Lithium-sodium double-ion de-intercalation phosphate positive electrode material, battery and preparation method thereof
By using Na as the outer layer and Li as the core of lithium-sodium integrated core-shell cathode material in lithium-sodium batteries, using the one-dimensional ion path design of phosphate materials, the problems of shortage of lithium battery resources and low sodium-voltage capacity are solved, and the specific capacity of sodium-voltage is improved. The specific capacity and cycling performance of the battery are obtained.
Patent Information
- Application Number
- CN202411175869.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
The shortage of existing lithium battery resources and low specific capacity of sodium batteries lead to poor circulation performance.
Using lithium-sodium integrated core-shell cathode material with Na as the outer layer and Li as the inner core, the phosphate material is used as the base material, and a one-dimensional ion path design is used to prevent lithium ions from transmissing to the material surface and keep sodium ions on the surface, thereby improving Specific capacity and cycling performance of the battery.
It improves the specific capacity and circulation performance of lithium-sodium batteries, reduces the free flow of core active substances, inhibits the formation of residual alkalis, and extends the service life of the battery.
Smart Images

Figure CN119069691A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrochemical technology, and in particular to a lithium-sodium dual ion deintercalation phosphate positive electrode material, a battery and a preparation method thereof. Background Art
[0002] With the rapid growth of global battery demand, lithium resources are beginning to face resource constraints. On the one hand, the total amount of lithium resources is limited, with an abundance of only 0.006% in the earth's crust. On the other hand, the spatial distribution of lithium resources is uneven. Lithium mines are mainly distributed in Australia and South America, while my country's lithium resource reserves account for only 6% of the world's lithium reserves. In addition, the mining cost is relatively high, and the current dependence on lithium for battery production is too high.
[0003] Sodium-ion batteries have the characteristics of low cost, high safety performance, and a wide operating temperature range. Sodium-ion batteries also have the advantages of abundant sodium resources and lower electrolyte concentration. There is no over-discharge phenomenon, and they have certain competitiveness in the fields of communication base stations, power grid energy storage, and low-speed electric vehicles. In addition, the working principle of sodium-ion batteries is the same as that of lithium-ion batteries, and both achieve charging and discharging by embedding and extracting ions back and forth between two electrodes. However, the specific capacity of sodium-ion batteries is low and the core active substances easily migrate to the surface of the material, resulting in a high residual alkali on the surface of the positive electrode material, which in turn leads to poor cycle performance of the positive electrode material. Summary of the invention
[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects of the existing lithium battery resources shortage, low sodium battery specific capacity and poor cycle performance due to high residual alkali on the surface of the positive electrode material, thereby providing a lithium-sodium dual ion deintercalation phosphate positive electrode material, battery and preparation method thereof to solve the above problems.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] A lithium-sodium dual ion deintercalation phosphate positive electrode material, comprising a lithium-sodium integrated core-shell positive electrode material with Na as the outer layer and Li as the inner core, the chemical formula of which is Na y Li x FePO 4 , 0.1<y≤0.5, 0.5≤x<0.9, x+y=1.
[0007] The present invention also provides a method for preparing the above-mentioned lithium sodium dual ion deintercalation phosphate positive electrode material, comprising:
[0008] The lithium source, iron phosphate and solvent are ground and mixed and dried to obtain a first precursor, and the first precursor is placed in an inert atmosphere for sintering to obtain a sintered product Li x FePO 4 ;
[0009] The sodium source and the calcined product Li x FePO 4 , and the solvent are ground and mixed and dried to obtain a second precursor, and the second precursor is placed in an inert atmosphere for sintering to obtain a lithium sodium dual ion deintercalation phosphate positive electrode material Na y Li x FePO 4 .
[0010] Preferably, the lithium source is Li 2 CO 3 ;
[0011] And / or, the sodium source is at least one of sodium gluconate, sodium dodecylbenzene sulfonate and sodium oxalate;
[0012] And / or, the solvent is water.
[0013] Preferably, the sintering temperature is 600-700°C;
[0014] And / or, the sintering treatment time is 8-12h;
[0015] And / or, the grinding is ball milling and / or sand milling;
[0016] And / or, the drying process is spray drying.
[0017] Preferably, the inlet temperature of the spray drying is 180-220°C;
[0018] And / or, the outlet temperature of the spray drying is 100-120°C;
[0019] And / or, the spray drying atmosphere is an inert atmosphere.
[0020] Preferably, the inert atmosphere is nitrogen and / or argon.
[0021] The present invention also provides a lithium-sodium dual-ion battery, comprising: a positive electrode sheet containing the above-mentioned lithium-sodium dual-ion deintercalation phosphate positive electrode material or the lithium-sodium dual-ion deintercalation phosphate positive electrode material prepared by the preparation method of the above-mentioned lithium-sodium dual-ion deintercalation phosphate positive electrode material, a hard carbon negative electrode sheet, a separator, and an electrolyte containing sodium salt and lithium salt.
[0022] The present invention also provides a method for preparing the above-mentioned lithium-sodium dual-ion battery, comprising: stacking a positive electrode sheet containing a lithium-sodium dual-ion deintercalation phosphate positive electrode material, a separator, and a hard carbon negative electrode sheet in sequence, winding and loading them into a battery shell, injecting an electrolyte containing a sodium salt and a lithium salt, and sealing and welding to obtain the battery.
