Composite diaphragm for semi-solid lithium battery as well as preparation method and application of composite diaphragm

The composite separator for semi-solid lithium batteries, featuring a base layer with aramid and h-BN-LATP, stabilizes LATP and enhances bonding, addressing the issues of reduction and powder falling, thereby improving ionic conductivity and cycle stability.

CN119069956AActive Publication Date: 2024-12-03SINOMA LITHIUM BATTERY SEPARATOR CO LTD

Patent Information

Application Number
CN202310647500.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

The direct contact of lithium aluminum titanium phosphate (LATP) with the metal lithium negative electrode leads to reduction, and the poor dispersion of inorganic heat-resistant materials with high molecular polymers results in powder falling off the coating surface, affecting the performance of semi-solid lithium-ion battery separators.

Method used

A composite separator for semi-solid lithium batteries is developed, comprising a base layer with a coating layer of aramid and h-BN-LATP (modified lithium aluminum titanium phosphate) and optionally a PEO layer, which stabilizes LATP and improves bonding, preventing it from reacting with metal lithium and enhancing the binding force between layers.

Benefits of technology

The composite separator effectively prevents LATP reduction, improves ionic conductivity, and enhances cycle stability by stabilizing the coating and reducing interface impedance, thus improving the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069956A_ABST
    Figure CN119069956A_ABST
Patent Text Reader

Abstract

The invention provides a composite diaphragm for a semi-solid lithium battery as well as a preparation method and application of the composite diaphragm. The composite diaphragm comprises a base layer and a PEO layer positioned on one side or two sides of the base layer, the base layer comprises a base film and a coating layer positioned on one side of the base film; the coating layer is prepared from aramid fibers and h-BN-LATP (h-BN-LATP); the h-BN-LATP is obtained by carrying out hydroxyl modification on a hexagonal boron nitride layer coated on the surface of the LATP. According to the composite diaphragm, the layers are matched with one another, so that the LATP can be effectively prevented from being in direct contact with a metal lithium negative electrode, and meanwhile, the binding force of the LATP and aramid fibers is improved. Meanwhile, the liquid absorption and retention capability and heat resistance of the diaphragm and the ionic conductivity of the diaphragm are improved, the interface impedance between the coating and an electrode is reduced, and the cycle performance of the battery is favorably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium-ion battery separators, and in particular relates to a composite separator for a semi-solid lithium battery and a preparation method and application thereof. Background Art

[0002] The core of a traditional liquid lithium-ion battery is composed of a positive electrode, a negative electrode, an electrolyte (lithium-containing electrolyte dissolved in an organic compound) and a diaphragm, wherein the diaphragm separates the positive and negative electrodes in the lithium-ion battery and allows lithium ions to pass freely while blocking electronic conduction to prevent short circuits between the positive and negative electrodes; at the same time, the porous diaphragm absorbs the electrolyte to form an ion channel. Ion conduction is one of the main functions of lithium-ion battery diaphragms, specifically, it is through the dissociation of lithium salts and the solvation of lithium ions that the conduction of lithium ions inside the battery is achieved. However, solvents are flammable, volatilizable and leak at high temperatures. Moreover, lithium hexafluorophosphate, as one of the most commonly used electrolytes in commercial lithium-ion batteries, has disadvantages such as poor thermal stability and easy deliquesce and hydrolysis, and the PF generated by thermal decomposition at high temperatures 5 It will cause fluorination of solvent impurities. In addition, lithium hexafluorophosphate can also react with water, alcohol, phenol, aldehyde, active hydrogen, etc. to generate HF, all of which will lead to reduced battery capacity, shortened cycle life, and even cause safety issues such as fire or explosion.

[0003] Compared with all-liquid lithium-ion batteries, semi-solid lithium battery separators greatly reduce the amount of liquid electrolyte added, thereby greatly reducing the risk of battery fire or explosion, and improving the safety performance of lithium-ion batteries. At present, most traditional semi-solid lithium-ion batteries are in the form of coating solid electrolytes on the separator, and solid electrolytes are the core components of semi-solid lithium-ion battery separators and the focus of research on semi-solid lithium-ion batteries. The various performance parameters of semi-solid lithium-ion batteries such as power density, cycle stability, safety performance, high and low temperature performance and service life depend to a large extent on the solid electrolyte material coated on the separator. Among them, oxides (such as NASICON system, LISICON system and the general formula ABO 3 Perovskite structure) solid electrolytes have been widely studied and have good stability in air, but their interface compatibility with electrode materials is poor. Polymer electrolytes have the advantages of excellent mechanical processing performance, light weight, and low electrode / electrolyte interface impedance, but their ionic conductivity is lower than that of oxide solid electrolytes.

