Method for preparing cathode active material and cathode active material obtained thereby
Through multi-step calcination and instantaneous heat treatment technology, a single crystal cathode active material with high Ni NCM was prepared, which solved the problems of poor shape and complex washing steps, and achieved efficient industrial-scale production and improved battery performance.
Patent Information
- Application Number
- CN202380034655.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-18
- Filing Date
- 2023-04-12
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to efficiently prepare single crystal cathode active materials with good shape on industrial scale, and commonly used methods require additional washing steps to remove residual flux, which increases cost and complexity.
Using a multi-step calcination process, including heating at a temperature between 300°C and 600°C and 750°C to 900°C, combined with instantaneous heat treatment (TTT) to form a single crystal cathode active material with an octahedral structure, using stoichiometric of LiNixCoyMnzO2 High Ni NCM was prepared by a co-precipitation and drying step with the lithium source.
It has achieved the improvement of high voltage density and conductivity, and formed a single crystal NCM with a uniform octahedral shape, simplified the production process, is suitable for industrial-scale production, and improved the energy density and charging and discharge rate of the battery.
Smart Images

Figure BDA0005089123580000121 
Figure BDA0005089123580000122 
Figure HDA0005089123590000011
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing a cathode active material, and more particularly to a method for preparing a single crystal cathode active material having an octahedral structure. Background Art
[0002] Lithium-ion batteries are widely used in various fields, from small devices such as mobile phones and laptops to car batteries and other batteries for electric vehicles. The electrodes, electrolytes and separators, which are the main parts of the battery, together determine the performance of the battery. Among them, the cathode active material (CAM) accounts for about 30% of the total cost of battery manufacturing, thus playing a key role in lithium-ion battery technology. And commonly used cathode active materials include lithium iron phosphate, lithium cobalt oxide and lithiated nickel-cobalt-manganese oxide ("NCM").
[0003] NCM is a preferred choice because Li ions have a higher diffusion rate and electron mobility, and thus achieve a higher energy density. And high Ni NCM, i.e., NCM with a Ni content of at least 80% by mole based on the total molar number of Ni, Co and Mn, has been developed to meet the requirements of electric vehicles (EVs). Examples of high Ni NCM include LiNi 0.80 Co 0.10 Mn 0.10 O2(Ni80),LiNi 0.83 Co 0.12 Mn 0.05 O2(Ni83),LiNi 0.88 Co 0.06 Mn 0.06 O2(Ni88),LiNi 0.90 Co 0.05 Mn 0.05 O2(Ni90) and LiNi 0.92 Co 0.04 Mn 0.04 O2(Ni92).
[0004] Meanwhile, single-crystal CAM (SCM) is becoming more and more attractive due to fewer phase boundaries and exposed surfaces compared with polycrystalline materials, which can effectively reduce structural degradation, electrolyte side reactions and gas generation and further improve the cycle stability and safety of cathode active materials. However, SCM on the market shows irregular and unshaped bulk morphology, which obviously does not meet the definition of SCM, i.e., a regular polyhedral shape with different edges.
[0005] It has been reported that adding Na2SO4 and NaCl as fluxes during the calcination step of producing SCM can form well-shaped SCM, however, a washing step is required to remove the residual Na2SO4 and NaCl, which brings additional cost and also makes the process more complicated, especially when scaling up the preparation from laboratory to large-scale production.
[0006] Therefore, there is still a need to provide a method for producing well-shaped SCMs suitable for industrial scale. Summary of the invention
[0007] In one aspect, the present invention provides a method for preparing a cathode active material having formula (I), the method comprising the following steps:
[0008] LiNi x Co y Mn z O2(I)
[0009] i) Preparing precursors of hydroxides or carbonates of Ni, Co and Mn;
[0010] ii). mixing the precursor obtained from step i) with a Li source; and
[0011] iii). calcining the mixture obtained from step ii), wherein said step iii) comprises a multi-step calcination, wherein x is in the range of 0.80 to 0.95 and preferably 0.80 to 0.92, y is in the range of 0.01 to 0.15 and preferably 0.01 to 0.12, and z is in the range of 0.01 to 0.15 and preferably 0.01 to 0.12, and the sum of x, y and z is 1.
