Nanocellulose / meta-aramid composite battery diaphragm material and preparation method thereof
Through the composite material of nanocellulose and metaaramid, the separator is prepared by phase conversion method, which solves the problems of low ionic conductivity and uneven pore size distribution of the existing separator, realizes high-performance separator materials, and improves battery safety and electrochemical properties, and simplify the process flow.
Patent Information
- Application Number
- CN202411203741.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing cellulose/aramid composite separators have problems such as low ionic conductivity, uneven pore size distribution and complex preparation process.
Using nanocellulose/meta-aramid composite battery separator, nanocellulose gel is dispersed ultrasonically through an ultrasonic cell crusher, combined with meta-aramid short fibers, and prepared by phase conversion method to regulate the pore structure and thickness of the separator to reduce Use organic solvents to simplify the process.
It realizes a separator material with adjustable pore structure, excellent thermal stability, high flame retardancy, good wetting and good electrochemical performance, improves the safety and electrochemical performance of the battery, simplifies the preparation process and reduces costs.
Smart Images

Figure CN119069951A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer materials and lithium / sodium ion batteries, and specifically relates to a nano cellulose / meta-aramid composite battery diaphragm material and a preparation method thereof. Background Art
[0002] Diaphragm materials are key components in lithium / sodium ion batteries. They not only physically separate the positive and negative electrodes of the battery to avoid short circuits, but also play the role of transporting ions and isolating electrons. At present, lithium / sodium battery separators are mainly divided into polyethylene terephthalate (PET) separators, meta-aramid (PMIA) separators, polyvinylidene fluoride (PVDF) separators, polyimide (PI) separators, polyacrylonitrile (PAN) separators, cellulose separators, polyolefin separators and glass fiber separators. At present, polyolefin separators have been commercialized, such as polyethylene (PE), polypropylene (PP) and PP-PE-PP composite separators, but their thermal stability and electrolyte wettability are poor, which seriously affects the safety and electrochemical performance of the battery. The high-cost glass fiber separator is usually 675μm thick, which reduces the overall volume energy density of the battery. The high-crystallinity PVDF separator has a hydrophobic surface, which causes a certain degree of ion transmission obstruction. The renewable cellulose separator has high electrolyte affinity and thermal decomposition temperature (240°C), but it is hygroscopic due to its strong hydrophilicity and difficult to control the pore size. The meta-aramid separator has high strength, high flame retardancy and excellent thermal stability, with a thermal decomposition temperature of up to 430°C, but its electrolyte affinity is poor and its ion transport performance is weak. The composite strategy of meta-aramid and cellulose can achieve a battery separator with high flame retardancy, excellent thermal stability, ion transport performance and good electrolyte wettability.
[0003] At present, the preparation methods of cellulose / aramid composite membranes mainly include electrospinning process, coating method, wet papermaking process, and phase inversion method. Zhang et al. mixed ZiF-8 particle / bacterial cellulose (BC) suspension dispersion and para-aramid fiber (ANFs) suspension dispersion, and then prepared a porous bacterial cellulose / aramid composite membrane by filtration, but the pore size distribution of the membrane was uneven, and it was very easy to agglomerate after the aramid concentration increased, which seriously affected the wettability of the composite membrane (Journal of Membrane Science 652 (2022) 120461). Liu et al. combined cellulose microfibrils (CNF) with meta-aramid / para-aramid fibers (PMIA / PPTA) and prepared a heat-resistant and highly wettable composite membrane through traditional heterogeneous papermaking process. However, the preparation process is very complicated (International Journal of Biological Macromolecules 225 (2023) 1476-1486). At the same time, the interfacial compatibility and dispersibility between aramid and cellulose are poor, resulting in uneven pore size distribution and low ionic conductivity of the composite membrane. Summary of the invention
[0004] In view of the problems of low ion conductivity, uneven pore size distribution and complicated preparation process in the current composite diaphragm of cellulose and aramid, one of the purposes of the present invention is to provide a nanocellulose / meta-aramid composite battery diaphragm material, which has the advantages of adjustable pore structure, excellent thermal stability, high flame retardancy, high wettability and good electrochemical performance. The second purpose of the present invention is to provide a method for preparing the above-mentioned diaphragm material, which is not only flexible and adjustable, but also can reduce the use of a large amount of organic solvents and has large-scale production capacity.