[0004] In view of the above problems, the prior art uses a mixture of heat-resistant materials, high molecular polymers and solid electrolytes to form a coating layer on the surface of the base film. The coating layer formed on the surface of the base film by the functional diaphragm has good adhesion to the battery pole piece, and has high ionic conductivity, while having good insulation and heat resistance. The battery assembled using the functional diaphragm is not easy to deform and has a small internal resistance, and has good rate and power performance. It also has high needle puncture and high temperature hot box safety performance and good cycle performance. However, the lithium aluminum titanium phosphate LATP used in this scheme is easily reduced and ineffective when it is directly in contact with the metal lithium negative electrode, resulting in a short battery life. In addition, the poor dispersion of inorganic heat-resistant materials and LATP with high molecular polymers can easily cause the problem of powder falling off the coating surface, affecting the physical properties of the diaphragm. Summary of the invention

[0005] Based on the technical problems existing in the prior art and the direction of improvement, the present invention provides a composite separator for a semi-solid lithium battery, which is used to solve the problem in the prior art that LATP is reduced due to direct contact with the metal lithium negative electrode and powder falls off in the coating due to the weak bonding between LATP and aramid.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] A composite diaphragm for a semi-solid lithium battery, the composite diaphragm comprising a base layer and a PEO (polyethylene oxide) layer located on one side or both sides of the base layer;

[0008] The base layer includes a base film and a coating layer located on one side of the base film; the coating layer includes aramid and h-BN-LATP (modified lithium aluminum titanium phosphate); when the PEO layer is located on one side of the base layer, the PEO layer is located on one side of the coating layer;

[0009] The h-BN-LATP is obtained by modifying the hexagonal boron nitride layer coated on the surface of LATP with hydroxyl groups.

[0010] The composite separator for semi-solid lithium battery provided by the present invention is formed by arranging a coating layer including aramid and h-BN-LATP on one side of the base film to form a base layer, and further arranging a PEO layer on one side (one side of the coating layer) or both sides of the base layer, and the layers cooperate with each other, which can effectively prevent LATP from directly contacting the metal lithium negative electrode, and at the same time improve the binding force between LATP and aramid. Specifically, using chemically inert hexagonal boron nitride as the LATP wrapping layer can effectively inhibit its reduction reaction with the metal lithium negative electrode. Hydroxylated hexagonal boron nitride forms hydrogen bonds with the amino groups in the aramid molecules, stabilizing LATP while improving the bonding force between h-BN-LATP and aramid. The h-BN-LATP in the resulting coating has better dispersibility and a high degree of bonding with aramid, preventing the coating from falling off. Moreover, the three-dimensional network structure of aramid fibers can serve as a carrier of h-BN-LATP, while improving the liquid absorption and retention capacity and heat resistance of the diaphragm. h-BN-LATP is filled in the three-dimensional structure of aramid, which can reduce the air permeability of the coating layer, which is beneficial to improving the ionic conductivity of the diaphragm. Combined with a single-sided or double-sided PEO layer, it can reduce the interface impedance between the coating and the electrode, which helps to improve the battery cycle performance.

[0011] Optionally, in the coating layer, the mass ratio of the aramid to the h-BN-LATP is (1-10):(1-5).

[0012] Optionally, the base film is a polyolefin base film with a microporous structure; preferably, the base film is made of polyethylene, or a copolymer of ethylene and propylene; more preferably, the base film has a thickness of 5-13.5 μm.

[0013] Optionally, the aramid is selected from poly(m-phenylene isophthalamide) (aramid 1313) and / or poly(p-phenylene terephthalamide) (aramid 1414, aramid II).

[0014] Optionally, the thickness of the composite membrane is less than 20 μm, the thickness of the coating layer is 2-4 μm, and the thickness of the PEO layer is 0.5-2.5 μm.