[0012] In another aspect, the present invention provides a single crystal cathode active material having an octahedral structure and having formula (I):
[0013] LiNi x Co y Mn z O2(I)
[0014] wherein x is in the range of 0.80 to 0.95 and preferably 0.80 to 0.02, y is in the range of 0.01 to 0.15 and 0.01 to 0.12, and z is in the range of 0.01 to 0.15 and preferably 0.01 to 0.12, and the sum of a, b and c is 1; wherein the lattice parameters a, b, c are respectively and Wherein the single crystal has an average particle size of 3.5um to 4.5um measured according to PSD (particle size distribution), a pressing density of 3.0g / ml to 4.0g / ml measured by a powder resistivity measuring unit MCP-PD51 provided by MITSUBISHI Mitsubishi Chemical Analytech Co., Ltd., and an electrical conductivity of 0.004S / m to 0.08S / m according to JIS K7194 / JIS R 1637.
[0015] In another aspect, the present invention provides a cathode comprising
[0016] (A) 50% to 98.99% by weight of a cathode active material obtained by the process of the present invention,
[0017] (B) 1 to 5% by weight of carbon in an electrically conductive state,
[0018] (C) 0.01% to 5% by weight of a binder, and
[0019] (D) 0 to 50% by weight of a solid electrolyte, based on the total weight of components (A), (B), (C) and (D). DETAILED DESCRIPTION
[0020] The present invention provides a method for preparing a cathode active material having formula (I), the method comprising the following steps:
[0021] LiNi x Co y Mn z O2(I)
[0022] i) Preparing precursors of hydroxides or carbonates of Ni, Co and Mn;
[0023] ii). mixing the precursor obtained from step i) with a Li source; and
[0024] iii). calcining the mixture obtained from step ii), wherein said step iii) comprises a multi-step calcination, wherein x is in the range of 0.80 to 0.95 and preferably 0.80 to 0.92, y is in the range of 0.01 to 0.15 and preferably 0.01 to 0.12, and z is in the range of 0.01 to 0.15 and preferably 0.01 to 0.12, and the sum of x, y and z is 1.
[0025] The cathode active material of formula (I) is a high Ni NCM product comprising at least 80% by mole of elemental Ni based on the total moles of elemental Ni, Co and Mn. An example may be LiNi 0.80Co 0.10 Mn 0.10 O2(Ni80),LiNi 0.83 Co 0.12 Mn 0.05 O2(Ni83),LiNi 0.88 Co 0.06 Mn 0.06 O2(Ni88),LiNi 0.90 Co 0.05 Mn 0.05 O2(Ni90) and LiNi 0.92 Co 0.04 Mn 0.04 O2(Ni92), preferably LiNi 0.83 Co 0.12 Mn 0.05 O2(Ni83),LiNi 0.88 Co 0.06 Mn 0.06 O2(Ni88),LiNi 0.90 Co 0.05 Mn 0.05 O2(Ni90) and LiNi 0.92 Co 0.04 Mn 0.04 O2(Ni92), more preferably LiNi 0.88 Co 0.06 Mn 0.06 O2(Ni88),LiNi 0.90 Co 0.05 Mn 0.05 O2(Ni90) and LiNi 0.92 Co 0.04 Mn 0.04 O2(Ni92) and even more preferably LiNi 0.90 Co 0.05 Mn 0.05 O2(Ni90) and LiNi 0.92 Co 0.04 Mn 0.04 O2(Ni92).
[0026] Steps (i) to (iii) of the method of the present invention are carried out in sequence and can be carried out with or without one or more intermediate steps. In some embodiments, the precursor in step (i) can be prepared by coprecipitating Ni, Co and Mn as hydroxides. In this case, a solution of a water-soluble salt containing nickel, cobalt and manganese is contacted with an alkali, such as a solution of an alkali metal hydroxide or an alkali metal carbonate, preferably a solution of an alkali metal hydroxide. Examples of alkali metal hydroxides are potassium hydroxide and sodium hydroxide. Examples of alkali metal carbonates are sodium carbonate, sodium bicarbonate, potassium carbonate and potassium bicarbonate. Contact with an alkali can be carried out by simultaneously feeding an alkali with a solution of one or more water-soluble salts of nickel, cobalt and manganese into a container (preferably under stirring). Such contact is preferably carried out by feeding a solution of an alkali metal hydroxide and a solution of a water-soluble salt of cobalt, nickel and manganese according to the molar ratio in formula (I). In the context of the present invention, water-soluble shall mean that the salt has a solubility of at least 20 g / l in distilled water at 20° C., the amount of salt being determined omitting crystal water and water from the aqueous complex. The water-soluble salts of nickel, cobalt and manganese may preferably be Ni 2+ 、Co 2+ and Mn 2+ The corresponding water-soluble salts.
