Bendable perovskite solar cell based on high anti-reflection electrode and preparation method thereof

The flexible perovskite cell with a high anti-reflection electrode structure addresses manufacturing inefficiencies by using a bendable substrate and transparent electrode layer, improving light utilization and durability while reducing costs.

CN119072208APending Publication Date: 2024-12-03DALIAN JIAOTONG UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411121749.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Current perovskite solar cells face high manufacturing costs, low transmittance, high square resistance, and poor flexibility due to the use of FTO or ITO films as front electrodes, which require thick films and expensive materials, leading to inefficient light utilization and poor performance.

Method used

A flexible perovskite cell design featuring a high anti-reflection electrode structure with a bendable substrate, stacked refractive layers, a transparent electrode layer composed of metal oxide and alloy films, and an electron transport layer, allowing for efficient light trapping and reduced material costs.

Benefits of technology

The design achieves high light transmittance, low square resistance, and excellent flexibility, enhancing power generation efficiency and durability, enabling operation in extreme environments with reduced production time and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072208A_ABST
    Figure CN119072208A_ABST
Patent Text Reader

Abstract

The invention relates to the field of solar cells, in particular to a bendable perovskite solar cell based on a high anti-reflection electrode and a preparation method of the bendable perovskite solar cell. The perovskite cell sequentially comprises a flexible substrate with an anti-reflection structure, a microstructure layer, a transparent electrode layer, an electron transport layer, a perovskite thin film and modification layer, a hole transport layer and a top electrode layer from bottom to top. The perovskite solar cell has the advantages that the production is convenient, the finished product is bendable, the electrode has extremely high light transmittance and lower sheet resistance, the power generation power of the cell can be improved, and the thermal stability of the perovskite solar cell is ensured by adopting an all-solid-state material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of solar cells, and in particular to a flexible perovskite solar cell based on a high anti-reflection electrode and a preparation method thereof. Background Art

[0002] Photovoltaic power generation is one of the most promising energy sources to alleviate the energy crisis and replace fossil fuels. Perovskite can adopt organic-inorganic hybridization and is the most promising new photovoltaic technology.

[0003] However, current perovskite solar cells mainly use FTO film or ITO film as the front electrode. The thickness of the FTO film must reach 600-800nm ​​to achieve good photoelectric performance indicators, and a large amount of money is needed to purchase high-purity F and Sn materials. The manufacturing cost is high and the coating time is long. Due to the problem of material selection, there are still problems such as low transmittance, high square resistance and high preparation cost, and the performance of flexible perovskite cells is relatively poor. Summary of the invention

[0004] The present invention aims to overcome the deficiencies in the prior art and provide a method for preparing a perovskite cell with a highly light-transmitting electrode.

[0005] In order to achieve the above object, the technical solution of the present invention is as follows:

[0006] On one hand, the present invention provides a flexible perovskite cell based on a high anti-reflection electrode, wherein the perovskite cell comprises, from bottom to top, a flexible substrate with an anti-reflection structure, a microstructure layer, a transparent electrode layer, an electron transport layer, a perovskite film and a modification layer, a hole transport layer, and a top electrode layer;

[0007] The flexible substrate is bendable glass, and the upper surface roughness is 50-200 nm;

[0008] The anti-reflection structure is a first high-refractive layer, a first low-refractive layer, a second high-refractive layer, and a second low-refractive layer stacked in sequence from top to bottom on the bottom surface of the flexible substrate;

[0009] The first high refractive layer and the second high refractive layer are independently TiO x 、TiO x N y 、TaO x , WO x 、NbO x 、ZrO x Any one of the thin films, with a thickness of 20 to 200 nm and a refractive index of 2.0 to 2.6;

[0010] The first low-refractive layer is SiO2 microspheres or MgO microspheres with a diameter of 20 to 200 nm and a refractive index of 1.45 to 1.6;

[0011] The second low refractive layer is SiO2, SiO x N y , any one of MgO thin films, with a thickness of 10 to 100 nm and a refractive index of 1.45 to 1.7;

[0012] The microstructure layer is SiO2 microspheres with a diameter of 20 to 200 nm and a refractive index ranging from 1.45 to 1.6;

[0013] The transparent electrode layer is composed of a first metal oxide film, a first alloy film, a second metal oxide film and a second alloy film stacked in sequence from bottom to top;

[0014] The first metal oxide film and the second metal oxide film are independently any two or more combinations of ZnO, SnO2, ITO, and AZO films, and have a thickness of 15 to 90 nm;

[0015] The first alloy film is composed of an N-ion doped alloy film and an alloy film stacked in sequence from bottom to top, with a thickness of 5 to 20 nm, the thickness of the N-ion doped alloy film is 2 nm, the N-ion doping amount is 0.2% to 0.5%, and the alloy film is synthesized by at least one of Zr, Mo, V, and W metals and Ag metal, wherein the mass fraction of Ag metal is 90% to 99%;

[0016] The second alloy film is an N-ion doped alloy film with a thickness of 2 to 4 nm and an N-ion doping amount of 0.1 to 0.6%. The alloy film is synthesized from at least one of Zr, Mo, V, and W metals and Ag metal, wherein the mass fraction of Ag metal is 40% to 50%.

[0017] In the above technical solution, further, the electron transport layer is N or C doped TiO x The film has a thickness of 30 to 200 nm and is distributed with spherical titanium oxide, and the diameter of the spheres is 20 to 180 nm.