[0023] Preferably, the preparation process of the positive electrode sheet comprises: weighing a lithium sodium dual ion deintercalation phosphate positive electrode material, conductive carbon black and a binder, adding the weighed materials into a solvent and mixing them to obtain a positive electrode slurry, uniformly coating the positive electrode slurry on an aluminum foil, drying, rolling and cutting the positive electrode sheet;
[0024] And / or, the preparation process of the hard carbon negative electrode sheet includes: weighing hard carbon and a binder and mixing them to obtain a negative electrode slurry, uniformly coating the negative electrode slurry on a copper foil, drying, rolling, and cutting to obtain a hard carbon negative electrode sheet.
[0025] Preferably, the mass ratio of the lithium sodium dual ion deintercalation phosphate positive electrode material, the conductive carbon black and the binder is 90:7:3;
[0026] And / or, the mass ratio of the total mass of the lithium sodium dual ion deintercalation phosphate positive electrode material, the conductive carbon black and the binder to the mass ratio of the solvent is 1:1;
[0027] And / or, the positive electrode slurry loading on the aluminum foil is 30-40 mg / cm 2 ;
[0028] and / or, the mass ratio of the hard carbon to the binder is 94:6;
[0029] And / or, the negative electrode slurry loading on the copper foil is 8-10 mg / cm 2 ;
[0030] And / or, the solvent is N-methylpyrrolidone (NMP);
[0031] And / or, the binder is polyvinylidene fluoride (PVDF).
[0032] Preferably, the drying is at 105°C;
[0033] And / or, the drying is for 1 hour.
[0034] Preferably, the diaphragm is a PP / PE / PP composite film;
[0035] And / or, the lithium salt in the electrolyte is LiPF 6 ;
[0036] And / or, the sodium salt in the electrolyte is NaPF 6 ;
[0037] and / or, the concentration of the lithium salt in the electrolyte is 0.5-1.0 mol / L, preferably 1.0 mol / L;
[0038] and / or, the concentration of sodium salt in the electrolyte is 0.5-1.0 mol / L, preferably 1.0 mol / L;
[0039] And / or, the solvent in the electrolyte is ethylene carbonate (EC) and / or dimethyl carbonate (DMC).
[0040] In the grinding process of the present invention, the amount of solvent can be adjusted according to the grinding conditions of the material. In the present invention, based on 500g of solvent, the amount of phosphate added is 10 mol.
[0041] The technical solution of the present invention has the following advantages:
[0042] 1. A lithium-sodium dual ion deintercalation phosphate positive electrode material, comprising a lithium-sodium integrated core-shell positive electrode material with Na as the outer layer and Li as the inner core, the chemical formula of which is Na y Li x FePO 4 , 0.1<y≤0.5, 0.5≤x<0.9, x+y=1. The present invention adopts phosphate material as the base material, and uses a step-by-step sintering method to prepare a lithium-sodium integrated core-shell positive electrode material with Na as the outer layer and Li as the inner core, which combines the advantages of high performance of lithium electricity and low cost of sodium electricity. Among them, the present invention adopts a phosphate material base material combined with a core-shell design with Na as the outer layer and Li as the inner core, and utilizes the characteristics of the one-dimensional ion path of phosphate (ions must first pass through the external wide path and then enter the internal narrow path), so that lithium ions with small ion radius cannot reach the material surface through the translation path, and sodium ions with large ion radius stay on the material surface, so that during the charge and discharge process, the positive electrode material still maintains a structure with Li ions inside and Na ions outside. Such a path design not only reduces the freeing of the inner core active material to the material surface, inhibits the formation of residual alkali, but also promotes Li ions to enter the bulk phase through the surface, improves the reversible deintercalation capacity, and thus improves the specific capacity and cycle performance of the battery.
