Electrode material and preparation method thereof, electrode plate and preparation method thereof, battery and electric device

The electrode material with a pre-lithiated substrate and inorganic lithium compound layer addresses SEI-related capacity decay by uniformly replenishing lithium ions and forming a stable protective film, enhancing energy density and cycle life in secondary batteries.

CN119069654AActive Publication Date: 2024-12-03CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
CN202310628920.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

Secondary batteries experience irreversible capacity loss due to the formation and rupture of the solid electrolyte interface (SEI) film, leading to decreased energy density and shortened cycle life.

Method used

An electrode material with a pre-lithiated substrate and a coated inorganic lithium compound layer, comprising lithium oxide, nitride, carbonate, fluoride, or sulfide, forms a stable protective film, replenishing active lithium ions and enhancing environmental stability.

Benefits of technology

The electrode material improves energy density and extends cycle life by uniformly replenishing lithium ions, forming a dense protective film that reduces irreversible losses and stabilizes the electrode environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069654A_ABST
    Figure CN119069654A_ABST
Patent Text Reader

Abstract

The invention provides an electrode material and a preparation method thereof, an electrode plate and a preparation method thereof, a battery and an electric device. The electrode material comprises a base material and a first inorganic lithium compound layer coating at least part of the surface of the base material, and the base material comprises a pre-lithiated electrode active material; the first inorganic lithium compound layer comprises at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to an electrode material and a preparation method thereof, an electrode plate and a preparation method thereof, a battery and an electrical device. Background Art

[0002] Secondary batteries rely on the reciprocating insertion and extraction of active ions between the positive and negative electrodes to charge and discharge. They have outstanding characteristics such as high energy density, long cycle life, no pollution, and no memory effect. Therefore, as a clean energy, secondary batteries have gradually spread from electronic products to large-scale devices such as electric vehicles to adapt to the sustainable development strategy of the environment and energy. As a result, higher requirements are also placed on the energy density and cycle performance of secondary batteries. Summary of the invention

[0003] In order to achieve the above-mentioned objectives, the present application provides an electrode material and a preparation method thereof, an electrode plate and a preparation method thereof, a battery and an electrical device. The electrode material and the electrode plate are applied to secondary batteries to improve the energy density and cycle performance of the battery.

[0004] In a first aspect, an embodiment of the present application provides an electrode material, comprising: a substrate, the substrate comprising a pre-lithiation electrode active material; and a first inorganic lithium compound layer coated on at least a portion of the surface of the substrate, the first inorganic lithium compound layer comprising at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide.

[0005] Without intending to be limited by any theory or explanation, the substrate of the electrode material of the embodiment of the present application includes a pre-lithiation electrode active material, and the pre-lithiation electrode active material has been pre-embedded with some active lithium ions. During the first charge or discharge process, the pre-lithiation electrode active material can release active lithium ions, thereby compensating for the loss of active lithium ions in the battery formation process. Compared with the technical solution of directly compounding a metal lithium layer on the surface of the negative electrode pole piece in the related art, the electrode material of the embodiment of the present application has the advantage of more uniform lithium replenishment. In addition, the electrode material of the embodiment of the present application includes a first inorganic lithium compound layer, which can isolate the substrate from the air on the one hand, improve the stability of the chemical properties of the substrate, so that the electrode material maintains a high lithium replenishment efficiency; on the other hand, the first inorganic lithium compound layer can form a dense, uniform and stable protective film on the surface of the electrode pole piece, which can play a role similar to that of the SEI film, thereby improving the environmental stability of the electrode, reducing the irreversible loss of active lithium ions, and slowing down the capacity decay of the secondary battery. Therefore, the electrode material of the embodiment of the present application is applied to the secondary battery, which can improve the energy density of the secondary battery and extend the cycle life of the secondary battery.

[0006] In any embodiment of the present application, the first inorganic lithium compound layer includes at least two of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride or lithium sulfide.

[0007] Optionally, based on the total mass of the first inorganic lithiation layer, the first inorganic lithiation layer includes 18%-90% lithium nitride, 0-28% lithium fluoride, 0-80% lithium oxide, 0-2% lithium carbonate, and 0-20% lithium sulfide.

[0008] More optionally, based on the total mass of the first inorganic lithiation layer, the first inorganic lithiation layer includes 70%-90% of lithium nitride, 0-30% of lithium oxide, and 0-10% of lithium sulfide.

[0009] When the first inorganic lithium compound layer has the above composition, it is beneficial to protect the substrate and inhibit the side reaction between the substrate and the air, so that the electrode material maintains a high lithium replenishment efficiency. In addition, when the first inorganic lithium compound layer has the above composition, it is applied to a secondary battery, which is beneficial to form a uniform, dense and stable protective film on the surface of the electrode plate, thereby further improving the cycle stability of the secondary battery.

[0010] In any embodiment of the present application, the thickness of the first inorganic lithium compound layer is 2nm-5000nm, and can be optionally 20nm-1000nm.

[0011] The thickness of the first inorganic lithium compound layer satisfies the given range, which can not only improve the stability of the chemical properties of the substrate, but also enable the electrode material to maintain a high substrate content. Thus, the lithium replenishment efficiency of the electrode material can be significantly improved. In addition, the thickness of the first inorganic lithium compound layer is within the above-mentioned suitable range, which also helps to improve the environmental stability of the electrode. Thus, the capacity decay of the secondary battery can be suppressed and the cycle life of the secondary battery can be extended.

[0012] In any embodiment of the present application, the volume distribution particle size Dv50 of the electrode material is 0.6 μm-60 μm, and can be 5 μm-15 μm. This is conducive to the release of active lithium ions from the electrode material, improving the lithium replenishment efficiency of the electrode material, thereby helping to further delay the capacity decay of the secondary battery and extend the cycle life of the secondary battery.

[0013] In any embodiment of the present application, the electrode material is a positive electrode material, and the lithium supplement content of the positive electrode material is 1%-30%, and can be 5%-20%; the lithium supplement content of the positive electrode material is determined by (C1-C 10 ) / C 10 ×100%, where C1 is the actual gram capacity of the positive electrode material in mAh / g, C 10The theoretical gram capacity of the positive electrode active material is expressed in mAh / g. Thus, the secondary battery can have both good cycle performance and high reliability.

[0014] In any embodiment of the present application, the electrode material is a negative electrode material, and the lithium supplement content of the negative electrode material is 1%-100%, and can be 30%-50%; the lithium supplement content of the negative electrode material is determined by (C 20 -C2) / C 20 ×100%, where C2 is the actual gram capacity of the negative electrode material in mAh / g, and C 20 The theoretical gram capacity of the negative electrode active material is expressed in mAh / g. Thus, the secondary battery can have both good cycle performance and high reliability.

[0015] In a second aspect, an embodiment of the present application provides a method for preparing an electrode material, comprising:

[0016] Mixing lithium metal with a complexing agent solution to allow the lithium metal to react with the complexing agent to obtain a liquid-phase lithiating agent;

[0017] contacting a liquid-phase lithiating agent with an electrode active material so that the liquid-phase lithiating agent pre-lithiates the electrode active material to obtain a pre-lithiated electrode active material;

[0018] contacting the pre-lithiated electrode active material with a reactant to form a first inorganic lithiation layer on at least a portion of the surface of the pre-lithiated electrode active material to obtain an electrode material;

[0019] Among them, the electrode material includes: a substrate, the substrate includes a pre-lithiation electrode active material; and a first inorganic lithium compound layer coated on at least a portion of the surface of the substrate, the first inorganic lithium compound layer includes at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide.

[0020] The method provided in the embodiment of the present application is simple to operate, has mild conditions and is easy to control. The substrate of the prepared electrode material has been pre-embedded with some active lithium ions. During the first charge or discharge process, the electrode material can release active lithium ions, thereby compensating for the loss of active lithium ions in the battery formation process. In addition, the electrode material prepared by the method of the embodiment of the present application can also form a dense, uniform and stable protective film on the surface of the electrode pole piece through the first inorganic lithium compound layer. The protective film can play a similar role to the SEI film, thereby improving the environmental stability of the electrode, reducing the irreversible loss of active lithium ions, and slowing down the capacity decay of the secondary battery. Therefore, the electrode material prepared in the embodiment of the present application is applied to secondary batteries, which can improve the energy density of the secondary batteries and extend the cycle life of the secondary batteries.

[0021] In any embodiment of the present application, the preparation method further comprises:

[0022] Providing a complexing reagent solution includes uniformly mixing the complexing reagent and the solvent to obtain the complexing reagent solution.

[0023] Optionally, the complexing reagent includes at least one of naphthalene and its derivatives, biphenyl and its derivatives, phenanthrene and its derivatives, pyrene and its derivatives, fluorene and its derivatives, indene and its derivatives or aromatic hydrocarbon derivatives containing heteroatom functional groups, and more optionally includes at least one of 2-methylnaphthalene, 1-naphthonitrile, 2,2-dimethylbiphenyl, 2-ethylindene, 1-methyl-3-ethylpyrene or benzophenone.

[0024] Optionally, the solvent includes at least one of alkanes and their derivatives, aromatic hydrocarbons and their derivatives, ether compounds and their derivatives, furan compounds and their derivatives, pyran compounds and their derivatives, or esters and their derivatives, and more optionally includes at least one of benzene, toluene, xylene, ethylbenzene, ethylene glycol dimethyl ether, 2-methyltetrahydrofuran, pyran or fluoroethylene carbonate.

[0025] The complexing agent selected from the above types can react with lithium metal to generate a liquid-phase lithiating agent with a lower redox potential. As a result, the liquid-phase lithiating agent is more likely to pre-lithiate the electrode active material and embed active lithium ions in the electrode active material, which is beneficial to improving the lithium replenishment efficiency of the electrode material. Furthermore, the use of the above-mentioned types of solvents to dissolve the complexing agent is beneficial to further adjust the redox potential of the liquid-phase lithiating agent within a suitable range, thereby further improving the efficiency of pre-lithiation and further improving the lithium replenishment efficiency of the electrode material.

[0026] In any embodiment of the present application, the redox potential of the liquid-phase lithiating agent is 0.05 V-1.5 V, and can be optionally 0.1 V-0.5 V. Thus, the efficiency of pre-lithiation can be further improved, thereby improving the lithium replenishment efficiency of the electrode material.

[0027] In any embodiment of the present application, the molar ratio of lithium metal to the complexing agent is (0.5:1)-(10:1), and can be optionally (1:1)-(4:1).

[0028] In any embodiment of the present application, the molar concentration of lithium element in the liquid-phase lithiating agent is 0.01 mol / L-10 mol / L, and can be optionally 0.01 mol / L-5 mol / L.

[0029] When the molar ratio of lithium metal to the complexing agent is within the above range, it not only helps to improve the reaction efficiency of lithium metal and the complexing agent, but also helps to adjust the content of lithium in the liquid-phase lithiating agent within a suitable range. In the liquid-phase lithiating agent, the content of lithium in a suitable range can improve the pre-lithiation efficiency of the liquid-phase lithiating agent for the electrode active material.

[0030] In any embodiment of the present application, the molar ratio of lithium element to electrode active material in the liquid phase lithiating agent is (0.05:1)-(10:1), and can be (0.1:1)-(5:1). Thus, during the battery formation process, the electrode material can release an appropriate amount of active lithium ions to supplement the active lithium ions lost during the first cycle of charge and discharge cycles.

[0031] In any embodiment of the present application, the volume distribution particle size Dv50 of the electrode active material is 0.5 μm-40 μm. This is conducive to the release of active lithium ions from the electrode material, improving the lithium replenishment efficiency of the electrode material, thereby helping to further delay the capacity decay of the secondary battery and extend the cycle life of the secondary battery.

[0032] In any embodiment of the present application, the reactants include at least one of air, water, oxygen, carbon dioxide, nitrogen, nitric oxide, nitrogen dioxide, nitrogen pentoxide, hydrogen fluoride, fluorine, sulfur, hydrogen sulfide, sulfur dioxide, sulfur trioxide or red phosphorus, and can optionally include at least one of carbon dioxide, fluorine, nitrogen, sulfur dioxide or red phosphorus.

[0033] By selecting appropriate reactants, the composition of the first inorganic lithium compound layer can be regulated. The first inorganic lithium compound layer has an appropriate composition, which is beneficial to suppress the side reaction between the substrate and the air, so that the electrode material maintains a high lithium replenishment efficiency, and is beneficial to regulating the composition of the protective film on the electrode surface, thereby improving the stability of the electrode environment. This helps to further improve the cycle stability of the secondary battery and extend the cycle life of the secondary battery.

[0034] In a third aspect, an embodiment of the present application provides an electrode plate, comprising a current collector and an electrode film layer located on at least one side of the current collector, wherein the electrode film layer comprises an electrode material; the electrode material comprises: a substrate, the substrate comprises a pre-lithiation electrode active material; and a first inorganic lithium compound layer coated on at least a portion of the surface of the substrate, the first inorganic lithium compound layer comprises at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide.

[0035] The electrode plate of the third aspect includes an electrode material, and the substrate of the electrode material has been pre-embedded with some active lithium ions. During the first charge or discharge process, the electrode material can release active lithium ions, thereby compensating for the loss of active lithium ions during the battery formation process. In addition, the electrode material can also form a dense, uniform and stable protective film on the surface of the electrode plate through the first inorganic lithium compound layer. The protective film can play a similar role to the SEI film, thereby improving the environmental stability of the electrode, reducing the irreversible loss of active lithium ions, and slowing down the capacity decay of the secondary battery. Therefore, the electrode plate of the embodiment of the present application is applied to the secondary battery, which can improve the energy density of the secondary battery and extend the cycle life of the secondary battery.

[0036] In any embodiment of the present application, the electrode plate also includes a second inorganic lithium compound layer attached to at least a portion of the surface of the electrode film layer, and the second inorganic lithium compound layer includes at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide.

[0037] When the electrode plate further includes a second inorganic lithium compound layer attached to at least a portion of the surface of the electrode film layer, it is beneficial to further improve the stability of the electrode environment during the charge and discharge cycle, thereby improving the cycle stability of the secondary battery.

[0038] In any embodiment of the present application, the first inorganic lithium compound layer includes at least two of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride or lithium sulfide.

[0039] Optionally, based on the total mass of the first inorganic lithiation layer, the first inorganic lithiation layer includes 18%-90% lithium nitride, 0-28% lithium fluoride, 0-80% lithium oxide, 0-2% lithium carbonate, and 0-20% lithium sulfide.

[0040] More optionally, based on the total mass of the first inorganic lithiation layer, the first inorganic lithiation layer includes 70%-90% of lithium nitride, 0-30% of lithium oxide, and 0-10% of lithium sulfide.

[0041] When the first inorganic lithium compound layer has the above composition, it is beneficial to protect the substrate and inhibit the side reaction between the substrate and the air, so that the electrode material maintains a high lithium replenishment efficiency. In addition, when the first inorganic lithium compound layer has the above composition, it is also beneficial to form a uniform, dense and stable protective film on the surface of the electrode plate, thereby further improving the cycle stability of the secondary battery.

[0042] In a fourth aspect, an embodiment of the present application provides a method for preparing an electrode plate, including method A or method B.

[0043] Method A:

[0044] Mixing lithium metal with a complexing agent solution to allow the lithium metal to react with the complexing agent to obtain a liquid-phase lithiating agent;

[0045] contacting a liquid-phase lithiating agent with an electrode active material so that the liquid-phase lithiating agent pre-lithiates the electrode active material to obtain a pre-lithiated electrode active material;

[0046] contacting the pre-lithiated electrode active material with a reactant to form a first inorganic lithiation layer on at least a portion of the surface of the pre-lithiated electrode active material to obtain an electrode material;

[0047] The electrode material includes: a substrate, the substrate includes a pre-lithiation electrode active material; and a first inorganic lithium compound layer coated on at least a portion of the surface of the substrate, the first inorganic lithium compound layer includes at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide;

[0048] An electrode sheet including an electrode material is prepared.

[0049] Method B:

[0050] Providing an initial pole piece, the initial pole piece comprising a current collector and an electrode film layer located on at least one side of the current collector, the electrode film layer comprising an electrode active material;

[0051] Mixing lithium metal with a complexing agent solution to allow the lithium metal to react with the complexing agent to obtain a liquid-phase lithiating agent;

[0052] contacting a liquid-phase lithiating agent with the electrode film layer so that the liquid-phase lithiating agent pre-lithiates the electrode active material to obtain a pole piece including the pre-lithiated electrode active material;

[0053] Contacting a pole piece including a pre-lithiated electrode active material with a reactant to form a first inorganic lithiation layer on a surface of the pre-lithiated electrode active material, thereby obtaining an electrode pole piece including an electrode material;

[0054] Among them, the electrode material includes: a substrate, the substrate includes a pre-lithiation electrode active material; and a first inorganic lithium compound layer coated on at least a portion of the surface of the substrate, the first inorganic lithium compound layer includes at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide.