[0018] In the above technical solution, further, the perovskite film and the modified layer are composed of a perovskite film and a modified layer grown on the surface of the perovskite film, and the perovskite film is cesium lead bromide (CsPbBr3), methylamine lead iodide (MAPbI3), methyl lead bromide (MAPbBr3), methyl lead chlorobromide (MAPbBr 3-x Cl x ), methyl lead iodide (MAPbI 3-x Cl x), lead bromide (PbBr2), methylammonium bromide (MABr) or cesium bromide (CsBr) film with a thickness of 200 to 680 nm, and the modification layer is any one of trimethylbenzylammonium iodide (TMPMAI), 3-bromo-N-methylbenzylamine, alkylphosphonic acid, ammonium halide, TiO2, and ZnO film with a thickness of 2 to 20 nm.

[0019] In the above technical solution, further, the hole transport layer is a zinc oxide (ZnO), scandium oxide (Sc2O3) or SnO2 thin film with a thickness of 70 to 180 nm.

[0020] In the above technical solution, further, the top electrode layer is an N-ion doped alloy film with a thickness of 2 to 4 nm, and the N-ion doping amount is 0.5% to 2%. The alloy film is synthesized by at least one of Zr, Mo, V, and W metals and Ag metal, wherein the mass percentage of Ag is 80% to 90%.

[0021] Another aspect of the present invention provides a method for preparing the above-mentioned perovskite battery, the method comprising the following steps:

[0022] Step 1: etching the upper surface of the flexible substrate using an etching solution;

[0023] Step 2: preparing a first high refractive layer, a first low refractive layer, a second high refractive layer and a second low refractive layer in sequence from top to bottom on the bottom surface of the flexible substrate;

[0024] Step 3: preparing a microstructure layer on the upper surface of the flexible substrate;

[0025] Step 4: sequentially preparing a first metal oxide film, a first alloy film, a second metal oxide film, and a second alloy film on the microstructure layer from bottom to top;

[0026] Step 5: preparing an electron transport layer on the second alloy film by a sol-gel method or a spin coating method;

[0027] Step 6: preparing a perovskite film and a modification layer on the electron transport layer;

[0028] Step 7: preparing a hole transport layer on the perovskite film and the modified layer;

[0029] Step 8: Prepare a top electrode layer on the hole transport layer.

[0030] In the above technical solution, further, in step one, the etching solution used in the etching treatment is a mixed solution of hydrofluoric acid and dilute hydrochloric acid or oxalic acid, or a mixed solution of hydrofluoric acid and, and the mass fraction of hydrofluoric acid in the etching solution is 20% to 70%.

[0031] In the above technical solution, further, in step 2, the first high refractive layer and the second high refractive layer are prepared by a sol-gel method, a spin coating method or a magnetron sputtering method;

[0032] The first low-refractive layer is prepared by a Czochralski method or a doctor blade coating method;

[0033] The second low-refractive layer is prepared by a sol-gel method, a spin coating method or a magnetron sputtering method.

[0034] In the above technical solution, further, in step three, the microstructure layer is prepared by a pulling method or a doctor blade coating method.

[0035] In the above technical scheme, further, in step four, the first metal oxide film and the second metal oxide film are prepared by co-sputtering, chemical vapor deposition or sol-gel method; the first alloy film and the second alloy film are prepared by co-sputtering, evaporation or metal organic chemical vapor deposition.

[0036] In the above technical solution, further, in step five, the electron transport layer is prepared by a sol-gel method or a spin coating method.

[0037] The beneficial effects of the present invention are:

[0038] The present invention significantly demonstrates the convenience of production and the high flexibility of the product. By integrating an anti-reflection structure, a flexible and bendable light-trapping substrate, an anti-reflection microstructure layer and a transparent electrode layer with high transmittance, the preparation process of the present invention does not require heating and can be efficiently completed at room temperature. The coating time is also greatly shortened, greatly improving production efficiency.

[0039] In particular, the design of the transparent electrode layer not only has excellent light transmission performance, but also has extremely low square resistance. The oxide film is superimposed on the metal alloy film and doped with N ions, which can effectively play the role of anti-reflection and anti-transmission, prevent the oxidation of the metal film, reduce the nucleation barrier of the metal film, and enhance the light transmittance on the basis of improving the electrical performance; this innovative design effectively reduces light loss, thereby significantly improving the power generation of perovskite solar cells. At the same time, the perfect combination of the anti-reflection substrate and the transparent electrode layer further enhances the utilization rate of light and optimizes the battery performance.

[0040] The solar cell of the present invention has excellent flexibility. The overall structure can be easily bent, deformed or even curled to a shape with a curvature radius of only a few centimeters, and can even be completely folded. This is due to the excellent mechanical durability of the materials used. Even in the case of repeated bending, it will not break or leave marks, ensuring the reliability and stability of the battery in complex environments.

[0041] In addition, the invention uses all-solid-state materials to effectively ensure the thermal stability of perovskite solar cells, allowing them to maintain excellent performance in high-temperature environments. This innovative design not only broadens the application scenarios of the battery, but also provides a solid guarantee for its stable operation in extreme environments.

