Lithium ion battery component with multiple layers of electrodes
A multilayer electrode structure with a silicon-rich and graphite-rich layer stabilizes silicon-based anodes, addressing mechanical degradation and enhancing lithium-ion battery performance by reducing swelling and improving cycle life.
Patent Information
- Application Number
- CN202410618534.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-17
- Publication Date
- 2024-12-03
AI Technical Summary
Conventional lithium-ion batteries face challenges with mechanical degradation and capacity loss due to the significant volume change of silicon-based anode materials during lithiation, leading to poor cycling performance.
A multilayer electrode structure is introduced, comprising a silicon-rich layer between a metal current collector and a graphite-rich layer, with a cross-linked binder to maintain mechanical integrity and disrupt the in-plane alignment of graphite particles, reducing swelling and enhancing electrochemical performance.
The multilayer structure improves energy density and cycle life by stabilizing the electrode against volume changes, maintaining electrical contact, and providing a less tortuous path for lithium ion migration.
Smart Images

Figure CN119069665A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to electrode materials for lithium-ion batteries. Background Art
[0002] Lithium-ion batteries are widely used in various applications. One of the contributing factors to the performance of lithium-ion batteries is the electrode structure, which plays a role in determining the battery cell performance, such as the battery's energy density, power density, and cycle life.
[0003] Graphite is commonly used as an anode material in lithium-ion batteries due to its low lithiation potential and reasonable capacity, high conductivity, and wide availability. However, graphite has been developed to near theoretical capacity and energy density maximums, so significant changes in battery cell performance may require the use of new and / or different anode materials.
[0004] Silicon-based materials (such as silicon oxide, silicon nanoparticles, and silicon / carbon composites) are considered promising anode materials due to their high theoretical capacity, but lithiation of silicon domains causes the material to expand and delithiate in a corresponding contraction. This volume change can lead to mechanical degradation of the anode and capacity loss during cycling. Although other materials undergo volume changes upon lithiation, the effect is very large for silicon lithiation, and these materials generally exhibit poor cycling performance. Summary of the invention
[0005] The present disclosure provides, in one embodiment, a lithium-ion battery comprising an electrode having a metal current collector and a multilayer active material coated on the metal current collector. The multilayer active material comprises a discrete graphite-rich layer of at least 85% by weight graphite and a discrete silicon-rich layer of at least 15% by weight silicon-based material, the silicon-rich layer being between the metal current collector and the graphite-rich layer and in direct contact with the metal current collector and the graphite-rich layer, so that the silicon-rich layer adheres to the metal current collector and adheres to the graphite-rich layer. In other embodiments, the silicon-rich layer comprises at least 20% by weight silicon-based material.
[0006] In one embodiment, the graphite-rich layer does not contain silicon-based materials. In another embodiment, the silicon-rich layer is a molecularly cross-linked silicon-rich layer. In yet another embodiment, the silicon-based material comprises silicon carbide or silicon monoxide. In another embodiment, the metal current collector is a metal foil.
[0007] The present disclosure also provides an electrode, which includes a metal current collector and a multilayer active material coated on the metal current collector. The multilayer active material comprises a discrete graphite particle layer suspended in a cross-linked binder and a discrete silicon-based material particle layer suspended in a cross-linked binder, and the silicon-based material particle layer is arranged between the metal current collector and the graphite particle layer. The layer defines an interface region, and the presence of silicon-based material particles in the interface region destroys the in-plane alignment of the graphite particles. The graphite particle layer comprises at least 85% by weight of graphite, and the silicon-based material particle layer comprises at least 15% by weight of silicon-based material. In other embodiments, the silicon-rich layer comprises at least 20% by weight of silicon-based material.
[0008] The present disclosure provides a method for forming an electrode. The method includes depositing a silicon-based slurry containing at least 15% by weight of a silicon-based material onto a metal current collector and drying to form a cured cross-linked layer. The method also includes depositing a top graphite-based slurry layer containing at least 85% by weight of graphite on the cured cross-linked layer, and drying to form a cured top cross-linked layer. In other embodiments, the silicon-rich layer contains at least 20% by weight of silicon-based material and / or these layers define an interfacial region, and the presence of silicon-based material particles in the interfacial region destroys the in-plane arrangement of the graphite particles. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 is a schematic cross-sectional view of an electrode structure according to one embodiment; and
[0010] Figure 2 is a schematic cross-sectional view of an electrode structure according to another embodiment. DETAILED DESCRIPTION
[0011] Embodiments are described herein. However, it should be understood that the disclosed embodiments are merely examples and that other embodiments may take various and alternative forms. The drawings are not necessarily drawn to scale. Some features may be enlarged or minimized to show details of particular components. Therefore, the specific structural details and functional details disclosed herein should not be interpreted as limiting, but merely as a representative basis for teaching those skilled in the art.