[0055] The electrode plate prepared according to method A or method B includes an electrode material, and the substrate of the electrode material has been pre-embedded with some active lithium ions. During the first charge or discharge process, the electrode material can release active lithium ions, thereby compensating for the loss of active lithium ions in the battery formation process. In addition, the electrode material can also form a dense, uniform and stable protective film on the surface of the electrode plate through the first inorganic lithium compound layer. The protective film can play a similar role to the SEI film, thereby improving the environmental stability of the electrode, reducing the irreversible loss of active lithium ions, and slowing down the capacity decay of the secondary battery. Therefore, the electrode plate prepared in the embodiment of the present application is applied to a secondary battery, which can improve the energy density of the secondary battery and extend the cycle life of the secondary battery.

[0056] In any embodiment of the present application, method A and / or method B further comprises:

[0057] Providing a complexing reagent solution includes uniformly mixing the complexing reagent and the solvent to obtain the complexing reagent solution.

[0058] Optionally, the complexing reagent includes at least one of naphthalene and its derivatives, biphenyl and its derivatives, phenanthrene and its derivatives, pyrene and its derivatives, fluorene and its derivatives, indene and its derivatives or aromatic hydrocarbon derivatives containing heteroatom functional groups, and more optionally includes at least one of 2-methylnaphthalene, 1-naphthonitrile, 2,2-dimethylbiphenyl, 2-ethylindene, 1-methyl-3-ethylpyrene or benzophenone.

[0059] Optionally, the solvent includes at least one of alkanes and their derivatives, aromatic hydrocarbons and their derivatives, ether compounds and their derivatives, furan compounds and their derivatives, pyran compounds and their derivatives, or esters and their derivatives, and more optionally includes at least one of benzene, toluene, xylene, ethylbenzene, ethylene glycol dimethyl ether, 2-methyltetrahydrofuran, pyran or fluoroethylene carbonate.

[0060] The complexing agent selected from the above types can react with lithium metal to generate a liquid-phase lithiating agent with a lower redox potential. As a result, the liquid-phase lithiating agent is more likely to pre-lithiate the electrode active material and embed active lithium ions in the electrode active material, which is beneficial to improving the lithium replenishment efficiency of the electrode material. Furthermore, the use of the above-mentioned types of solvents to dissolve the complexing agent is beneficial to further adjust the redox potential of the liquid-phase lithiating agent within a suitable range, thereby further improving the efficiency of pre-lithiation and further improving the lithium replenishment efficiency of the electrode plate.

[0061] In any embodiment of the present application, in method A and / or method B, the redox potential of the liquid phase lithiating agent is 0.05 V-1.5 V, and can be optionally 0.1 V-0.5 V. Thus, the efficiency of pre-lithiation can be further improved, thereby improving the lithium replenishment efficiency of the electrode plate.

[0062] In any embodiment of the present application, in method A and / or method B, the molar ratio of lithium metal to the complexing agent is (0.5:1)-(10:1), and can be optionally (1:1)-(4:1).

[0063] In any embodiment of the present application, in method A and / or method B, the molar concentration of lithium element in the liquid-phase lithiating agent is 0.01 mol / L-10 mol / L, and can be optionally 0.01 mol / L-5 mol / L.

[0064] When the molar ratio of lithium metal to the complexing agent is within the above range, it not only helps to improve the reaction efficiency of lithium metal and the complexing agent, but also helps to adjust the content of lithium in the liquid-phase lithiating agent within a suitable range. In the liquid-phase lithiating agent, the content of lithium in a suitable range can improve the pre-lithiation efficiency of the liquid-phase lithiating agent on the electrode active material, thereby improving the lithium replenishment efficiency of the electrode plate.

[0065] In any embodiment of the present application, in method A and / or method B, the molar ratio of lithium element to electrode active material in the liquid phase lithiating agent is (0.05:1)-(10:1), and can be (0.1:1)-(5:1). Thus, during the battery formation process, the electrode material can release an appropriate amount of active lithium ions to supplement the active lithium ions lost during the first cycle of charge and discharge cycles.

[0066] In any embodiment of the present application, in method A and / or method B, the volume distribution particle size Dv50 of the electrode active material is 0.5 μm-40 μm. This is conducive to the release of active lithium ions from the electrode material, improving the lithium replenishment efficiency of the electrode plate, thereby helping to further delay the capacity decay of the secondary battery and extend the cycle life of the secondary battery.

[0067] In any embodiment of the present application, in method A and / or method B, the reactants include at least one of air, water, oxygen, carbon dioxide, nitrogen, nitric oxide, nitrogen dioxide, nitrogen pentoxide, hydrogen fluoride, fluorine, sulfur, hydrogen sulfide, sulfur dioxide, sulfur trioxide or red phosphorus, and can optionally include at least one of carbon dioxide, fluorine, nitrogen, sulfur dioxide or red phosphorus.

[0068] By selecting appropriate reactants, the composition of the first inorganic lithium compound layer can be regulated. The first inorganic lithium compound layer has an appropriate composition, which is beneficial to suppress the side reaction between the substrate and the air, so that the electrode material maintains a high lithium replenishment efficiency, and is beneficial to regulating the composition of the protective film on the electrode surface, thereby improving the stability of the electrode environment. This helps to further improve the cycle stability of the secondary battery and extend the cycle life of the secondary battery.

[0069] In a fifth aspect, an embodiment of the present application provides a battery, comprising at least one of the electrode material of the first aspect, the electrode material prepared according to the preparation method of the second aspect, the electrode plate of the third aspect, or the electrode plate prepared according to the preparation method of the fourth aspect. Thus, it can have both high energy density and long cycle life.

[0070] In a sixth aspect, an embodiment of the present application provides an electrical device comprising the battery of the fifth aspect.

[0071] The electric device according to the embodiment of the present application includes the battery provided by the embodiment of the present application, and thus has at least the same advantages as the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0072] Figure 1 It is a schematic diagram of an implementation of a battery cell of the present application.

[0073] Figure 2 yes Figure 1 An exploded view of an embodiment of a battery cell of the present application is shown.

[0074] Figure 3 It is a schematic diagram of an embodiment of a battery module of the present application.

[0075] Figure 4 It is a schematic diagram of an embodiment of the battery pack of the present application.

[0076] Figure 5 yes Figure 4 An exploded view of an embodiment of a battery pack of the present application is shown.

[0077] Figure 6 It is a schematic diagram of an electrical device using the battery embodiment of the present application as a power source.

[0078] 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 battery cell; 51 shell; 52 electrode assembly; 53 cover plate. DETAILED DESCRIPTION

[0079] Below, the electrode material and its preparation method, electrode pole piece and its preparation method, battery and electric device of the present application are described in detail with appropriate reference to the drawings. However, there are cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0080] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0081] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0082] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0083] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0084] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0085] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0086] Herein, derivatives generally refer to products derived from the substitution of hydrogen atoms or atomic groups in a polymer by other atoms or atomic groups.

[0087] With the application and promotion of secondary batteries in various electronic products and new energy vehicles and other industries, higher requirements are placed on the energy density and cycle performance of secondary batteries.

[0088] During the first charge of a secondary battery, a solid electrolyte interface (SEI) film is inevitably formed on the surface of the negative electrode active material, causing irreversible consumption of active ions, thereby leading to irreversible capacity loss of the secondary battery. In addition, during the charge and discharge cycle, the SEI film may rupture due to expansion of the negative electrode active material, and active lithium ions need to be continuously consumed to form a new SEI film, which further aggravates the capacity decay of the battery, resulting in a decrease in the energy density of the battery and a shortened cycle life.

[0089] To this end, the present application provides an electrode material and a preparation method thereof, wherein the electrode material can effectively replenish consumed active lithium ions; the present application also provides an electrode plate comprising the electrode material and a preparation method thereof, a battery and an electrical device.

[0090] Electrode Materials

[0091] In a first aspect, an embodiment of the present application proposes an electrode material, comprising a substrate and a first inorganic lithium compound layer, wherein the first inorganic lithium compound layer is coated on at least a portion of the surface of the substrate; the substrate comprises a pre-lithiation electrode active material, and the first inorganic lithium compound layer comprises at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide.

[0092] Without intending to be limited by any theory or explanation, the substrate of the electrode material of the embodiment of the present application includes a pre-lithiation electrode active material, and the pre-lithiation electrode active material has been pre-embedded with some active lithium ions. During the first charge or discharge process, the pre-lithiation electrode active material can release active lithium ions, thereby compensating for the loss of active lithium ions in the battery formation process. Compared with the technical solution of directly compounding a metal lithium layer on the surface of the negative electrode pole piece in the related art, the electrode material of the embodiment of the present application has the advantage of more uniform lithium replenishment. In addition, the electrode material of the embodiment of the present application includes a first inorganic lithium compound layer, which can isolate the substrate from the air on the one hand, improve the stability of the chemical properties of the substrate, so that the electrode material maintains a high lithium replenishment efficiency; on the other hand, the first inorganic lithium compound layer can form a dense, uniform and stable protective film on the surface of the electrode pole piece, which can play a role similar to that of the SEI film, thereby improving the environmental stability of the electrode, reducing the irreversible loss of active lithium ions, and slowing down the capacity decay of the secondary battery. Therefore, the electrode material of the embodiment of the present application is applied to the secondary battery, which can improve the energy density of the secondary battery and extend the cycle life of the secondary battery.

[0093] The pre-lithiation electrode active material has a meaning known in the art, which may refer to an electrode active material pre-embedded with active lithium ions. The electrode active material may include an electrode active material known in the art that has not been pre-lithiation treated, and the present application does not limit the specific type of the electrode active material. As an example, the electrode active material may include at least one positive electrode active material known in the art, or include at least one negative electrode active material known in the art.

[0094] The type of positive electrode active material is not specifically limited, and positive electrode active materials for secondary batteries known in the art can be used. For example, the positive electrode active material may include at least one of the following positive electrode active materials: lithium transition metal oxide, lithium phosphate containing olivine structure and their respective modified compounds. Examples of lithium transition metal oxides may include, but are not limited to, at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide and their modified compounds. Examples of lithium phosphate containing olivine structure may include, but are not limited to, lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, lithium iron manganese phosphate and carbon composite materials and their respective modified compounds. The embodiments of the present application are not limited to these materials, and other conventionally known materials that can be used as positive electrode active materials for secondary batteries can also be used. These positive electrode active materials can be used alone or in combination of two or more.

[0095] Optionally, in some embodiments, the positive electrode active material may include at least one of the following positive electrode active materials: lithium iron phosphate, nickel-cobalt-manganese ternary material, cobalt-free positive electrode material, lithium iron manganese phosphate, and lithium manganate.

[0096] The type of negative electrode active material is not specifically limited, and negative electrode active materials for secondary batteries known in the art can be used. As an example, the negative electrode active material may include at least one of the following negative electrode active materials: graphite, soft carbon, hard carbon, mesophase carbon microspheres, silicon-based materials, tin-based materials, lithium titanate. Silicon-based materials may include one or more of elemental silicon, silicon oxide, silicon-carbon composites, silicon-nitrogen composites, and silicon alloy materials. Tin-based materials may include one or more of elemental tin, tin oxide, and tin alloy materials. The present application is not limited to these materials, and other conventionally known materials that can be used as negative electrode active materials for secondary batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0097] Optionally, in some embodiments, the negative electrode active material may include at least one of the following negative electrode active materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based material, tin-based material, phosphorus-based material, lithium titanate.

[0098] In some embodiments, based on the total mass of the first inorganic lithiation layer, the first inorganic lithiation layer may include 0-80% lithium oxide, 0-100% lithium carbonate, 0-100% lithium fluoride, 0-45% lithium phosphide, 0-90% lithium nitride, and 0-55% lithium sulfide.

[0099] Optionally, in some embodiments, based on the total mass of the first inorganic lithium compound layer, the first inorganic lithium compound layer may include 0-100% lithium fluoride, 0-80% lithium oxide, 0-50% lithium nitride, 0-100% lithium carbonate, and 0-55% lithium sulfide.

[0100] In some embodiments, the first inorganic lithiation layer may include at least two of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, or lithium sulfide.

[0101] Optionally, in some embodiments, based on the total mass of the first inorganic lithium compound layer, the first inorganic lithium compound layer may include 18%-90% lithium nitride, 0-28% lithium fluoride, 0-80% lithium oxide, 0-2% lithium carbonate, and 0-20% lithium sulfide.

[0102] More optionally, in some embodiments, based on the total mass of the first inorganic lithiation layer, the first inorganic lithiation layer may include 70%-90% lithium nitride, 0-30% lithium oxide, and 0-10% lithium sulfide.

[0103] When the first inorganic lithium compound layer has the above composition, it is beneficial to protect the substrate and inhibit the side reaction between the substrate and the air, so that the electrode material maintains a high lithium replenishment efficiency. In addition, when the first inorganic lithium compound layer has the above composition, it is applied to a secondary battery, which is beneficial to form a uniform, dense and stable protective film on the surface of the electrode plate, thereby further improving the cycle stability of the secondary battery.

[0104] The composition of the first inorganic lithium compound layer can be determined by methods and equipment known in the art. As an example, the content of each element (such as O, N, P, S, F, C, Li and other elements) in the first inorganic lithium compound layer can be determined by X-ray photoelectron spectroscopy (XPS). According to the ratio of the content of each element and the chemical formula of the inorganic lithium compound, the components included in the first inorganic lithium compound layer and the content of each component can be determined. As another example, when sampling from a battery, the composition of the first inorganic lithium compound layer can also be determined by the following steps: disassembling the battery and taking out the electrode plate; soaking the electrode plate with an organic solvent to remove the electrolyte and additives in the electrode plate; after drying the electrode plate, randomly selecting an area for cross-section, and determining the position of the first inorganic lithium compound layer by scanning electron microscopy (SEM) at a magnification of more than 3000 times (for example, 3000 times, 10000 times, or 100000 times, etc.), and the first inorganic lithium compound layer distributed in the field of view is divided into the following sections. The position of the inorganic lithium compound layer is marked as the target area; then, an area of ​​a certain size is selected at a magnification of 500 times or more (for example, 500 times or 1000 times) (for example, when the magnification is 500 times, a 100 μm*100 μm area can be selected; when the magnification is 1000 times, a 10 μm*10 μm area can be selected) for EDS surface scanning for 2 minutes to obtain the element types and contents of the target area, and determine the composition of the first inorganic lithium compound layer according to the content ratio of each element and the chemical formula of the inorganic lithium compound.

[0105] In some embodiments, the thickness of the first inorganic lithium compound layer can be 2nm-5000nm, for example, 2nm, 5nm, 10nm, 50nm, 100nm, 300nm, 500nm, 1000nm, 2000nm, 3000nm, 4000nm, 5000nm, or a range consisting of any two of the above values. For example, the thickness of the first inorganic lithium compound layer can be 2nm-5000nm, 2nm-4000nm, 2nm-3000nm, 2nm-2000nm, 2nm-1000nm, 5nm-5000nm, 5nm-3000nm, 5nm-1000nm, 5nm-500nm, 5nm-300nm, 10nm-4000nm, 10nm-2000nm, 10nm-500nm, 50nm-5000nm, 50nm-3000nm, 50nm-1000nm, 50nm-500nm and the like.

[0106] Optionally, in some embodiments, the thickness of the first inorganic lithium compound layer may also be 20 nm-1000 nm, for example, 20 nm, 50 nm, 100 nm, 300 nm, 500 nm, 800 nm, 1000 nm, or a range consisting of any two of the above values. For example, the thickness of the first inorganic lithium compound layer can be 20nm-1000nm, 20nm-800nm, 20nm-500nm, 20nm-300nm, 20nm-100nm, 20nm-50nm, 50nm-1000nm, 50nm-800nm, 50nm-500nm, 50nm-300nm, 50nm-100nm, 100nm-1000nm, 100nm-800nm, 100nm-500nm, 100nm-300nm, 300nm-1000nm, 500nm-1000nm and the like.

[0107] It is not intended to be limited by any theory or explanation. The thickness of the first inorganic lithium compound layer is within the above-mentioned suitable range. On the one hand, it can effectively isolate the substrate from direct contact with the air, thereby improving the stability of the chemical properties of the substrate, and on the other hand, it can keep the electrode material at a high substrate content. Thus, the lithium replenishment efficiency of the electrode material can be significantly improved. In addition, the thickness of the first inorganic lithium compound layer is within the above-mentioned suitable range, which also helps to form a dense, uniform and stable protective film on the surface of the electrode pole piece, thereby further improving the environmental stability of the electrode. Thus, the capacity decay of the secondary battery can be suppressed and the cycle life of the secondary battery can be extended.

[0108] The thickness of the first inorganic lithiation layer has a well-known meaning in the art and can be measured using equipment and methods known in the art. For example, the thickness of the first inorganic lithiation layer on the surface of the lithiated material can be observed using a transmission electron microscope (TEM) or a scanning electron microscope (SEM).