[0042] In summary, the present invention, with its unique anti-reflection structure, flexible and bendable design, high-transmittance transparent electrode layer and all-solid-state material construction, demonstrates excellent performance and innovative advantages in the field of perovskite solar cells, and opens up a new path for the future development of solar cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 It is a schematic structural diagram of a bendable perovskite solar cell based on a high antireflection electrode of the present invention;

[0044] Among them: 1. Flexible substrate, 2. Microstructure layer, 3. Transparent electrode, 4. Electron transport layer, 5. Perovskite film and modified layer, 6. Hole transport layer, 7. Top electrode layer;

[0045] 01, first high refractive layer, 02, first low refractive layer, 03, second high refractive layer, 04, second low refractive layer;

[0046] 31. a first metal oxide film, 32. a first alloy film, 33. a second metal oxide film, 34. a second alloy film;

[0047] Figure 2 is a light transmittance spectrum of a flexible substrate with an anti-reflection structure according to Example 3 of the present invention;

[0048] Figure 3 is a light transmittance spectrum of the transparent electrode layer in Example 3 of the present invention;

[0049] Figure 4 is the photoelectric conversion efficiency of the perovskite cell in Example 3 of the present invention. DETAILED DESCRIPTION

[0050] The following examples may enable those skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.

[0051] Unless otherwise specified, the materials used in the embodiments of the present invention can be obtained through commercial channels or prepared according to conventional methods well known to those skilled in the art.

[0052] Example 1

[0053] like Figure 1As shown, a flexible perovskite solar cell based on a high anti-reflection electrode includes, from bottom to top: a flexible substrate 1 with an anti-reflection structure, a microstructure layer 2, a transparent electrode layer 3, an electron transport layer 4, a perovskite film and a modified layer 5, a hole transport layer 6, and a top electrode layer 7;

[0054] The flexible substrate 1 is a bendable glass with a thickness of 0.3 mm and a top surface roughness of 100 nm;

[0055] The anti-reflection structure is a first high-refractive layer 01, a first low-refractive layer 02, a second high-refractive layer 03, and a second low-refractive layer 04 stacked in sequence from top to bottom on the bottom surface of the flexible substrate 1;

[0056] The first high refractive layer 01 is TiO x , with a thickness of 40nm and a refractive index of 2.21; the first low-refractive layer 02 is SiO2 microspheres, with a diameter of 100nm and a refractive index of 1.51; the second high-refractive layer 03 is TiO x , with a thickness of 40nm and a refractive index of 2.21; the second low-refractive layer 04 is a SiO2 film with a thickness of 40nm and a refractive index of 1.53;

[0057] Microstructure layer 2 is SiO2 microspheres with a diameter of 100 nm and a refractive index of 1.51;

[0058] The transparent electrode layer 3 is composed of a first metal oxide film 31, a first alloy film 32, a second metal oxide film 33 and a second alloy film 34 stacked in sequence from bottom to top;

[0059] The first metal oxide film 31 and the second metal oxide film 33 are SnO2 and AZO films co-doped, and have a thickness of 25 nm;

[0060] The first alloy film 32 is composed of a 0.3% N ion-doped ZrAg alloy film and a ZrAg alloy film stacked in sequence from bottom to top, the mass fraction of Ag metal in the ZrAg alloy is 99%, the thickness of the first alloy film 32 is 6nm, and the thickness of the 0.3% N ion-doped ZrAg alloy film is 2nm;

[0061] The second alloy film 34 is a 0.3% N ion doped ZrAg alloy film with a thickness of 2nm, and the mass fraction of Ag metal in the ZrAg alloy is 50%;

[0062] The electron transport layer 4 is N-doped TiO x The film has a thickness of 60nm and is distributed with spherical titanium oxide with a sphere diameter of 50nm;

[0063] The perovskite film and modification layer 5 consist of a CsPbBr3 film with a thickness of 380 nm and a modification layer of trimethylbenzyl ammonium iodide film grown on the surface thereof, and the thickness of the TMPMAI modification layer is 3 nm;

[0064] The hole transport layer 6 is a ZnO thin film with a thickness of 70 nm;

[0065] The top electrode layer 7 is a 1% N ion doped ZrAg alloy film with a thickness of 2 nm. The mass fraction of Ag in the ZrAg alloy is 90%.

[0066] The method for preparing the above-mentioned flexible perovskite solar cell based on a high antireflection electrode comprises the following steps:

[0067] (1) Covering the bottom surface of the flexible substrate 1 with a layer of protective paper, and then covering the protective paper with a layer of film, ensuring that the film completely covers the protective paper, and sticking it to the edge of the etching surface, and performing ultrasonic etching for 5 minutes with a solution of 40% hydrofluoric acid: 1% dilute hydrochloric acid = 50%: 50% (unit: mass fraction) to obtain a self-trapping light glass with a roughness of 100 nm;

[0068] (2) Using the sol-gel method, a mixed solution of butyl titanate and anhydrous ethanol is dripped into a mixed solution of anhydrous ethanol and nitric acid at a rate of 2 drops / second to form a gel, which is then coated on the unetched surface of the flexible substrate 1 and then heat treated in an oven at 400°C for 3 hours to convert the gel into a dense TiO x The first high refractive layer 01 is obtained by immersing the sample obtained above into a 1% ethanol SiO2 microsphere solvent with a diameter of 100nm, and the substrate is vertically pulled out from the suspension at a speed of 2 mm / s. During the pulling process, due to the capillary force and the liquid flow caused by the evaporation of the solvent, the microspheres will form a uniform SiO2 microsphere layer on both sides of the substrate, and the first low refractive layer 02 is obtained by drying at 100°C in an oven for 4 hours; the second high refractive layer 03 is prepared on the surface of the first low refractive layer 02 by the same preparation method as the first high refractive layer 01; the mixed solution of tetraethyl orthosilicate and anhydrous ethanol is dripped into the mixed solution of anhydrous ethanol and concentrated hydrochloric acid at a speed of 3 drops / second by the sol-gel method, and the mixture is stirred evenly, and the mixture is allowed to stand for aging for 2 days to form a sol coating on the second high refractive layer 03, and then the mixture is dried at 100°C in a drying oven for 2 hours, and heat-treated at 500°C for 1 hour to form a dense SiO2 film, and the second low refractive layer 04 is obtained;