[0015] The composite diaphragm for semi-solid lithium battery provided by the present invention cooperates with each other between the layers to prevent the surface powder of the composite diaphragm from falling off, thereby significantly improving the ionic conductivity, air permeability and cycle stability of the composite diaphragm. Among them, the PEO layer and h-BN modification synergistically stabilize LATP, especially when metallic lithium is used as the negative electrode, LATP can be avoided from reacting with lithium, and PEO is distributed in particles on the surface of the composite diaphragm. Compared with the single-side coating of the PEO layer on the base layer, the PEO layer is coated on both sides of the base layer, which will affect the air permeability of the composite diaphragm, but the impact will not be great, and the ionic conductivity will be correspondingly lower. Aramid, as a heat-resistant skeleton material, can cooperate with h-BN-LATP, and h-BN-LATP has a pore-forming effect in aramid, thereby improving the ionic conductivity and air permeability of the composite diaphragm.

[0016] The present invention also provides a method for preparing the above-mentioned composite diaphragm for semi-solid lithium battery, comprising the following steps:

[0017] h-BN-LATP: A hexagonal boron nitride coating is formed on the surface of LATP by chemical vapor deposition, and then the boron nitride coating is modified by hydroxylation to obtain h-BN-LATP;

[0018] Aramid glue solution: dissolve aramid in a solvent and control the solid content of aramid to be 1.8%-2.2% to obtain aramid glue solution;

[0019] h-BN-LATP suspension: Disperse h-BN-LATP and solvent evenly to form a suspension, thus obtaining h-BN-LATP suspension;

[0020] Coating slurry: after the aramid glue solution and the h-BN-LATP suspension are mixed and dispersed evenly, the mixture is filtered and degassed to obtain a coating slurry;

[0021] PEO glue: mix PEO and solvent evenly to obtain PEO glue;

[0022] Composite diaphragm: the coating slurry is coated on one side of the base film, and treated with water vapor and deionized water in sequence to obtain a base layer; then the PEO glue is coated on one side or both sides of the base layer, and dried to obtain a composite diaphragm for a semi-solid lithium battery.

[0023] Optionally, the steps for preparing a hexagonal boron nitride coating layer formed on the surface of LATP by chemical vapor deposition are as follows:

[0024] At 750~1200℃, BH 3 -NH 3 In the case of pure N 2A chemical vapor deposition reaction is carried out on the surface of LATP under an atmosphere to obtain LATP with a surface coated with a hexagonal boron nitride layer; preferably, the thickness of the hexagonal boron nitride coating layer is 5-10 nm.

[0025] By adopting the chemical vapor deposition method, chemically inert hexagonal boron nitride with a certain thickness and more defects can be obtained at a lower deposition temperature, thereby ensuring that the deposited layer has a higher lithium ion pass rate.

[0026] Optionally, the method for hydroxylation modification of the boron nitride coating is not specifically limited, and conventional physical methods or chemical methods in the industry can be used, such as the physical method can be ball milling, and the chemical method can be molten hydroxide or hydrogen peroxide. The steps of hydroxylation modification of the boron nitride coating recommended by the present invention are as follows:

[0027] The LATP with a hexagonal boron nitride layer on the surface is placed in a 1-10 mol / L alkali solution (conventional inorganic alkali solutions such as potassium hydroxide and sodium hydroxide are acceptable, without specific limitation), heated to 80-150° C. under stirring and maintained for 12-24 hours, separated, and the obtained solid is washed with deionized water until the pH of the filtrate is neutral, and dried to obtain h-BN-LATP.

[0028] Optionally, the aramid glue solution further contains a co-solvent, and the mass content of the co-solvent in the aramid glue solution is ≤10%; preferably, the co-solvent is selected from CaCl 2 , at least one of KOH, LiCl and pyridine;

[0029] In the h-BN-LATP suspension, the mass ratio of the h-BN-LATP to the solvent is 1:5-12.

[0030] Optionally, the solvent is selected from an organic solvent and / or water, and the organic solvent is selected from at least one of NMP, DMSO, DMF and DMAc;

[0031] The coating method is not specifically limited and any conventional method in the industry may be used, such as blade coating, roller coating, wire rod coating, and dip coating.