[0109] In some embodiments, the volume distribution particle size Dv50 of the electrode material can be 0.6μm-60μm, for example, 0.6μm, 1μm, 5μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, or a range of any two of the above values. For example, the volume distribution particle size Dv50 of the electrode material can be 0.6μm-60μm, 0.6μm-30μm, 0.6μm-10μm, 0.6μm-5μm, 1μm-50μm, 1μm-40μm, 1μm-20μm, 5μm-55μm, 5μm-45μm, 5μm-35μm, 5μm-25μm, 5μm-15μm, and the like.

[0110] Optionally, in some embodiments, the volume distribution particle size Dv50 of the electrode material can also be 5μm-15μm, for example, it can be 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, or a range consisting of any two of the above values.

[0111] Without intending to be limited by any theory or explanation, when the volume distribution particle size Dv50 of the electrode material is within the above-mentioned suitable range, the electrode material can not only have a suitable lithium ion transmission path, but also have good electrolyte infiltration performance. Therefore, it is beneficial for active lithium ions to escape from the electrode material, improve the lithium replenishment efficiency of the electrode material, and thus help to further delay the capacity decay of the secondary battery and extend the cycle life of the secondary battery.

[0112] The volume distribution particle size Dv50 of the electrode material has a well-known meaning in the art, which can represent the particle size corresponding to the cumulative particle size distribution percentage reaching 50% in the volume-based particle size distribution of the electrode material. The volume distribution particle size Dv50 can be measured using equipment and methods known in the art. For example, it can be measured with reference to GB / T 19077-2016 particle size distribution laser diffraction method using a laser particle size analyzer (e.g., Malvern Master Size 3000).

[0113] In some embodiments, the electrode material is a positive electrode material. The positive electrode material may refer to an electrode material whose substrate includes a pre-lithiated positive electrode active material.

[0114] The lithium supplement content of the positive electrode material may be 1%-30%, for example, 1%, 5%, 10%, 15%, 20%, 25%, 30%, or a range consisting of any two of the above values.

[0115] Optionally, in some embodiments, the lithium supplement content of the positive electrode material can also be 5%-20%, for example, it can be 5%, 8%, 10%, 12%, 15%, 18%, 20%, or a range consisting of any two of the above values.

[0116] The lithium content of the positive electrode material can be calculated by (C1-C 10 ) / C 10 ×100%, where C1 is the actual gram capacity of the positive electrode material in mAh / g, C 10 It is the theoretical gram capacity of the positive electrode active material, in mAh / g.

[0117] The actual gram capacity C1 of the positive electrode material has a well-known meaning in the art, and may represent the ratio of the capacitance that the positive electrode material can actually release to the mass of the positive electrode material.

[0118] Theoretical gram capacity C of positive electrode active material 10 It has a well-known meaning in the art, and can represent the ratio of the theoretically released capacity of the positive electrode active material to the mass of the positive electrode active material. The positive electrode active material corresponds to the positive electrode material. For example, when the positive electrode active material is lithium iron phosphate, the positive electrode material includes pre-lithiated lithium iron phosphate and a first inorganic lithium compound layer coated on at least a portion of the surface of the pre-lithiated lithium iron phosphate; when the positive electrode active material is a nickel-cobalt-manganese ternary material, the positive electrode material includes a pre-lithiated nickel-cobalt-manganese ternary material and a first inorganic lithium compound layer coated on at least a portion of the surface of the pre-lithiated nickel-cobalt-manganese ternary material.

[0119] Without intending to be limited by any theory or explanation, when the positive electrode material has a suitable lithium supplement content, it can be applied to the positive electrode of the secondary battery to release a suitable amount of active lithium ions to supplement the active lithium ions lost during the first cycle of charge and discharge, and reduce the risk of lithium precipitation due to excessive lithium supplement. Therefore, the positive electrode material applied to the secondary battery can make the secondary battery have both good cycle performance and high reliability.

[0120] The lithium supplement content of the positive electrode material can be determined by methods and equipment known in the art. The actual gram capacity C1 of the positive electrode material can be determined by equipment and methods known in the art. Those skilled in the art can determine the theoretical gram capacity C1 of the positive electrode active material according to the type and chemical composition of the positive electrode active material. 10 .

[0121] As an example, C1 can be determined by testing the capacity of lithium that can be extracted from the positive electrode material. Specifically, the positive electrode material can be mixed with an appropriate amount of a conductive agent and a binder in a certain proportion to prepare a single-sided coated positive electrode plate; the lithium half-cell can be directly charged to the rated voltage using a button type to test the removable lithium capacity CmAh of the positive electrode plate containing m1 g of positive electrode material. The actual gram capacity C1 of the positive electrode material can be calculated by the formula C1=C / m1. The above-mentioned rated voltage has a well-known meaning in the art, which can represent the rated voltage corresponding to the substrate of the positive electrode material. For example, when the substrate is pre-lithiated lithium iron phosphate, the rated voltage can be 3.8V; when the substrate is a pre-lithiated nickel-cobalt-manganese ternary material, the rated voltage can be 4.2V-4.4V.

[0122] In some embodiments, the electrode material is a negative electrode material. The negative electrode material may refer to an electrode material whose substrate includes a pre-lithiated negative electrode active material.

[0123] The lithium supplement content of the negative electrode material can be 1%-100%, for example, it can be 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 80%, 100% or a range consisting of any two of the above values.

[0124] Optionally, in some embodiments, the lithium supplement content of the negative electrode material can also be 30%-50%, for example, it can be 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%, or a range consisting of any two of the above values.

[0125] The lithium content of the negative electrode material can be measured by (C 20 -C2) / C 20 ×100%, where C2 is the actual gram capacity of the negative electrode material in mAh / g, and C 20 It is the theoretical gram capacity of the negative electrode active material, in mAh / g.

[0126] The actual gram capacity C2 of the negative electrode material has a well-known meaning in the art, and may represent the ratio of the capacitance that the negative electrode material can actually release to the mass of the negative electrode material.

[0127] Theoretical gram capacity C of negative electrode active material 20 It has a well-known meaning in the art, and can represent the ratio of the theoretically released capacity of the negative electrode active material to the mass of the negative electrode active material. The negative electrode active material corresponds to the negative electrode material. For example, when the negative electrode active material is graphite, the negative electrode material includes pre-lithiated graphite and a first inorganic lithium compound layer coated on at least a portion of the surface of the pre-lithiated graphite; when the negative electrode active material is lithium titanate, the negative electrode material includes pre-lithiated lithium titanate and a first inorganic lithium compound layer coated on at least a portion of the surface of the pre-lithiated lithium titanate.

[0128] Without intending to be limited by any theory or explanation, when the negative electrode material has a suitable amount of lithium supplement, it can release a suitable amount of active lithium ions when applied to the negative electrode of a secondary battery to supplement the active lithium ions lost during the first cycle of charge and discharge, and reduce the risk of lithium precipitation due to excessive lithium supplement. Therefore, the negative electrode material applied to the secondary battery can enable the secondary battery to have both good cycle performance and high reliability.

[0129] The lithium supplement content of the negative electrode material can be determined by methods and equipment known in the art. Among them, the actual gram capacity C2 of the negative electrode material can be determined by equipment and methods known in the art. Those skilled in the art can determine the theoretical gram capacity C2 of the negative electrode active material according to the type and chemical composition of the negative electrode active material. 20 .

[0130] As an example, C2 can be determined by testing the embeddable lithium capacity of the negative electrode material. Specifically, the negative electrode material can be mixed with an appropriate amount of a conductive agent and a binder in a certain proportion to prepare a single-sided coated negative electrode plate; a button-type lithium half-cell is used to discharge to a preset voltage to test the embeddable lithium capacity C'mAh of the negative electrode plate containing m2 g of negative electrode material; the actual gram capacity C2 of the negative electrode material can be calculated by the formula C2=C' / m2. The above preset voltage can represent the discharge voltage required for the negative electrode active material corresponding to the substrate of the negative electrode material to reach a fully embedded lithium state. As an example, the preset voltage of graphite, soft carbon, hard carbon, mesophase carbon microspheres, silicon-based materials, and tin-based materials can be 0.01V, and the preset voltage of lithium titanate can be 2.0V.

[0131] Preparation method of electrode material

[0132] In a second aspect, an embodiment of the present application provides a method for preparing an electrode material, comprising the following steps S110-S130.

[0133] S110, mixing lithium metal with a complexing agent solution to allow the lithium metal to react with the complexing agent to obtain a liquid-phase lithiating agent.

[0134] In step S110, the lithium metal can be in any form, for example, it can include at least one of a lithium block, a lithium foil, and a lithium powder, which is not limited here. The coordination reagent may include a reagent known in the art that can react with lithium metal, and those skilled in the art may select it as needed, which is not limited here. In some embodiments, mixing the lithium metal with the coordination reagent solution may include mixing the lithium metal with the coordination reagent and stirring it evenly, and the stirring temperature and time are not specifically limited, and those skilled in the art may adjust it as needed. As an example, the stirring temperature may be 0°C-60°C, optionally 10°C-40°C, and the stirring time may be 0.1h-12h, optionally 1h-6h.

[0135] S120, contacting a liquid-phase lithiating agent with an electrode active material so that the liquid-phase lithiating agent pre-lithiates the electrode active material to obtain a pre-lithiated electrode active material.

[0136] In step S120, the contact between the liquid-phase lithiating agent and the electrode active material can be achieved in a variety of ways, which are not limited in this application. In some embodiments, the electrode active material can be impregnated with a liquid-phase lithiating agent so that the liquid-phase lithiating agent pre-lithiates the electrode active material. In step S120, the temperature and time for the liquid-phase lithiating agent to pre-lithiate the electrode active material are not specifically limited, and those skilled in the art can adjust them as needed. As an example, the pre-lithiation temperature can be 0°C-80°C, optionally 10°C-50°C, and the pre-lithiation time can be 1min-6h, optionally 5min-30min.

[0137] S130, contacting the pre-lithiation electrode active material with a reactant to form a first inorganic lithiation layer on at least a portion of the surface of the pre-lithiation electrode active material to obtain an electrode material.

[0138] In step S130, the reactant may be a substance that can react with a liquid-phase lithium agent or a pre-lithiation electrode active material to generate at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide, and lithium phosphide, and those skilled in the art may select it as needed. After the pre-lithiation electrode active material contacts the reactant, the reactant may react with the residual liquid-phase lithium agent on at least a portion of the surface of the pre-lithiation electrode active material to form a first inorganic lithium compound layer on at least a portion of the surface of the pre-lithiation electrode active material; and / or, the reactant may react with the material on the surface of the pre-lithiation electrode active material to form a first inorganic lithium compound layer on at least a portion of the surface of the pre-lithiation electrode active material. The reaction temperature and reaction time of step S130 are not specifically limited, and those skilled in the art may adjust them as needed. As an example, the reaction temperature of step S130 may be 0°C-80°C, optionally 10°C-50°C, and the reaction time may be 1min-60min, optionally 2min-10min.

[0139] The electrode material prepared according to the above steps S110 to S130 includes a substrate and a first inorganic lithium compound layer, wherein the first inorganic lithium compound layer is coated on at least a portion of the surface of the substrate. The substrate includes a pre-lithiation electrode active material, and the first inorganic lithium compound layer includes at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide.

[0140] The method provided in the embodiment of the present application is simple to operate, has mild conditions and is easy to control. The substrate of the prepared electrode material has been pre-embedded with some active lithium ions. During the first charge or discharge process, the electrode material can release active lithium ions, thereby compensating for the loss of active lithium ions in the battery formation process. In addition, the electrode material prepared by the method of the embodiment of the present application can also form a dense, uniform and stable protective film on the surface of the electrode pole piece through the first inorganic lithium compound layer. The protective film can play a similar role to the SEI film, thereby improving the environmental stability of the electrode, reducing the irreversible loss of active lithium ions, and slowing down the capacity decay of the secondary battery. Therefore, the electrode material prepared in the embodiment of the present application is applied to secondary batteries, which can improve the energy density of the secondary batteries and extend the cycle life of the secondary batteries.

[0141] In some embodiments, the preparation method may further include: providing a complexing reagent solution, including uniformly mixing the complexing reagent and the solvent to obtain the complexing reagent solution.

[0142] In some embodiments, the coordination agent may include at least one of naphthalene and its derivatives, biphenyl and its derivatives, phenanthrene and its derivatives, pyrene and its derivatives, fluorene and its derivatives, indene and its derivatives, and aromatic hydrocarbon derivatives containing heteroatom functional groups. Alternatively, in some embodiments, the coordination agent may include at least one of 2-methylnaphthalene, 1-naphthonitrile, 2,2-dimethylbiphenyl, 2-ethylindene, 1-methyl-3-ethylpyrene, benzophenone, pyridine, and quinoline.

[0143] In some embodiments, the solvent may include at least one of alkanes and their derivatives, aromatic hydrocarbons and their derivatives, ether compounds and their derivatives, furan compounds and their derivatives, pyran compounds and their derivatives, esters and their derivatives. Alternatively, the solvent may include at least one of benzene, toluene, xylene, ethylbenzene, ethylene glycol dimethyl ether, 2-methyltetrahydrofuran, pyran or fluoroethylene carbonate.

[0144] Without intending to be limited by any theory or explanation, the complexing agent selected from the above types can react with lithium metal to generate a liquid-phase lithiating agent with a lower redox potential. As a result, the liquid-phase lithiating agent is more likely to pre-lithiate the electrode active material and embed active lithium ions in the electrode active material, which is beneficial to improve the lithium replenishment efficiency of the electrode material. Furthermore, the use of the above-mentioned types of solvents to dissolve the complexing agent is beneficial to further adjust the redox potential of the liquid-phase lithiating agent within a suitable range, thereby further improving the efficiency of pre-lithiation and thus improving the lithium replenishment efficiency of the electrode material.

[0145] In some embodiments, the redox potential of the liquid-phase lithiating agent may be 0.05 V to 1.5 V, for example, 0.05 V, 0.10 V, 0.20 V, 0.30 V, 0.40 V, 0.50 V, 0.60 V, 0.70 V, 0.80 V, 0.90 V, 1.0 V, 1.5 V, or a range consisting of any two of the above values.

[0146] Optionally, in some embodiments, the redox potential of the liquid-phase lithiating agent may also be 0.1V-0.5V, 0.1V-0.4V, 0.1V-0.3V, 0.1V-0.2V, 0.2V-0.5V, 0.2V-0.4V, 0.2V-0.3V, 0.3V-0.5V, 0.3V-0.4V, 0.4V-0.5V and the like.

[0147] The redox potential of the liquid-phase lithiating agent is within the above-mentioned suitable range, which can further improve the efficiency of pre-lithiation, thereby improving the lithium replenishment efficiency of the electrode material.

[0148] The redox potential of the liquid-phase lithiating agent has a well-known meaning in the art and can be measured by equipment and methods known in the art, for example, cyclic voltammetry can be used. Specifically, Pt can be used as a working electrode, Li can be used as a reference electrode and a counter electrode, and an electrolytic cell can be formed with the liquid-phase lithiating agent. The open circuit voltage is scanned to 0.01V, and then cycled three times at 0.01V-1.5V to obtain the redox peak of the liquid-phase lithiating agent and measure the redox potential of the liquid-phase lithiating agent.

[0149] In some embodiments, the molar ratio of lithium metal to the complexing agent can be (0.5:1)-(10:1), for example, 0.5:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, or a range consisting of any two of the above ratios. Alternatively, the molar ratio of lithium metal to the complexing agent can be (1:1)-(4:1), (1:1)-(3.5:1), (1:1)-(3:1), (1:1)-(2.5:1), (1:1)-(2:1), (1:1)-(1.5:1), and the like.

[0150] In some embodiments, the content of lithium in the liquid-phase lithiation agent can be 0.01mol / L-10mol / L, for example, 0.01mol / L, 0.1mol / L, 0.5mol / L, 1mol / L, 2mol / L, 5mol / L, 8mol / L, 10mol / L, or a range consisting of any two of the above values. Optionally, the content of lithium in the liquid-phase lithiation agent can also be 0.01mol / L-5mol / L, 0.01mol / L-4mol / L, 0.01mol / L-3mol / L, 0.01mol / L-2mol / L, 0.01mol / L-1mol / L, 0.5mol / L-5mol / L, 0.5mol / L-3mol / L, 0.5mol / L-1mol / L, 1mol / L-5mol / L, 2mol / L-4mol / L, etc.

[0151] Without intending to be limited by any theory or explanation, when the molar ratio of lithium metal to the complexing agent is within the above range, it not only helps to improve the reaction efficiency of lithium metal and the complexing agent, but also helps to adjust the content of lithium element in the liquid-phase lithiating agent within a suitable range. In the liquid-phase lithiating agent, the content of lithium element is within a suitable range, which can improve the pre-lithiation efficiency of the liquid-phase lithiating agent for the electrode active material.