[0069] (3) preparing SiO2 microspheres on the etched surface of the flexible substrate 1, and simultaneously completing the SiO2 microspheres of the first low-refractive layer 02 by using a Czochralski method to obtain a microstructure layer 2;

[0070] (4) using a co-sputtering method with a working pressure of 0.5 Pa and a sputtering power of 100 W of SnO2 target and 100 W of AZO target (ZnO: Al2O3 = 97%: 3%) to prepare a SnO2 and AZO co-doped film to obtain a first metal oxide film 31;

[0071] The first alloy film 32 is an alloy film synthesized from Zr and Ag metals. The co-sputtering method is adopted, the working pressure is 0.5Pa, the sputtering power is 2W for Zr target and 200W for Ag target, and the Zr and Ag alloy film with a mass percentage of 1%:99% and a thickness of 6nm is prepared. At the same time, the first 2nm alloy film is doped with N ions by the ion source assisted method, 1sccm of N2 is introduced, the power is 10W, and the ZrAg alloy film is protected from oxidation;

[0072] The second metal oxide film 33 repeats the preparation steps of the first metal oxide film 31;

[0073] The second alloy film 34 is a ZrAg alloy film, which is prepared by co-sputtering with a working pressure of 0.5 Pa, a Zr target of 100 W and an Ag target of 110 W, and a ZrAg alloy film with a mass percentage of 49.7%:50% and a thickness of 2 nm. At the same time, an ion source assisted method is adopted, 2 sccm of N2 is introduced, the power is 10 W, and 0.3% N ions are doped to protect the ZrAg alloy film from being oxidized by contact with the second metal oxide film 33 and the electron transport layer 4.

[0074] (5) By spin coating, a mixture of tetrabutyl titanate and ethanol is added dropwise to a mixture of anhydrous ethanol and nitric acid, and then ammonia and spherical titanium oxide with a diameter of 40 nm are added, and the mixture is stirred thoroughly to form a gel, which is coated on the second alloy film 34, and then heat treated in an oven (heat treated at 400° C. for 3 hours) to convert the gel into a dense N-TiO2 film with spherical titanium oxide evenly and discretely distributed therein. x Thin film, obtaining an electron transport layer 4;

[0075] (6) Using a solution method, lead bromide (PbBr2) and cesium bromide (CsBr) were dissolved in dimethylformamide solvent to form a lead source solution and a cesium source solution, and then ligand oleylamine (OA) was added as a precursor solution, and the solutions were heated to 60°C. The cesium source solution was then quickly injected into the lead source solution to form a CsPbBr3 solution, ethanol was added, and the solution was coated on the electron transport layer 4, and dried in an oven at 50°C for 24 hours to obtain a CsPbBr3 solution with a thickness of 380 nm. 3 film; at the same time, a modified layer of trimethylbenzyl ammonium iodide (TMPMAI) film is grown on it, and the film is prepared by spin coating. The trimethylbenzyl solution is added with ethanol solvent, and then ammonium iodide reagent is added to form a uniform trimethylbenzyl ammonium iodide solution. The solution is heated to 60°C, and the solution is evenly spin-coated on the CsPbBr3 film at 1000r / min, and dried in an oven at 50°C for 12h to obtain a trimethylbenzyl ammonium iodide (TMPMAI) film with a thickness of 3nm;

[0076] (7) Using a sol-gel method, Zn(NO3)2·6H2O and ethanol were mixed and stirred until no obvious precipitation was observed, ethanolamine was added as a stabilizer, and the mixture was stirred continuously to obtain a sol, which was allowed to stand for 48 hours. The solution was evenly spin-coated on the perovskite film 5 and placed at 50°C for 48 hours to obtain a ZnO film with a thickness of 70 nm, thereby obtaining a hole transport layer 6;

[0077] (8) A co-sputtering method was adopted with a working pressure of 0.5 Pa and a sputtering power of 5 W for Zr target and 50 W for Ag target to prepare a Zr and Ag alloy film with a mass percentage of approximately 9%:90% and a thickness of 2 nm. At the same time, an ion source assisted method was adopted with 3 sccm of N2 and a power of 20 W to dope 1.0% N ions to protect the ZrAg alloy film from being oxidized by contact with the outside world.

[0078] This structure has excellent optical and electrical properties, and also has an anti-reflection effect. The transmittance of the substrate with an anti-reflection structure can be as high as 93.1%, and the transmittance of the transparent electrode can be as high as 84.5%, which can effectively increase the power generation of the perovskite cell; the photoelectric conversion efficiency of the perovskite cell is 13.86%.

