one or more of -OH, -COOH, and -NH2. For example, the conductive agent may include carbon nanotubes and / or reduced graphene oxide modified by one or more of -OH, -COOH, and -NH2.

[0092] Without intending to be limited by any theory or explanation, the modified conductive carbon material can interact with the aqueous binder to form hydrogen bonds. As a result, the mechanical properties of the conductive coating can be further improved, and the structural changes of the conductive coating caused by the insertion and extraction of sodium can be suppressed. In addition, the presence of polar groups further reduces the overpotential of sodium metal deposition. When the conductive carbon material includes the above-mentioned modifying groups, sodium metal can be more evenly deposited on the surface of the negative electrode. As a result, not only can the formation of sodium dendrites be suppressed, thereby improving the reliability and long-term cycle performance of the battery; but also the irreversible loss of active sodium is reduced, thereby improving the energy density and cycle life of the battery.

[0093] The conductive carbon material modified with one or more of -OH, -COOH, and -NH2 can be purchased commercially or prepared by methods known in the art, which are not limited here.

[0094] As an example, -OH-modified carbon nanotubes can be prepared by the following steps: the carbon nanotubes are mixed with a mixed solution of concentrated nitric acid and concentrated sulfuric acid (68% by mass concentrated nitric acid and 98% by mass concentrated sulfuric acid mixed in a volume ratio of 2:1), and then treated in a constant temperature water bath at 55°C-65°C for 3 hours to introduce carboxyl groups into the carbon nanotubes; the treated carbon nanotubes are mixed with a phosphorous acid reducing agent to reduce the carboxyl groups to hydroxyl groups to obtain -OH-modified carbon nanotubes.

[0095] As an example, -COOH-modified carbon nanotubes can be prepared by the following steps: carbon nanotubes are mixed with a mixed solution of concentrated nitric acid and concentrated sulfuric acid (68% by mass concentrated nitric acid and 98% by mass concentrated sulfuric acid mixed in a volume ratio of 2:1), and then treated in a constant temperature water bath at 55°C-65°C for 3 hours; the treated carbon nanotubes are transferred into a beaker, sodium hydroxide solution is added to the pH value of 7, and then washed with deionized water 3 times to obtain -COOH-modified carbon nanotubes.

[0096] As an example, -NH2-modified carbon nanotubes can be prepared by the following steps: reacting -COOH-modified carbon nanotubes with amine compounds (such as ethylenediamine, diethylamine, aniline, etc.) to obtain -NH2-modified carbon nanotubes.

[0097] It should be noted that the preparation steps of the modified conductive carbon material are only used as examples to explain the present application, rather than to limit the present application. Those skilled in the art can adjust the preparation conditions and raw materials according to actual needs to obtain the modified conductive carbon material of the embodiment of the present application. In some embodiments, the sodium deposition potential of the conductive coating can be 2.6V-2.75V.

[0098] Without intending to be bound by any theory or explanation, in the negative electrode sheet of the embodiment of the present application, the conductive coating has a specific composition, which can increase the sodium-philic nucleation sites on the surface of the conductive coating, so that the conductive coating has the above-mentioned lower sodium deposition potential. This is conducive to the uniform deposition of sodium metal on the negative electrode surface, thereby facilitating the improvement of the cycle performance of the battery.

[0099] The sodium deposition potential has a well-known meaning in the art and can be measured by equipment and methods known in the art. For example, the positive electrode active material NFPP (such as Na4Fe3(PO4)2P2O7) can be mixed with the positive electrode binder and the conductive agent in a mass ratio of 96:2:2, and N-methylpyrrolidone (NMP) can be added and stirred to obtain a positive electrode slurry; the positive electrode slurry is coated on an aluminum foil, and then dried, cold pressed, and cut to obtain a positive electrode sheet; the positive electrode sheet and the negative electrode sheet are assembled into a button-type full battery, and the button-type battery is charged using a battery charge and discharge instrument to obtain a first-cycle voltage-capacity curve, and the sodium deposition potential can be determined according to the voltage platform in the first-cycle voltage-capacity curve.