[0152] In some embodiments, the molar ratio of lithium element to electrode active material in the liquid-phase lithiating agent may be (0.05:1)-(10:1), and may be (0.1:1)-(5:1).

[0153] Without intending to be bound by any theory or explanation, the molar ratio of lithium element in the liquid phase lithiating agent to the electrode active material is within the above-mentioned suitable range, and an appropriate amount of active lithium ions can be embedded in the electrode active material. Therefore, during the battery formation process, the electrode material can release an appropriate amount of active lithium ions to supplement the active lithium ions lost during the first cycle of charge and discharge cycles.

[0154] In some embodiments, the volume distribution particle size Dv50 of the electrode active material can be 0.5μm-40μm, 0.5μm-30μm, 0.5μm-20μm, 0.5μm-15μm, 2.5μm-35μm, 2.5μm-25μm, 2.5μm-15μm, 2.5μm-10μm, 4.5μm-37.5μm, 4.5μm-27.5μm, 4.5μm-17.5μm, 4.5μm-15μm, 4.5μm-12.5μm, and the like.

[0155] Without intending to be limited by any theory or explanation, when the volume distribution particle size Dv50 of the electrode active material is within the above-mentioned suitable range, not only can the prepared electrode material have a suitable lithium ion transmission path, but also the electrode material can have good electrolyte infiltration performance. Therefore, it is beneficial for the active lithium ions to escape from the electrode material, improve the lithium replenishment efficiency of the electrode material, and thus help to further delay the capacity decay of the secondary battery and extend the cycle life of the secondary battery.

[0156] The volume distribution particle size Dv50 of the electrode active material can be determined by referring to the test method for the volume distribution particle size Dv50 of the electrode material.

[0157] In some embodiments, the reactants may include at least one of air, water, oxygen, carbon dioxide, nitrogen, nitric oxide, nitrogen dioxide, nitrogen pentoxide, hydrogen fluoride, fluorine, sulfur, hydrogen sulfide, sulfur dioxide, sulfur trioxide, or red phosphorus. Alternatively, the reactants may include at least one of carbon dioxide, fluorine, nitrogen, sulfur dioxide, or red phosphorus.

[0158] The reactants selected from the above types can react with the liquid phase lithium agent and / or the pre-lithiation electrode active material. By selecting suitable reactants, the composition of the first inorganic lithium compound layer can be regulated. The first inorganic lithium compound layer has a suitable composition, which is beneficial to suppress the side reaction between the substrate and the air, so that the electrode material maintains a high lithium replenishment efficiency, and is beneficial to regulate the composition of the protective film on the electrode surface, thereby improving the stability of the electrode environment. As a result, it helps to further improve the cycle stability of the secondary battery and extend the cycle life of the secondary battery.

[0159] The contact between the above-mentioned reactants and the pre-lithiation electrode active material can be achieved in a variety of ways, and the present application does not limit this. In some embodiments, when the reactant is a gas, the reactant can be directly introduced into the slurry obtained in step S120. In some embodiments, when the reactant is a solid, the reactant can be dissolved in an organic solvent to obtain a reactant solution, and then the reactant solution is mixed evenly with the slurry obtained in step S120. This allows the reactant to be in contact with the pre-lithiation electrode active material more evenly and fully, which is conducive to the smooth progress of the reaction. The above-mentioned organic solvent may include at least one of alkanes, aromatic hydrocarbons, ethers, esters and their halides, for example, it may include at least one of benzene, dimethyl carbonate, ethylene carbonate, fluoroethylene carbonate, tetrahydrofuran, dimethyl ether, hydrofluoroether, and 1,1,1,3,3,3-hexafluoroisopropyl methyl ether. In the reactant solution, the mass fraction of the reactant may be 0.1%-20%.

[0160] In some embodiments, the preparation method may further include: drying the electrode material.

[0161] The present application does not limit the dry atmosphere, and the dry atmosphere may include any atmosphere that does not react with the electrode material. In some embodiments, the dry atmosphere may include nitrogen, argon, dry air, or a combination thereof. Alternatively, in some embodiments, the dry atmosphere may include nitrogen, argon, or a combination thereof. The present application does not limit the drying temperature and time, and those skilled in the art may adjust as needed. In some embodiments, the drying temperature may be 0°C-200°C, optionally 20°C-120°C, and the drying time may be 5min-6h. Thus, the stability of the chemical properties of the electrode material can be improved.

[0162] Electrode

[0163] In a third aspect, an embodiment of the present application provides an electrode plate, which includes a current collector and an electrode film layer located on at least one side of the current collector, the electrode film layer includes an electrode material; the electrode material includes a substrate and a first inorganic lithium compound layer, the first inorganic lithium compound layer is coated on at least a portion of the surface of the substrate, the substrate includes a pre-lithiation electrode active material, and the first inorganic lithium compound layer includes at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide.

[0164] The electrode plate of the third aspect includes an electrode material, and the substrate of the electrode material has been pre-embedded with some active lithium ions. During the first charge or discharge process, the electrode material can release active lithium ions, thereby compensating for the loss of active lithium ions during the battery formation process. In addition, the electrode material can also form a dense, uniform and stable protective film on the surface of the electrode plate through the first inorganic lithium compound layer. The protective film can play a similar role to the SEI film, thereby improving the environmental stability of the electrode, reducing the irreversible loss of active lithium ions, and slowing down the capacity decay of the secondary battery. Therefore, the electrode plate of the embodiment of the present application is applied to the secondary battery, which can improve the energy density of the secondary battery and extend the cycle life of the secondary battery.

[0165] It should be noted that in the embodiments of the present application, the structure of the electrode material in the electrode film layer can be determined by equipment and methods known in the art. As an example, it can be tested by the following method: obtain the electrode pole piece (when sampling from the battery, the battery can be directly disassembled, the electrode pole piece can be taken out and dried); randomly select an area, perform argon ion cross-section polishing, and take a transmission electron microscope image (TEM image) of the electrode film layer, with a magnification of 3000 times or more (for example, it can be 3000 times, 30000 times, 100000 times, or 500000 times, etc.); process the TEM image, adjust the appropriate contrast, and the substrate of the electrode material and the first inorganic lithium compound layer can be observed. The thickness of the first inorganic lithium compound layer can also be determined by the TEM image.

[0166] It should be noted that in the embodiments of the present application, the volume distribution particle size Dv50 of the electrode material in the electrode film layer can be determined by equipment and methods known in the art. As an example, it can be tested by the following method: obtain the electrode plate (when sampling from the battery, the battery can be directly disassembled, the electrode plate can be taken out and dried); randomly select an area, perform argon ion cross-section polishing, and take an electron microscope image (SEM image) of the electrode film layer with a magnification of 500 times or more (for example, it can be 500 times, 1000 times, or 5000 times, etc.); process the SEM image, adjust the appropriate contrast, and the electrode material can be observed. The particle size of the electrode material in the statistical field of view can determine the volume distribution particle size Dv50 of the electrode material.

[0167] In some embodiments, the electrode plate may further include a second inorganic lithium compound layer attached to at least a portion of the surface of the electrode film layer. The second inorganic lithium compound layer includes at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide, or lithium phosphide.

[0168] In this embodiment, the second inorganic lithium compound layer may be a separable layered structure formed separately on at least a portion of the surface of the electrode film layer.

[0169] In some embodiments, the composition of the second inorganic lithiation layer may be the same as that of the first inorganic lithiation layer.

[0170] Without intending to be limited by any theory or explanation, when the electrode plate further includes a second inorganic lithium compound layer attached to at least a portion of the surface of the electrode film layer, it is beneficial to further improve the stability of the electrode environment during the charge and discharge cycle, thereby improving the cycle stability of the secondary battery.

[0171] In some embodiments, based on the total mass of the first inorganic lithiation layer, the first inorganic lithiation layer may include 0-80% lithium oxide, 0-100% lithium carbonate, 0-100% lithium fluoride, 0-45% lithium phosphide, 0-90% lithium nitride, and 0-55% lithium sulfide.

[0172] Optionally, in some embodiments, based on the total mass of the first inorganic lithium compound layer, the first inorganic lithium compound layer may include 0-100% lithium fluoride, 0-80% lithium oxide, 0-50% lithium nitride, 0-100% lithium carbonate, and 0-55% lithium sulfide.

[0173] In some embodiments, the first inorganic lithiation layer may include at least two of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, or lithium sulfide.

[0174] Optionally, in some embodiments, based on the total mass of the first inorganic lithium compound layer, the first inorganic lithium compound layer may include 18%-90% lithium nitride, 0-28% lithium fluoride, 0-80% lithium oxide, 0-2% lithium carbonate, and 0-20% lithium sulfide.

[0175] More optionally, in some embodiments, based on the total mass of the first inorganic lithiation layer, the first inorganic lithiation layer may include 70%-90% lithium nitride, 0-30% lithium oxide, and 0-10% lithium sulfide.

[0176] When the first inorganic lithium compound layer has the above composition, it is beneficial to protect the substrate and inhibit the side reaction between the substrate and the air, so that the electrode material maintains a high lithium replenishment efficiency. In addition, when the first inorganic lithium compound layer has the above composition, it is also beneficial to form a uniform, dense and stable protective film on the surface of the electrode plate, thereby further improving the cycle stability of the secondary battery.

[0177] In some embodiments, based on the total mass of the second inorganic lithiation layer, the second inorganic lithiation layer may include 0-80% lithium oxide, 0-100% lithium carbonate, 0-100% lithium fluoride, 0-45% lithium phosphide, 0-90% lithium nitride, and 0-55% lithium sulfide.

[0178] Optionally, in some embodiments, based on the total mass of the second inorganic lithium compound layer, the second inorganic lithium compound layer may include 0-100% lithium fluoride, 0-80% lithium oxide, 0-50% lithium nitride, 0-100% lithium carbonate, and 0-55% lithium sulfide.

[0179] In some embodiments, the second inorganic lithiation layer may include at least two of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, or lithium sulfide.

[0180] Optionally, in some embodiments, based on the total mass of the second inorganic lithium compound layer, the second inorganic lithium compound layer may include 18%-90% lithium nitride, 0-28% lithium fluoride, 0-80% lithium oxide, 0-2% lithium carbonate, and 0-20% lithium sulfide.

[0181] More optionally, in some embodiments, based on the total mass of the second inorganic lithiation layer, the second inorganic lithiation layer may include 70%-90% lithium nitride, 0-30% lithium oxide, and 0-10% lithium sulfide.

[0182] The electrode plate of the embodiment of the present application can be a positive electrode plate or a negative electrode plate. When the electrode plate is a positive electrode plate, the electrode material is a positive electrode material. When the electrode plate is a negative electrode plate, the electrode material is a negative electrode material.

[0183] In some embodiments, the electrode plate is a positive electrode plate, and the electrode material is a positive electrode material. The electrode film layer may also include other positive electrode active materials.

[0184] Optionally, in some embodiments, based on the total mass of the positive electrode film layer, the mass percentage of the positive electrode material is 15wt%-98wt%, optionally 50wt%-98wt%. The mass percentage of other positive electrode active materials is less than or equal to 95wt%,

[0185] In some embodiments, the electrode plate is a negative electrode plate, and the electrode material is a negative electrode material. The electrode film layer may also include other negative electrode active materials.

[0186] Optionally, in some embodiments, based on the total mass of the negative electrode film layer, the mass percentage of the negative electrode material may be 10wt%-98wt%, optionally 50wt-98wt%. The mass percentage of other negative electrode active materials may be less than or equal to 95wt%.

[0187] When the mass percentage of the electrode material in the electrode film layer is within the above-mentioned appropriate range, an appropriate amount of active lithium ions can be released to supplement the active lithium ions lost during the first cycle of charge and discharge, and reduce the risk of lithium precipitation due to excessive lithium supplementation. This allows the secondary battery to have both good cycle performance and high reliability.

[0188] The above-mentioned other positive electrode active materials may include positive electrode active materials of the same type as the pre-lithiation positive electrode active materials, or may include positive electrode active materials of different types from the pre-lithiation positive electrode active materials. Other negative electrode active materials may include negative electrode active materials of the same type as the pre-lithiation negative electrode active materials, or may include negative electrode active materials of different types from the pre-lithiation negative electrode active materials. The embodiments of the electrode active materials have been described and explained in detail above, and will not be repeated here.

[0189] In some embodiments, the electrode plate is a positive electrode plate, and the lithium supplement content of the positive electrode plate may be 1%-30%.

[0190] The lithium content of the positive electrode can be calculated by (C3-C 30 ) / C 30 ×100%, where C3 is the actual gram capacity of the positive electrode active material contained in the positive electrode sheet, in mAh / g; C 30 The theoretical gram capacity of the non-pre-lithiated positive electrode active material, in units of mAh / g. The positive electrode active material may include the positive electrode material and other positive electrode active materials contained in the positive electrode sheet.

[0191] The lithium supplement content of the positive electrode sheet can be determined by methods and equipment known in the art. Among them, C3 can be determined by referring to the test method of the actual gram capacity C1 of the positive electrode material, which is not described in detail here. The theoretical gram capacity C of the non-pre-lithiated positive electrode active material 30 It can be determined according to the type, chemical composition and content of the positive electrode active material. As an example, the positive electrode active material includes m3 g of the first positive electrode active material and m4 g of the positive electrode material, and the substrate of the positive electrode material is the pre-lithiated second positive electrode active material. The theoretical gram capacity C of the non-pre-lithiated positive electrode active material is 30 =[m3 / (m3+m4)]×C 31 +[m4 / (m3+m4)]×C 32 , where C 31 is the theoretical gram capacity of the first positive electrode active material, in mAh / g; C 32 is the theoretical gram capacity of the second positive electrode active material, in mAh / g.

[0192] In some embodiments, the electrode plate is a negative electrode plate, and the lithium supplement content of the negative electrode plate may be 1%-50%. Optionally, the lithium supplement content of the negative electrode plate may be 30%-50%.

[0193] The lithium content of the negative electrode can be measured by (C 40 -C4) / C 40 ×100%, where C4 is the actual gram capacity of the negative electrode active material contained in the negative electrode sheet, in mAh / g, and C 40 The theoretical gram capacity of the non-pre-lithiated negative electrode active material, in units of mAh / g. The negative electrode active material may include the negative electrode material and other negative electrode active materials contained in the negative electrode sheet.

[0194] The lithium supplement content of the negative electrode sheet can be determined by methods and equipment known in the art. Among them, C4 can be determined by referring to the test method of the actual gram capacity C2 of the negative electrode material, which is not described here. The theoretical capacity C of the negative electrode active material without pre-lithiation 40 It can be determined according to the type, chemical composition and content of the negative electrode active material. 40 The determination process can be compared with C 30 Similar, I will not elaborate on it here.

[0195] When the lithium supplement content of the electrode plate meets the given range, when used in a secondary battery, it can release an appropriate amount of active lithium ions to replenish the active lithium ions lost during the first week of charge and discharge cycles, and reduce the risk of lithium precipitation due to excessive lithium supplementation. Therefore, the application of the electrode plate in a secondary battery can enable the secondary battery to have both good cycle performance and high reliability.

[0196] Method for preparing electrode sheet

[0197] In a fourth aspect, an embodiment of the present application provides a method for preparing an electrode plate, which may include method A or method B.

[0198] Method A may include the following steps S210 to S240.

[0199] S210, mixing lithium metal with a complexing agent solution so that the lithium metal reacts with the complexing agent to obtain a liquid-phase lithiating agent.

[0200] S220, contacting a liquid-phase lithiating agent with an electrode active material so that the liquid-phase lithiating agent pre-lithiates the electrode active material to obtain a pre-lithiated electrode active material.

[0201] S230, contacting a pre-lithiation electrode active material with a reactant to form a first inorganic lithiation layer on at least a portion of the surface of the pre-lithiation electrode active material to obtain an electrode material; wherein the electrode material comprises: a substrate, the substrate comprising the pre-lithiation electrode active material; and a first inorganic lithiation layer coated on at least a portion of the surface of the substrate, the first inorganic lithiation layer comprising at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide.

[0202] S240, preparing an electrode plate including an electrode material.

[0203] The implementation of steps S210 to S230 may be the same as that of steps S110 to S130. The implementation of steps S110 to S130 has been described and illustrated in detail above, and will not be repeated here. Step S240 may be implemented by a method known in the art, and is not limited here.

[0204] The electrode plate prepared according to method A includes an electrode material, and the substrate of the electrode material has been pre-embedded with some active lithium ions. During the first charge or discharge process, the electrode material can release active lithium ions, thereby compensating for the loss of active lithium ions in the battery formation process. In addition, the electrode material can also form a dense, uniform and stable protective film on the surface of the electrode plate through the first inorganic lithium compound layer. The protective film can play a similar role to the SEI film, thereby improving the environmental stability of the electrode, reducing the irreversible loss of active lithium ions, and slowing down the capacity decay of the secondary battery. Therefore, the electrode plate prepared in the embodiment of the present application is applied to a secondary battery, which can improve the energy density of the secondary battery and extend the cycle life of the secondary battery.