[0079] Example 2

[0080] like Figure 1 As shown, a flexible perovskite solar cell based on a high anti-reflection electrode includes, from bottom to top: a flexible substrate 1 with an anti-reflection structure, a microstructure layer 2, a transparent electrode layer 3, an electron transport layer 4, a perovskite film and a modified layer 5, a hole transport layer 6, and a top electrode layer 7;

[0081] The flexible substrate 1 is a bendable glass with a thickness of 0.1 mm and a top surface roughness of 120 nm;

[0082] The anti-reflection structure is a first high-refractive layer 01, a first low-refractive layer 02, a second high-refractive layer 03, and a second low-refractive layer 04 stacked in sequence from top to bottom on the bottom surface of the flexible substrate 1;

[0083] The first high refractive layer 01 is TaO x , with a thickness of 50nm and a refractive index of 2.26; the first low-refractive layer 02 is SiO2 microspheres with a diameter of 150nm and a refractive index of 1.49; the second high-refractive layer 03 is TaO x , with a thickness of 50nm and a refractive index of 2.26; the second low refractive layer 04 is SiO x N y Thin film, thickness 50nm, refractive index 1.54;

[0084] Microstructure layer 2 is SiO2 microspheres with a diameter of 150 nm and a refractive index of 1.51;

[0085] The transparent electrode layer 3 is composed of a first metal oxide film 31, a first alloy film 32, a second metal oxide film 33 and a second alloy film 34 stacked in sequence from bottom to top;

[0086] The first metal oxide film 31 and the second metal oxide film 33 are SnO2 co-doped with ITO films, and have a thickness of 30 nm;

[0087] The first alloy film 32 is composed of a 0.2% N ion-doped MoAg alloy film and a MoAg alloy film stacked sequentially from bottom to top, the mass fraction of Ag metal in the MoAg alloy is 99.4%, the thickness of the first alloy film 32 is 7nm, and the thickness of the 0.2% N ion-doped MoAg alloy film is 2nm;

[0088] The second alloy film 34 is a 0.1% N ion doped MoAg alloy film, the mass fraction of Ag metal in the MoAg alloy is 55%, and the thickness is 3nm;

[0089] The electron transport layer 4 is C-doped TiO x The film has a thickness of 90nm and is distributed with spherical titanium oxide with a sphere diameter of 70nm;

[0090] The perovskite film and the modified layer 5 are composed of methyl lead iodide (MAPbI 3-x Cl x ) film and a modified layer 3-bromo-N-methylbenzylamine film grown on the surface thereof, the modified layer thickness being 5 nm;

[0091] The hole transport layer 6 is a Sc2O3 film with a thickness of 110 nm;

[0092] The top electrode layer 7 is a 1.5% N ion-doped MoAg alloy film with a thickness of 5 nm. The mass percentage of Ag in the MoAg alloy is 94%.

[0093] The method for preparing the above-mentioned flexible perovskite solar cell based on a high antireflection electrode comprises the following steps:

[0094] (1) Covering the bottom surface of the flexible substrate 1 with a layer of protective paper, and then covering the protective paper with a layer of film, ensuring that the film completely covers the protective paper, and sticking it to the edge of the etching surface, and etching it through a solution of 40% hydrofluoric acid: 1% dilute hydrochloric acid = 60%: 40% (mass fraction) and ultrasonic etching for 5 minutes to obtain a self-trapping light glass with a roughness of 120 nm;

[0095] (2) Spin coating of TaO x The solution was coated on a spin coater at a rate of 2000 rpm, and then placed in an oven for heat treatment at 200 °C for 1 hour, and repeated once to obtain TaO x The film was obtained to obtain the first high refractive layer 01; the sample obtained above was placed on a doctor blade, 1 ml of ethanol SiO2 microsphere solvent was taken, and a uniform SiO2 microsphere layer with a diameter of 150 nm was obtained by doctor blade coating at a rate of 2 cm / s to obtain the first low refractive layer 02; the sample obtained above was coated with TaO x The solution was coated on a spin coater at a rate of 2000 rpm, and then placed in an oven for heat treatment at 200 °C for 1 hour, and repeated once to obtain TaO x The second high refractive layer 03 is obtained; the above-obtained sample is coated with SiO x N y The solution was coated on a spin coater at a rate of 1500 rpm, and then placed in an oven for heat treatment at 200 °C for 1 hour, and repeated once to obtain SiO x N y The film obtains the second low refractive layer 04;

[0096] (3) Place the sample obtained above on a doctor blade coater, take 1 ml of ethanol SiO2 microsphere solvent, with a diameter of 150 nm, and apply it on the etched surface of the flexible substrate 1 at a rate of 2 cm / s to obtain a uniform SiO2 microsphere layer, thereby obtaining a microstructure layer 2;

[0097] (4) The first metal oxide film 31 and the second metal oxide film 33 are prepared by chemical vapor deposition, using indium acetylacetonate (In(C5H7O2)3):tetramethyltin ((CH3)4Sn) = 7:3 (mass ratio) as precursors, heating to 300° C., introducing 10 sccm of oxygen and 30 sccm of argon, and forming SnO2 and ITO co-doped films;

[0098] The first alloy film 32 is a MoAg film deposited by vacuum evaporation. The Mo source is heated and baked to 900°C with an evaporation power of 10W, and the Ag source is heated and baked to 600°C with an evaporation power of 150W. At the same time, 1sccm of N2 is introduced in the first 10s to dope N ions to protect the MoAg alloy film from oxidation.