[0032] The present invention also provides a semi-solid lithium ion battery, comprising the above-mentioned composite diaphragm for a semi-solid lithium battery or a composite diaphragm for a semi-solid lithium battery prepared by the above-mentioned method for preparing the composite diaphragm for a semi-solid lithium battery. Description of the drawings:

[0033] Figure 1 This is a scanning electron microscope image of the composite diaphragm for a semi-solid lithium battery prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0034] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0035] The thickness of the boron nitride coating involved in the following embodiments and comparative examples is calculated based on the deposition rate and time, and other membrane-related thickness values ​​are measured using a Mahr thickness gauge.

[0036] Example 1

[0037] This embodiment provides a composite diaphragm for a semi-solid lithium battery, and the preparation method thereof is as follows:

[0038] Preparation of h-BN-LATP: 3 -NH 3 . To prepare the precursor for boron nitride, pure N 2 The LATP surface was subjected to chemical vapor deposition under an atmosphere to obtain LATP with a 10 nm hexagonal boron nitride coating on the surface. Then, it was added to a 5 mol / L potassium hydroxide solution, heated in an oil bath at 150°C for 24 hours under continuous mechanical stirring, and the obtained mixture was filtered and washed with deionized water several times until the pH value of the filtrate was 7, and finally dried to obtain LATP with a surface hydroxylation-modified hexagonal boron nitride coating, namely h-BN-LATP.

[0039] Preparation of h-BN-LATP suspension: 2 parts by weight of h-BN-LATP was added to 12 parts by weight of N-methylpyrrolidone (NMP), and the suspension of h-BN-LATP was obtained after high-speed dispersion for 20 minutes;

[0040] Preparation of aramid glue solution: Take 8 parts of calcium chloride and 90 parts of N-methylpyrrolidone NMP and fully dissolve them under high-speed dispersion conditions, then add 2 parts of aramid 1414 to the above mixed solvent, and then disperse it at high speed for 5 hours to obtain aramid glue solution.

[0041] Preparation of coating slurry: 50 parts by weight of the aramid glue solution and the h-BN-LATP suspension solution were mixed, and then dispersed at high speed for 30 minutes, and then filtered with a 400-mesh filter, and vacuum-debubbled for 5 minutes to obtain a coating slurry;

[0042] Preparation of PEO glue: 0.5 parts by weight of PEO was mixed with 200 parts by weight of deionized water, and then subjected to high-speed dispersion treatment for 120 minutes to obtain PEO glue;

[0043] Preparation of composite diaphragm: The above-mentioned coating slurry is evenly coated on one side of a 13.5μm thick polyethylene porous substrate using a wire rod, and the coated wet film is retained in a water vapor atmosphere of 65°C and 85% RH for 60s, then transferred to a pure water tank for washing for 5min, and then transferred to the above-mentioned PEO glue solution and taken out after 5s, and finally dried in an oven at 65°C for 15min to obtain a composite diaphragm for a semi-solid lithium battery with a total thickness of about 3μm for the double-sided PEO layer and the coating layer.

[0044] The composite membrane was scanned by electron microscope. Figure 1 As shown. Figure 1 It can be seen that the h-BN-LATP solid electrolyte is evenly wrapped by aramid fibers inside the coating, with no obvious exposed particles on the surface, and the surface of the obtained coated diaphragm is not easy to fall off.

[0045] Example 2

[0046] This embodiment provides a composite diaphragm for a semi-solid lithium battery, and the preparation method thereof is as follows:

[0047] The preparation methods of h-BN-LATP, h-BN-LATP suspension, aramid glue and coating slurry are the same as those in Example 1.

[0048] Preparation of PEO glue: 1 part by weight of PEO was mixed with 200 parts by weight of deionized water, and then subjected to high-speed dispersion treatment for 120 minutes to obtain PEO glue;

[0049] Preparation of composite diaphragm: The above-mentioned coating slurry is evenly coated on one side of a 7μm thick polyethylene porous substrate using a wire rod, and the coated wet film is retained in a water vapor atmosphere of 65°C and 85% RH for 60s, then transferred to a pure water tank for washing for 5min, and then transferred to the above-mentioned PEO glue solution and taken out after 5s, and finally dried in an oven at 65°C for 15min to obtain a composite diaphragm for a semi-solid lithium battery with a total thickness of about 3μm for the double-sided PEO layer and the coating layer.