[0100] In some embodiments, the thickness of the conductive coating may be 1 μm-5 μm, for example, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, or a range consisting of any two of the above values.

[0101] Optionally, in some embodiments, the thickness of the conductive coating may also be 2 μm-3 μm, for example, 2 μm, 2.2 μm, 2.5 μm, 2.8 μm, 3 μm, or a range consisting of any two of the above values.

[0102] Without intending to be bound by any theory or explanation, the negative electrode sheet of the embodiment of the present application contains a specific aqueous binder, which can allow the conductive coating to have both a small thickness and a high interface flatness. Thus, while reducing the thickness of the negative electrode sheet, sodium metal can be uniformly deposited on the surface of the negative electrode sheet, thereby improving the energy density of the battery.

[0103] The thickness of the conductive coating has a well-known meaning in the art and can be measured by equipment and methods known in the art. For example, a scanning electron microscope (such as ZEISS Sigma300) can be used to obtain a cross-sectional scanning electron microscope (SEM) image of the negative electrode sheet with reference to JY / T 0584-2020. As an example, the test can be carried out as follows: randomly select multiple areas on the cross section of the negative electrode sheet, measure the thickness of the conductive coating at least five times at a certain magnification, count the measured values ​​of different areas, and take the average as the thickness of the conductive coating.

[0104] In some embodiments, based on the total mass of the conductive coating, the mass percentage of the aqueous binder can be less than or equal to 5%, for example, 5%, 4.5%, 4%, 3.5%, 3%, 2.5%, 2%, 1.5%, or a range consisting of any two of the above values.

[0105] Optionally, in some embodiments, based on the total mass of the conductive coating, the mass percentage of the aqueous binder can also be 2%-2.6%, for example, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, or a range consisting of any two of the above values.

[0106] Without intending to be limited by any theory or explanation, when the mass percentage of the aqueous binder in the conductive coating satisfies the given range, the conductive coating can have a suitable content of the conductive agent while improving the interface flatness and structural stability of the conductive coating. Thus, the conductive coating surface can have a suitable amount of sodium-philic nucleation sites, which is beneficial to improving the cycle performance of the battery.

[0107] In some embodiments, the Fourier transform infrared spectroscopy (FTIR) spectrum of the conductive coating has at least one of the characteristic peaks located at: 1300 cm -1 -1050cm -1 ; 3300cm -1 -2500cm -1 ; 3400cm -1 -3200cm -1 .

[0108] Above 1300cm -1 -1050cm -1 The characteristic peak of is used to characterize -OH; located at 3300cm -1 -2500cm -1 The characteristic peak of is used to characterize -COOH; located at 3400cm -1 -3200cm -1 The characteristic peak of is the characteristic peak used to characterize -NH2.

[0109] Without intending to be limited by any theory or explanation, when the conductive coating contains one or more of the above characteristic peaks, it means that the conductive coating contains a conductive agent and / or an aqueous binder modified by the above polar groups. As a result, the molecules modified by the polar groups can interact with each other to form hydrogen bonds. As a result, the mechanical properties of the conductive coating can be further improved, and the structural changes of the conductive coating caused by the insertion and extraction of sodium can be suppressed. In addition, there is a lower binding energy between sodium metal and the polar groups. When the conductive coating includes the above-mentioned modified groups, sodium metal can be deposited more evenly on the surface of the negative electrode. As a result, not only can the formation of sodium dendrites be suppressed, thereby improving the reliability and long-term cycle performance of the battery; but also the difficulty of sodium metal extraction can be reduced, and the irreversible loss of active sodium ions can be reduced, thereby improving the energy density and cycle life of the battery.

[0110] The negative electrode sheet includes a negative electrode current collector and a conductive coating disposed on at least one side of the negative electrode current collector. For example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the conductive coating is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0111] In some embodiments, the negative electrode sheet can be prepared in the following manner: the raw materials for preparing the conductive coating, such as the conductive agent, the aqueous binder and any other components are dispersed in a solvent (such as deionized water) to form a conductive coating slurry; the conductive coating slurry is coated on one or both surfaces of the negative electrode collector; after drying, cold pressing and other processes, the negative electrode sheet of the embodiment of the present application can be obtained.