[0012] The various features shown and described with reference to any one of the accompanying drawings may be combined with features shown in one or more other drawings to produce embodiments not explicitly shown or described. The combinations of features shown provide representative embodiments for typical applications. However, for specific applications or implementations, various combinations and modifications of features consistent with the teachings of the present disclosure may be desired.
[0013] Silicon oxide or silicon carbon composites (silicon X materials) have been developed that provide increased anode energy density compared to graphite (typically 800 mAh / g to 1800 mAh / g), while significantly reducing the amount of electrode swelling relative to elemental silicon, and reducing anode or electrolyte degradation that can lead to irreversible capacity, gas formation and material fragmentation and rapid cycle life loss. These silicon X active materials remain electrochemically active similar to silicon in that they are conversion materials that reversibly form lithiated silicon alloys when reduced in an electrochemical cell. However, these materials use an oxide or carbon substrate as a matrix to promote performance in the cell. Typically, these silicon X materials are blended with graphite to further promote cycle life and electrode stability, thereby accepting a trade-off between anode energy density and cell cycle life and anode stability.
[0014] The present disclosure relates to lithium ion batteries with enhanced electrode structures and methods for forming such electrode structures. In some examples, a lithium ion battery is provided with an electrode comprising a metal current collector and a multilayer active material coated on the metal current collector. The multilayer active material comprises discrete graphite-rich layers and discrete silicon-rich layers, and the multilayer active material provides increased electrochemical performance, energy density, and cycle life compared to conventional lithium ion batteries.
[0015] In the enhanced electrode structure, the active material comprises both silicon particles and graphite particles. At least a certain weight percent of the silicon particles are incorporated into the silicon-rich layer, and at least a certain weight percent of the graphite particles are incorporated into the graphite-rich layer.
[0016] The binder material in the multilayer anode helps maintain the mechanical and structural integrity of the electrode. In some embodiments, the binder material comprises a crosslinker that enhances adhesion between the particles and the current collector and between the silicon-rich layer and the graphite-rich layer. The crosslinked binder also helps to alleviate the mechanical stress caused by the volume expansion and contraction of the silicon particles during the charge and discharge cycles.
[0017] The expansion of silicon particles during charge and discharge cycles is a well-known phenomenon that can lead to capacity loss and mechanical degradation of lithium-ion batteries. As will be appreciated by those skilled in the art, the novel feature of the present disclosure is the disruption of the in-plane arrangement of graphite particles, which is achieved by the presence of silicon-based material particles at the interface region between the graphite-rich layer and the silicon-rich layer. This disruption helps prevent the expansion effect of the silicon particles from propagating throughout the graphite layer.
[0018] Figure 1 is a schematic cross-sectional view of an electrode structure 10 according to one embodiment. The electrode structure 10 includes a metal current collector 12, a first discrete silicon-rich layer 14, and a top discrete graphite-rich layer 16.
[0019] The metal current collector 12 can be made of a material such as copper, aluminum or other suitable metal or metal alloy. The first discrete silicon-rich layer 14 is adhered to the metal current collector 12 and contains at least 15 weight percent of a silicon-based material, which can be silicon carbide, silicon monoxide or other suitable silicon-based materials. The top discrete graphite-rich layer 16 is in direct contact with the first discrete silicon-rich layer 14 and contains at least 85 weight percent graphite. However, in some embodiments, the silicon-rich layer contains at least 20 weight percent of a silicon-based material, thereby further promoting the performance of the electrode.
[0020] Figure 2 is a schematic cross-sectional view of an electrode structure 15 according to another embodiment. The electrode structure 15 includes a metal current collector 22, a first layer 24 including silicon particles, and a top layer 26 including graphite particles.
[0021] The metal current collector 22 can be made of a material such as copper, aluminum or other suitable metal or metal alloy. A first layer 24 containing silicon particles is formed on the current collector 22. The silicon particles in the first layer 24 can be suspended in a cross-linked binder material. A top layer 26 containing graphite particles is formed on the first layer 24. The graphite particles in the top layer 26 can also be suspended in a cross-linked binder material. At the interface region 28 between the first layer 24 and the top layer 26, the presence of the silicon particles disrupts the orientation of the graphite particles.
