Binder for positive electrode of lithium-sulfur battery as well as preparation method and application of binder
By using composite water-based binders prepared with sodium carboxymethylcellulose and acrylic modified chitosan derivatives, the low conductivity and volume expansion of sulfur in lithium-sulfur batteries are solved, and better cycling performance and flexibility are achieved , extends the battery life.
Patent Information
- Application Number
- CN202410948843.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-12-03
AI Technical Summary
Due to the low conductivity and volume expansion of sulfur, lithium-sulfur batteries have impeded electron/ion transfer, slow redox kinetics and shuttle effects, which affect their charge and discharge capacity and cycle stability. Existing binders such as PVDF are harmful to the human body. And the inhibitory ability is limited.
Using sodium carboxymethylcellulose and acrylic modified chitosan derivatives as binders, prepared by magnetic stirring, to form a non-toxic, natural green composite water-based binder, used for the positive electrode of lithium sulfur battery, inhibiting multiple The shuttle effect and volume expansion of sulfides improve cycling performance.
The binder is non-toxic and harmless, easy to prepare, has good mechanical properties and pulping properties, can effectively suppress the shuttle effect, improve the circulation performance and flexibility of lithium-sulfur batteries, and extend the battery service life.
Smart Images

Figure CN119069703A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a binder, in particular to a binder for a positive electrode of a lithium-sulfur battery, and also to a preparation method of the binder and application of the binder in a positive electrode sheet of a lithium-sulfur battery. Background Art
[0002] As a next-generation battery technology that is expected to replace lithium-ion batteries, lithium-sulfur batteries have attracted widespread attention and in-depth research in the military and civilian fields. Compared with the current commercial lithium-ion batteries, they have the following two advantages: 1. High energy density (2600Wh / kg). Its energy density is about 3 to 5 times the specific energy of current commercial lithium batteries. After integrating the battery cells, its actual energy density is still as high as 300 to 900Wh / kg, which is still much higher than the current lithium-ion power battery level of 100 to 300Wh / kg; 2. Low cost advantage. Sulfur, the raw material of lithium-sulfur batteries, is an abundant and inexpensive element with environmentally friendly advantages. my country has abundant and independently controllable content, and does not contain rare metals such as cobalt, so it has outstanding cost advantages.
[0003] However, although lithium-sulfur batteries have great application potential, there are still some technical challenges that need to be addressed.
[0004] First, the electrical conductivity of sulfur at room temperature is very low (5×10 -3 S / cm), and the conductivity of its discharge final product, lithium sulfide (Li2S), is also very low (1×10 -13 S / cm). This low conductivity property will seriously hinder the electron / ion transfer, resulting in low sulfur utilization and slow redox kinetics, thus affecting the charge and discharge capacity and rate performance of lithium-sulfur batteries; the density of sulfur is about 2.07g / cm 3 The density of lithium sulfide (Li2S) is about 1.66 g / cm 3 This will cause the volume of lithium sulfide generated during the charge and discharge process of the lithium-sulfur battery to be larger than the total volume of the original sulfur and lithium. Therefore, during the charge and discharge process of the battery, a volume expansion / contraction of nearly 80% will occur.
[0005] Secondly, lithium-sulfur batteries have a notorious problem, which is the troublesome "shuttle effect". This process consumes lithium ions in the electrolyte, resulting in loss of active materials, reduced Coulombic efficiency (CE), rapid capacity decay, and severe corrosion of the lithium negative electrode, thus affecting the cycle stability and service life of the battery. These problems have greatly hindered its commercial development.
[0006] Since the binder is an important component of the positive electrode of lithium-sulfur batteries, a small amount can greatly affect the structure and morphology of the positive electrode, and can fix polysulfides, inhibit volume expansion, and can bind active material particles and provide mechanical and chemical stability. Therefore, the performance of lithium-sulfur battery positive electrode materials can be improved starting from the binder. The binders currently used, such as polyvinylidene fluoride (PVDF) and carboxymethyl cellulose (CMC), have great limitations in aspects such as chemical adsorption of lithium polysulfide, inhibition of the shuttle effect of polysulfides, and relief of volume expansion. In addition, N-methylpyrrolidone (NMP), a commonly used dispersant for PVDF, is harmful to the human body. In order to solve these limitations, it is necessary to develop some new binders. Summary of the invention
[0007] The first technical problem to be solved by the present invention is to provide a binder for the positive electrode of a lithium-sulfur battery with high electrochemical performance in view of the above-mentioned technical status.