[0112] In addition, the negative electrode plate of the embodiment of the present application does not exclude other additional functional layers besides the conductive coating. For example, in some embodiments, the negative electrode plate of the embodiment of the present application further includes a protective layer covering the surface of the conductive coating.

[0113] Battery

[0114] The second aspect of the embodiment of the present application provides a battery. The battery mentioned in the embodiment of the present application may include one or more battery cells to provide a single physical module with higher voltage and capacity. When there are multiple battery cells, the multiple battery cells are connected in series, in parallel or in mixed connection through a busbar.

[0115] The battery cell may be a secondary battery, which is also called a rechargeable battery or storage battery, and refers to a battery cell that can be recharged to activate the active material after the battery cell is discharged and continue to be used. The embodiment of the present application has no particular limitation on the type of secondary battery, and in particular, the secondary battery may be a sodium metal battery.

[0116] Typically, a battery cell includes an electrode assembly and an electrolyte, and the electrode assembly includes a positive electrode sheet, a negative electrode sheet, and a separator.

[0117] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0118] [Positive electrode]

[0119] The positive electrode plate included in the battery of the embodiment of the present application includes a positive electrode current collector and a positive electrode film layer located on at least one side of the positive electrode current collector, and the positive electrode film layer includes a positive electrode active material.

[0120] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0121] In the positive electrode sheet of the embodiment of the present application, the positive electrode active material may be a positive electrode active material for sodium batteries known in the art. As an example, the positive electrode active material may include but is not limited to at least one of a sodium-containing transition metal oxide, a polyanion material (such as phosphate, fluorophosphate, pyrophosphate, sulfate, etc.), and a Prussian blue material.

[0122] As an example, the positive electrode active material may include NaFeO2, NaCoO2, NaCrO2, NaMnO2, NaNiO2, NaNi 1 / 2Ti 1 / 2 O2、NaNi 1 / 2 Mn 1 / 2 O2、Na 2 / 3 Fe 1 / 3Mn 2 / 3 O2、NaNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, NaFePO4, NaMnPO4, NaCoPO4, Prussian blue materials, general formula X p M' q (PO4) r O x Y 3-x In the general formula X p M' q (PO4) r O x Y 3-x , 0<p≤4, 0<q≤2, 1≤r≤3, 0≤x≤2, X is selected from H + , Li + 、Na + , K + and NH4 + At least one of, M' is a transition metal cation, optionally at least one of V, Ti, Mn, Fe, Co, Ni, Cu and Zn, and Y is a halogen anion, optionally at least one of F, Cl and Br.

[0123] The modified compounds of the above-mentioned positive electrode active materials may be the ones that undergo doping modification and / or surface coating modification on the positive electrode active materials.

[0124] In some embodiments, the positive electrode film layer may further include a positive electrode conductive agent. The present application has no particular restrictions on the type of the positive electrode conductive agent. As an example, the positive electrode conductive agent includes at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0125] In some embodiments, the positive electrode film layer may further optionally include a positive electrode binder. The present application has no particular restrictions on the type of positive electrode binder. As an example, the positive electrode binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin.

[0126] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base and a metal material layer formed on at least one surface of the polymer material base. As an example, the metal material may include at least one of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).

[0127] The positive electrode film layer is usually formed by coating the positive electrode slurry on the positive electrode current collector, drying and cold pressing. The positive electrode slurry is usually formed by dispersing the positive electrode active material, optional conductive agent, optional binder and any other components in a solvent and stirring them uniformly. The solvent can be N-methylpyrrolidone (NMP), but is not limited thereto.