[0043] 2. In the lithium-sodium dual-ion battery provided by the present invention, on the basis of adopting a lithium-sodium dual-ion deintercalation phosphate positive electrode material, a lithium-sodium dual-ion battery is prepared by combining a hard carbon negative electrode and an electrolyte containing a mixed solute of lithium salt and sodium salt, and the battery is optimized from an overall perspective, thereby ensuring that the prepared battery has excellent specific capacity and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0045] Figure 1 It is Na obtained in Example 1 of the present invention.0.5 Li 0.5 FePO 4 XRD diffraction pattern of positive electrode material;
[0046] Figure 2 It is a test diagram of the cycle performance of the positive electrode materials prepared in the embodiments of the present invention and the comparative examples. DETAILED DESCRIPTION
[0047] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0048] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0049] Example 1
[0050] This embodiment provides a method for preparing a lithium sodium dual-ion battery, and the specific steps are as follows:
[0051] (1) Weigh 2.5 mol Li 2 CO 3 、10.0mol FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 200℃, the outlet temperature was 110℃, N 2 The first precursor was spray-dried in a nitrogen atmosphere to obtain a first precursor, and the first precursor was sintered at 650° C. for 10 h in a nitrogen atmosphere to obtain a lithium-deficient first sintered product Li 0.5 FePO 4 ;
[0052] (2) 5 mol of sodium gluconate and 10 mol of the calcined product Li prepared in step (1) 0.5 FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 200℃, the outlet temperature was 110℃, N 2 The second precursor was spray-dried in a nitrogen atmosphere to obtain a second precursor, and the second precursor was sintered at 650° C. for 10 h in a nitrogen atmosphere to obtain a lithium-sodium dual ion deintercalation phosphate positive electrode material Na 0.5 Li 0.5 FePO 4 The prepared lithium sodium dual ion deintercalation phosphate cathode material Na0.5 Li 0.5 FePO 4 The XRD diffraction results are as follows Figure 1 As shown;
[0053] (3) Weigh the Na obtained in step (2) at a mass ratio of 90:7:3 0.5 Li 0.5 FePO 4 The positive electrode material, conductive carbon black and PVDF were added into NMP solvent at a solid-liquid mass ratio of 1:1 and mixed to obtain positive electrode slurry. The positive electrode slurry was evenly coated on aluminum foil with a loading of 30 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled by a roller press, and cut and shaped to obtain a positive electrode sheet;
[0054] (4) Weigh hard carbon and PVDF in a mass ratio of 94:6 and stir to mix evenly to obtain a negative electrode slurry, and evenly coat the negative electrode slurry on copper foil with a loading of 8 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled on a roller press, and cut and shaped to obtain a hard carbon negative electrode sheet;
[0055] (5) The positive electrode sheet, the separator (PP / PE / PP composite film) prepared in step (3), and the negative electrode sheet prepared in step (4) are stacked in sequence, wound, and loaded into a 18650 battery shell, and an electrolyte (1 mol / L NaPF 6 and 1 mol / L LiPF 6 As the solute, EC and DMC with a mass ratio of 1:1 as the solvent), sealed and welded, and assembled into a 18650 lithium-sodium battery.
[0056] Example 2
[0057] This embodiment provides a method for preparing a lithium sodium dual-ion battery, and the specific steps are as follows:
[0058] (1) Weigh 3 mol Li 2 CO 3 、10.0mol FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 220℃, the outlet temperature was 120℃, N 2 The first precursor was spray-dried in a nitrogen atmosphere to obtain a first precursor, and the first precursor was sintered at 700° C. for 12 h in a nitrogen atmosphere to obtain a lithium-deficient first sintered product Li 0.6 FePO 4 ;
[0059] (2) 2 mol of sodium oxalate and 10 mol of the calcined product Li prepared in step (1) were added.0.6 FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 220℃, the outlet temperature was 120℃, N 2 The second precursor was spray-dried in a nitrogen atmosphere to obtain a second precursor, and the second precursor was sintered at 700 ° C for 12 h in a nitrogen atmosphere to obtain a lithium-sodium dual ion deintercalation phosphate positive electrode material Na 0.4 Li 0.6 FePO 4 ;
[0060] (3) Weigh the Na obtained in step (2) at a mass ratio of 90:7:3 0.4 Li 0.6 FePO 4 The positive electrode material, conductive carbon black and PVDF were added into NMP solvent at a solid-liquid mass ratio of 1:1 and mixed to obtain positive electrode slurry. The positive electrode slurry was evenly coated on aluminum foil with a loading of 40 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled by a roller press, and cut and shaped to obtain a positive electrode sheet;
[0061] (4) Weigh hard carbon and PVDF in a mass ratio of 94:6 and stir to mix evenly to obtain a negative electrode slurry, and evenly coat the negative electrode slurry on copper foil with a loading of 10 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled on a roller press, and cut and shaped to obtain a hard carbon negative electrode sheet;
[0062] (5) The positive electrode sheet, the separator (PP / PE / PP composite film) prepared in step (3), and the negative electrode sheet prepared in step (4) are stacked in sequence, wound, and loaded into a 18650 battery shell, and an electrolyte (1 mol / L NaPF 6 and 1 mol / L LiPF 6 As the solute, EC and DMC with a mass ratio of 1:1 as the solvent), sealed and welded, and assembled into a 18650 lithium-sodium battery.
[0063] Example 3
[0064] This embodiment provides a method for preparing a lithium-sodium dual-ion battery, and the specific steps are as follows:
[0065] (1) Weigh 2.5 mol Li 2 CO 3 、10.0mol FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 180℃, the outlet temperature was 100℃, N 2The first precursor was spray-dried in a nitrogen atmosphere to obtain a first precursor, and the first precursor was sintered at 600° C. for 8 h in a nitrogen atmosphere to obtain a lithium-deficient first sintered product Li 0.5 FePO 4 ;
[0066] (2) 5 mol of sodium gluconate and 10 mol of the calcined product Li prepared in step (1) 0.5 FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 180℃, the outlet temperature was 100℃, N 2 The second precursor was spray-dried in a nitrogen atmosphere to obtain a second precursor, and the second precursor was sintered at 600 ° C for 8 h in a nitrogen atmosphere to obtain a lithium-sodium dual ion deintercalation phosphate positive electrode material Na 0.5 Li 0.5 FePO 4 ;
[0067] (3) Weigh the Na obtained in step (2) at a mass ratio of 90:7:3 0.5 Li 0.5 FePO 4 The positive electrode material, conductive carbon black and PVDF were added into NMP solvent at a solid-liquid mass ratio of 1:1 and mixed to obtain positive electrode slurry. The positive electrode slurry was evenly coated on aluminum foil with a loading of 30 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled by a roller press, and cut and shaped to obtain a positive electrode sheet;
[0068] (4) Weigh hard carbon and PVDF in a mass ratio of 94:6 and stir to mix evenly to obtain a negative electrode slurry, and evenly coat the negative electrode slurry on copper foil with a loading of 8 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled on a roller press, and cut and shaped to obtain a hard carbon negative electrode sheet;
[0069] (5) The positive electrode sheet, the separator (PP / PE / PP composite film) prepared in step (3), and the negative electrode sheet prepared in step (4) are stacked in sequence, wound, and loaded into a 18650 battery shell, and an electrolyte (1 mol / L NaPF 6 and 1 mol / L LiPF 6 As the solute, EC and DMC with a mass ratio of 1:1 as the solvent), sealed and welded, and assembled into a 18650 lithium-sodium battery.