[0008] The second technical problem to be solved by the present invention is to provide a method for preparing a binder with high electrochemical performance for the positive electrode of a lithium-sulfur battery in view of the above-mentioned technical status.
[0009] The third technical problem to be solved by the present invention is to provide a binder for lithium-sulfur battery positive electrode with high electrochemical performance for use in lithium-sulfur battery positive electrode plates in response to the above-mentioned technical status.
[0010] The technical solution adopted by the present invention to solve the above-mentioned first technical problem is: a binder for the positive electrode of a lithium-sulfur battery, characterized in that it includes the following components: sodium carboxymethyl cellulose, an acrylic acid-modified chitosan derivative and deionized water, wherein the mass ratio of the total mass of the solid matter to the mass of the deionized water is 1:20-40; the mass ratio of the sodium carboxymethyl cellulose to the acrylic acid-modified chitosan derivative is 0-2:1-2.
[0011] Preferably, the aqueous solution of the acrylic acid-modified chitosan derivative has a solid content of 14.8-15.2% and a viscosity of ≥3000 cps at 25°C.
[0012] The technical solution adopted by the present invention to solve the above second technical problem is: a method for preparing a binder for a positive electrode of a lithium-sulfur battery, characterized in that it comprises the following steps:
[0013] ① Weigh sodium carboxymethyl cellulose and acrylic acid-modified chitosan derivative, mix, and add deionized water;
[0014] ② Stirring on a magnetic stirrer at a stirring speed of 400-1500 r / min, a stirring temperature of 30-70° C., and a stirring time of 6-24 hours to obtain a binder.
[0015] Preferably, the stirring speed of the magnetic stirrer is 400-1500 r / min.
[0016] Preferably, the stirring temperature of the magnetic stirrer is 30-70°C.
[0017] Preferably, the stirring time of the magnetic stirrer is 6 to 24 hours.
[0018] The technical solution adopted by the present invention to solve the third technical problem is: a positive electrode plate for a lithium-sulfur battery, characterized in that the positive electrode plate for a lithium-sulfur battery is prepared by the following steps:
[0019] The positive electrode active material, sulfur-carrying material, conductive agent and binder are mixed evenly, stirred to form slurry, and then the slurry is coated on aluminum foil, and vacuum dried to obtain the positive electrode sheet of the lithium-sulfur battery.
[0020] Preferably, the weight ratio of the positive electrode active material, the sulfur-carrying material, the conductive agent and the binder is 7:1:1:1.
[0021] Preferably, the positive electrode active material is sublimated sulfur. The sulfur-carrying material is carbon nanotubes.
[0022] Compared with the prior art, the advantages of the present invention are: the binder of the present invention is non-toxic, harmless, natural and green; the raw materials are easily available and easy to prepare; it has good mechanical properties, which is beneficial to buffering the volume expansion of the electrode; it has good pulping performance; the acrylic acid-modified chitosan derivative (NV-1A) contains polar carboxyl and hydroxyl groups, which can chemically capture and adsorb polysulfides, inhibit the shuttle effect of polysulfides, and improve the cycle performance of lithium-sulfur batteries.
[0023] The sulfur positive electrode prepared using NV-1A as a binder is relatively less flexible. Considering that different types of batteries, such as soft-pack batteries and cylindrical batteries, may have different requirements for positive electrode flexibility, the flexibility of the electrode can be improved after mixing sodium carboxymethyl cellulose (CMC) as a binder. The higher the proportion of CMC, the higher the electrode flexibility. However, as the content of NV-1A decreases, the ability to inhibit the shuttle effect will also decrease. Compared with chitosan, acrylic acid-modified chitosan derivatives (NV-1A) have higher viscosity and can be used as a binder alone without having to be used with other binders.
[0024] Instruction Manual
[0025] Figure 1 It is a coordinate diagram of the cycle performance of the lithium-sulfur battery positive electrode sheets prepared in Examples 5, 6, 7, 8 and Comparative Example 1 when applied to Li-S batteries. DETAILED DESCRIPTION
[0026] The present invention is further described in detail below in conjunction with embodiments and drawings.
[0027] Example 1, a lithium-sulfur battery positive electrode composite aqueous binder, the binder is composed of sodium carboxymethyl cellulose (CMC), acrylic acid modified chitosan derivative (NV-1A) and deionized water. The specific preparation steps are as follows:
[0028] Weigh according to the mass ratio of NV-1A:CMC=1:0, add appropriate amount of deionized water, stir on a magnetic stirrer at a stirring speed of 1500r / min, stirring temperature at 30°C, stirring time for 24 hours, and obtain a composite sugar-based binder.