[0128] [Negative electrode]

[0129] The negative electrode sheet included in the battery of the embodiment of the present application includes the negative electrode sheet of the first aspect of the embodiment of the present application. The embodiment of the negative electrode sheet has been described and illustrated in detail above, and will not be repeated here. It can be understood that the battery of the embodiment of the present application can achieve the beneficial effects of any of the above embodiments of the negative electrode sheet of the embodiment of the present application.

[0130] [Isolation film]

[0131] The separator is disposed between the positive electrode sheet and the negative electrode sheet to play a role of isolation. The embodiment of the present application has no particular limitation on the type of separator, and any known porous structure separator with good chemical stability and mechanical stability can be selected.

[0132] In some embodiments, the material of the isolation membrane can be selected from one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer are the same or different, without special restrictions.

[0133] [Electrolytes]

[0134] The electrolyte plays a role in conducting ions between the positive electrode and the negative electrode. The present application embodiment has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid or gel.

[0135] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0136] In some embodiments, the electrolyte salt may include, but is not limited to, at least one of sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium hexafluoroarsenate (NaAsF6), sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), sodium trifluoromethanesulfonate (NaTFS), sodium difluorooxalatoborate (NaDFOB), sodium dioxalatoborate (NaBOB), sodium difluorophosphate (NaPO2F2), sodium difluorobis(oxalatophosphate) (NaDFOP), and sodium tetrafluorooxalatophosphate (NaTFOP).

[0137] In some embodiments, the solvent may include, but is not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).

[0138] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.

[0139] In some embodiments, the battery cell further includes a housing for accommodating the electrode assembly and the electrolyte. The housing of the battery cell may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The housing of the battery cell may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0140] The embodiment of the present application has no particular limitation on the shape of the battery cell, which can be cylindrical, square or any other shape. Figure 1 The battery cell 5 is a square structure as an example.

[0141] In some embodiments, reference Figure 2, the shell may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0142] The preparation method of the battery cell of the embodiment of the present application is well known. In some embodiments, the electrode assembly can be placed in a housing, dried, injected with electrolyte, and then vacuum packaged, allowed to stand, formed, shaped, etc. to obtain a battery cell.

[0143] In some embodiments, the battery mentioned in the embodiments of the present application refers to a single physical module including one or more battery cells to provide higher voltage and capacity. For example, the battery mentioned in the embodiments of the present application can be a battery module or a battery pack. The battery generally includes a box for encapsulating one or more battery cells. The box can prevent liquid or other foreign matter from affecting the charging or discharging of the battery cells.

[0144] In some embodiments, there may be multiple battery cells in the battery, and the multiple battery cells may be connected in series, in parallel, or in a hybrid connection. A hybrid connection means that the multiple battery cells are both connected in series and in parallel. The multiple battery cells may be directly connected in series, in parallel, or in a hybrid connection, and then the whole formed by the multiple battery cells is accommodated in the box; of course, multiple battery cells may be first connected in series, in parallel, or in a hybrid connection to form a battery module, and then the multiple battery modules are connected in series, in parallel, or in a hybrid connection to form a whole, and then accommodated in the box.

[0145] Figure 3 FIG. 4 is a schematic diagram of a battery module 4 as an example. Figure 3 As shown, there are multiple battery cells 5, and the multiple battery cells 5 are first connected in series, in parallel, or in mixed connection to form a battery module 4. The multiple battery cells 5 in the battery module 4 can be electrically connected through a busbar component to realize the series connection, parallel connection, or mixed connection of the multiple battery cells 5 in the battery module 4. In the battery module 4, the multiple battery cells 5 can be arranged in sequence along the length direction of the battery module 4. Of course, they can also be arranged in any other manner. Further, the multiple battery cells 5 can be fixed by fasteners.

[0146] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0147] Figure 4 and Figure 5 FIG. 1 is a schematic diagram of a battery pack 1 as an example. Figure 4 and Figure 5 As shown, the battery pack 1 may include a box body and a plurality of battery modules 4 disposed in the box body. The plurality of battery modules 4 in the battery pack 1 may be electrically connected through a busbar component to achieve series connection, parallel connection, or mixed connection of the plurality of battery modules 4 in the battery pack 1. The box body includes an upper box body 2 and a lower box body 3, wherein the upper box body 2 is used to cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box in any manner.