[0070] Example 4
[0071] This embodiment provides a method for preparing a lithium-sodium dual-ion battery, and the specific steps are as follows:
[0072] (1) Weigh 4.0 mol Li 2 CO 3 、10.0mol FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 200℃, the outlet temperature was 110℃, N 2 The first precursor was spray-dried in a nitrogen atmosphere to obtain a first precursor, and the first precursor was sintered at 650° C. for 10 h in a nitrogen atmosphere to obtain a lithium-deficient first sintered product Li 0.8 FePO 4 ;
[0073] (2) 2 mol of sodium gluconate and 10 mol of the calcined product Li prepared in step (1) 0.8 FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 200℃, the outlet temperature was 110℃, N 2 The second precursor was spray-dried in a nitrogen atmosphere to obtain a second precursor, and the second precursor was sintered at 650° C. for 10 h in a nitrogen atmosphere to obtain a lithium-sodium dual ion deintercalation phosphate positive electrode material Na 0.2 Li 0.8 FePO 4 The prepared lithium sodium dual ion deintercalation phosphate cathode material Na 0.2 Li 0.8 FePO 4 The XRD diffraction results are as follows Figure 1 As shown;
[0074] (3) Weigh the Na obtained in step (2) at a mass ratio of 90:7:3 0.2 Li 0.8 FePO 4 The positive electrode material, conductive carbon black and PVDF were added into NMP solvent at a solid-liquid mass ratio of 1:1 and mixed to obtain positive electrode slurry. The positive electrode slurry was evenly coated on aluminum foil with a loading of 30 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled by a roller press, and cut and shaped to obtain a positive electrode sheet;
[0075] (4) Weigh hard carbon and PVDF in a mass ratio of 94:6 and stir to mix evenly to obtain a negative electrode slurry, and evenly coat the negative electrode slurry on copper foil with a loading of 8 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled on a roller press, and cut and shaped to obtain a hard carbon negative electrode sheet;
[0076] (5) The positive electrode sheet, the separator (PP / PE / PP composite film) prepared in step (3), and the negative electrode sheet prepared in step (4) are stacked in sequence, wound, and loaded into a 18650 battery shell, and an electrolyte (1 mol / L NaPF 6 and 1 mol / L LiPF 6 As the solute, EC and DMC with a mass ratio of 1:1 as the solvent), sealed and welded, and assembled into a 18650 lithium-sodium battery.
[0077] Comparative Example 1
[0078] This comparative example provides a method for preparing a lithium-sodium dual-ion battery, and the specific steps are as follows:
[0079] (1) Weigh 1 mol Li 2 CO 3 、10.0mol FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 200℃, the outlet temperature was 110℃, N 2 The first precursor was spray-dried in a nitrogen atmosphere to obtain a first precursor, and the first precursor was sintered at 650° C. for 10 h in a nitrogen atmosphere to obtain a lithium-deficient first sintered product Li 0.2 FePO 4 ;
[0080] (2) 8 mol of sodium gluconate and 10 mol of the calcined product Li prepared in step (1) were added. 0.2 FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 200℃, the outlet temperature was 110℃, N 2 The second precursor was spray-dried in a nitrogen atmosphere to obtain a second precursor, and the second precursor was sintered at 650° C. for 10 h in a nitrogen atmosphere to obtain a lithium-sodium dual ion deintercalation phosphate positive electrode material Na 0.8 Li 0.2 FePO 4 ;
[0081] (3) Weigh the Na obtained in step (2) at a mass ratio of 90:7:3 0.8 Li 0.2 FePO 4 The positive electrode material, conductive carbon black and PVDF were added into NMP solvent at a solid-liquid mass ratio of 1:1 and mixed to obtain positive electrode slurry. The positive electrode slurry was evenly coated on aluminum foil with a loading of 30 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled by a roller press, and cut and shaped to obtain a positive electrode sheet;
[0082] (4) Weigh hard carbon and PVDF in a mass ratio of 94:6 and stir to mix evenly to obtain a negative electrode slurry, and evenly coat the negative electrode slurry on copper foil with a loading of 8 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled on a roller press, and cut and shaped to obtain a hard carbon negative electrode sheet;
[0083] (5) The positive electrode sheet, the separator (PP / PE / PP composite film) prepared in step (3), and the negative electrode sheet prepared in step (4) are stacked in sequence, wound, and loaded into a 18650 battery shell, and an electrolyte (1 mol / L NaPF 6 and 1 mol / L LiPF 6 As the solute, EC and DMC with a mass ratio of 1:1 as the solvent), sealed and welded, and assembled into a 18650 lithium-sodium battery.