[0005] In order to achieve the above-mentioned purpose, the technical scheme of the present invention is as follows: a nanocellulose / meta-aramid composite battery separator material, wherein the nanocellulose of the separator material is uniformly dispersed in the porous network structure of the meta-aramid fiber, and the thickness is 9 to 30 μm.
[0006] A method for preparing a nanocellulose / meta-aramid composite battery separator material comprises the following steps:
[0007] (1) dispersing nanocellulose gel (CNC) in an organic solvent by ultrasonic cell crusher to obtain a nanocellulose solution;
[0008] (2) adding dried meta-aramid staple fibers (PMIA) to the nanocellulose solution obtained in step (1), then adding an appropriate amount of a solvent, heating and stirring under the protection of an inert gas to dissolve until the solution becomes clear and transparent, thereby obtaining a uniform casting solution;
[0009] (3) The casting liquid obtained in step (2) is scraped into a liquid film, placed in a coagulation bath, and gradient replacement is performed using water / organic solvents of different concentrations, and the operation is repeated until solidification into a film.
[0010] (4) repeatedly washing the cured film until the residual porogen and organic solvent are removed, and finally drying the film under vacuum or at normal pressure to obtain a nanocellulose / meta-aramid composite battery separator material.
[0011] Furthermore, in the step (1), the size of the nanocellulose gel is 100 to 200 nm; the organic solvent is one of N,N-dimethylacetamide (DMAc), dimethyl sulfoxide (DMSO), dimethylformamide (DMF), etc.; in the step (1), the concentration of the nanocellulose solution is 1wt% to 10wt%.
[0012] Furthermore, in the step (1), the ultrasonic power is 100 to 300 W, and the ultrasonic fragmentation time is 0.5 to 2 h.
[0013] Furthermore, in the step (2), the co-solvent is one of anhydrous lithium chloride (LiCl) and polyethylene glycol (PEG), and its concentration is 2wt% to 10wt%.
[0014] Furthermore, in step (2), the inert gas atmosphere is nitrogen (N 2 ) or one of argon (Ar); the heating dissolution temperature is 60-100°C, the stirring speed is 300-800rpm, the dissolution time is 4-8h; the casting solution concentration is 6wt%-14wt%.
[0015] Furthermore, in step (3), the concentration gradients (volume ratio) of coagulation bath water / organic solvent are 3:7, 5:5, 7:3 and 10:0 respectively.
[0016] Furthermore, in step (4), the detergent is deionized water, the drying temperature is 50-100° C., and the drying time is ≥3 hours.
[0017] The present invention also provides a lithium / sodium ion battery comprising the nano-cellulose / meta-aramid composite battery separator material.
[0018] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows:
[0019] (1) The present invention provides a nanocellulose / meta-aramid composite battery separator material. The nanocellulose has excellent electrolyte affinity characteristics, which effectively improves the wettability of the separator, thereby improving the rate performance and cycle performance; the meta-aramid has high thermal stability and flame retardancy characteristics, which effectively improves the safety of the separator, thereby enhancing the safety of the battery.
[0020] (2) The phase inversion preparation method used in the present invention can achieve precise control of the pore structure of the nanocellulose / meta-aramid composite membrane. The porous network structure and thickness of the composite membrane can be adjusted by adjusting the concentration gradient of water / organic solvent used for replacement and the concentration of meta-aramid during the curing process, thereby achieving performance optimization of the composite membrane.
[0021] (3) The phase conversion method of the present invention is simple and flexible to operate, and the organic solvent used is recyclable, and is expected to be used on a large scale in industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to further illustrate the technical solutions and implementation cases in the present invention, the following is a brief description of the test drawings used in the existing examples or technical processes. It is worth noting that the drawings listed below are only some implementation cases in the present invention. For technicians in the same field, other drawings can be obtained based on the provided drawings without creative work.