[0148] Electrical devices

[0149] The embodiment of the present application also provides an electric device, the electric device includes a battery cell provided in the embodiment of the present application, and the battery cell is used to provide electrical energy. The battery cell can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0150] As the electrical device, a battery cell, a battery module including a plurality of battery cells, or a battery pack may be selected according to its usage requirements.

[0151] Figure 6 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the requirements of the power consumption device for high power and high energy density, a battery pack or a battery module can be used.

[0152] As another example, the power-consuming device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be light and thin, and a battery cell may be used as a power source.

[0153] Example

[0154] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0155] Example 1

[0156] Preparation of negative electrode

[0157] The aqueous binder carboxymethyl cellulose (CMC) and the conductive agent carbon nanotube (CNT) are mixed in a mass ratio of 2.6:97.4, and dispersed in deionized water to obtain a conductive coating slurry; the conductive coating slurry is evenly coated on the surface of the negative electrode current collector aluminum foil, and dried, cold pressed, and cut to obtain a negative electrode sheet, which includes an aluminum foil and a conductive coating on the surface of the aluminum foil. Among them, the average polymerization degree of CMC is 1500, the viscosity is 2000mPa·s, and the mass percentage w of the aqueous binder in the conductive coating is 2.6%.

[0158] Preparation of positive electrode

[0159] The positive electrode active material Na4Fe3(PO4)2P2O7, the positive electrode binder polyvinylidene fluoride (PVDF), and the conductive agent carbon black (Super-P) are mixed in a mass ratio of 96:2:2, N-methylpyrrolidone (NMP) is added, and the mixture is stirred evenly to obtain a positive electrode slurry; the positive electrode slurry is coated on an aluminum foil, and then dried, cold pressed, and cut to obtain a positive electrode sheet.

[0160] Isolation film

[0161] Polypropylene film is used as the isolation film.

[0162] Preparation of electrolyte

[0163] NaPF6 was dissolved in a solvent prepared by diethylene glycol dimethyl ether and tetraethylene glycol dimethyl ether in a volume ratio of 1:1 to obtain an electrolyte with a NaPF6 concentration of 1 mol / L.

[0164] Preparation of secondary batteries

[0165] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order to obtain an electrode assembly; the electrode assembly is placed in a packaging shell, and a secondary battery is obtained through processes such as drying, liquid injection, vacuum packaging, standing, forming, and shaping.

[0166] Preparation of button cells

[0167] The negative electrode sheet was punched into a small disc with a diameter of 14 mm using a puncher, and the positive electrode sheet was punched into a small disc with a diameter of 13 mm. In a drying room, the small disc negative electrode and the separator (Celgard 2300 model), the small disc positive electrode sheet and the button battery shell were assembled into a button battery, and the above-mentioned electrolyte was added dropwise, and the button battery packaging machine was used to package to obtain a button battery.

[0168] Example 2-22

[0169] Based on the preparation process of the negative electrode sheet in Example 1, at least one of the type of aqueous binder, the average degree of polymerization n of the aqueous binder, the mass percentage w of the aqueous binder in the conductive coating, and the type of the conductive agent is adjusted as shown in Table 1 to prepare the negative electrode sheets of Examples 2-22. The preparation of the positive electrode sheets, separators, electrolytes, secondary batteries, and button batteries of Examples 2-22 is the same as that of Example 1. Among them, the aqueous binders of Examples 12-14 and 20-22 are CMC modified by graft copolymerization-blending of modified raw materials; the conductive agents of Examples 15-22 are conductive agents modified by modified groups, as shown in Table 1 for details.

[0170] Comparative Example 1-2

[0171] Based on the preparation process of the positive electrode sheet, the negative electrode sheet, the separator, the electrolyte, the secondary battery and the button battery of Example 1, as shown in Table 1, the positive electrode sheet, the negative electrode sheet, the separator, the electrolyte, the secondary battery and the button battery of Comparative Examples 1-2 were prepared by adjusting at least one of the type of aqueous binder, the average degree of polymerization n of the aqueous binder, the mass percentage w of the aqueous binder in the conductive coating, and the type of the conductive agent.