[0084] Comparative Example 2
[0085] This comparative example provides a method for preparing a lithium-sodium dual-ion battery, and the specific steps are as follows:
[0086] (1) Weigh 2.5 mol Li 2 CO 3 、10.0mol FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 200℃, the outlet temperature was 110℃, N 2 The first precursor was spray-dried in a nitrogen atmosphere to obtain a first precursor, and the first precursor was sintered at 650° C. for 10 h in a nitrogen atmosphere to obtain a lithium-deficient first sintered product Li 0.5 FePO 4 ;
[0087] (2) 5 mol of sodium gluconate and 10 mol of the calcined product Li prepared in step (1) 0.5 FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 200℃, the outlet temperature was 110℃, N 2 The second precursor was spray-dried in a nitrogen atmosphere to obtain a second precursor, and the second precursor was sintered at 650° C. for 10 h in a nitrogen atmosphere to obtain a lithium-sodium dual ion deintercalation phosphate positive electrode material Na 0.5 Li 0.5 FePO 4 ;
[0088] (3) Weigh the Na obtained in step (2) at a mass ratio of 90:7:3 0.5 Li 0.5 FePO 4The positive electrode material, conductive carbon black and PVDF were added into NMP solvent at a solid-liquid mass ratio of 1:1 and mixed to obtain positive electrode slurry. The positive electrode slurry was evenly coated on aluminum foil with a loading of 30 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled by a roller press, and cut and shaped to obtain a positive electrode sheet;
[0089] (4) Weigh soft carbon and PVDF in a mass ratio of 94:6 and stir to mix evenly to obtain a negative electrode slurry, and evenly coat the negative electrode slurry on copper foil with a loading of 8 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled on a roller press, and cut and shaped to obtain a soft carbon negative electrode sheet;
[0090] (5) The positive electrode sheet, the separator (PP / PE / PP composite film) prepared in step (3), and the negative electrode sheet prepared in step (4) are stacked in sequence, wound, and loaded into a 18650 battery shell, and an electrolyte (1 mol / L NaPF 6 and 1 mol / L LiPF 6 As the solute, EC and DMC with a mass ratio of 1:1 as the solvent), sealed and welded, and assembled into a 18650 lithium-sodium battery.
[0091] Comparative Example 3
[0092] This comparative example provides a method for preparing a lithium-sodium dual-ion battery, and the specific steps are as follows:
[0093] (1) Weigh 2.5 mol Na 2 CO 3 、10.0mol FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 200℃, the outlet temperature was 110℃, N 2 The first precursor was spray-dried in a nitrogen atmosphere to obtain a first precursor, and the first precursor was sintered at 650° C. for 10 h in a nitrogen atmosphere to obtain a sodium-deficient first sintered product Na 0.5 FePO 4 ;
[0094] (2) 5 mol of lithium gluconate and 10 mol of the calcined product Na 0.5 FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 200℃, the outlet temperature was 110℃, N 2 The second precursor was spray-dried in a nitrogen atmosphere to obtain a second precursor, and the second precursor was sintered at 650° C. for 10 h in a nitrogen atmosphere to obtain a lithium-sodium dual ion deintercalation phosphate positive electrode material Li 0.5 Na0.5 FePO 4 ;
[0095] (3) Weigh the Li obtained in step (2) at a mass ratio of 90:7:3 0.5 Na 0.5 FePO 4 The positive electrode material, conductive carbon black and PVDF were added into NMP solvent at a solid-liquid mass ratio of 1:1 and mixed to obtain positive electrode slurry. The positive electrode slurry was evenly coated on aluminum foil with a loading of 30 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled by a roller press, and cut and shaped to obtain a positive electrode sheet;
[0096] (4) Weigh hard carbon and PVDF in a mass ratio of 94:6 and stir to mix evenly to obtain a negative electrode slurry, and evenly coat the negative electrode slurry on copper foil with a loading of 8 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled on a roller press, and cut and shaped to obtain a hard carbon negative electrode sheet;
[0097] (5) The positive electrode sheet, the separator (PP / PE / PP composite film) prepared in step (3), and the negative electrode sheet prepared in step (4) are stacked in sequence, wound, and loaded into a 18650 battery shell, and an electrolyte (1 mol / L NaPF 6 and 1 mol / L LiPF 6 As the solute, EC and DMC with a mass ratio of 1:1 as the solvent), sealed and welded, and assembled into a 18650 lithium-sodium battery.