[0050] Example 3

[0051] This embodiment provides a composite diaphragm for a semi-solid lithium battery, and the preparation method thereof is as follows:

[0052] Preparation of h-BN-LATP: 3 -NH 3 To prepare the precursor for boron nitride, pure N 2The LATP surface was subjected to chemical vapor deposition under an atmosphere to obtain LATP with a 5 nm hexagonal boron nitride coating on the surface. Then, it was added to a 5 mol / L sodium hydroxide solution, heated in an oil bath at 150°C for 24 hours under continuous mechanical stirring, and the obtained mixture was filtered and washed with deionized water for multiple times until the pH value of the filtrate was 7, and finally dried to obtain LATP with a surface hydroxylation-modified hexagonal boron nitride coating, namely h-BN-LATP.

[0053] The preparation methods of aramid glue and PEO glue are the same as those in Example 1, and the preparation methods of h-BN-LATP suspension and coating slurry are similar to those in Example 1, with the only difference being that h-BN-LATP in this example is used in the preparation of h-BN-LATP suspension, and h-BN-LATP suspension in this example is used in the preparation of coating slurry.

[0054] Preparation of composite diaphragm: The above-mentioned coating slurry is evenly coated on one side of a 9μm thick polyethylene porous substrate using a wire rod, and the coated wet film is retained in a water vapor atmosphere of 65°C and 85% RH for 60s, then transferred to a pure water tank for washing for 5min, and then transferred to the above-mentioned PEO glue solution and taken out after 5s, and finally dried in an oven at 65°C for 15min to obtain a composite diaphragm for a semi-solid lithium battery with a total thickness of about 3μm for the double-sided PEO layer and the coating layer.

[0055] Example 4

[0056] This embodiment provides a composite diaphragm for a semi-solid lithium battery, and the preparation method thereof is as follows:

[0057] The preparation methods of h-BN-LATP, aramid glue and PEO glue are the same as those in Example 1. The preparation method of the coating slurry is similar to that in Example 1, with the only difference being that the h-BN-LATP suspension in this example is used in the preparation of the coating slurry.

[0058] Preparation of h-BN-LATP suspension: 1 part by weight of h-BN-LATP was added to 12 parts by weight of N-methylpyrrolidone (NMP), and the suspension of h-BN-LATP was obtained after high-speed dispersion for 20 minutes;

[0059] Preparation of composite diaphragm: The above-mentioned coating slurry is evenly coated on one side of a 12μm thick polyethylene porous substrate using a wire rod, and the coated wet film is retained in a water vapor atmosphere of 65°C and 85% RH for 60s, then transferred to a pure water tank for washing for 5min, and then transferred to the above-mentioned PEO glue solution and taken out after 5s, and finally dried in an oven at 65°C for 15min to obtain a composite diaphragm for a semi-solid lithium battery with a total thickness of about 3μm for the double-sided PEO layer and the coating layer.

[0060] Example 5

[0061] This embodiment provides a composite diaphragm for a semi-solid lithium battery, and the preparation method thereof is as follows:

[0062] The preparation methods of h-BN-LATP, h-BN-LATP suspension, aramid glue, coating slurry and PEO glue are the same as those in Example 1.

[0063] Preparation of composite diaphragm: The above-mentioned coating slurry is evenly coated on one side of a 13.5μm thick polyethylene porous substrate using a wire rod, and the coated wet film is retained in a water vapor atmosphere of 65°C and 85%RH for 60s, and then transferred to a pure water tank for washing for 5min. Then the above-mentioned PEO glue is evenly coated on one side of the coating layer using a wire rod, and finally dried in an oven at 65°C for 15min to obtain a composite diaphragm for semi-solid lithium batteries with a total thickness of about 3μm for the single-side PEO layer and the coating layer.

[0064] Example 6

[0065] This embodiment provides a composite diaphragm for a semi-solid lithium battery, and the preparation method thereof is as follows:

[0066] The preparation methods of h-BN-LATP, aramid glue and PEO glue are the same as those in Example 1. Preparation of h-BN-LATP suspension:

[0067] 0.2 parts by weight of h-BN-LATP was added to 1.2 parts by weight of N-methylpyrrolidone (NMP), and dispersed at high speed for 20 minutes to obtain a suspension of h-BN-LATP;

[0068] The method for preparing the coating slurry is similar to that of Example 1, except that the h-BN-LATP suspension in this example is used.