[0172] Test Section

[0173] The following tests were performed on Examples 1-22 and Comparative Examples 1-2, and the test results are shown in Table 2.

[0174] (1) Sodium deposition potential test

[0175] Use a battery charger and discharger to test the button cell. Set the charging voltage of the button cell to 100mV vs Na / Na + , the current density was set to 1 mA / cm 2 , and the voltage-capacity curve is obtained. The sodium deposition potential can be determined based on the voltage platform in the voltage-capacity curve.

[0176] (2) Battery DC resistance (DCR) test

[0177] At 25°C, the secondary battery was allowed to stand for 30 minutes, and then charged to 3.65V at a constant current of 0.33C; then charged to a cut-off current of 0.05C at a constant voltage of 3.65V; after standing for 30 minutes, the battery was discharged at a constant current of 0.33C for 90 minutes to a cut-off current of 0.5C, and the voltage at this time was recorded as U0; after standing for 30 minutes, the battery was discharged at a rate of 4C for 30 seconds, and the discharge current was recorded as I, and the voltage at the 5th, 10th, 20th, and 30th seconds of discharge was recorded as U n , n are 5, 10, 20, 30 respectively; let it stand for 5 minutes and end the test.

[0178] Calculating DCRn =(U n -U0) / I, get the DCR at 5s, 10s, 20s, and 30s of discharge, and take the average value as the DCR of the battery.

[0179] (3) Normal temperature cycle performance test

[0180] At 25°C, let the secondary battery stand for 30 minutes, then discharge it at 0.33C to 1.5V. After standing for 30 minutes, charge it at 0.33C constant current to 3.65V, then charge it at 3.65V constant voltage to a cut-off current of 0.05C; let it stand for 30 minutes; discharge it at 0.33C to 1.5V; let it stand for 30 minutes. This is a charge and discharge process, and the discharge capacity at this time is recorded as the discharge capacity of the first cycle of the battery. Repeat the charge and discharge cycles in this way, and record the number of cycles when the capacity is reduced to 80%.

[0181] Table 1

[0182]

[0183] Table 2

[0184] Serial number Sodium deposition potential / V DCR / mΩ Cycle life / cycle Example 1 2.70 1.2 1900 Example 2 2.75 1.1 1800 Example 3 2.75 1.3 1700 Example 4 2.73 1.4 1750 Example 5 2.70 1.3 1800 Example 6 2.70 1.2 1850 Example 7 2.70 1.2 1850 Example 8 2.65 0.8 1800 Example 9 2.65 1.1 1800 Example 10 2.74 4.3 1850 Embodiment 11 2.74 5.4 1820 Example 12 2.68 0.8 2300 Example 13 2.60 0.7 2500 Embodiment 14 2.65 1.1 2500 Embodiment 15 2.60 1.75 2200 Example 16 2.63 1.63 2100 Embodiment 17 2.60 0.8 2200 Embodiment 18 2.70 2.2 1800 Embodiment 19 2.75 2.5 1800 Embodiment 20 2.60 1.2 2150 Embodiment 21 2.60 0.98 2300 Embodiment 22 2.60 0.85 2173 Comparative Example 1 2.80 3.5 1200 Comparative Example 2 2.75 3 1500

[0185] It can be seen from Table 1 and Table 2 that the negative electrode plate provided in the embodiment of the present application is applied to a sodium battery, which can effectively improve the cycle performance of the battery.

[0186] In contrast, Comparative Example 1 uses a binder of styrene-butadiene rubber (SBR) and a conventional conductive agent CNT, and its sodium deposition potential and DCR are relatively high, which is not conducive to the uniform deposition of sodium metal and the stable cycle of the battery. Therefore, the cycle performance of the battery of Comparative Example 1 is far inferior to that of Examples 1 to 22. Although Comparative Example 2 uses CNT modified with -OH, thereby reducing the sodium deposition potential and DCR to a certain extent, the cycle performance of its battery is still not ideal.