[0022] Therefore, the present disclosure contemplates forming a multilayer anode structure that blends silicon X and graphite active materials, wherein the first deposited layer on the metal current collector is a blend of silicon X and a graphite active material having a relatively high silicon X content (greater than 5% by weight of silicon X, and especially greater than 20% by weight of silicon X), and the one or more outer layers are composed of a graphite active material having less than 15% by weight or no silicon X content. All of these layers also contain a binder, and sometimes contain conductive additives and other components that produce a functional electrode. Each layer can be applied by placing the slurry on the electrode surface and then drying. The thickness of each deposited layer can be 5um to 100um.
[0023] The present disclosure also contemplates stabilizing the sublayers by crosslinking prior to coating the cover layer. Crosslinking can be achieved by adding a molecular crosslinking agent to the slurry or to the layer after coating, and then chemically crosslinking with a chemical reagent, ultraviolet light, or thermal process. This can form a multilayer coated anode by preventing redissolution or significant swelling of the coating layer when a new layer is deposited.
[0024] An example of such a crosslinking chemistry is the use of dipentaerythritol penta / hexaacrylate or tetramethylolmethane tetraacrylate as molecular crosslinkers, which form crosslinks after reaction with a free radical source such as benzoyl peroxide. The crosslinker and activator can be added during slurry coating or after the coating is applied. Typical crosslink densities can be 0.5% to 4%. Additional layers can then be applied without dissolving or significantly swelling the crosslinked layer.
[0025] The proposed multilayer approach can show different performance advantages over a single layer by embedding the X-rich silicon layer within a strongly bonded layer adjacent to the current collector. This can reduce sublayer swelling and reduce the loss of electrical contact with the silicon X particles.
[0026] The proposed multilayer approach can also produce electrodes in which the average alignment of graphite particles is reduced compared to anodes having only a single layer of graphite or a blend of graphite and silicon X active material. This effect occurs due to the relatively high presence of silicon X particles in the sublayer. The silicon X particles are not stratified and are relatively non-deformable and isotropic, which reduces the ability of compression to induce alignment in this sublayer. This can also reduce subsequent alignment in the overlying layer. The overall reduction in the alignment of graphite flakes results in less anisotropic cell swelling perpendicular to the cell stacking direction, as well as a less tortuous path for lithium ions to migrate through the wetted electrode, and thereby produces electrochemical performance benefits to the anode.
[0027] Other solutions to boost the performance of silicon X-graphite blend anodes may involve replacing the carboxymethyl cellulose / styrene-butadiene binder system with a less flexible binder such as polyacrylic acid or polyurethane.
[0028] The proposed arrangement can maintain a closer contact between the silicon X and the current collector, provide a simple method to optimize the mechanical properties of the silicon X-graphite layer by varying the crosslink density, and reduce the overall graphite particle alignment in the anode layer.
[0029] Although exemplary embodiments are described above, these embodiments are not intended to describe all possible forms encompassed by the claims. The words used in the specification are words of description rather than limitation, and it should be understood that various changes can be made without departing from the spirit and scope of these disclosed materials.
[0030] As previously mentioned, the features of the various embodiments may be combined to form further embodiments of the invention which may not have been explicitly described or shown.
[0031] Although various embodiments may have been described as providing advantages or being preferred over other embodiments or prior art implementations with respect to one or more desired characteristics, one of ordinary skill in the art will recognize that one or more features or characteristics may be compromised to achieve desired overall system properties, depending on the specific application and implementation. These properties may include, but are not limited to, strength, durability, marketability, appearance, packaging, size, serviceability, weight, manufacturability, ease of assembly, etc. Therefore, embodiments that are described as less desirable than other embodiments or prior art implementations with respect to one or more characteristics are within the scope of the present disclosure and may be desirable for particular applications.
[0032] According to the present invention, a lithium ion battery is provided, which has: an electrode, the electrode having a metal current collector and a multilayer active material coated on the metal current collector, the multilayer active material comprising a discrete graphite-rich layer of at least 85 weight % graphite and a discrete silicon-rich layer of at least 15 weight % silicon-based material, the silicon-rich layer being between the metal current collector and the graphite-rich layer and in direct contact with the metal current collector and the graphite-rich layer, so that the silicon-rich layer adheres to the metal current collector and to the graphite-rich layer.
[0033] According to an embodiment, the silicon-rich layer contains at least 20 wt. % of silicon-based material.
[0034] According to an embodiment, the graphite rich layer is free of silicon-based materials.