[0029] Example 2, a lithium-sulfur battery positive electrode composite aqueous binder, the binder is composed of sodium carboxymethyl cellulose (CMC), acrylic acid modified chitosan derivative (NV-1A) and deionized water. The specific preparation steps are as follows:
[0030] Weigh according to the mass ratio of NV-1A:CMC=2:1, add appropriate amount of deionized water, stir on a magnetic stirrer at a stirring speed of 1500r / min, stirring temperature at 30°C, stirring time for 24 hours, and obtain a composite sugar-based binder.
[0031] Example 3, a lithium-sulfur battery positive electrode composite aqueous binder, the binder is composed of sodium carboxymethyl cellulose (CMC), acrylic acid modified chitosan derivative (NV-1A) and deionized water. The specific preparation steps are as follows:
[0032] Weigh according to the mass ratio of NV-1A:CMC=1:1, add appropriate amount of deionized water, stir on a magnetic stirrer at a stirring speed of 1500r / min, stirring temperature at 30°C, stirring time for 24 hours, and obtain a composite sugar-based binder.
[0033] Example 4, a lithium-sulfur battery positive electrode composite aqueous binder, the binder is composed of sodium carboxymethyl cellulose (CMC), acrylic acid modified chitosan derivative (NV-1A) and deionized water. The specific preparation steps are as follows:
[0034] Weigh according to the mass ratio of NV-1A:CMC=1:2, add appropriate amount of deionized water, stir on a magnetic stirrer at a stirring speed of 1500r / min, stirring temperature at 30°C, stirring time for 24 hours, and obtain a composite sugar-based binder.
[0035] Embodiment 5, a positive electrode plate of a lithium-sulfur battery, the positive electrode plate comprising a positive electrode active material, a sulfur-carrying material, a conductive agent and a binder, the ratio of which is positive electrode active material: sulfur-carrying material: conductive agent: binder = 7:1:1:1. The binder is the composite sugar-based binder for the positive electrode of the lithium-sulfur battery in Embodiment 1. The positive electrode active material and the sulfur-carrying material are kept at 160°C for 24 hours in an Ar atmosphere, then uniformly ground with the conductive agent for 60 minutes, dry mixed at 1000r / min on a magnetic stirrer for 24 hours, the binder described in Embodiment 1 is added to form a slurry, and the slurry is coated on an aluminum foil, and vacuum dried at 60°C for 12 hours to obtain a positive electrode plate for a lithium-sulfur battery.
[0036] Embodiment 6, a positive electrode plate of a lithium-sulfur battery, the positive electrode plate comprising a positive electrode active material, a sulfur-carrying material, a conductive agent and a binder, the ratio of which is positive electrode active material: sulfur-carrying material: conductive agent: binder = 7:1:1:1. The binder is the composite sugar-based binder for the positive electrode of the lithium-sulfur battery in Embodiment 2. The positive electrode active material and the sulfur-carrying material are kept at 160°C for 24 hours in an Ar atmosphere, then uniformly ground with the conductive agent for 60 minutes, dry mixed at 1000r / min on a magnetic stirrer for 24 hours, the binder described in Embodiment 2 is added to form a slurry, and the slurry is coated on an aluminum foil, and vacuum dried at 60°C for 12 hours to obtain a positive electrode plate for a lithium-sulfur battery.
[0037] Embodiment 7, a positive electrode plate of a lithium-sulfur battery, the positive electrode plate comprising a positive electrode active material, a sulfur-carrying material, a conductive agent and a binder, the ratio of which is positive electrode active material: sulfur-carrying material: conductive agent: binder = 7:1:1:1. The binder is the composite sugar-based binder for the positive electrode of the lithium-sulfur battery in embodiment 3. The positive electrode active material and the sulfur-carrying material are kept at 160°C in an Ar atmosphere for 24 hours, then uniformly ground with the conductive agent for 60 minutes, dry mixed at 1000r / min on a magnetic stirrer for 24 hours, the binder described in embodiment 3 is added to form a slurry, and the slurry is coated on an aluminum foil, and vacuum dried at 60°C for 12 hours to obtain a positive electrode plate for a lithium-sulfur battery.