[0069] Preparation of composite diaphragm: The above-mentioned coating slurry is evenly coated on one side of a 13.5μm thick polyethylene porous substrate using a wire rod, and the coated wet film is retained in a water vapor atmosphere of 65°C and 85%RH for 60s, and then transferred to a pure water tank for washing for 5min. Then the above-mentioned PEO glue is evenly coated on one side of the coating layer using a wire rod, and finally dried in an oven at 65°C for 15min to obtain a composite diaphragm for semi-solid lithium batteries with a total thickness of about 3μm for the single-side PEO layer and the coating layer.

[0070] Comparative Example 1

[0071] This comparative example provides a composite diaphragm for a semi-solid lithium battery, and the preparation method thereof is as follows:

[0072] Preparation of LATP suspension: 2 parts by weight of LATP was added to 12 parts by weight of N-methylpyrrolidone (NMP), and dispersed at high speed for 20 minutes to obtain a suspension of LATP;

[0073] The preparation method of the aramid glue is the same as that of Example 1, and the preparation method of the coating slurry is similar to that of Example 1, the only difference being that the LATP suspension in this comparative example is used instead of the h-BN-LATP suspension in Example 1.

[0074] Preparation of composite diaphragm: The preparation method is similar to that of Example 6, except that the coating slurry in this comparative example is used.

[0075] Comparative Example 2

[0076] This embodiment provides a composite diaphragm for a semi-solid lithium battery, and the preparation method thereof is as follows:

[0077] Preparation of LATP suspension: 2 parts by weight of LATP was added to 12 parts by weight of N-methylpyrrolidone (NMP), and dispersed at high speed for 20 minutes to obtain a suspension of LATP;

[0078] The preparation of aramid glue and PEO glue is the same as that in Example 1.

[0079] Preparation of coating slurry: 50 parts by weight of the aramid glue solution and the LATP suspension solution were mixed, and then dispersed at high speed for 30 minutes, and then filtered with a 400-mesh filter, and vacuum-debubbled for 5 minutes to obtain coating slurry;

[0080] Preparation of composite diaphragm: The preparation method is similar to that of Example 1, except that the coating slurry in this comparative example is used.

[0081] Comparative Example 3

[0082] This comparative example provides a composite diaphragm for a semi-solid lithium battery, and the preparation method thereof is as follows:

[0083] Preparation of aramid glue: the same as the preparation method in Example 1.

[0084] Preparation of coating slurry: 50 parts by weight of the above aramid glue and 12 parts by weight of N-methylpyrrolidone (NMP) were mixed and dispersed at high speed for 20 minutes, filtered with a 400-mesh filter, and vacuum-debubbled for 5 minutes to obtain coating slurry.

[0085] Preparation of PEO glue: the same as the preparation method in Example 1.

[0086] Preparation of composite diaphragm: The preparation method is similar to that of Example 6, except that the coating slurry in this comparative example is used.

[0087] Comparative Example 4

[0088] This comparative example provides a composite diaphragm for a semi-solid lithium battery, and the preparation method thereof is as follows:

[0089] Preparation of aramid glue: the same as the preparation method in Example 1.

[0090] Preparation of coating slurry: The preparation method is the same as that of Comparative Example 3.

[0091] Preparation of PEO glue: the same as the preparation method in Example 1.

[0092] Preparation of composite membrane: the preparation method is the same as that in Example 1.

[0093] Comparative Example 5

[0094] This comparative example provides a composite diaphragm for a semi-solid lithium battery, and the preparation method thereof is as follows:

[0095] Preparation of h-BN-LATP: The preparation method is the same as that in Example 1.

[0096] Preparation of h-BN-LATP suspension: 2 parts by weight of h-BN-LATP was added to 12 parts by weight of N, N-dimethylacetamide (DMAc), and dispersed at high speed for 20 minutes to obtain a suspension of h-BN-LATP;

[0097] Preparation of aramid adhesive solution: Take 8 parts of calcium chloride and 90 parts of N, N-dimethylacetamide (DMAc) and fully dissolve them under high-speed dispersion conditions, then add 2 parts of aramid 1414 to the above mixed solvent, and then disperse it at high speed for 5 hours to obtain aramid adhesive solution.