[0205] In some embodiments, method A may further include: providing a complexing reagent solution, including uniformly mixing the complexing reagent and the solvent to obtain the complexing reagent solution.

[0206] In some embodiments, the coordination agent may include at least one of naphthalene and its derivatives, biphenyl and its derivatives, phenanthrene and its derivatives, pyrene and its derivatives, fluorene and its derivatives, indene and its derivatives, and aromatic hydrocarbon derivatives containing heteroatom functional groups. Alternatively, in some embodiments, the coordination agent may include at least one of 2-methylnaphthalene, 1-naphthonitrile, 2,2-dimethylbiphenyl, 2-ethylindene, 1-methyl-3-ethylpyrene, benzophenone, pyridine, and quinoline.

[0207] In some embodiments, the solvent may include at least one of alkanes and their derivatives, aromatic hydrocarbons and their derivatives, ether compounds and their derivatives, furan compounds and their derivatives, pyran compounds and their derivatives, esters and their derivatives. Alternatively, the solvent may include at least one of benzene, toluene, xylene, ethylbenzene, ethylene glycol dimethyl ether, 2-methyltetrahydrofuran, pyran or fluoroethylene carbonate.

[0208] Without intending to be limited by any theory or explanation, the complexing agent selected from the above types can react with lithium metal to generate a liquid-phase lithiating agent with a lower redox potential. As a result, the liquid-phase lithiating agent is more likely to pre-lithiate the electrode active material and embed active lithium ions in the electrode active material, which is beneficial to improve the lithium replenishment efficiency of the electrode material. Furthermore, the use of the above-mentioned types of solvents to dissolve the complexing agent is beneficial to further adjust the redox potential of the liquid-phase lithiating agent within a suitable range, thereby further improving the efficiency of pre-lithiation and further improving the lithium replenishment efficiency of the electrode plate.

[0209] In some embodiments, in method A, the redox potential of the liquid-phase lithiating agent can be 0.05V-1.5V, for example, 0.05V, 0.10V, 0.20V, 0.30V, 0.40V, 0.50V, 0.60V, 0.70V, 0.80V, 0.90V, 1.0V, 1.5V, or a range consisting of any two of the above values.

[0210] Optionally, in some embodiments, in method A, the redox potential of the liquid-phase lithiating agent can also be 0.1V-0.5V, 0.1V-0.4V, 0.1V-0.3V, 0.1V-0.2V, 0.2V-0.5V, 0.2V-0.4V, 0.2V-0.3V, 0.3V-0.5V, 0.3V-0.4V, 0.4V-0.5V and the like.

[0211] The redox potential of the liquid-phase lithiating agent is within the above-mentioned suitable range, which can further improve the efficiency of pre-lithiation, thereby improving the lithium replenishment efficiency of the electrode plate.

[0212] In some embodiments, in method A, the molar ratio of lithium metal to the complexing agent can be (0.5:1)-(10:1), for example, 0.5:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, or a range consisting of any two of the above ratios. Alternatively, the molar ratio of lithium metal to the complexing agent can be (1:1)-(4:1), (1:1)-(3.5:1), (1:1)-(3:1), (1:1)-(2.5:1), (1:1)-(2:1), (1:1)-(1.5:1), and the like.

[0213] In some embodiments, the content of lithium in the liquid-phase lithiation agent can be 0.01mol / L-10mol / L, for example, 0.01mol / L, 0.1mol / L, 0.5mol / L, 1mol / L, 2mol / L, 5mol / L, 8mol / L, 10mol / L, or a range consisting of any two of the above values. Optionally, the content of lithium in the liquid-phase lithiation agent can also be 0.01mol / L-5mol / L, 0.01mol / L-4mol / L, 0.01mol / L-3mol / L, 0.01mol / L-2mol / L, 0.01mol / L-1mol / L, 0.5mol / L-5mol / L, 0.5mol / L-3mol / L, 0.5mol / L-1mol / L, 1mol / L-5mol / L, 2mol / L-4mol / L, etc.

[0214] Without intending to be limited by any theory or explanation, when the molar ratio of lithium metal to the complexing agent is within the above range, it not only helps to improve the reaction efficiency of lithium metal and the complexing agent, but also helps to adjust the content of lithium in the liquid-phase lithiating agent within a suitable range. In the liquid-phase lithiating agent, the content of lithium in a suitable range can improve the pre-lithiation efficiency of the liquid-phase lithiating agent for the electrode active material, thereby improving the lithium replenishment efficiency of the electrode plate.

[0215] In some embodiments, in method A, the molar ratio of lithium element to electrode active material in the liquid-phase lithiating agent may be (0.05:1)-(10:1), and may be (0.1:1)-(5:1).

[0216] Without intending to be bound by any theory or explanation, the molar ratio of lithium element in the liquid phase lithiating agent to the electrode active material is within the above-mentioned suitable range, and an appropriate amount of active lithium ions can be embedded in the electrode active material. Therefore, during the battery formation process, the electrode material can release an appropriate amount of active lithium ions to supplement the active lithium ions lost during the first cycle of charge and discharge cycles.

[0217] In some embodiments, in method A, the volume distribution particle size Dv50 of the electrode active material can be 0.5μm-40μm, 0.5μm-30μm, 0.5μm-20μm, 0.5μm-15μm, 2.5μm-35μm, 2.5μm-25μm, 2.5μm-15μm, 2.5μm-10μm, 4.5μm-37.5μm, 4.5μm-27.5μm, 4.5μm-17.5μm, 4.5μm-15μm, 4.5μm-12.5μm, and the like.

[0218] Without intending to be limited by any theory or explanation, when the volume distribution particle size Dv50 of the electrode active material is within the above-mentioned suitable range, not only can the prepared electrode material have a suitable lithium ion transmission path, but also the electrode material can have good electrolyte infiltration performance. Therefore, it is beneficial for the active lithium ions to escape from the electrode material, improve the lithium replenishment efficiency of the electrode plate, and thus help to further delay the capacity decay of the secondary battery and extend the cycle life of the secondary battery.

[0219] In some embodiments, in method A, the reactants may include at least one of air, water, oxygen, carbon dioxide, nitrogen, nitric oxide, nitrogen dioxide, nitrogen pentoxide, hydrogen fluoride, fluorine, sulfur, hydrogen sulfide, sulfur dioxide, sulfur trioxide, or red phosphorus. Alternatively, the reactants may include at least one of carbon dioxide, fluorine, nitrogen, sulfur dioxide, or red phosphorus.

[0220] The reactants selected from the above types can react with the liquid phase lithium agent and / or the pre-lithiation electrode active material. By selecting suitable reactants, the composition of the first inorganic lithium compound layer can be regulated. The first inorganic lithium compound layer has a suitable composition, which is beneficial to suppress the side reaction between the substrate and the air, so that the electrode material maintains a high lithium replenishment efficiency, and is beneficial to regulate the composition of the protective film on the electrode surface, thereby improving the stability of the electrode environment. As a result, it helps to further improve the cycle stability of the secondary battery and extend the cycle life of the secondary battery.

[0221] The contact between the above-mentioned reactants and the pre-lithiation electrode active material can be achieved in a variety of ways, and the present application does not limit this. In some embodiments, when the reactant is a gas, the reactant can be directly introduced into the slurry obtained in step S220. In some embodiments, when the reactant is a solid, the reactant can be dissolved in an organic solvent to obtain a reactant solution, and then the reactant solution is mixed evenly with the slurry obtained in step S220. This allows the reactant to be in contact with the pre-lithiation electrode active material more evenly and fully, which is conducive to the smooth progress of the reaction. The above-mentioned organic solvent may include at least one of alkanes, aromatic hydrocarbons, ethers, esters and their halides, for example, it may include at least one of benzene, dimethyl carbonate, ethylene carbonate, fluoroethylene carbonate, tetrahydrofuran, dimethyl ether, hydrofluoroether, and 1,1,1,3,3,3-hexafluoroisopropyl methyl ether. In the reactant solution, the mass fraction of the reactant may be 0.1%-20%.

[0222] In some embodiments, method A may further include: drying the electrode material.

[0223] The present application does not limit the dry atmosphere, and the dry atmosphere may include any atmosphere that does not produce side reactions with the electrode material. In some embodiments, the dry atmosphere may include nitrogen, argon, dry air, or a combination thereof. Optionally, in some embodiments, the dry atmosphere may include nitrogen, argon, or a combination thereof. The present application does not limit the drying temperature and time, and those skilled in the art may adjust them as needed. In some embodiments, the drying temperature may be 0°C-200°C, optionally 20°C-120°C, and the drying time may be 5min-6h. Thus, the stability of the chemical properties of the electrode material can be improved, thereby improving the stability of the chemical properties of the electrode plate.

[0224] In some embodiments, step S240 may include the following steps (1)-(2).

[0225] (1) The electrode material, optional other electrode active materials, and optional additives are uniformly mixed in an aprotic solvent to obtain an electrode slurry, wherein the other electrode active materials include other positive electrode active materials known in the art or other negative electrode active materials known in the art.

[0226] (2) The electrode slurry is coated on at least one side of the current collector, and then dried and cold pressed to obtain an electrode sheet.

[0227] In some embodiments, step S240 may include the following steps (3)-(4).

[0228] (3) Evenly mixing the electrode material, other optional electrode active materials, and optional additives to obtain electrode powder, wherein the other electrode active materials include other positive electrode active materials known in the art or other negative electrode active materials known in the art.

[0229] (4) Extruding and rolling the electrode powder into an electrode film, and pressing the electrode film and the current collector together to obtain an electrode plate.

[0230] Method B may include the following steps S310 to S340.

[0231] S310, providing an initial electrode sheet, the initial electrode sheet comprising a current collector and an electrode film layer located on at least one side of the current collector, the electrode film layer comprising an electrode active material.

[0232] S320, mixing lithium metal with a complexing agent solution so that the lithium metal reacts with the complexing agent to obtain a liquid-phase lithiating agent.

[0233] In step S320, the lithium metal can be in any form, for example, it can include at least one of a lithium block, a lithium foil, and a lithium powder, which is not limited here. The coordination reagent may include a reagent known in the art that can react with lithium metal, and those skilled in the art may select it as needed, which is not limited here. In some embodiments, mixing the lithium metal with the coordination reagent solution may include mixing the lithium metal with the coordination reagent and stirring it evenly, and the stirring temperature and time are not specifically limited, and those skilled in the art may adjust it as needed. As an example, the stirring temperature can be 0°C-60°C, optionally 10°C-40°C, and the stirring time can be 0.1h-12h, optionally 1h-6h.

[0234] S330, bringing a liquid-phase lithiating agent into contact with the electrode film layer, so that the liquid-phase lithiating agent pre-lithiates the electrode active material, thereby obtaining a pole piece including the pre-lithiated electrode active material.

[0235] In step S330, the contact between the liquid-phase lithiating agent and the electrode film layer can be achieved in a variety of ways, which are not limited in this application. In some embodiments, the electrode film layer can be impregnated with a liquid-phase lithiating agent, or the liquid-phase lithiating agent can be applied to the surface of the electrode film layer so that the liquid-phase lithiating agent pre-lithiates the electrode active material in the electrode film layer. The coating method can be brushing, shower coating, roller coating, nitrogen spraying, air spraying, electrostatic spraying, electrophoretic spraying, high-pressure airless spraying, etc., which are not limited here. In step S330, the temperature and time for the liquid-phase lithiating agent to pre-lithiate the electrode active material are not specifically limited, and those skilled in the art can adjust them as needed. As an example, the pre-lithiation temperature can be 0°C-80°C, optionally 10°C-50°C, and the pre-lithiation time can be 1min-6h, optionally 5min-30min.

[0236] S340, bringing an electrode plate including a pre-lithiation electrode active material into contact with a reactant to form a first inorganic lithium compound layer on at least a portion of the surface of the pre-lithiation electrode active material, thereby obtaining an electrode plate including the electrode material; wherein the electrode material includes: a substrate, the substrate includes the pre-lithiation electrode active material; and a first inorganic lithium compound layer coated on at least a portion of the surface of the substrate, the first inorganic lithium compound layer including at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide.

[0237] In step S340, the reactant may be a substance that can react with a liquid-phase lithiating agent or a pre-lithiated electrode active material to generate at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide, and lithium phosphide, and those skilled in the art may select it as needed. In step S340, after the pole piece including the pre-lithiated electrode active material contacts the reactant, the reactant may react with the liquid-phase lithiating agent remaining on at least a portion of the surface of the pre-lithiated electrode active material or the material on the surface of the pre-lithiated electrode active material to form a first inorganic lithium compound layer on at least a portion of the surface of the pre-lithiated electrode active material, thereby obtaining an electrode pole piece including the electrode material.

[0238] In some embodiments, the reactant may also react with the liquid-phase lithiation agent remaining on the surface of the electrode film layer to form a second inorganic lithium compound layer on at least a portion of the surface of the electrode film layer. The implementation of the second inorganic lithium compound layer has been described and illustrated in detail above and will not be repeated here. The reaction temperature and reaction time of step S340 are not specifically limited, and those skilled in the art may adjust them as needed. As an example, the reaction temperature of step S340 may be 0°C-80°C, optionally 10°C-50°C, and the reaction time may be 1min-60min, optionally 2min-10min.

[0239] The electrode plate prepared according to method B includes an electrode material, and the substrate of the electrode material has been pre-embedded with some active lithium ions. During the first charge or discharge process, the electrode material can release active lithium ions, thereby compensating for the loss of active lithium ions in the battery formation process. In addition, the electrode material can also form a dense, uniform and stable protective film on the surface of the electrode plate through the first inorganic lithium compound layer. The protective film can play a similar role to the SEI film, thereby improving the environmental stability of the electrode, reducing the irreversible loss of active lithium ions, and slowing down the capacity decay of the secondary battery. Therefore, the electrode plate prepared in the embodiment of the present application is applied to a secondary battery, which can improve the energy density of the secondary battery and extend the cycle life of the secondary battery.

[0240] It should be noted that by regulating the above steps S310 to S340, the composition of the electrode film layer in the electrode plate can be regulated. As an example, by regulating the reaction raw materials and reaction conditions of step S330, part of the electrode active materials can be pre-lithiated, or all of the electrode active materials can be pre-lithiated. By regulating the reaction raw materials and reaction conditions of step S330, the degree of pre-lithiation of the electrode active materials can also be regulated to regulate the lithium supplement content of the electrode plate. As an example, by regulating the reaction raw materials and reaction conditions of step S340, a first inorganic lithium compound layer can be formed on the surface of part of the pre-lithiated electrode active materials, or a first inorganic lithium compound layer can be formed on the surface of all pre-lithiated electrode active materials. As an example, by regulating the reaction raw materials and reaction conditions of steps S330 and S340, a second inorganic lithium compound layer can also be formed on at least part of the surface of the electrode plate. Those skilled in the art can understand that no matter what composition the electrode film layer in the electrode plate has, as long as it contains the above-mentioned electrode material, it can fall within the scope of this application.

[0241] In some embodiments, method B may further include: providing a complexing reagent solution, including uniformly mixing the complexing reagent and the solvent to obtain the complexing reagent solution.

[0242] In some embodiments, the coordination agent may include at least one of naphthalene and its derivatives, biphenyl and its derivatives, phenanthrene and its derivatives, pyrene and its derivatives, fluorene and its derivatives, indene and its derivatives, and aromatic hydrocarbon derivatives containing heteroatom functional groups. Alternatively, in some embodiments, the coordination agent may include at least one of 2-methylnaphthalene, 1-naphthonitrile, 2,2-dimethylbiphenyl, 2-ethylindene, 1-methyl-3-ethylpyrene, benzophenone, pyridine, and quinoline.

[0243] In some embodiments, the solvent may include at least one of alkanes and their derivatives, aromatic hydrocarbons and their derivatives, ether compounds and their derivatives, furan compounds and their derivatives, pyran compounds and their derivatives, esters and their derivatives. Alternatively, the solvent may include at least one of benzene, toluene, xylene, ethylbenzene, ethylene glycol dimethyl ether, 2-methyltetrahydrofuran, pyran or fluoroethylene carbonate.

[0244] Without intending to be limited by any theory or explanation, the complexing reagent selected from the above types can react with lithium metal to generate a liquid-phase lithiating agent with a lower redox potential. As a result, the liquid-phase lithiating agent is more likely to pre-lithiate the electrode active material and embed active lithium ions in the electrode active material, which is beneficial to improve the lithium replenishment efficiency of the electrode plate. Furthermore, the use of the above-mentioned types of solvents to dissolve the complexing reagent is beneficial to further adjust the redox potential of the liquid-phase lithiating agent within a suitable range, thereby further improving the efficiency of pre-lithiation and thereby improving the lithium replenishment efficiency of the electrode plate.