[0099] The second alloy film 34 is vacuum-deposited with N-ion-doped MoAg film. The Mo source is heated and baked to 900°C with a evaporation power of 100W. The Ag source is heated and baked to 600°C with a evaporation power of 120W. 1sccm of N2 is introduced to prepare MoAgN X film;

[0100] (5) Prepared by spin coating, high-purity TiO2 powder and organic carbon source are dissolved in ethanol solution, TiO2 powder: organic carbon source = 90%: 5%, then mixed with 5% of spherical titanium oxide solution with a diameter of 70nm, coated at a speed of 2500 rpm, and then placed in an oven for heat treatment at 300°C for 1 hour, repeated once, to obtain an electron transport layer 4;

[0101] (6) Methyl lead iodide (MAPbI) prepared by liquid phase method 3-x Cl x ) The film thickness is 420nm; at the same time, a modification layer of 3-bromo-N-methylbenzylamine is grown on it by a liquid phase method to obtain a perovskite film and a modification layer 5;

[0102] (7) preparing a scandium oxide (Sc2O3) thin film by a sol-gel method to obtain a hole transport layer 6;

[0103] (8) MoAg alloy thin film was deposited by vacuum evaporation. The Mo source was heated and baked to 900°C with a evaporation power of 30 W; the Ag source was heated and baked to 600°C with a evaporation power of 120 W. At the same time, 3 sccm of N2 was introduced to obtain a MoAgN alloy with a mass percentage of 14.5%:94%:1.5%. X .

[0104] This structure has excellent optical and electrical properties, and also has an anti-reflection effect. The transmittance of the substrate with an anti-reflection structure can be as high as 94.3%, and the transmittance of the transparent electrode can be as high as 85.8%, which can effectively increase the power generation of the perovskite cell; the photoelectric conversion efficiency of the perovskite cell is 14.69%.

[0105] Example 3

[0106] like Figure 1As shown, a flexible perovskite solar cell based on a high anti-reflection electrode includes, from bottom to top: a flexible substrate 1 with an anti-reflection structure, a microstructure layer 2, a transparent electrode layer 3, an electron transport layer 4, a perovskite film and a modified layer 5, a hole transport layer 6, and a top electrode layer 7;

[0107] The flexible substrate 1 is a bendable glass with a thickness of 0.06 mm and a top surface roughness of 150 nm;

[0108] The anti-reflection structure is a first high-refractive layer 01, a first low-refractive layer 02, a second high-refractive layer 03, and a second low-refractive layer 04 stacked in sequence from top to bottom on the bottom surface of the flexible substrate 1;

[0109] The first high refractive layer 01 is NbO x , with a thickness of 60nm and a refractive index of 2.32; the first low-refractive layer 02 is MgO microspheres, with a diameter of 110nm and a refractive index of 1.51; the second high-refractive layer 03 is NbO x , with a thickness of 60nm and a refractive index of 2.32; the second low-refractive layer 04 is a MgO film, with a thickness of 80nm and a refractive index of 1.53;

[0110] Microstructure layer 2 is MgO microspheres with a diameter of 110 nm and a refractive index range of 1.51;

[0111] The transparent electrode layer 3 is composed of a first metal oxide film 31, a first alloy film 32, a second metal oxide film 33 and a second alloy film 34 stacked in sequence from bottom to top;

[0112] The first metal oxide film 31 and the second metal oxide film 33 are co-doped with ITO and AZO, and have a thickness of 40 nm;

[0113] The first alloy film 32 is composed of a 0.2% N ion-doped WAG alloy film and a WAG alloy film stacked in sequence from bottom to top, the mass fraction of Ag metal in the WAG alloy is 99%, the thickness of the first alloy film 32 is 8nm, and the thickness of the 0.2% N ion-doped MoAg alloy film is 2nm;

[0114] The second alloy film 34 is a 0.5% N ion doped Wag alloy film, the mass fraction of Ag metal in the Wag alloy is 50%, and the thickness is 3nm;

[0115] The electron transport layer 4 is N-doped TiO x The film has a thickness of 140nm and is distributed with spherical titanium oxide with a sphere diameter of 100nm;

[0116] The perovskite film and the modified layer 5 consist of a cesium bromide (CsBr) film with a thickness of 510 nm and a modified ammonium halide film grown on the surface thereof, and the modified layer thickness is 6 nm;

[0117] The hole transport layer 6 is a SnO2 thin film with a thickness of 90 nm;

[0118] The top electrode layer 7 is a 1.3% N ion doped Wag alloy film with a thickness of 6 nm. The mass percentage of Ag in the Wag alloy is 90%.

[0119] The method for preparing the above-mentioned flexible perovskite solar cell based on a high antireflection electrode comprises the following steps:

[0120] (1) Covering the bottom surface of the flexible substrate 1 with a layer of protective paper, and then covering the protective paper with a layer of film, ensuring that the film completely covers the protective paper, and sticking it to the edge of the etching surface, and etching it through a solution of 40% hydrofluoric acid: 1% dilute hydrochloric acid = 70%: 30% (mass fraction) and ultrasonic etching for 6 minutes to obtain a self-trapping light glass with a roughness of 150 nm;

[0121] (2) The first high-refractive layer 01 and the second high-refractive layer 03 are prepared by magnetron sputtering, using NbO x The target material was sputtered at a power of 100 W, a pressure of 0.4 Pa, 40 sccm of argon gas, and the sputtering time was controlled to obtain NbO with a thickness of 60 nm and a refractive index of 2.32. x film;

[0122] The first low-refractive layer 02 is MgO microspheres. The sample obtained above is vertically immersed in a 1.5% ethanol MgO microsphere solvent with a diameter of 110 nm. The substrate is vertically pulled out of the suspension at a speed of 1 mm / s. During the pulling process, due to the capillary force and the liquid flow caused by the evaporation of the solvent, the microspheres will form a uniform MgO microsphere layer on both sides of the substrate. The substrate is dried in an oven at 100°C for 2 hours to obtain the first low-refractive layer 01.