[0187] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A negative electrode sheet for a sodium battery, comprising: Anode current collector; as well as The conductive coating is located on at least one side of the negative electrode current collector, and the conductive coating comprises a conductive agent and an aqueous binder, wherein the aqueous binder is selected from aqueous binders with a relative dielectric constant greater than or equal to 2.

5.

2. The negative electrode sheet according to claim 1, wherein: The aqueous binder includes at least one of carboxymethyl cellulose and its derivatives, polyacrylic acid and its derivatives, acrylonitrile multipolymer, sodium alginate and its derivatives, polyacrylate and its derivatives; Optionally, the aqueous binder includes at least one of carboxymethyl cellulose and its derivatives.

3. The negative electrode sheet according to claim 1 or 2, wherein: The aqueous binder includes a chemically blended modified aqueous binder; Optionally, the aqueous binder includes chemically blended modified carboxymethyl cellulose.

4. The negative electrode sheet according to any one of claims 1 to 3, wherein: The aqueous binder includes carboxymethyl cellulose modified by graft copolymerization-blending of one or more of acrylic acid, o-hydroxyphenylethylamine and polyvinyl alcohol.

5. The negative electrode sheet according to any one of claims 1 to 4, wherein: The average polymerization degree of the aqueous binder is 50-2500, and can be optionally 800-2000.

6. The negative electrode sheet according to any one of claims 1 to 5, wherein: The viscosity of the aqueous binder is 600mPa·s-2000mPa·s, and can be optionally 600mPa·s-1200mPa·s.

7. The negative electrode sheet according to any one of claims 1 to 6, wherein: The purity of the aqueous binder is above 95%, and can be selected to be above 95%-99%.

8. The negative electrode sheet according to any one of claims 1 to 7, wherein: The conductive agent includes a conductive carbon material; Optionally, the conductive agent includes one or more of carbon nanotubes, graphene, and conductive carbon fibers; More optionally, the conductive agent includes carbon nanotubes and / or reduced graphene oxide.

9. The negative electrode sheet according to any one of claims 1 to 8, wherein: The conductive agent includes a modified conductive carbon material; Optionally, the conductive agent includes a conductive carbon material modified by one or more of -OH, -COOH, and -NH2; More optionally, the conductive agent includes carbon nanotubes and / or reduced graphene oxide modified with one or more of -OH, -COOH, and -NH2.

10. The negative electrode sheet according to any one of claims 1 to 9, wherein: The sodium deposition potential of the conductive coating is 2.6V-2.75V.

11. The negative electrode sheet according to any one of claims 1 to 10, wherein: The thickness of the conductive coating is 1 μm-5 μm, optionally 2 μm-3 μm.

12. The negative electrode sheet according to any one of claims 1 to 11, wherein: Based on the total mass of the conductive coating, the mass percentage of the aqueous binder is less than or equal to 5%, and can be optionally 2%-2.6%.

13. The negative electrode sheet according to any one of claims 1 to 12, wherein: The Fourier transform infrared spectrum FTIR spectrum of the conductive coating has at least one of the characteristic peaks located at the following positions: 1300cm -1 -1050cm -1 ;3300cm -1 -2500cm -1 ;3400cm -1 -3200cm -1 。 14. A battery comprising the negative electrode sheet according to any one of claims 1 to 13.

15. An electrical device comprising the battery according to claim 14.

Citation Information

Patent Citations

  • Negative pole piece of sodium ion battery, electrochemical device and electronic device

    CN113437254A

  • Sodium metal battery and electrochemical device

    CN114824167A

  • Electrochemical device and electric device

    CN115036464A

  • Sodium-electricity composite negative electrode plate, preparation method and application of sodium-electricity composite negative electrode plate

    CN115939323A

  • In-situ crosslinking polymer binder for lithium-ion battery, and electrode manufactured by using same