[0245] In some embodiments, in method B, the redox potential of the liquid-phase lithiating agent can be 0.05V-1.5V, for example, 0.05V, 0.10V, 0.20V, 0.30V, 0.40V, 0.50V, 0.60V, 0.70V, 0.80V, 0.90V, 1.0V, 1.5V, or a range consisting of any two of the above values.

[0246] Optionally, in some embodiments, in method B, the redox potential of the liquid-phase lithiating agent can also be 0.1V-0.5V, 0.1V-0.4V, 0.1V-0.3V, 0.1V-0.2V, 0.2V-0.5V, 0.2V-0.4V, 0.2V-0.3V, 0.3V-0.5V, 0.3V-0.4V, 0.4V-0.5V and the like.

[0247] The redox potential of the liquid-phase lithiating agent is within the above-mentioned suitable range, which can further improve the efficiency of pre-lithiation, thereby improving the lithium replenishment efficiency of the electrode plate.

[0248] In some embodiments, in method B, the molar ratio of lithium metal to the complexing agent can be (0.5:1)-(10:1), for example, 0.5:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, or a range consisting of any two of the above ratios. Alternatively, the molar ratio of lithium metal to the complexing agent can be (1:1)-(4:1), (1:1)-(3.5:1), (1:1)-(3:1), (1:1)-(2.5:1), (1:1)-(2:1), (1:1)-(1.5:1), and the like. In some embodiments, the content of lithium in the liquid-phase lithiation agent can be 0.01mol / L-10mol / L, for example, 0.01mol / L, 0.1mol / L, 0.5mol / L, 1mol / L, 2mol / L, 5mol / L, 8mol / L, 10mol / L, or a range consisting of any two of the above values. Optionally, the content of lithium in the liquid-phase lithiation agent can also be 0.01mol / L-5mol / L, 0.01mol / L-4mol / L, 0.01mol / L-3mol / L, 0.01mol / L-2mol / L, 0.01mol / L-1mol / L, 0.5mol / L-5mol / L, 0.5mol / L-3mol / L, 0.5mol / L-1mol / L, 1mol / L-5mol / L, 2mol / L-4mol / L, etc.

[0249] Without intending to be limited by any theory or explanation, when the molar ratio of lithium metal to the complexing agent is within the above range, it not only helps to improve the reaction efficiency of lithium metal and the complexing agent, but also helps to adjust the content of lithium in the liquid-phase lithiating agent within a suitable range. In the liquid-phase lithiating agent, the content of lithium in a suitable range can improve the pre-lithiation efficiency of the liquid-phase lithiating agent for the electrode active material, thereby improving the lithium replenishment efficiency of the electrode plate.

[0250] In some embodiments, in method B, the molar ratio of lithium element to electrode active material in the liquid-phase lithiating agent may be (0.05:1)-(10:1), and may be (0.1:1)-(5:1).

[0251] Without intending to be bound by any theory or explanation, the molar ratio of lithium element in the liquid phase lithiating agent to the electrode active material is within the above-mentioned suitable range, and an appropriate amount of active lithium ions can be embedded in the electrode active material. Therefore, during the battery formation process, the electrode material can release an appropriate amount of active lithium ions to supplement the active lithium ions lost during the first cycle of charge and discharge cycles.

[0252] In some embodiments, in method B, the volume distribution particle size Dv50 of the electrode active material can be 0.5μm-40μm, 0.5μm-30μm, 0.5μm-20μm, 0.5μm-15μm, 2.5μm-35μm, 2.5μm-25μm, 2.5μm-15μm, 2.5μm-10μm, 4.5μm-37.5μm, 4.5μm-27.5μm, 4.5μm-17.5μm, 4.5μm-15μm, 4.5μm-12.5μm, and the like.

[0253] Without intending to be limited by any theory or explanation, when the volume distribution particle size Dv50 of the electrode active material is within the above-mentioned suitable range, not only can the prepared electrode material have a suitable lithium ion transmission path, but also the electrode material can have good electrolyte infiltration performance. Therefore, it is beneficial for the active lithium ions to escape from the electrode material, improve the lithium replenishment efficiency of the electrode plate, and thus help to further delay the capacity decay of the secondary battery and extend the cycle life of the secondary battery.

[0254] In some embodiments, in method B, the reactants may include at least one of air, water, oxygen, carbon dioxide, nitrogen, nitric oxide, nitrogen dioxide, nitrogen pentoxide, hydrogen fluoride, fluorine, sulfur, hydrogen sulfide, sulfur dioxide, sulfur trioxide, or red phosphorus. Alternatively, the reactants may include at least one of carbon dioxide, fluorine, nitrogen, sulfur dioxide, or red phosphorus.

[0255] The reactants selected from the above types can react with the pre-lithiation electrode active material. By selecting suitable reactants, the composition of the first inorganic lithium compound layer can be regulated. The first inorganic lithium compound layer has a suitable composition, which is beneficial to suppress the side reaction between the substrate and the air, so that the electrode plate maintains a high lithium replenishment efficiency, and is beneficial to regulate the composition of the protective film on the electrode surface, thereby improving the stability of the electrode environment. This helps to further improve the cycle stability of the secondary battery and extend the cycle life of the secondary battery.

[0256] The above-mentioned reactants can be brought into contact with the pole piece including the pre-lithiation electrode active material in a variety of ways, which are not limited in this application. In some embodiments, when the reactant is a gas, the surface of the pole piece is directly purged with the reactant gas. In some embodiments, when the reactant is a solid, the reactant can be dissolved in an organic solvent to obtain a reactant solution, and then the reactant solution is applied to the surface of the pole piece. The coating method can be brushing, shower coating, roller coating, nitrogen spraying, air spraying, electrostatic spraying, electrophoretic spraying, high-pressure airless spraying, etc., which are not limited here. Thereby, the reactant can be more evenly and fully contacted with the surface of the pole piece, which is conducive to the smooth progress of the reaction. When the reactant contacts the pole piece in the form of a reactant solution, the reactant solution can also infiltrate into the pores of the electrode film layer, and react with the pre-lithiation electrode active material inside the electrode film layer, thereby further improving the efficiency of the reaction. The organic solvent may include at least one of alkanes, aromatic hydrocarbons, ethers, esters and halogenated products thereof, for example, benzene, dimethyl carbonate, ethylene carbonate, fluoroethylene carbonate, tetrahydrofuran, dimethyl ether, hydrofluoroether, 1,1,1,3,3,3-hexafluoroisopropyl methyl ether. In the reactant solution, the mass fraction of the reactant may be 0.1%-20%.

[0257] In some embodiments, method B may further include: drying the electrode plate.

[0258] The present application does not limit the dry atmosphere, and the dry atmosphere may include any atmosphere that does not produce side reactions with the electrode plate. In some embodiments, the dry atmosphere may include nitrogen, argon, dry air, or a combination thereof. Optionally, in some embodiments, the dry atmosphere may include nitrogen, argon, or a combination thereof. The present application does not limit the drying temperature and time, and those skilled in the art may adjust them as needed. In some embodiments, the drying temperature may be 0°C-200°C, optionally 20°C-120°C, and the drying time may be 5min-6h. In this way, the stability of the chemical properties of the electrode plate can be improved.

[0259] Battery

[0260] In a fifth aspect, an embodiment of the present application provides a battery. The battery mentioned in the embodiment of the present application may include one or more battery cells to provide a single physical module with higher voltage and capacity. When there are multiple battery cells, the multiple battery cells are connected in series, in parallel, or in mixed connection through a busbar.

[0261] The battery cell may be a secondary battery, which is also called a rechargeable battery or storage battery, and refers to a battery cell that can be recharged to activate the active material after the battery cell is discharged and continue to be used. The present application embodiment has no particular limitation on the type of secondary battery, for example, the secondary battery may be a lithium ion battery, a lithium metal battery, etc., and in particular, the secondary battery may be a lithium ion battery.

[0262] Generally, a battery cell includes an electrode assembly and an electrolyte, and the electrode assembly includes a positive electrode sheet, a negative electrode sheet and a separator. The separator is arranged between the positive electrode sheet and the negative electrode sheet, and mainly plays the role of preventing the positive and negative electrodes from short-circuiting, while allowing active ions to pass through.

[0263] The battery cell of the embodiment of the present application includes at least one of the electrode material of the first aspect, the electrode material prepared according to the preparation method of the second aspect, the electrode plate of the third aspect, or the electrode plate prepared according to the preparation method of the fourth aspect.

[0264] [Positive electrode]

[0265] In the battery cell of the present application, the positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector and including a positive electrode active material. For example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0266] In some embodiments, the positive electrode sheet includes the electrode material of the first aspect, and the electrode material is a positive electrode material. The embodiments of the electrode material have been described and illustrated in detail above, and will not be repeated here. It can be understood that the battery of the present application can achieve the beneficial effects of any of the above embodiments of the electrode material of the present application.

[0267] In some embodiments, the positive electrode sheet includes an electrode material prepared according to the method of the second aspect, and the electrode material is a positive electrode material. The embodiments of the method for preparing the electrode material have been described and illustrated in detail above, and will not be repeated here. It can be understood that the battery of the present application can achieve the beneficial effects of any of the above embodiments of the method for preparing the electrode material of the present application.

[0268] In some embodiments, the positive electrode plate includes the electrode plate of the third aspect. The embodiments of the electrode plate have been described and illustrated in detail above, and will not be repeated here. It can be understood that the battery of the present application can achieve the beneficial effects of any of the above embodiments of the electrode plate of the present application.

[0269] In some embodiments, the positive electrode sheet includes an electrode sheet prepared according to the preparation method of the fourth aspect. The embodiments of the preparation method of the electrode sheet have been described and illustrated in detail above, and will not be repeated here. It can be understood that the battery of the present application can achieve the beneficial effects of any of the above embodiments of the preparation method of the electrode sheet of the present application.

[0270] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0271] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0272] In some embodiments, the positive electrode film layer may further include a conductive agent and an optional dispersant. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0273] [Negative electrode]

[0274] In the battery cell of the present application, the negative electrode plate includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector and including a negative electrode active material. For example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0275] In some embodiments, the negative electrode plate includes the electrode material of the first aspect, and the electrode material is a negative electrode material. The embodiments of the electrode material have been described and illustrated in detail above, and will not be repeated here. It can be understood that the battery of the present application can achieve the beneficial effects of any of the above embodiments of the electrode material of the present application.

[0276] In some embodiments, the negative electrode sheet includes an electrode material prepared according to the method of the second aspect, and the electrode material is a negative electrode material. The embodiments of the method for preparing the electrode material have been described and illustrated in detail above, and will not be repeated here. It can be understood that the battery of the present application can achieve the beneficial effects of any of the above embodiments of the method for preparing the electrode material of the present application.

[0277] In some embodiments, the negative electrode plate includes the electrode plate of the third aspect. The embodiments of the electrode plate have been described and illustrated in detail above, and will not be repeated here. It can be understood that the battery of the present application can achieve the beneficial effects of any of the above embodiments of the electrode plate of the present application.

[0278] In some embodiments, the negative electrode sheet includes an electrode sheet prepared according to the preparation method of the fourth aspect. The embodiment of the preparation method of the electrode sheet has been described and illustrated in detail above, and will not be repeated here. It can be understood that the battery of the present application can achieve the beneficial effects of any of the above embodiments of the preparation method of the electrode sheet of the present application.

[0279] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, copper foil or aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0280] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).

[0281] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0282] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0283] In addition, the negative electrode plate of the present application does not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode plate described in the present application may also include a conductive primer layer (e.g., composed of a conductive agent and a binder) disposed between the negative electrode current collector and the negative electrode film layer. In other embodiments, the negative electrode plate described in the present application also includes a protective layer covering the surface of the negative electrode film layer.

[0284] [Isolation film]

[0285] The separator is disposed between the positive electrode sheet and the negative electrode sheet to play a role of isolation. The present application has no particular limitation on the type of separator, and any known porous structure separator with good chemical stability and mechanical stability can be selected.

[0286] In some embodiments, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer are the same or different, without special restrictions.

[0287] [Electrolytes]

[0288] Generally speaking, a battery cell also includes an electrolyte, which plays a role in conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid, gel or all-solid.

[0289] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0290] In some embodiments, the electrolyte salt can be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0291] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0292] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.

[0293] In some embodiments, the outer shell of the battery cell may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer shell of the battery cell may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0294] The present application has no particular limitation on the shape of the battery cell, which may be cylindrical, square or any other shape. Figure 1 The battery cell 5 is a square structure as an example.

[0295] In some embodiments, reference Figure 2 , the shell may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0296] The preparation method of the battery cell of the present application is well known. In some embodiments, the electrode assembly can be placed in a housing, dried, injected with electrolyte, and subjected to vacuum packaging, standing, forming, shaping and other processes to obtain a battery cell.

[0297] In some embodiments, the battery mentioned in the present application may be a battery module or a battery pack, etc. A battery module or a battery pack generally includes a box for encapsulating one or more battery cells. The box can prevent liquid or other foreign matter from affecting the charging or discharging of the battery cells.

[0298] In some embodiments, there may be multiple battery cells in a battery module or battery pack, and the multiple battery cells may be connected in series, in parallel, or in a hybrid connection. A hybrid connection means that the multiple battery cells are connected in series and in parallel. The multiple battery cells may be directly connected in series, in parallel, or in a hybrid connection, and then the whole formed by the multiple battery cells is accommodated in a box; of course, multiple battery cells may be first connected in series, in parallel, or in a hybrid connection to form a battery module, and then the multiple battery modules may be connected in series, in parallel, or in a hybrid connection to form a whole, and then accommodated in a box.

[0299] Figure 3 FIG. 4 is a schematic diagram of a battery module 4 as an example. Figure 3 As shown, there are multiple battery cells 5, and the multiple battery cells 5 are first connected in series, in parallel, or in mixed connection to form a battery module 4. The multiple battery cells 5 in the battery module 4 can be electrically connected through a busbar component to realize the series connection, parallel connection, or mixed connection of the multiple battery cells 5 in the battery module 4. In the battery module 4, the multiple battery cells 5 can be arranged in sequence along the length direction of the battery module 4. Of course, they can also be arranged in any other manner. Further, the multiple battery cells 5 can be fixed by fasteners.

[0300] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0301] Figure 4 and Figure 5 FIG. 1 is a schematic diagram of a battery pack 1 as an example. Figure 4 and Figure 5 As shown, the battery pack 1 may include a box body and a plurality of battery modules 4 disposed in the box body. The plurality of battery modules 4 in the battery pack 1 may be electrically connected through a busbar component to achieve series connection, parallel connection, or mixed connection of the plurality of battery modules 4 in the battery pack 1. The box body includes an upper box body 2 and a lower box body 3, wherein the upper box body 2 is used to cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box in any manner.

[0302] Electrical devices

[0303] The present application also provides an electrical device, the electrical device includes a battery provided by the present application, and the battery is used to provide electrical energy. The battery can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0304] As the electrical device, a battery cell, a battery module including a plurality of battery cells, or a battery pack may be selected according to its usage requirements.

[0305] Figure 6 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the requirements of the power consumption device for high power and high energy density, a battery pack or a battery module can be used.

[0306] As another example, the power-consuming device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be light and thin, and a battery cell may be used as a power source.

[0307] Example

[0308] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0309] Example 1

[0310] Preparation of electrode materials

[0311] Step a: Dissolve 1 mol of the complexing reagent 2-methylbiphenyl in 1 L of tetrahydrofuran solvent, then add 1 mol of lithium flakes, and stir at room temperature 25° C. for 4 h to obtain a liquid phase lithiating agent of 1 mol / L lithium-[2-methylbiphenyl]-tetrahydrofuran.

[0312] Step b: Volume distribution particle size Dv 1 The electrode active material silicon oxide with a size of 10 μm is added to the liquid-phase lithiating agent obtained in step a, and stirred under the first reaction conditions to obtain a lithiated electrode slurry, wherein the molar ratio M of the lithium element in the liquid-phase lithiating agent to the electrode active material is 5, and the first reaction conditions are: reaction temperature 25° C., reaction time 6 h.

[0313] Step c: introducing the reactants (a mixed gas of 2% HF, 2% CO2, 20% O2 and 76% N2) into the lithiated electrode slurry at a flow rate of 0.5 L / min, and continuing the reaction under the second reaction conditions, wherein the second reaction conditions are: reaction temperature 25°C, reaction time 10 min.

[0314] Step d: The slurry after the reaction in step c is filtered under reduced pressure and dried at 120° C. for 1 hour to obtain an electrode material. The electrode material includes a substrate (pre-lithiated silicon oxide) and a first inorganic lithium compound layer coated on the surface of the substrate. The volume distribution volume Dv of the electrode material is 2 50 is 15 μm, the thickness d of the first inorganic lithium compound layer is 1 μm, and the first inorganic lithium compound layer includes 40% by weight of Li2O, 30% by weight of Li3N, 2% by weight of Li2CO3, and 28% by weight of LiF. The lithium supplement content of the electrode material is measured by the method described in the specification of this application, and the measured value is 50%.