[0023] Figure 1 This is an electronic photograph of the nanocellulose / meta-aramid composite battery separator material prepared in Example 1;
[0024] Figure 2 This is a scanning electron microscope image of the nanocellulose / meta-aramid composite battery separator material prepared in Example 1;
[0025] Figure 3 This is the infrared spectrum of the nanocellulose / meta-aramid composite battery separator material prepared in Example 2;
[0026] Figure 4 This is a thermogravimetric analysis diagram of the nanocellulose / meta-aramid composite battery separator material prepared in Example 3;
[0027] Figure 5 This is a contact angle diagram of the nanocellulose / meta-aramid composite battery separator material prepared in Example 4; DETAILED DESCRIPTION
[0028] The following will further describe the process and technology of the embodiment of the present invention in detail in conjunction with the accompanying drawings of the test results of the embodiment of the present invention. In addition, the embodiments described in this patent are only some examples of the present invention, not all. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] (1) 0.6 g of 2 wt% nanocellulose gel (CNC) was added to 26 g of N,N-dimethylacetamide solvent, and the nanocellulose gel was uniformly dispersed in DMAc using an ultrasonic cell crusher with an ultrasonic power of 100 to 300 W and an ultrasonic crushing time of 0.5 to 2 h to obtain a nanocellulose solution with a concentration of 2 wt%;
[0031] (2) Weigh 2.4 g of dried meta-aramid staple fiber (PMIA) and add it to the nanocellulose solution obtained in step (1), and add 0.6 g of lithium chloride (LiCl), a co-solvent, corresponding to a concentration of 2 wt %, in an inert gas nitrogen (N 2 ) under the protection of 80 ° C., the stirring rate is 300 rpm, and the reaction is carried out in an oil bath for 6 hours, and the solution is dissolved until it is clear and transparent to obtain a uniform casting solution with a concentration of 8 wt%;
[0032] (3) The casting liquid obtained in step (2) is scraped into a liquid film with a thickness of 100 μm, and placed in a water / DMAc coagulation bath, and gradient replacement is performed according to the concentrations of 3:7, 5:5, 7:3 and 10:0, and the coagulation bath is replaced every 2 hours. The operation is repeated 3 times until it slowly solidifies into a film.
[0033] (4) The composite membrane was repeatedly washed with deionized water until the residual porogen and organic solvent were completely removed, and vacuum dried at 50°C for 3 h to finally prepare a nanocellulose / meta-aramid composite battery separator material with a thickness of 14.6 μm.
[0034] Example 2
[0035] (1) 0.9 g of 2 wt% nanocellulose gel (CNC) was added to 26 g of dimethylformamide solvent, and the nanocellulose gel was uniformly dispersed in DMF using an ultrasonic cell crusher with an ultrasonic power of 100 to 300 W and an ultrasonic crushing time of 0.5 to 2 h to obtain a nanocellulose solution with a concentration of 3 wt%;
[0036] (2) Weighing 3.0 g of dried meta-aramid staple fiber (PMIA), adding it to the nanocellulose solution obtained in step (1), and adding 0.9 g of co-solvent lithium chloride (LiCl), corresponding to a concentration of 3 wt%, under the protection of inert gas argon (Ar), the dissolution temperature is 90 ° C, the stirring rate is 400 rpm, and the oil bath reaction is carried out for 5 h, dissolving until clear and transparent, and obtaining a uniform casting solution with a concentration of 10 wt%;
[0037] (3) The casting liquid obtained in step (2) is scraped into a liquid film with a thickness of 100 μm, and placed in a water / DMF coagulation bath, and gradient replacement is performed according to the concentrations of 3:7, 5:5, 7:3 and 10:0, and the coagulation bath is replaced every 2 hours. The operation is repeated 3 times until it slowly solidifies into a film.
[0038] (4) The composite membrane was repeatedly washed with deionized water until the residual porogen and organic solvent were completely removed, and vacuum dried at 55°C for 3 h to finally prepare a nanocellulose / meta-aramid composite battery separator material with a thickness of 16.8 μm.
[0039] Example 3
[0040] (1) 1.5 g of 2 wt% nanocellulose gel (CNC) was added to 26 g of N,N-dimethylacetamide solvent and uniformly dispersed in DMAc using an ultrasonic cell crusher with an ultrasonic power of 100 to 300 W and an ultrasonic crushing time of 0.5 to 2 h to obtain a nanocellulose solution with a concentration of 5 wt%;
[0041] (2) Weighing 3.6 g of dried meta-aramid staple fiber (PMIA), adding it to the nanocellulose solution obtained in step (1), and adding 1.2 g of co-solvent lithium chloride (LiCl), corresponding to a concentration of 4 wt%, under the protection of inert gas argon (Ar), the dissolution temperature is 85 ° C, the stirring rate is 600 rpm, and the oil bath reaction is carried out for 4 h, dissolving until clear and transparent, and obtaining a uniform casting solution with a concentration of 12 wt%;
[0042] (3) The casting liquid obtained in step (2) is scraped into a liquid film with a thickness of 100 μm, and placed in a water / DMAc coagulation bath, and gradient replacement is performed according to the concentrations of 3:7, 5:5, 7:3 and 10:0, and the coagulation bath is replaced every 2 hours. The operation is repeated 3 times until it slowly solidifies into a film.