[0038] Embodiment 8, a positive electrode plate of a lithium-sulfur battery, the positive electrode plate comprising a positive electrode active material, a sulfur-carrying material, a conductive agent and a binder, the ratio of which is positive electrode active material: sulfur-carrying material: conductive agent: binder = 7:1:1:1. The binder is the composite sugar-based binder for the positive electrode of the lithium-sulfur battery in Embodiment 4. The positive electrode active material and the sulfur-carrying material are kept at 160°C in an Ar atmosphere for 24 hours, then uniformly ground with the conductive agent for 60 minutes, dry mixed at 1000r / min on a magnetic stirrer for 24 hours, the binder described in Embodiment 3 is added to form a slurry, and the slurry is coated on an aluminum foil, and vacuum dried at 60°C for 12 hours to obtain a positive electrode plate for a lithium-sulfur battery.
[0039] The acrylic acid-modified chitosan derivative in the above embodiment uses a water-based adhesive of model NV-1A produced by Zhejiang Zhongke Lide New Materials Co., Ltd.
[0040] Comparative Example 1, a positive electrode plate for a lithium-sulfur battery, the positive electrode plate comprising a positive electrode active material, a sulfur-carrying material, a conductive agent and a binder, the ratio of which is positive electrode active material: sulfur-carrying material: conductive agent: binder = 7:1:1:1. The binder is CMC. The positive electrode active material and the sulfur-carrying material are kept at 160°C for 24 hours in an Ar atmosphere, then uniformly ground with the conductive agent for 60 minutes, dry-mixed on a magnetic stirrer at 1000r / min for 24 hours, the binder described in Example 3 is added to form a slurry, and the slurry is coated on an aluminum foil, and vacuum dried at 60°C for 12 hours to obtain a positive electrode plate for a lithium-sulfur battery.
[0041] Performance test, compare the cycle performance of the lithium-sulfur battery positive electrode sheet prepared in Examples 5, 6, 7, 8 and Comparative Example 1 when applied to Li-S batteries. Figure 1 As shown, compared with the commercial CMC binder, the sulfur positive electrode prepared using the binder in Example 1 has better cycle performance. The initial discharge capacity of Example 5 is 740 mAh / g, and the discharge capacity remains at 605 mAh / g after 50 cycles, with a capacity retention rate of 81.7%. As the NV-1A content decreases, the capacity retention rate decreases accordingly. As shown in Comparative Example 1, the initial discharge capacity of the positive electrode prepared entirely using commercial CMC as the binder is 703 mAh / g, and the discharge capacity remains at 469 mAh / g after 50 cycles, with a capacity retention rate of only 66.7%.
Claims
1. A binder for a lithium-sulfur battery positive electrode, characterized in that The invention comprises the following components: sodium carboxymethyl cellulose, acrylic acid modified chitosan derivative and deionized water, wherein the mass ratio of the total mass of solid matter to the deionized water is 1:20-40; the mass ratio of sodium carboxymethyl cellulose to acrylic acid modified chitosan derivative is 0-2:1-2.
2. The binder for the positive electrode of a lithium-sulfur battery according to claim 1, characterized in that The solid content of the acrylic acid modified chitosan derivative aqueous solution is 14.8-15.2%, and the viscosity at 25°C is ≥3000cps.
3. A method for preparing the binder for the positive electrode of a lithium-sulfur battery according to claim 1, characterized in that The steps include: ① Weigh sodium carboxymethyl cellulose and acrylic acid-modified chitosan derivative, mix, and add deionized water; ② Stirring on a magnetic stirrer at a stirring speed of 400-1500 r / min, a stirring temperature of 30-70° C., and a stirring time of 6-24 hours to obtain a binder.
4. The preparation method according to claim 3, characterized in that The stirring speed of the magnetic stirrer is 400-1500 r / min.
5. The preparation method according to claim 3, characterized in that The stirring temperature of the magnetic stirrer is 30-70°C.
6. The preparation method according to claim 3, characterized in that The stirring time of the magnetic stirrer is 6 to 24 hours.
7. A positive electrode plate for a lithium-sulfur battery, characterized in that The positive electrode plate of the lithium-sulfur battery is prepared by the following steps: The positive electrode active material, the sulfur-carrying material, the conductive agent and the binder according to any one of claims 1 or 2 are uniformly mixed and stirred to form a slurry, and then the slurry is coated on an aluminum foil and vacuum dried to obtain a positive electrode sheet for a lithium-sulfur battery.
8. The positive electrode plate of a lithium-sulfur battery according to claim 7, characterized in that The weight ratio of the positive electrode active material, the sulfur-carrying material, the conductive agent and the binder is 7:1:1:
1.
9. The positive electrode plate of a lithium-sulfur battery according to claim 7, characterized in that The positive electrode active material is sublimated sulfur.
10. The positive electrode plate of a lithium-sulfur battery according to claim 7, characterized in that The sulfur-carrying material is carbon nanotube.