[0315] Preparation of positive electrode

[0316] The positive electrode active material LiFePO4, the conductive agent carbon black and the binder PVDF are mixed in a ratio of 84:8:8, the solvent NMP is added, and the mixture is stirred evenly to obtain a positive electrode slurry; the positive electrode slurry is coated on a carbon-coated aluminum foil, and the positive electrode sheets are obtained through drying, cold pressing and slitting.

[0317] Preparation of negative electrode

[0318] The negative electrode active material artificial graphite, electrode material, conductive agent carbon black, binder SBR, and thickener CMC-Na are mixed in a mass ratio of 87:10:0.5:1.25:1.25, and a solvent NMP is added and stirred evenly to obtain a negative electrode slurry; the negative electrode slurry is coated on a copper foil, and the negative electrode sheet is obtained through drying, cold pressing, and slitting.

[0319] Isolation film

[0320] Polypropylene film is used as the isolation film.

[0321] Preparation of electrolyte

[0322] LiPF6 was dissolved in a solvent prepared by ethylene carbonate, ethyl methyl carbonate and diethyl carbonate in a volume ratio of 1:1:1 to obtain an electrolyte with a LiPF6 concentration of 1 mol / L.

[0323] Preparation of secondary batteries

[0324] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order to obtain an electrode assembly; the electrode assembly is placed in a packaging shell, and after drying, the electrolyte is injected, and after vacuum packaging, standing, forming, shaping and other processes, a secondary battery is obtained.

[0325] Example 2-15

[0326] Based on the preparation process of the electrode material in Example 1, the preparation parameters of the electrode material were adjusted as shown in Table 1 to prepare the electrode materials of Examples 2-15. The preparation of the positive electrode sheet, negative electrode sheet, separator, electrolyte and secondary battery of Examples 2-15 was the same as that of Example 1.

[0327] Example 16

[0328] Preparation of electrode materials

[0329] Step a: 0.05 mol of the complexing agent naphthalene is dissolved in 1 L of the solvent 2-methylfuran, and then 0.05 mol of lithium flakes is added, and stirred at room temperature 25°C for 4 hours to obtain 0.05 mol / L of the liquid phase lithiating agent lithium-naphthalene-[2-methylfuran].

[0330] Step b: Volume distribution particle size Dv 1 The electrode active material LiFePO4 with a size of 10 μm is added to the liquid-phase lithiating agent obtained in step a, and stirred under the first reaction conditions to obtain a lithiated electrode slurry, wherein the molar ratio M of the lithium element in the liquid-phase lithiating agent to the electrode active material is 1, and the first reaction conditions are: reaction temperature 25° C., reaction time 5 min.

[0331] Step c: Pass the reactant (a mixed gas of 80% O2 and 20% N2) into the lithiated electrode slurry at a flow rate of 0.1 L / min, and continue the reaction under the second reaction conditions. The second reaction conditions are: reaction temperature 25°C, reaction time 2 min.

[0332] Step d: The slurry after the reaction in step c is filtered under reduced pressure and dried at 120°C for 1 hour to obtain an electrode material. The electrode material includes a substrate (pre-lithiated LiFePO4) and a first inorganic lithium compound layer coated on the surface of the substrate. The volume distribution volume Dv of the electrode material is 2 50 is 10 μm, the thickness d of the first inorganic lithium compound layer is 80 nm, and the first inorganic lithium compound layer includes 30% by mass of Li2O and 70% by mass of Li3N. The lithium supplement content of the electrode material is measured by the method described in the specification of this application, and the measured value is 30%.

[0333] Preparation of positive electrode

[0334] The electrode material, the positive electrode active material LiFePO4, the conductive agent carbon black and the binder PVDF are mixed in a ratio of 15:69:8:8, the solvent NMP is added, and the mixture is stirred evenly to obtain the positive electrode slurry; the positive electrode slurry is coated on the carbon-coated aluminum foil, and the positive electrode sheets are obtained through drying, cold pressing and slitting.

[0335] Preparation of negative electrode

[0336] The negative electrode active material artificial graphite, the negative electrode active material silicon oxide, the conductive agent carbon black, the binder SBR, and the thickener CMC-Na are mixed in a mass ratio of 67:30:0.5:1.25:1.25, and the solvent NMP is added and stirred evenly to obtain the negative electrode slurry; the negative electrode slurry is coated on the copper foil, and the negative electrode sheet is obtained through drying, cold pressing and cutting.

[0337] Isolation film

[0338] Polypropylene film is used as the isolation film.

[0339] Preparation of electrolyte

[0340] LiPF6 was dissolved in a solvent prepared by ethylene carbonate, ethyl methyl carbonate and diethyl carbonate in a volume ratio of 1:1:1 to obtain an electrolyte with a LiPF6 concentration of 1 mol / L.

[0341] Preparation of secondary batteries

[0342] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order to obtain an electrode assembly; the electrode assembly is placed in a packaging shell, and after drying, the electrolyte is injected, and after vacuum packaging, standing, forming, shaping and other processes, a secondary battery is obtained.

[0343] Examples 17-18

[0344] Based on the preparation process of the electrode material in Example 16, the preparation parameters of the electrode material were adjusted as shown in Table 2 to prepare the electrode materials of Examples 17-18. The preparation of the positive electrode sheet, negative electrode sheet, separator, electrolyte and secondary battery of Examples 17-18 was the same as that of Example 16.

[0345] Embodiment 19

[0346] Preparation of negative electrode

[0347] The negative electrode active material (artificial graphite and silicon oxide are mixed in a mass ratio of 95:5), the conductive agent carbon black, the binder SBR, and the thickener CMC-Na are mixed in a mass ratio of 97:0.5:1.25:1.25, the solvent NMP is added, and the mixture is stirred evenly to obtain the negative electrode slurry; the negative electrode slurry is coated on a copper foil, and the initial negative electrode sheet is obtained through drying, cold pressing, and slitting.

[0348] 1 mol of the complexing agent 2-methylbiphenyl was dissolved in 1 L of tetrahydrofuran solvent, and then 1 mol of lithium flakes was added, and stirred at room temperature at 25°C for 4 hours to obtain 1 mol / L of the liquid phase lithium-[2-methylbiphenyl]-tetrahydrofuran.

[0349] The initial negative electrode plate is immersed in a liquid-phase lithiating agent, and the liquid-phase lithiating agent reacts with the negative electrode active material under the first reaction condition to obtain a plate including a pre-lithiated negative electrode active material. The molar ratio M of the lithium element in the liquid-phase lithiating agent to the negative electrode active material in the initial negative electrode plate is 0.3, and the first reaction condition is: reaction temperature 40°C, reaction time 20min.

[0350] Place the electrode sheet including the pre-lithiation negative electrode active material in the reactant gas flow, continuously introduce the reactant (a mixed gas of 25% H2S and 75% N2) at a flow rate of 0.22L / min, and continue the reaction under the second reaction condition, which is: reaction temperature 25°C, reaction time 10min. Subsequently, dry at normal pressure at 120°C for 1h to obtain the negative electrode sheet. The negative electrode sheet includes an electrode material, which includes a substrate and a first inorganic lithium compound layer coated on the surface of the substrate. The thickness d of the first inorganic lithium compound layer is 800nm, and the first inorganic lithium compound layer includes 10% Li2S and 90% Li3N by mass. The lithium supplement content of the negative electrode sheet is 50% as measured by the method described in the specification of this application.

[0351] The preparation process of the positive electrode plate, isolation membrane, electrolyte and secondary battery of Example 19 is the same as that of Example 1.

[0352] Examples 20-32

[0353] Based on the preparation process of the negative electrode sheet in Example 19, the preparation parameters of the negative electrode sheet were adjusted as shown in Table 3 to prepare the negative electrode sheets of Examples 20 to 32. The preparation of the positive electrode sheets, separators, electrolytes and secondary batteries of Examples 20 to 32 was the same as that of Example 19.

[0354] Embodiment 33

[0355] Preparation of positive electrode

[0356] The positive electrode active material LiFePO4, the conductive agent carbon black and the binder PVDF are mixed in a ratio of 84:8:8, the solvent NMP is added, and the mixture is stirred evenly to obtain a positive electrode slurry; the positive electrode slurry is coated on a carbon-coated aluminum foil, and the initial positive electrode sheet is obtained through drying, cold pressing and cutting.

[0357] 0.05 mol of the complexing agent naphthalene was dissolved in 1 L of the solvent 2-methylfuran, and then 0.05 mol of lithium flakes was added, and stirred at room temperature 25°C for 4 hours to obtain 0.05 mol / L of the liquid phase lithiating agent lithium-naphthalene-[2-methylfuran].

[0358] The initial positive electrode plate is immersed in a liquid-phase lithiating agent, and the liquid-phase lithiating agent reacts with the positive electrode active material under the first reaction condition to obtain a plate including a pre-lithiated positive electrode active material. The molar ratio M of the lithium element in the liquid-phase lithiating agent to the positive electrode active material in the initial positive electrode plate is 1, and the first reaction condition is: reaction temperature 25°C, reaction time 15min.

[0359] Place the electrode sheet including the pre-lithiated positive electrode active material in the reactant gas flow, continuously introduce the reactant (a mixed gas of 80% O2 and 20% N2) at a flow rate of 1L / min, and continue the reaction under the second reaction condition, which is: reaction temperature 25°C, reaction time 10min. Subsequently, dry at normal pressure at 120°C for 1h to obtain the positive electrode sheet. The positive electrode sheet includes an electrode material, which includes a substrate (pre-lithiated LiFePO4) and a first inorganic lithium compound layer coated on the surface of the substrate. The thickness d of the first inorganic lithium compound layer is 100nm, and the first inorganic lithium compound layer includes 30% Li2O and 70% Li3N by mass. The lithium supplement content of the positive electrode sheet is 30% as determined by the method described in the specification of this application.

[0360] The preparation of the negative electrode plate, isolation membrane, electrolyte and secondary battery of Example 33 is the same as that of Example 16.

[0361] Examples 34-35

[0362] Based on the preparation process of the positive electrode sheet in Example 33, the preparation parameters of the positive electrode sheet were adjusted as shown in Table 4 to prepare the positive electrode sheets of Examples 34-35. The preparation of the negative electrode sheets, separators, electrolytes and secondary batteries of Examples 34-35 was the same as that of Example 33.

[0363] Comparative Examples 1-3

[0364] The preparation process of the positive electrode sheet, negative electrode sheet, separator, electrolyte and secondary battery of Comparative Examples 1-3 is the same as that of Example 1, except that the electrode material is replaced with an equal mass of electrode active material, as shown in Table 1 for details.

[0365] Comparative Example 4

[0366] Based on the preparation process of the electrode material in Example 1, the preparation parameters of the electrode material were adjusted as shown in Table 1 to prepare the electrode material of Comparative Example 4. The preparation of the positive electrode sheet, negative electrode sheet, separator, electrolyte and secondary battery of Comparative Example 4 was the same as that of Example 1.

[0367] Comparative Example 5

[0368] The preparation process of the positive electrode sheet, negative electrode sheet, isolation membrane, electrolyte and secondary battery of Comparative Example 5 is the same as that of Example 16, except that the electrode material is replaced with an equal mass of electrode active material, as shown in Table 2 for details.

[0369] Comparative Example 6

[0370] Based on the preparation process of the electrode material in Example 16, the preparation parameters of the electrode material were adjusted as shown in Table 2 to prepare the electrode material of Comparative Example 6. The preparation of the positive electrode sheet, negative electrode sheet, separator, electrolyte and secondary battery of Comparative Example 6 was the same as that of Example 16.

[0371] Comparative Example 7

[0372] The preparation process of the positive electrode plate, isolation membrane, electrolyte and secondary battery of Comparative Example 7 is the same as that of Example 19, except that the negative electrode plate is replaced with the initial negative electrode plate to prepare the secondary battery of Comparative Example 7.

[0373] Comparative Example 8

[0374] Based on the preparation process of the negative electrode sheet in Example 19, the preparation parameters of the negative electrode sheet were adjusted as shown in Table 3 to prepare the negative electrode sheet of Comparative Example 8. The preparation of the positive electrode sheet, separator, electrolyte and secondary battery of Comparative Example 8 was the same as that of Example 19.

[0375] Comparative Example 9

[0376] The preparation process of the negative electrode plate, isolation membrane, electrolyte and secondary battery of Comparative Example 9 is the same as that of Example 33, except that the positive electrode plate is replaced with the initial positive electrode plate to prepare the secondary battery of Comparative Example 9.

[0377] Comparative Example 10

[0378] Based on the preparation process of the positive electrode sheet in Example 33, the preparation parameters of the positive electrode sheet were adjusted as shown in Table 4 to prepare the positive electrode sheet of Comparative Example 10. The preparation of the negative electrode sheet, separator, electrolyte and secondary battery of Comparative Example 10 was the same as that of Example 33.

[0379] The following tests were performed on Examples 1-35 and Comparative Examples 1-10, and the test results are shown in Tables 1 to 4, respectively.

[0380] Characterization of materials

[0381] (1)Dv 1 50's Representation

[0382] According to GB / T 19077-2016 particle size distribution laser diffraction method, the volume distribution particle size Dv of the electrode active material was determined by a laser particle size analyzer (MalvemMaster Size 3000). 1 50.

[0383] (2)Dv 2 50's Representation

[0384] According to GB / T 19077-2016 particle size distribution laser diffraction method, the volume distribution particle size Dv of the electrode material was determined using a laser particle size analyzer (MalvernMaster Size 3000). 2 50.

[0385] (3) Characterization of the thickness d of the first inorganic lithium compound layer

[0386] Example 1-18: The prepared electrode material is dispersed in an ethanol solvent, and dropped onto a micro-gate support film. The thickness d of the first inorganic lithium compound layer in the electrode material is measured by a high-resolution transmission electron microscope (magnification of 10,000-300,000 times).

[0387] Example 19-32: Take the prepared negative electrode plate; randomly select an area, perform argon ion cross-section polishing, and take a transmission electron microscope image (TEM image) with a magnification of 30,000 times; process the TEM image, adjust the appropriate contrast, and measure the thickness d of the first inorganic lithium compound layer.

[0388] Examples 33-35: Take the prepared positive electrode plate; randomly select an area, perform argon ion cross-section polishing, and take a transmission electron microscope image (TEM image) with a magnification of 10,000 times; process the TEM image, adjust the appropriate contrast, and measure the thickness d of the first inorganic lithium compound layer.

[0389] (4) Characterization of the composition of the first inorganic lithium compound layer

[0390] Example 1-18: The types of elements and their contents on the surface of the electrode material are measured by X-ray photoelectron spectroscopy (XPS), and the composition of the first inorganic lithiation layer is determined according to the content ratio of each element and the chemical formula of the inorganic lithiation.

[0391] Examples 19-32: Take the prepared negative electrode plate, randomly select an area for cross-section, determine the position of the first inorganic lithium compound layer by scanning electron microscopy (SEM) at a magnification of 10,000 times, and mark the position where the first inorganic lithium compound layer is distributed in the field of view as the target area; then select an area of ​​10 μm*10 μm at a magnification of 1,000 times for EDS surface scanning for 2 minutes to obtain the element types and contents of the target area, and determine the composition of the first inorganic lithium compound layer according to the content ratio of each element and the chemical formula of the inorganic lithium compound.

[0392] Examples 33-35: Take the prepared positive electrode plate, randomly select an area for cross-section, determine the position of the first inorganic lithium compound layer by scanning electron microscopy (SEM) at a magnification of 10,000 times, and mark the position where the first inorganic lithium compound layer is distributed in the field of view as the target area; then select an area of ​​10μm*10μm at a magnification of 1000 times for EDS surface scanning for 2 minutes to obtain the element types and contents of the target area, and determine the composition of the first inorganic lithium compound layer according to the content ratio of each element and the chemical formula of the inorganic lithium compound.

[0393] Battery performance test

[0394] (1) First week coulomb efficiency test

[0395] At 25°C, charge the secondary battery to 3.65V at 0.1C constant current, then charge at constant voltage until the current is less than or equal to 0.05C, then leave it for 5 minutes, the charging capacity this time is recorded as the first charging capacity C0 (mAh / g); then discharge to 2.5V at 0.2C constant current, the discharge capacity this time is recorded as the first discharge capacity D0 (mAh / g). First week coulomb efficiency = D0 / C0×100%.

[0396] (2) Normal temperature cycle performance test

[0397] At 25°C, the formed secondary battery was charged to 3.65V at a constant current of 0.2C, then charged to a current of 0.05C at a constant voltage of 3.65V, left for 5 minutes, and then discharged to 2.5V at 0.5C. The resulting capacity was recorded as the initial capacity C. 初始 Repeat the above steps for the same battery and record the discharge capacity C of the battery after the 300th cycle. 300 , calculate the battery capacity retention rate P 300 (%) = C 300 / C 初始 ×100%.