[0098] Preparation of coating slurry: 0.5 parts by weight of PEO, 200 parts by weight of N,N-dimethylacetamide (DMAc), 50 parts by weight of the above aramid glue and the above h-BN-LATP suspension were mixed, and then dispersed at high speed for 120 minutes, and then filtered with a 400-mesh filter, and vacuum-debubbled for 5 minutes to obtain a coating slurry;

[0099] Preparation of composite diaphragm: The above-mentioned coating slurry is evenly coated on one side of a 13.5μm thick polyethylene porous substrate using a wire rod, and the coated wet film is retained in a water vapor atmosphere of 65°C and 85% RH for 60s, then transferred to a pure water tank for washing for 5min, and finally dried in an oven at 65°C for 15min to obtain a composite diaphragm for a semi-solid lithium battery with a single-side coating layer thickness of about 3μm.

[0100] The composite membranes prepared in the above embodiments and comparative examples were assembled into stainless steel|composite membrane|stainless steel symmetrical cells, and the impedance values ​​of each cell were tested to calculate the ionic conductivity value of the membrane. 0.33 Mn 0.33 Co 0.33 O 2 The electrochemical performance of the (NMC) / composite separator / Li full battery was tested. The specific test data are shown in Table 1.

[0101] Table 1

[0102]

[0103] Note: The more ☆ in the battery cycle stability, the better the cycle stability

[0104] It can be seen from the data in the above table that the composite diaphragm for semi-solid lithium batteries provided by the present invention cooperates with each other between the layers to prevent the surface of the composite diaphragm from falling off, and significantly improves the ionic conductivity, air permeability and cycle stability of the composite diaphragm. Specifically, in Examples 1-4, the PEO layer is coated on both sides of the base layer, and the surface of the obtained composite diaphragm does not fall off. In Example 1, LATP has high stability and the highest ionic conductivity. Compared with Example 1, the PEO concentration in the PEO glue of Example 2 is relatively large, and the ionic conductivity of the composite diaphragm obtained is slightly lower; in Example 3, the temperature of chemical vapor deposition during the preparation of h-BN-LATP is increased, and the final LATP stability and ionic conductivity of the composite diaphragm are lower than those in Example 1; in Example 4, the amount of h-BN-LATP is reduced, and the final LATP stability is high, but the ionic conductivity is low. In Examples 5 and 6, a PEO layer is coated on one side of the coating layer, and the LATP in the obtained composite diaphragm is highly stable and does not fall off, but the ionic conductivity is slightly lower than that of Examples 1-4.

[0105] Compared with the above-mentioned embodiments, the surfaces of the composite diaphragms obtained in the comparative examples all lose powder. Specifically, in Comparative Examples 1, 3 and 5, a PEO layer is coated on one side of the coating layer, and in Comparative Examples 2 and 4, a PEO layer is coated on both sides of the base layer. In Comparative Examples 1 and 2, LATP is not modified, and the composite diaphragms finally obtained have poor stability, lose powder, and have low ionic conductivity. No LATP is added in Comparative Examples 3 and 4, and the composite diaphragms finally obtained have low ionic conductivity, poor air permeability, and poor cyclic stability. In Comparative Example 5, a mixed coating method of PEO and h-BN-LATP is adopted. During the mixed coating process, PEO particles are filled into the pores of the aramid fibers, and the porosity in the coating is reduced, which leads to increased air permeability (poor air permeability) and reduced ionic conductivity.

[0106] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various specific technical features in any appropriate manner. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations. However, these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A composite diaphragm for a semi-solid lithium battery, characterized in that: The composite diaphragm comprises a base layer and a PEO layer located on one side or both sides of the base layer; The base layer includes a base film and a coating layer located on one side of the base film; the coating layer includes aramid and h-BN-LATP; The h-BN-LATP is obtained by modifying the hexagonal boron nitride layer coated on the surface of LATP with hydroxyl groups.

2. The composite separator for a semi-solid lithium battery according to claim 1, characterized in that: In the coating layer, the mass ratio of the aramid fiber to the h-BN-LATP is (1-10):(1-5).

3. The composite separator for a semi-solid lithium battery according to claim 1, characterized in that: The base film is a polyolefin base film with a microporous structure; the material of the base film is polyethylene or ethylene-propylene copolymer.

4. The composite separator for a semi-solid lithium battery according to claim 3, characterized in that: The base film has a thickness of 5-13.5 μm.

5. The composite separator for a semi-solid lithium battery according to claim 1, characterized in that: The aramid is selected from poly(m-phenylene isophthalamide) and / or poly(p-phenylene terephthalamide).