[0098] Comparative Example 4
[0099] This comparative example provides a method for preparing a lithium-sodium dual-ion battery, and the specific steps are as follows:
[0100] (1) Weigh 2.5 mol Li 2 CO 3 、10.0mol FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 200℃, the outlet temperature was 110℃, N 2 The first precursor was spray-dried in a nitrogen atmosphere to obtain a first precursor, and the first precursor was sintered at 650° C. for 10 h in a nitrogen atmosphere to obtain a lithium-deficient first sintered product Li 0.5 FePO 4 ;
[0101] (2) 5 mol of sodium gluconate and 10 mol of the calcined product Li prepared in step (1) 0.5 FePO 4, 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 200℃, the outlet temperature was 110℃, N 2 The second precursor was spray-dried in a nitrogen atmosphere to obtain a second precursor, and the second precursor was sintered at 650° C. for 10 h in a nitrogen atmosphere to obtain a lithium-sodium dual ion deintercalation phosphate positive electrode material Na 0.5 Li 0.5 FePO 4 ;
[0102] (3) Weigh the Na obtained in step (2) at a mass ratio of 90:7:3 0.5 Li 0.5 FePO 4 The positive electrode material, conductive carbon black and PVDF were added into NMP solvent at a solid-liquid mass ratio of 1:1 and mixed to obtain positive electrode slurry. The positive electrode slurry was evenly coated on aluminum foil with a loading of 30 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled by a roller press, and cut and shaped to obtain a positive electrode sheet;
[0103] (4) Weigh hard carbon and PVDF in a mass ratio of 94:6 and stir to mix evenly to obtain a negative electrode slurry, and evenly coat the negative electrode slurry on copper foil with a loading of 8 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled on a roller press, and cut and shaped to obtain a hard carbon negative electrode sheet;
[0104] (5) The positive electrode sheet, the separator (PP / PE / PP composite film) prepared in step (3), and the negative electrode sheet prepared in step (4) are stacked in sequence, wound, and loaded into a 18650 battery shell, and an electrolyte (1 mol / L NaPF 6 As the solute, EC and DMC with a mass ratio of 1:1 as the solvent), sealed and welded, and assembled into a 18650 lithium-sodium battery.
[0105] Comparative Example 5
[0106] This comparative example provides a method for preparing a lithium-sodium dual-ion battery, and the specific steps are as follows:
[0107] (1) Weigh 2.5 mol Li 2 CO 3 、10.0mol FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 200℃, the outlet temperature was 110℃, N 2 The first precursor was spray-dried in a nitrogen atmosphere to obtain a first precursor, and the first precursor was sintered at 650° C. for 10 h in a nitrogen atmosphere to obtain a lithium-deficient first sintered product Li 0.5FePO 4 ;
[0108] (2) 5 mol of sodium gluconate and 10 mol of the calcined product Li prepared in step (1) 0.5 FePO 4 , 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 200℃, the outlet temperature was 110℃, N 2 The second precursor was spray-dried in a nitrogen atmosphere to obtain a second precursor, and the second precursor was sintered at 650° C. for 10 h in a nitrogen atmosphere to obtain a lithium-sodium dual ion deintercalation phosphate positive electrode material Na 0.5 Li 0.5 FePO 4 ;
[0109] (3) Weigh the Na obtained in step (2) at a mass ratio of 90:7:3 0.5 Li 0.5 FePO 4 The positive electrode material, conductive carbon black and PVDF were added into NMP solvent at a solid-liquid mass ratio of 1:1 and mixed to obtain positive electrode slurry. The positive electrode slurry was evenly coated on aluminum foil with a loading of 30 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled by a roller press, and cut and shaped to obtain a positive electrode sheet;
[0110] (4) Weigh hard carbon and PVDF in a mass ratio of 94:6 and stir to mix evenly to obtain a negative electrode slurry, and evenly coat the negative electrode slurry on copper foil with a loading of 8 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled on a roller press, and cut and shaped to obtain a hard carbon negative electrode sheet;
[0111] (5) The positive electrode sheet, the separator (PP / PE / PP composite film) prepared in step (3), and the negative electrode sheet prepared in step (4) are stacked in sequence, wound, and loaded into a 18650 battery shell, and an electrolyte (1 mol / L LiPF 6 As the solute, EC and DMC with a mass ratio of 1:1 as the solvent), sealed and welded, and assembled into a 18650 lithium-sodium battery.
[0112] Comparative Example 6
[0113] This comparative example provides a method for preparing a lithium-sodium dual-ion battery, and the specific steps are as follows:
[0114] (1) Weigh 2.5 mol Li 2 CO 3 , 5 mol sodium gluconate, 10.0 mol FePO 4, 500g pure water were ball-milled and mixed evenly, and then pumped into the spray drying equipment with a pump. The inlet temperature was 200℃, the outlet temperature was 110℃, N 2 The first precursor was spray-dried in a nitrogen atmosphere to obtain a first precursor, and the first precursor was sintered at 650° C. for 10 h in a nitrogen atmosphere to obtain a lithium-sodium dual ion deintercalation phosphate positive electrode material Na 0.5 Li 0.5 FePO 4 ;
[0115] (2) Weigh the Na obtained in step (1) at a mass ratio of 90:7:3 0.5 Li 0.5 FePO 4 The positive electrode material, conductive carbon black and PVDF were added into NMP solvent at a solid-liquid mass ratio of 1:1 and mixed to obtain positive electrode slurry. The positive electrode slurry was evenly coated on aluminum foil with a loading of 30 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled by a roller press, and cut and shaped to obtain a positive electrode sheet;
[0116] (3) Weigh hard carbon and PVDF in a mass ratio of 94:6 and stir to mix evenly to obtain a negative electrode slurry, and evenly coat the negative electrode slurry on copper foil with a loading of 8 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled on a roller press, and cut and shaped to obtain a hard carbon negative electrode sheet;
[0117] (4) The positive electrode sheet, the separator (PP / PE / PP composite film) prepared in step (2), and the negative electrode sheet prepared in step (3) are stacked in sequence, wound, and loaded into a 18650 battery shell, and an electrolyte (1 mol / L NaPF 6 and 1 mol / L LiPF 6 As the solute, EC and DMC with a mass ratio of 1:1 as the solvent), sealed and welded, and assembled into a 18650 lithium-sodium battery.