[0398] (3) Discharge capacity test

[0399] At 25°C, charge the formed secondary battery at a constant current of 0.2C to 3.65V, then charge at a constant voltage of 3.65V to a current of 0.05C, leave for 5 minutes, and then discharge at 0.5C to 2.5V. Repeat the above steps for the same battery, and record the discharge capacity C of the battery after the 100th cycle. 100 , calculate the battery's discharge capacity in grams = C 100 / (mass of positive electrode active material + mass of electrode material).

[0400]

[0401]

[0402]

[0403]

[0404]

[0405]

[0406]

[0407] In Tables 1 to 4, the percentage of the gaseous component in the reactant refers to the volume percentage of the component in the mixed gas, for example, "25% H2S + 75% N2" refers to a gas formed by a mixture of H2S and N2 at a volume ratio of 25:75. The percentage of the solute in the reactant solution refers to the mass percentage concentration of the solute in the solution, for example, "[5% S + 5% P] / THF mixed solution" means that in a mixed solution of S and P with THF as the solvent, the mass percentage concentration of S is 5%, and the mass percentage concentration of P is 5%.

[0408] It can be seen from Tables 1 to 4 above that the electrode materials and electrode plates provided in the embodiments of the present application are applied to secondary batteries, which can effectively compensate for the loss of active lithium ions in the secondary batteries, thereby improving the cycle performance of the batteries.

[0409] From Examples 1-7, it can be seen that by regulating the composition of the first inorganic lithium compound layer, the lithium replenishment efficiency of the electrode material can be controlled, thereby regulating the cycle performance of the battery. From Examples 3, 8-10, it can be seen that when other conditions are the same, as the lithium replenishment content of the electrode material increases, the first-week coulombic efficiency and cycle performance of the battery are improved. From Examples 3, 11-13, it can be seen that when other conditions remain unchanged, regulating the thickness of the first inorganic lithium compound layer within a suitable range can improve the lithium replenishment efficiency of the electrode material while improving the cycle performance of the battery.

[0410] In contrast, in Comparative Example 1, the electrode material is replaced with silicon oxide of equal mass, and the first cycle coulombic efficiency and cycle performance of the battery are not as good as those of Examples 1-13; in Comparative Examples 2 and 3, the electrode material is replaced with tin and phosphorus of equal mass, and the first cycle coulombic efficiency and cycle performance of the battery are also not as good as those of the corresponding Examples 14 and 15. Although Comparative Example 4 uses pre-lithiated silicon oxide, the first inorganic lithium compound layer is not coated on the surface of the pre-lithiated silicon oxide, so the lithium replenishment efficiency of the pre-lithiated silicon oxide is reduced, and the cycle performance of the battery is not ideal.

[0411] Based on the test results of Examples 16-18 in Table 2, it can be seen that pre-lithiation of the positive electrode active material and coating the surface of the first inorganic lithium compound layer can effectively replenish the active lithium ions lost by the secondary battery. Therefore, the secondary battery can still maintain a relatively high discharge capacity after 100 charge and discharge cycles.

[0412] In contrast, in Comparative Example 5, the electrode material is replaced with an equal mass of LiFePO4, and the discharge capacity and cycle performance are far inferior to those of Examples 16 to 18. Although Comparative Example 6 uses pre-lithiated LiFePO4, the first inorganic lithium compound layer is not coated on the surface of the pre-lithiated LiFePO4, so the lithium replenishment efficiency of the pre-lithiated LiFePO4 is reduced, resulting in that the discharge capacity of Comparative Example 6 is not as good as that of Example 17, and the cycle performance is also not as good as that of Examples 16 to 18.

[0413] From the test results in Table 3, it can be seen that pre-lithiation of the negative electrode active material in the negative electrode plate and treatment of the negative electrode plate with reactants so that the negative electrode plate contains electrode materials can effectively improve the first-week coulombic efficiency and cycle performance of the battery.

[0414] In contrast, the negative electrode plate of Comparative Example 7 was not subjected to pre-lithiation treatment, and the first-cycle coulombic efficiency and cycle performance of the battery were much lower than those of Examples 19 to 32. Although Comparative Example 8 used a pre-lithiation treatment on the negative electrode active material in the negative electrode plate, no first inorganic lithium compound layer was formed on the surface of the pre-lithiation negative electrode active material, and thus, the first-cycle coulombic efficiency of the battery was lower than that of Examples 19 to 25 and Examples 29 to 32, and the cycle performance was also lower than that of Examples 19 to 32.

[0415] From the test results in Table 4, it can be seen that pre-lithiation of the positive active material in the positive electrode plate and treating the positive electrode plate with a reactant so that the positive electrode plate contains electrode materials can effectively replenish the active lithium ions lost by the secondary battery. As a result, the secondary battery can still maintain a high discharge capacity after 100 cycles of charge and discharge.

[0416] In contrast, the positive electrode plate of Comparative Example 9 was not subjected to pre-lithiation treatment, and the discharge capacity in grams and the cycle performance after 100 charge-discharge cycles were much lower than those of Examples 33 to 35. Although the positive electrode active material in the positive electrode plate of Comparative Example 10 was subjected to pre-lithiation treatment, the first inorganic lithium compound layer was not formed on the surface of the pre-lithiation positive electrode active material, and thus the discharge capacity in grams after 100 charge-discharge cycles was lower than that of Example 33, and the cycle performance was also lower than that of Example 33.

[0417] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. An electrode material, characterized in that: include: a substrate comprising a pre-lithiated electrode active material; as well as A first inorganic lithium compound layer is coated on at least a portion of the surface of the substrate, wherein the first inorganic lithium compound layer includes at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide.

2. The electrode material according to claim 1, characterized in that The first inorganic lithium compound layer includes at least two of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride or lithium sulfide; Optionally, based on the total mass of the first inorganic lithium compound layer, the first inorganic lithium compound layer comprises 18%-90% of lithium nitride, 0-28% of lithium fluoride, 0-80% of lithium oxide, 0-2% of lithium carbonate, and 0-20% of lithium sulfide; More optionally, based on the total mass of the first inorganic lithiation layer, the first inorganic lithiation layer includes 70%-90% of lithium nitride, 0-30% of lithium oxide, and 0-10% of lithium sulfide.

3. The electrode material according to claim 1 or 2, characterized in that The thickness of the first inorganic lithium compound layer is 2nm-5000nm, and can be optionally 20nm-1000nm.

4. The electrode material according to any one of claims 1 to 3, characterized in that The volume distribution particle size Dv50 of the electrode material is 0.6 μm-60 μm, and can be optionally 5 μm-15 μm.

5. The electrode material according to any one of claims 1 to 4, characterized in that The electrode material is a positive electrode material, and the lithium supplement content of the positive electrode material is 1%-30%, and can be optionally 5%-20%; The lithium supplement content of the positive electrode material is determined by (C1-C 10 ) / C 10 ×100%, where C1 is the actual gram capacity of the positive electrode material in mAh / g, C 10 It is the theoretical gram capacity of the positive electrode active material, in mAh / g.

6. The electrode material according to any one of claims 1 to 4, characterized in that The electrode material is a negative electrode material, and the lithium supplement content of the negative electrode material is 1%-100%, and can be optionally 30%-50%; The lithium supplement content of the negative electrode material is determined by (C 20 -C2) / C 20 ×100%, where C2 is the actual gram capacity of the negative electrode material in mAh / g, and C 20 It is the theoretical gram capacity of the negative electrode active material, in mAh / g.

7. A method for preparing an electrode material, characterized in that: include: Mixing lithium metal with a complexing agent solution so that the lithium metal reacts with the complexing agent to obtain a liquid-phase lithiating agent; contacting the liquid-phase lithiating agent with an electrode active material so that the liquid-phase lithiating agent pre-lithiates the electrode active material to obtain a pre-lithiated electrode active material; contacting the pre-lithiation electrode active material with a reactant to form a first inorganic lithiation layer on at least a portion of the surface of the pre-lithiation electrode active material to obtain an electrode material; Among them, the electrode material includes: a substrate, the substrate includes the pre-lithiation electrode active material; and the first inorganic lithium compound layer coated on at least a portion of the surface of the substrate, the first inorganic lithium compound layer includes at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide.

8. The preparation method according to claim 7, characterized in that: The preparation method further comprises: Providing the complexing reagent solution, including uniformly mixing the complexing reagent with a solvent to obtain the complexing reagent solution; Optionally, the complexing agent includes at least one of naphthalene and its derivatives, biphenyl and its derivatives, phenanthrene and its derivatives, pyrene and its derivatives, fluorene and its derivatives, indene and its derivatives, or aromatic hydrocarbon derivatives containing heteroatom functional groups, and more preferably includes at least one of 2-methylnaphthalene, 1-naphthonitrile, 2,2-dimethylbiphenyl, 2-ethylindene, 1-methyl-3-ethylpyrene, or benzophenone; Optionally, the solvent includes at least one of alkanes and their derivatives, aromatic hydrocarbons and their derivatives, ether compounds and their derivatives, furan compounds and their derivatives, pyran compounds and their derivatives, or esters and their derivatives, and more optionally includes at least one of benzene, toluene, xylene, ethylbenzene, ethylene glycol dimethyl ether, 2-methyltetrahydrofuran, pyran or fluoroethylene carbonate.

9. The preparation method according to claim 7 or 8, characterized in that: The redox potential of the liquid-phase lithiating agent is 0.05V-1.5V, and can be optionally 0.1V-0.5V.

10. The preparation method according to any one of claims 7 to 9, characterized in that: The molar ratio of the lithium metal to the complexing agent is (0.5:1)-(10:1), and can be optionally (1:1)-(4:1); And / or, the molar concentration of lithium element in the liquid-phase lithiating agent is 0.01 mol / L-10 mol / L, and can be optionally 0.01 mol / L-5 mol / L; And / or, the molar ratio of lithium element in the liquid-phase lithiating agent to the electrode active material is (0.05:1)-(10:1), and can be optionally (0.1:1)-(5:1); And / or, the volume distribution particle size Dv50 of the electrode active material is 0.5 μm-40 μm.

11. The preparation method according to any one of claims 7 to 10, characterized in that: The reactants include at least one of air, water, oxygen, carbon dioxide, nitrogen, nitric oxide, nitrogen dioxide, nitrogen pentoxide, hydrogen fluoride, fluorine, sulfur, hydrogen sulfide, sulfur dioxide, sulfur trioxide or red phosphorus, and can optionally include at least one of carbon dioxide, fluorine, nitrogen, sulfur dioxide or red phosphorus.

12. An electrode plate, characterized in that: It comprises a current collector and an electrode film layer located on at least one side of the current collector, wherein the electrode film layer comprises an electrode material; The electrode material comprises: a substrate comprising a pre-lithiated electrode active material; and A first inorganic lithium compound layer is coated on at least a portion of the surface of the substrate, wherein the first inorganic lithium compound layer includes at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide.

13. The electrode plate according to claim 12, characterized in that: The electrode plate also includes a second inorganic lithium compound layer attached to at least a portion of the surface of the electrode film layer, and the second inorganic lithium compound layer includes at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide.

14. The electrode plate according to claim 12 or 13, characterized in that: The first inorganic lithium compound layer includes at least two of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride or lithium sulfide; Optionally, based on the total mass of the first inorganic lithium compound layer, the first inorganic lithium compound layer comprises 18%-90% of lithium nitride, 0-28% of lithium fluoride, 0-80% of lithium oxide, 0-2% of lithium carbonate, and 0-20% of lithium sulfide; More optionally, based on the total mass of the first inorganic lithiation layer, the first inorganic lithiation layer includes 70%-90% of lithium nitride, 0-30% of lithium oxide, and 0-10% of lithium sulfide.

15. A method for preparing an electrode sheet, characterized in that: include: Method A: Mixing lithium metal with a complexing agent solution so that the lithium metal reacts with the complexing agent to obtain a liquid-phase lithiating agent; contacting the liquid-phase lithiating agent with an electrode active material so that the liquid-phase lithiating agent pre-lithiates the electrode active material to obtain a pre-lithiated electrode active material; contacting the pre-lithiation electrode active material with a reactant to form a first inorganic lithiation layer on at least a portion of the surface of the pre-lithiation electrode active material to obtain an electrode material; The electrode material comprises: a substrate, the substrate comprising the pre-lithiation electrode active material; and a first inorganic lithium compound layer coated on at least a portion of the surface of the substrate, the first inorganic lithium compound layer comprising at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide; Preparing an electrode sheet comprising the electrode material; Or method B: Providing an initial pole piece, the initial pole piece comprising a current collector and an electrode film layer located on at least one side of the current collector, the electrode film layer comprising an electrode active material; Mixing lithium metal with a complexing agent solution so that the lithium metal reacts with the complexing agent to obtain a liquid-phase lithiating agent; The liquid-phase lithiating agent is brought into contact with the electrode film layer, so that the liquid-phase lithiating agent pre-lithiates the electrode active material to obtain a pole piece including the pre-lithiated electrode active material; The electrode sheet including the pre-lithiation electrode active material is brought into contact with a reactant to form a first inorganic lithiation layer on the surface of the pre-lithiation electrode active material, thereby obtaining an electrode sheet including the electrode material; Among them, the electrode material includes: a substrate, the substrate includes the pre-lithiation electrode active material; and the first inorganic lithium compound layer coated on at least a portion of the surface of the substrate, the first inorganic lithium compound layer includes at least one of lithium oxide, lithium nitride, lithium carbonate, lithium fluoride, lithium sulfide or lithium phosphide.

16. The preparation method according to claim 15, characterized in that: The method A and / or method B further comprises: Providing the complexing reagent solution, including uniformly mixing the complexing reagent with a solvent to obtain the complexing reagent solution; Optionally, the complexing agent includes at least one of naphthalene and its derivatives, biphenyl and its derivatives, phenanthrene and its derivatives, pyrene and its derivatives, fluorene and its derivatives, indene and its derivatives, or aromatic hydrocarbon derivatives containing heteroatom functional groups, and more preferably includes at least one of 2-methylnaphthalene, 1-naphthonitrile, 2,2-dimethylbiphenyl, 2-ethylindene, 1-methyl-3-ethylpyrene, or benzophenone; Optionally, the solvent includes at least one of alkanes and their derivatives, aromatic hydrocarbons and their derivatives, ether compounds and their derivatives, furan compounds and their derivatives, pyran compounds and their derivatives, or esters and their derivatives, and more optionally includes at least one of benzene, toluene, xylene, ethylbenzene, ethylene glycol dimethyl ether, 2-methyltetrahydrofuran, pyran or fluoroethylene carbonate.

17. The preparation method according to claim 15 or 16, characterized in that: In the method A and / or the method B, the redox potential of the liquid-phase lithiating agent is 0.05V-1.5V, and can be optionally 0.1V-0.5V.

18. The preparation method according to any one of claims 15 to 17, characterized in that: In the method A and / or method B, The molar ratio of the lithium metal to the complexing agent is (0.5:1)-(10:1), and can be optionally (1:1)-(4:1); And / or, the molar concentration of lithium element in the liquid-phase lithiating agent is 0.01 mol / L-10 mol / L, and can be optionally 0.01 mol / L-5 mol / L; And / or, the molar ratio of lithium element in the liquid-phase lithiating agent to the electrode active material is (0.05:1)-(10:1), and can be optionally (0.1:1)-(5:1); And / or, the volume distribution particle size Dv50 of the electrode active material is 0.5 μm-40 μm.

19. The preparation method according to any one of claims 15 to 18, characterized in that: In the method A and / or method B, The reactants include at least one of air, water, oxygen, carbon dioxide, nitrogen, nitric oxide, nitrogen dioxide, nitrogen pentoxide, hydrogen fluoride, fluorine, sulfur, hydrogen sulfide, sulfur dioxide, sulfur trioxide or red phosphorus, and can optionally include at least one of carbon dioxide, fluorine, nitrogen, sulfur dioxide or red phosphorus.

20. A battery, comprising at least one of the electrode material according to any one of claims 1 to 6, the electrode material prepared according to the preparation method according to any one of claims 7 to 11, the electrode plate according to any one of claims 12 to 14, or the electrode plate prepared according to the preparation method according to any one of claims 15 to 19.

21. An electrical device comprising the battery according to claim 20.

Citation Information

Patent Citations

  • Pre-lithiated positive electrode slurry as well as preparation method and application thereof

    CN113764672A

  • Interface regulation and control liquid for pre-lithiation electrode, preparation method and application

    CN115000489A

  • Negative pole piece and preparation method thereof, secondary battery, battery module, battery pack and power utilization device

    CN115842094A

  • Pre-lithiated pole piece and preparation method thereof, secondary battery and power utilization device

    CN115842096A

  • Composite negative plate and preparation method thereof, and lithium ion battery and preparation method thereof

    CN115863537A

Cited By

  • Electrode material and preparation method therefor, electrode sheet and preparation method therefor, battery and electric device

    EP4693591A1