[0035] According to an embodiment, the silicon-rich layer is a molecularly cross-linked silicon-rich layer.
[0036] According to an embodiment, the silicon-based material is silicon carbide or silicon monoxide.
[0037] According to an embodiment, the metal current collector is a metal foil.
[0038] According to the present invention, an electrode is provided, which has: a metal current collector and a multilayer active material coated on the metal current collector, the multilayer active material comprising a discrete graphite particle layer suspended in a cross-linked binder and a discrete silicon-based material particle layer suspended in a cross-linked binder, and the silicon-based material particle layer is arranged between the metal current collector and the graphite particle layer, these layers define an interface region, the presence of silicon-based material particles in the interface region destroys the in-plane arrangement of the graphite particles, the graphite particle layer contains at least 85 weight % of graphite, and the silicon-based material particle layer contains at least 15 weight % of silicon-based material.
[0039] According to an embodiment, the layer of silicon-based material particles contains at least 20 wt % silicon-based material.
[0040] According to an embodiment, the graphite particle layer does not contain silicon-based materials.
[0041] According to an embodiment, the metal current collector is a metal foil.
[0042] According to the present invention, a method for forming an electrode includes: depositing a silicon-based slurry containing at least 15 weight % of a silicon-based material onto a metal current collector; drying to form a cured cross-linked layer; depositing a top graphite-based slurry layer containing at least 85 weight % of graphite on the cured cross-linked layer; and drying to form a cured top cross-linked layer.
[0043] In one aspect of the invention, the cured cross-linked layer comprises at least 20 wt % of silicon-based material.
[0044] In one aspect of the invention, the layers define an interfacial region where the presence of the silicon-based material particles disrupts the in-plane alignment of the graphite particles.
[0045] In one aspect of the invention, the current collector is a metal foil.
[0046] In one aspect of the present invention, the cured top cross-linked layer is free of silicon-based materials.
Claims
1. A lithium ion battery comprising: An electrode having a metal current collector and a multilayer active material coated on the metal current collector, the multilayer active material comprising discrete graphite-rich layers of at least 85 weight percent graphite and discrete silicon-rich layers of at least 15 weight percent silicon-based material, the silicon-rich layers being between the metal current collector and the graphite-rich layers and in direct contact with the metal current collector and the graphite-rich layers, such that the silicon-rich layers adhere to the metal current collector and to the graphite-rich layers.
2. The lithium ion battery of claim 1, wherein the silicon-rich layer comprises at least 20 wt% silicon-based material.
3. The lithium ion battery of claim 1, wherein the graphite-rich layer does not contain silicon-based materials. 4 . The lithium ion battery as claimed in claim 1 , wherein the silicon-rich layer is a molecularly cross-linked silicon-rich layer.
5. The lithium ion battery of claim 1, wherein the silicon-based material is silicon carbide or silicon monoxide.
6. The lithium ion battery of claim 1, wherein the metal current collector is a metal foil.
7. An electrode comprising: A metal current collector and a multilayer active material coated on the metal current collector, wherein the multilayer active material comprises a discrete graphite particle layer suspended in a cross-linked binder and a discrete silicon-based material particle layer suspended in a cross-linked binder, and the silicon-based material particle layer is arranged between the metal current collector and the graphite particle layer, the layers define an interface region, the presence of the silicon-based material particles in the interface region destroys the in-plane arrangement of the graphite particles, the graphite particle layer comprises at least 85 weight % of graphite, and the silicon-based material particle layer comprises at least 15 weight % of silicon-based material.
8. The electrode of claim 7, wherein the silicon-based material particle layer comprises at least 20 wt% of silicon-based material.
9. The electrode of claim 7, wherein the graphite particle layer does not contain silicon-based materials.
10. The electrode of claim 7, wherein the metal current collector is a metal foil.
11. A method for forming an electrode, the method comprising: depositing a silicon-based slurry comprising at least 15 weight percent silicon-based material onto a metal current collector; drying to form a cured cross-linked layer; depositing a top graphite-based slurry layer comprising at least 85 wt.% graphite on the cured cross-linked layer; as well as Drying to form a cured top cross-linked layer.
12. The method of claim 11, wherein the cured cross-linked layer comprises at least 20 wt% of a silicon-based material.
13. The method of claim 11, wherein the layer defines an interfacial region in which the presence of the silicon-based material particles disrupts the in-plane alignment of the graphite particles.
14. The method of claim 11, wherein the current collector is a metal foil.
15. The method of claim 11, wherein the cured top cross-linked layer is free of silicon-based materials.