[0123] The second low-refractive layer 04 is prepared by magnetron sputtering, using MgO target material, sputtering power of 120W, pressure of 0.6Pa, introducing 40sccm of argon gas, and controlling the sputtering time to obtain a MgO film;

[0124] (3) preparing MgO microspheres on the etched surface of the flexible substrate 1, and simultaneously completing the MgO microspheres of the first low-refractive layer 02 by using a Czochralski method to obtain a microstructure layer 2;

[0125] (4) The first metal oxide film 31 and the second metal oxide film 33 are prepared by a sol-gel method. The precursors of ITO are In(NO3)3·xH2O and SnCl4·5H2O, which are dissolved in an ethanol solution and a trace amount of acetic acid stabilizer is added. The precursors of AZO are Zn(CH3COO)2·2H2O) and Al(NO3)3·9H2O), which are dissolved in an ethanol solution and a trace amount of ammonia stabilizer is added. Then, the required amount of precursors is calculated according to the mass ratio of ITO to AZO of 8:2, and the precursors are mixed and stirred to form a uniform composite sol. The coating machine is started and spin-coated at a speed of 1500 rpm, and then high-speed spin-coating is performed at 3000 rpm to form a uniform film. Drying treatment is performed at 100°C for 30 min. The spin-coating and drying treatment is performed 5 times to obtain an ITO and AZO co-doped film. Heat treatment is performed at 300°C for 30 min to obtain an ITO and AZO co-doped film.

[0126] The first alloy film 32 is formed by metal organic chemical vapor deposition, using metal organic compounds of tungsten W(CO)6 and metal organic compounds of silver dimethylsilver (CH3)2Ag. The reaction chamber is heated to 400°C, and argon gas Ar is introduced to carry the precursors into the reaction chamber respectively. The flow rates of different precursor carrier gases are controlled to adjust the ratios of different metals. At the same time, 1 sccm of N2 is introduced in the first 10 seconds for trace doping. The deposition reaction is continued for 30 seconds to obtain the first alloy film 32.

[0127] The second alloy film 34 is deposited by metal organic chemical vapor deposition, metal organic compound W(CO)6 of tungsten, metal organic compound dimethylsilver (CH3)2Ag of silver, the reaction chamber is heated to 400°C, argon gas Ar is introduced to carry the precursor into the reaction chamber, and 3sccm of N2 is introduced for trace doping;

[0128] (5) By spin coating, a mixture of tetrabutyl titanate and ethanol is added dropwise into a mixture of anhydrous ethanol and nitric acid, and then ammonia and spherical titanium oxide with a diameter of 100 nm are added, and the mixture is stirred thoroughly to form a gel, which is coated on the second alloy film 34, and then heat treated in an oven (heat treated at 400° C. for 3 hours) to convert the gel into a dense N-ion-doped TiO2 layer with spherical titanium oxide distributed therein. x Thin film, obtaining an electron transport layer 4;

[0129] (6) A cesium bromide (CsBr) film obtained by physical method, and at the same time, a modified layer of ammonium halide is grown on it by liquid phase method to obtain a perovskite film and a modified layer 5;

[0130] (7) A SnO2 thin film prepared by vapor deposition method is used to obtain a hole transport layer 6;

[0131] (8) Metal organic chemical vapor deposition (MOCVD) was used to prepare the metal organic compound of tungsten W(CO)6 and the metal organic compound of silver dimethylsilver (CH3)2Ag. The reaction chamber was heated to 400°C, and argon gas Ar was introduced to carry the precursors into the reaction chamber. 6 sccm of N2 was introduced for trace doping to obtain the top electrode layer 7.

[0132] This structure has excellent optical and electrical properties, and also has an anti-reflection effect. The transmittance of the substrate with an anti-reflection structure can be as high as 95.2%, and the transmittance of the transparent electrode can be as high as 87.4%, which can effectively increase the power generation of the perovskite cell; the photoelectric conversion efficiency of the perovskite cell is 15.7%.

[0133] The above embodiments are only preferred embodiments of the present invention and are not intended to limit the implementation methods. The protection scope of the present invention shall be subject to the scope defined in the claims. Other different forms of changes or modifications may be made based on the above description. Obvious changes or modifications derived therefrom are still within the protection scope of the present invention.