[0118] Comparative Example 7
[0119] This embodiment provides a method for preparing a lithium sodium dual-ion battery, and the specific steps are as follows:
[0120] (1) Weigh 2.5 mol Li 2 CO 3 、10.0mol Ni 1 / 3 Co 1 / 3 Mn 1 / 3 (OH) 2 After ball milling and mixing, the mixture was sintered at 850°C (the conventional temperature required for sintering NCM111 material) for 10 h in air atmosphere to obtain a lithium-deficient sintered product Li0.5 Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 ;
[0121] (2) 5 mol of sodium gluconate and 10 mol of the calcined product Li prepared in step (1) 0.5 Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 After ball milling and mixing, the mixture was sintered at 850 °C for 10 h in air atmosphere to obtain the lithium-sodium dual ion deintercalation ternary cathode material Na 0.5 Li 0.5 Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 ;
[0122] (3) Weigh the Na obtained in step (2) at a mass ratio of 90:7:3 0.5 Li 0.5 Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 The positive electrode material, conductive carbon black and PVDF were added into NMP solvent at a solid-liquid mass ratio of 1:1 and mixed to obtain positive electrode slurry. The positive electrode slurry was evenly coated on aluminum foil with a loading of 30 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled by a roller press, and cut and shaped to obtain a positive electrode sheet;
[0123] (4) Weigh hard carbon and PVDF in a mass ratio of 94:6 and stir to mix evenly to obtain a negative electrode slurry, and evenly coat the negative electrode slurry on copper foil with a loading of 8 mg / cm 2 , then placed in a vacuum oven at 105°C for 1 hour, rolled on a roller press, and cut and shaped to obtain a hard carbon negative electrode sheet;
[0124] (5) The positive electrode sheet, the separator (PP / PE / PP composite film) prepared in step (3), and the negative electrode sheet prepared in step (4) are stacked in sequence, wound, and loaded into a 18650 battery shell, and an electrolyte (1 mol / L NaPF 6 and 1 mol / L LiPF 6 As the solute, EC and DMC with a mass ratio of 1:1 as the solvent), sealed and welded, and assembled into a 18650 lithium-sodium battery.
[0125] Test Case
[0126] The batteries prepared in the embodiments and comparative examples were placed in a blue-electric test system for electrical performance testing. Among them, the charge / discharge specific capacity test: at room temperature, the battery was charged to 4.2V at a constant current of 0.1C, then discharged to 2.0V at a discharge rate of 0.1C, and then charged and discharged at 0.5C and 1C; the cycle test: 200 cycles of charge and discharge tests were performed between 2.0-4.2V at a rate of 0.1C / 0.1C to characterize the capacity retention rate of the battery after 200 cycles; the statistical results of the buckling performance of the embodiments and comparative examples are shown in Tables 1 and 2 below, and the cycle curves of the embodiments and comparative examples are shown in Tables 1 and 2 below. Figure 2 shown.
[0127] Table 1
[0128]
[0129]
[0130] Table 2
[0131]
[0132] According to the above test results, the specific capacity of the batteries prepared in Examples 1-4 at a charging rate of 0.1C is all above 162.3 mAh / g, and the 200 cycle retention rates are all above 93%, while the comprehensive performance (specific capacity and cycle performance) of the batteries prepared in Comparative Examples 1-7 is worse than that of Examples 1-4 of the present invention.
[0133] In Table 2, compared with Example 1 using the lithium-sodium integrated core-shell positive electrode material of the present invention with Na as the outer layer and Li as the inner core, Comparative Examples 1, 3, 6, and 7 all cause varying degrees of battery performance degradation due to the different positive electrode materials used. In this regard, the present invention believes that: in comparative example 1, there is too little Li in the core of the positive electrode material, and the performance of the positive electrode material is mainly determined by the properties of the shell material, which hinders the performance of the lithium electrical properties and completely replaces the properties of the sodium electrical properties, thereby reducing the battery performance; in comparative example 3, because the shell is Li, and the lithium ion diffusion path is narrow, the core Na ions cannot be deintercalated into the lattice, thereby reducing the battery performance; in comparative example 6, because lithium and sodium are added at the same time, the ion path is chaotic, there is a lithium ion path on the surface of the material, and the sodium ion radius is large and cannot pass through, resulting in the obstruction of sodium ion deintercalation, the specific capacity is reduced, and the cycle performance is deteriorated; in comparative example 7, because the NCM ternary material is a two-dimensional deintercalation path, some lithium ions cannot be deintercalated into the interior of the particles, and they are translated to the surface of the material along the two-dimensional plane, occupying the sodium position, and the ion path formed during the deintercalation process is narrow, which hinders the deintercalation of sodium ions. Therefore, after the ternary material is designed as a lithium core sodium shell structure material, after charging and discharging and deintercalation once, due to the influence of the two-dimensional deintercalation path, Li / Na mixed occupation occurs, affecting the next capacity, accompanied by reduced cycle performance.