[0043] (4) The composite membrane was repeatedly washed with deionized water until the residual porogen and organic solvent were completely removed, and vacuum dried at 45°C for 4 h to finally prepare a nanocellulose / meta-aramid composite battery separator material with a thickness of 18.9 μm.
[0044] Example 4
[0045] (1) 1.5 g of 2 wt% nanocellulose gel (CNC) was added to 26 g of dimethyl sulfoxide solvent, and the nanocellulose gel was uniformly dispersed in DMSO using an ultrasonic cell crusher, with an ultrasonic power of 100 to 300 W and an ultrasonic crushing time of 0.5 to 2 h to obtain a nanocellulose solution with a concentration of 5 wt%;
[0046] (2) Weigh 4.2 g of dried meta-aramid staple fiber (PMIA) and add it to the nanocellulose solution obtained in step (1), and add 1.5 g of lithium chloride (LiCl), a co-solvent, corresponding to a concentration of 5 wt %, in an inert gas nitrogen (N 2) under the protection of 95 ° C., the stirring rate is 800 rpm, and the reaction is carried out in an oil bath for 4 hours, and the solution is dissolved until it is clear and transparent to obtain a uniform casting solution with a concentration of 14 wt%;
[0047] (3) The casting liquid obtained in step (2) is scraped into a liquid film with a thickness of 100 μm, and placed in a water / DMSO coagulation bath, and gradient replacement is performed according to the concentrations of 3:7, 5:5, 7:3 and 10:0, and the coagulation bath is replaced every 2 hours. The operation is repeated 3 times until it slowly solidifies into a film.
[0048] (4) The composite membrane was repeatedly washed with deionized water until the residual porogen and organic solvent were completely removed, and vacuum dried at 60°C for 3 h to finally prepare a nanocellulose / meta-aramid composite battery separator material with a thickness of 20.7 μm.
[0049] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0050] The nanocellulose / meta-aramid composite battery separator materials prepared in each example were characterized and tested under the following test conditions:
[0051] (1) Scanning electron microscopy characterization
[0052] The morphology of the nanocellulose / meta-aramid composite battery separator material prepared in each implementation case was observed using a scanning electron microscope (S-4800) produced by HITACHI with an accelerating voltage of 15 KV.
[0053] (2) Fourier transform infrared spectroscopy (FTIR)
[0054] The freeze-dried sample was ground into a uniform powder with potassium bromide (KBr) in a mortar at a mass ratio of 1:100. The powder was pressed into a transparent sheet by tabletting and placed on the sample stage of an infrared spectrometer for FT-IR testing and analysis. The test parameters were set to a scanning range of 4000-400cm -1 , scanned 32 times, with a resolution of 4cm -1 .
[0055] (3) Thermogravimetric-differential thermal analysis
[0056] Thermogravimetric-Differential Thermal Analysis (TG-DTA) refers to measuring the mass fraction of active components in a sample and analyzing the thermal stability of the sample under a certain atmosphere and temperature. This experiment used a STA 2500 Regulus thermal analyzer under a nitrogen atmosphere with a heating rate of 10 °C min -1 The temperature was raised from room temperature to 500°C.
[0057] (4) Contact angle measurement
[0058] The contact angle of the liquid electrolyte on the nanocellulose / meta-aramid composite battery separator material prepared in each implementation case is measured to reflect the wettability of the electrolyte on the nanocellulose / meta-aramid composite battery separator material and to characterize the hydrophilicity and hydrophobicity of the separator surface.
[0059] Figure 1 This is an electronic photograph of the nanocellulose / meta-aramid composite battery separator material prepared in Example 1. It can be observed that the separator has a good shape and a smooth surface.