6. The composite separator for a semi-solid lithium battery according to claim 1, characterized in that: The thickness of the composite membrane is less than 20 μm, the thickness of the coating layer is 2-4 μm, and the thickness of the PEO layer is 0.5-2.5 μm.

7. A method for preparing a composite separator for a semi-solid lithium battery according to any one of claims 1 to 6, characterized in that: The steps include: h-BN-LATP: A hexagonal boron nitride coating is formed on the surface of LATP by chemical vapor deposition, and then the boron nitride coating is modified by hydroxylation to obtain h-BN-LATP; Aramid glue solution: dissolve aramid in a solvent and control the solid content of aramid to be 1.8%-2.2% to obtain aramid glue solution; h-BN-LATP suspension: Disperse h-BN-LATP and solvent evenly to form a suspension, thus obtaining h-BN-LATP suspension; Coating slurry: after the aramid glue solution and the h-BN-LATP suspension are mixed and dispersed evenly, the mixture is filtered and degassed to obtain a coating slurry; PEO glue: mix PEO and solvent evenly to obtain PEO glue; Composite diaphragm: the coating slurry is coated on one side of the base film, and treated with water vapor and deionized water in sequence to obtain a base layer; then the PEO glue is coated on one side or both sides of the base layer, and dried to obtain a composite diaphragm for a semi-solid lithium battery.

8. The method for preparing a composite diaphragm for a semi-solid lithium battery according to claim 7, characterized in that: The steps of forming a hexagonal boron nitride coating on the surface of LATP by chemical vapor deposition are as follows: At 750-1200° C., chemical vapor deposition reaction is carried out on the surface of LATP in a pure N2 atmosphere with BH3-NH3 as a boron source and a nitrogen source to obtain LATP with a hexagonal boron nitride layer coated on the surface; the thickness of the hexagonal boron nitride coating layer is 5-10 nm.

9. The method for preparing a composite separator for a semi-solid lithium battery according to claim 7, characterized in that: The steps of hydroxylating and modifying the boron nitride coating are as follows: The LATP with a hexagonal boron nitride layer on the surface is placed in a 1-10 mol / L alkali solution, heated to 80-150° C. under stirring and maintained for 12-24 hours, separated, and the obtained solid is washed with deionized water until the pH of the filtrate is neutral, and dried to obtain h-BN-LATP.

10. The method for preparing a composite separator for a semi-solid lithium battery according to claim 7, characterized in that: In the h-BN-LATP suspension, the mass ratio of the h-BN-LATP to the solvent is 1:5-12.

11. The method for preparing a composite diaphragm for a semi-solid lithium battery according to claim 7, wherein the aramid glue solution further contains a co-solvent, and the mass content of the co-solvent is ≤10%; The co-solvent is selected from at least one of CaCl2, KOH, LiCl and pyridine.

12. The method for preparing a composite separator for a semi-solid lithium battery according to claim 7, characterized in that: The solvent is selected from an organic solvent and / or water, and the organic solvent is selected from at least one of NMP, DMSO, DMF and DMAc; and / or The coating can be any one of blade coating, roller coating, wire rod coating and dip coating.

13. A semi-solid lithium ion battery, characterized in that: A composite diaphragm for a semi-solid lithium battery comprising the composite diaphragm for a semi-solid lithium battery as described in any one of claims 1 to 6 or a composite diaphragm for a semi-solid lithium battery as described in any one of claims 7 to 12.

Citation Information

Patent Citations

  • Composite coating lithium-ion battery separator and preparation method thereof

    CN105552284A

  • High-safety composite diaphragm and preparation method thereof

    CN111697187A

  • High-temperature-resistant diaphragm slurry with lithium pre-supplementing function, diaphragm and lithium battery

    CN113851782A

  • Preparation method of LATP-based solid electrolyte interface layer and preparation method of LATP-based solid lithium battery

    CN114883641A

  • Modified functional diaphragm for lithium metal battery and preparation method of modified functional diaphragm

    CN115764161A

Cited By

  • Composite diaphragm, preparation method thereof and lithium ion battery

    CN119994396A

  • Preparation method of high-temperature-resistant composite ceramic material

    CN120289189A

  • Composite diaphragm, preparation method thereof and application of composite diaphragm in semi-solid-state battery

    CN120581829A