[0134] As for the reasons why the battery performance of Comparative Examples 2, 4, and 5 deteriorates, the present invention believes that: in Comparative Example 2, the spacing between the soft carbon layers is small, and the sodium ions cannot be smoothly deintercalated, which leads to reduced battery performance; in Comparative Example 4, there is only sodium hexafluorophosphate in the electrolyte, and the Li ions enter the electrolyte after deintercalation, and the solvation ability is greatly weakened, which leads to reduced battery performance; in Comparative Example 5, there is only lithium hexafluorophosphate in the electrolyte, and the Na ions enter the electrolyte after deintercalation, and the solvation ability is greatly weakened, which leads to reduced battery performance.
[0135] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A lithium sodium dual ion deintercalation phosphate positive electrode material, characterized in that: It includes a lithium-sodium integrated core-shell cathode material with Na as the outer layer and Li as the inner core, and its chemical formula is Na y Li x FePO4, 0.1<y≤0.5, 0.5≤x<0.9, x+y=1.
2. The method for preparing the lithium sodium dual ion deintercalation phosphate positive electrode material according to claim 1, characterized in that: include: The lithium source, iron phosphate and solvent are ground and mixed and dried to obtain a first precursor, and the first precursor is placed in an inert atmosphere for sintering to obtain a sintered product Li x FePO4; The sodium source and the calcined product Li x The FePO4 and solvent are ground and mixed and dried to obtain a second precursor, and the second precursor is placed in an inert atmosphere for sintering to obtain a lithium sodium dual ion deintercalation phosphate positive electrode material Na y Li x FePO4.
3. The preparation method according to claim 2, characterized in that: The lithium source is Li2CO3; And / or, the sodium source is at least one of sodium gluconate, sodium dodecylbenzene sulfonate and sodium oxalate; And / or, the solvent is water.
4. The preparation method according to claim 2 or 3, characterized in that: The sintering temperature is 600-700°C; And / or, the sintering treatment time is 8-12h; And / or, the grinding is ball milling and / or sand milling; And / or, the drying process is spray drying.
5. The preparation method according to claim 4, characterized in that: The inlet temperature of the spray drying is 180-220°C; And / or, the outlet temperature of the spray drying is 100-120°C; And / or, the spray drying atmosphere is an inert atmosphere.
6. A lithium sodium dual ion battery, characterized in that: include: A positive electrode sheet, a hard carbon negative electrode sheet, a separator and an electrolyte containing sodium salt and lithium salt comprising the lithium-sodium dual ion deintercalation phosphate positive electrode material according to claim 1 or the lithium-sodium dual ion deintercalation phosphate positive electrode material prepared by the preparation method of the lithium-sodium dual ion deintercalation phosphate positive electrode material according to any one of claims 2 to 5.
7. The method for preparing a lithium sodium dual ion battery according to claim 6, characterized in that: include: The positive electrode sheet containing the lithium-sodium dual-ion deintercalation phosphate positive electrode material, the separator, and the hard carbon negative electrode sheet are stacked in sequence, wound and loaded into the battery shell, and the electrolyte containing the sodium salt and the lithium salt is injected, and the battery shell is sealed and welded.
8. The preparation method according to claim 7, characterized in that: The preparation process of the positive electrode sheet comprises: weighing a lithium sodium dual ion deintercalation phosphate positive electrode material, conductive carbon black and a binder, adding the weighed materials into a solvent and mixing them to obtain a positive electrode slurry, uniformly coating the positive electrode slurry on an aluminum foil, drying, rolling and cutting the positive electrode sheet; And / or, the preparation process of the hard carbon negative electrode sheet includes: weighing hard carbon and a binder and mixing them to obtain a negative electrode slurry, uniformly coating the negative electrode slurry on a copper foil, drying, rolling, and cutting to obtain a hard carbon negative electrode sheet.
9. The preparation method according to claim 8, characterized in that: The mass ratio of the lithium sodium dual ion deintercalation phosphate positive electrode material, the conductive carbon black and the binder is 90:7:3; And / or, the mass ratio of the total mass of the lithium sodium dual ion deintercalation phosphate positive electrode material, the conductive carbon black and the binder to the mass ratio of the solvent is 1:1; And / or, the positive electrode slurry loading on the aluminum foil is 30-40 mg / cm 2 ; and / or, the mass ratio of the hard carbon to the binder is 94:6; And / or, the negative electrode slurry loading on the copper foil is 8-10 mg / cm 2 ; And / or, the solvent is N-methylpyrrolidone; And / or, the binder is polyvinylidene fluoride.
10. The preparation method according to any one of claims 7 to 9, characterized in that: The diaphragm is a PP / PE / PP composite film; And / or, the lithium salt in the electrolyte is LiPF6; And / or, the sodium salt in the electrolyte is NaPF6; and / or, the concentration of lithium salt in the electrolyte is 0.5-1.0 mol / L, preferably 1.0 mol / L; and / or, the concentration of sodium salt in the electrolyte is 0.5-1.0 mol / L, preferably 1.0 mol / L; And / or, the solvent in the electrolyte is ethylene carbonate and / or dimethyl carbonate.