[0060] Figure 2 This is a scanning electron microscope image of the nanocellulose / meta-aramid composite battery separator material prepared in Example 1. It can be observed that the three-dimensional network porous structure of the composite separator and the uniform distribution of nanocellulose.
[0061] Figure 3 This is the infrared spectrum of the nanocellulose / meta-aramid composite battery separator material prepared in Example 2, where the X-axis represents the wave number, indicating the position of the absorption peak; the ordinate represents the transmittance, indicating the absorption intensity. Figure 1 It can be seen that at 3423cm -1 、2920cm -1 、1656cm -1 、1610cm -1 、1536cm -1 、1305cm -1 、1053cm -1 There are obvious absorption peaks, which correspond to the stretching vibration peak of the NH bond on PMIA, the stretching vibration peak of the methyl group (CH bond) on nanocellulose, the stretching vibration peak of the C=O bond on PMIA (amide I band), the stretching vibration peak of the aromatic ring, the NH in-plane bending and CN stretching coupling of the CNH group (amide II band) and the COC stretching vibration peak on nanocellulose. No new impurity peaks appear, indicating that nanocellulose and meta-aramid are well physically combined together.
[0062] Figure 4The thermogravimetric analysis diagram of the nanocellulose / meta-aramid composite battery separator material prepared in Example 3 shows that the separator material has almost no mass loss before 130°C, with a weight loss of about 2.55%, which is attributed to the removal of bound water and the breaking of hydrogen bonds; the obvious weight loss between 160 and 240°C is caused by the thermal breaking of glycosidic bonds in nanocellulose; the second obvious thermal weight loss begins at 438°C, corresponding to the breaking of amide bonds, and the thermal weight loss peak moves slightly to a higher temperature, which is related to the hydrogen bond between nanocellulose and meta-aramid. It is confirmed that the mixing of nanocellulose does not affect the high heat resistance of the nanocellulose / meta-aramid composite battery separator material, thereby improving the safety of the battery.
[0063] Figure 5 This is the contact angle diagram of the nanocellulose / meta-aramid composite battery separator material and the electrolyte prepared in Example 4. The electrolyte was all 1M LiPF 6 A mixed solution of FEC / DMC / EC = 10:45:45 (v) was dripped for 3s to record the contact angle between the composite separator and the electrolyte. It can be observed that the contact angle between the composite separator and the electrolyte is only 2.2°, indicating that the composite separator has good wettability with the electrolyte.
[0064] The nanocellulose / meta-aramid composite battery separator materials of different thicknesses prepared in each example are used as the separator layer of the lithium-ion battery. The negative electrode active material (graphite) is mixed with the binder (polyvinylidene fluoride PVDF) and the conductive agent (Super P) in a mass ratio of 8:1:1, and dimethylpyrrolidone (NMP) is added as a solvent to mix and stir into a uniform slurry. The slurry is evenly applied on the copper foil, and after drying, it is cut into thin sheets as the negative electrode. The 2032 button battery is assembled in a glove box filled with argon gas, which includes the positive electrode shell, electrode sheet, electrolyte, diaphragm, lithium sheet, gasket, shrapnel and negative electrode shell from bottom to top. Among them, the electrolyte is 1.0M lithium hexafluorophosphate (LiPF 6 ) was prepared from a solution of fluoroethylene carbonate (FEC), dimethyl carbonate (DMC) and ethylene carbonate (EC) (volume ratio of 10:45:45).
[0065] The above-assembled button batteries were tested using the Land battery tester produced by Wuhan Jinnuo Electronics Co., Ltd. The test conditions and results are as follows:
[0066] The button battery was subjected to constant current charge and discharge test, and the charge and discharge voltage range was 0.01 to 2.5 V. Among Examples 1 to 4, the battery assembled with the nanocellulose / meta-aramid composite battery separator material of Example 3 had the best electrochemical performance. The initial specific capacity of the battery was 358.1 mAh / g at a current density of 100 mA / g, and the capacity retention rate after 200 cycles was 92.08%, while the initial specific capacity of the battery of Examples 1, 2, and 4 at a current density of 100 mA / g was 336.5 mAh / g, 345.2 mAh / g, and 352.3 mAh / g, respectively. In addition, the capacity retention rates of Examples 1, 2, and 4 after 200 cycles at a current density of 100 mA / g were all greater than 90%, indicating that the electrochemical performance of the battery assembled with the composite separator was relatively stable.