Claims

1. A flexible perovskite cell based on a high antireflection electrode, Features: The perovskite cell comprises, from bottom to top, a flexible substrate with an anti-reflection structure (1), a microstructure layer (2), a transparent electrode layer (3), an electron transport layer (4), a perovskite film and a modified layer (5), a hole transport layer (6), and a top electrode layer (7); The flexible substrate (1) is bendable glass, and the upper surface roughness is 50 to 200 nm; The anti-reflection structure comprises a first high-refractive layer (01), a first low-refractive layer (02), a second high-refractive layer (03), and a second low-refractive layer (04) stacked in sequence from top to bottom on the bottom surface of the flexible substrate (1); The first high-refractive layer (01) and the second high-refractive layer (03) are independently TiO x 、TiO x N y 、TaO x , WO x 、NbO x 、ZrO x Any one of the thin films, with a thickness of 20 to 200 nm and a refractive index of 2.0 to 2.6; The first low refractive layer (02) is SiO 2 Microspheres or MgO microspheres, with a diameter of 20 to 200 nm and a refractive index of 1.45 to 1.6; The second low refractive layer (04) is SiO 2 、SiO x N y , any one of MgO thin films, with a thickness of 10 to 100 nm and a refractive index of 1.45 to 1.7; The microstructure layer (2) is SiO 2 Microspheres, with diameters of 20 to 200 nm and refractive indices ranging from 1.45 to 1.6; The transparent electrode layer (3) is composed of a first metal oxide film (31), a first alloy film (32), a second metal oxide film (33) and a second alloy film (34) which are stacked in sequence from bottom to top; The first metal oxide film (31) and the second metal oxide film (33) are independently ZnO, SnO 2 Any combination of two or more of ITO and AZO thin films, with a thickness of 15 to 90 nm; The first alloy film (32) is composed of an N-ion doped alloy film and an alloy film stacked in sequence from bottom to top, with a thickness of 5 to 20 nm, the thickness of the N-ion doped alloy film is 2 nm, the N-ion doping amount is 0.2% to 0.5%, and the alloy film is synthesized from at least one of Zr, Mo, V, and W metals and Ag metal, wherein the mass fraction of Ag metal is 90 to 99%; The second alloy film (34) is an N-ion doped alloy film with a thickness of 2 to 4 nm and an N-ion doping amount of 0.1% to 0.6%. The alloy film is synthesized from at least one of Zr, Mo, V, and W metals and Ag metal, wherein the mass fraction of Ag metal is 40% to 50%.

2. The bendable perovskite cell based on a high antireflection electrode according to claim 1, Features: The electron transport layer (4) is N or C doped TiO x The film has a thickness of 30 to 200 nm and is distributed with spherical titanium oxide, and the diameter of the spheres is 20 to 180 nm.

3. The bendable perovskite cell based on a high antireflection electrode according to claim 1, Features: The perovskite film and the modified layer (5) are composed of a perovskite film and a modified layer grown on the surface of the perovskite film. The perovskite film is cesium lead bromide, methylamine lead iodide, methyl lead bromide, methyl lead chlorobromide, methyl lead chloroiodide, lead bromide, methyl ammonium bromide or cesium bromide film, with a thickness of 200 to 680 nm. The modified layer is trimethylbenzyl ammonium iodide, 3-bromo-N-methylbenzylamine, alkylphosphonic acid, ammonium halide, TiO 2 , any one of ZnO thin films, with a thickness of 2 to 20 nm.

4. The bendable perovskite cell based on a high antireflection electrode according to claim 1, Features: The hole transport layer (6) is zinc oxide, scandium oxide or SnO 2 Thin film, thickness is 70~180nm.

5. The bendable perovskite cell based on a high antireflection electrode according to claim 1, Features: The top electrode layer (7) is an N-ion doped alloy film with a thickness of 2 to 4 nm and an N-ion doping amount of 0.5% to 2%. The alloy film is synthesized from at least one of Zr, Mo, V, and W metals and Ag metal, wherein the mass percentage of Ag is 80% to 90%.

6. A method for preparing a perovskite battery according to any one of claims 1 to 5, Features: The method comprises the following steps: Step 1: etching the upper surface of the flexible substrate (1) using an etching solution; Step 2: preparing a first high refractive layer (01), a first low refractive layer (02), a second high refractive layer (03) and a second low refractive layer (04) in sequence from top to bottom on the bottom surface of the flexible substrate (1); Step 3: preparing a microstructure layer (2) on the upper surface of the flexible substrate (1); Step 4: preparing a first metal oxide film (31), a first alloy film (32), a second metal oxide film (33) and a second alloy film (34) on the microstructure layer (2) from bottom to top; Step 5: preparing an electron transport layer (4) on the second alloy film (34) by a sol-gel method or a spin coating method; Step 6: preparing a perovskite film and a modification layer (5) on the electron transport layer (4); Step 7: preparing a hole transport layer (6) on the perovskite film and the modified layer (5); Step 8: Prepare a top electrode layer (7) on the hole transport layer (6).

7. The preparation method according to claim 6, Features: In step 2, the first high refractive layer (01) and the second high refractive layer (03) are prepared by a sol-gel method, a spin coating method or a magnetron sputtering method; The first low-refractive layer (02) is prepared by a Czochralski method or a doctor blade coating method; The second low-refractive layer (04) is prepared by a sol-gel method, a spin coating method or a magnetron sputtering method.

8. The preparation method according to claim 6, Features: In step three, the microstructure layer (2) is prepared by a pulling method or a scraping method.

9. The preparation method according to claim 6, Features: In step four, the first metal oxide film (31) and the second metal oxide film (33) are prepared by co-sputtering, chemical vapor deposition or sol-gel method; the first alloy film (32) and the second alloy film (34) are prepared by co-sputtering, evaporation or metal organic chemical vapor deposition.

10. The preparation method according to claim 6, Features: In step five, the electron transport layer (4) is prepared by a sol-gel method or a spin coating method.