[0067] See Table 1 for specific data
[0068] Table 1 Test results
[0069]
[0070] In summary, the nanocellulose / meta-aramid composite battery diaphragm material obtained by the present invention uses meta-aramid as the substrate, which effectively improves the thermal stability and flame retardancy of the diaphragm, and ensures the safety of the diaphragm material during use; at the same time, the introduction of nanocellulose effectively improves the problems of poor wettability and low ionic conductivity of the diaphragm. When the prepared composite diaphragm is applied to batteries, the rate performance and cycle performance are excellent. The present invention uses a phase inversion method to prepare a nanocellulose / meta-aramid composite battery diaphragm material, and adjusts the thickness and pore structure of the diaphragm by adjusting the concentration of meta-aramid and the substitution system, and the preparation process is simple and flexible.
[0071] The content of the present invention is not limited to the content of the above embodiments. The combination of one or more embodiments can also achieve the purpose of the present invention.
[0072] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the method disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part description.
[0073] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein but will conform to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A nanocellulose / meta-aramid composite battery separator material, characterized in that: The nanocellulose of the diaphragm material is uniformly dispersed in the porous network structure of the meta-aramid fiber and has a thickness of 9 to 30 μm.
2. A method for preparing a nanocellulose / meta-aramid composite battery separator material, characterized in that: The following steps are involved: (1) dispersing nanocellulose gel (CNC) in an organic solvent by ultrasonic cell crusher to obtain a nanocellulose solution; (2) adding dried meta-aramid staple fibers (PMIA) to the nanocellulose solution obtained in step (1), then adding an appropriate amount of a solvent, heating and stirring under the protection of an inert gas to dissolve until the solution becomes clear and transparent, and obtaining a uniform casting solution; (3) The casting liquid obtained in step (2) is scraped into a liquid film, placed in a coagulation bath, and gradient replacement is performed using water / organic solvents of different concentrations, and the operation is repeated until solidification into a film. (4) repeatedly washing the cured film until the residual porogen and organic solvent are removed, and finally drying the film under vacuum or at normal pressure to obtain a nanocellulose / meta-aramid composite battery separator material.
3. The method for preparing the nanocellulose / meta-aramid composite battery separator material according to claim 2, characterized in that: In the step (1), the size of the nanocellulose gel is 100 to 200 nm; the organic solvent is one of N,N-dimethylacetamide (DMAc), dimethyl sulfoxide (DMSO), dimethylformamide (DMF), etc.; in the step (1), the concentration of the nanocellulose solution is 1 wt% to 10 wt%.
4. The method for preparing the nanocellulose / meta-aramid composite battery separator material according to claim 2, characterized in that: In the step (1), the ultrasonic power is 100 to 300 W, and the ultrasonic fragmentation time is 0.5 to 2 h.
5. The method for preparing the nanocellulose / meta-aramid composite battery separator material according to claim 2, characterized in that: The co-solvent in step (2) is one of anhydrous lithium chloride (LiCl) and polyethylene glycol (PEG), and its concentration is 2wt% to 10wt%.
6. The method for preparing the nanocellulose / meta-aramid composite battery separator material according to claim 2, characterized in that: In the step (2), the inert gas atmosphere is one of nitrogen (N2) or argon (Ar); the heating and dissolving temperature is 60-100°C, the stirring rate is 300-800 rpm, and the stirring time is 4-8h; and the casting liquid concentration is 6wt%-14wt%.
7. The method for preparing the nanocellulose / meta-aramid composite battery separator material according to claim 2, characterized in that: In the step (3), the concentration gradients (volume ratio) of coagulation bath water / organic solvent are 3:7, 5:5, 7:3 and 10:0, respectively.
8. The method for preparing the nanocellulose / meta-aramid composite battery separator material according to claim 2, characterized in that: In the step (4), the detergent is deionized water, the drying temperature is 50-100° C., and the drying time is ≥3 hours.
9. A lithium / sodium ion battery comprising the nanocellulose / meta-aramid composite battery separator material according to claim 1.
Citation Information
Patent Citations
Method for preparing porous meta-aramid diaphragm through non-solvent induced phase separation method
CN113381122A
Preparation method of nano cellulose / aramid fiber lithium battery diaphragm material by heterogeneous process
CN114865218A