[0027] The coprecipitation in step (i) is preferably carried out at a temperature in the range of 10° C. to 85° C., more preferably 20° C. to 60° C. The coprecipitation in step (i) is preferably carried out at a pH value (measured in the mother liquor at 23° C.) in the range of 8 to 13, more preferably 11 to 12.5, and even more preferably 11.5 to 12.2. The coprecipitation is carried out at a pressure in the range of 0.5 bar to 20 bar, preferably at 1 atm.
[0028] Based on the total moles of the elements Ni, Co and Mn, a stoichiometric or excess amount of base, such as an alkali metal hydroxide, is used. The molar excess can be, for example, in the range of 1.01:1 or greater, and preferably a stoichiometric ratio is used. The aqueous solution of the alkali metal hydroxide has a concentration in the range of 1% to 50% by weight, preferably 10% to 25% by weight. The concentration of the aqueous solution of nickel, cobalt and manganese salts can be in a wide range, preferably in the range of 1 mol / L to 1.8 mol / L, more preferably 1.5 mol / L to 1.7 mol / L of the total moles of nickel, cobalt and manganese based on the volume of the solution.
[0029] The coprecipitation in step (i) is carried out in the presence of at least one compound L which can act as a ligand for at least one transition metal, such as an organic amine, preferably ammonia. The concentration of compound L (such as ammonia) is preferably in the range of 0.05 mol / L to 1 mol / L, more preferably 0.1 mol / L to 0.7 mol / L. Preferably, the amount of ammonia should be considered so that the soluble Ni in the mother liquor 2+ The amount of ions does not exceed 1000 ppm, more preferably does not exceed 500 ppm.
[0030] During the coprecipitation of step (i), mixing with a stirrer is preferably performed at a stirring speed of at least 1 W / l, more preferably at least 3 W / l and even more preferably at least 5 W / l and not more than 25 W / l. Preferably, no reducing agent, such as hydrazine, ascorbic acid, glucose and alkali metal sulfite, is used during the coprecipitation of step (i).
[0031] The coprecipitation in step (i) can be carried out in air, in an inert gas atmosphere (such as a rare gas or nitrogen atmosphere) or in a reducing atmosphere (such as SO2), and is preferably carried out in air or inert gas atmosphere.
[0032] The coprecipitation in step (i) provides a mixed hydroxide or carbonate, preferably a hydroxide of nickel, cobalt and manganese, in a mother liquor in the form of a slurry of particles. The particles preferably have a spherical shape. The spherical particles should include not only particles with a precise spherical shape, but also particles whose maximum and minimum diameters differ by no more than 10%, preferably no more than 5%.
[0033] In some embodiments of the present invention, the coprecipitation in step (i) is carried out for a period of 1 hour to 40 hours, preferably 2 hours to 30 hours. And in some other embodiments, step (i) is carried out with an intermediate step, and the time period excluding the intermediate step is in the range of 1 hour to 40 hours, preferably 2 hours to 30 hours.
[0034] The obtained precursor is removed from the mother liquor and dried in the presence of an oxygen-containing atmosphere. The removal can be achieved by filtering, centrifuging, decantation, spray drying, sedimentation or a combination thereof. Suitable equipment is, for example, a filter press, a belt filter, a spray dryer, a hydrocyclone, an inclined clarifier or a combination thereof.
[0035] After removal, the precursor can be washed. Washing can be achieved, for example, with pure water or with an aqueous solution of alkali metal carbonate or alkali metal hydroxide, preferably with an aqueous solution of sodium carbonate, potassium carbonate, sodium hydroxide, potassium hydroxide or ammonia, more preferably with an aqueous solution of water and sodium hydroxide. Washing can be achieved, for example, by adopting an elevated pressure or elevated temperature (e.g., 30° C. to 50° C.). In certain embodiments, washing is carried out at room temperature. Washing efficiency can be checked by analytical measurement. For example, the content of one or more transition metals in the washing water can be analyzed. If washing is achieved by water rather than an aqueous solution of alkali metal hydroxide, then after washing, the conductivity of the water can be used to check whether any water-soluble substances (e.g., water-soluble salts) can still be washed off.
[0036] After removal, drying can be carried out in the presence of oxygen. In this context, the presence of oxygen refers to the presence of an oxygen-containing gas, such as air, pure oxygen, a mixture of oxygen and air, and an air atmosphere diluted with an inert gas such as nitrogen. Drying can be carried out, for example, at a temperature in the range of 30° C. to 150° C.
[0037] To carry out step (ii) of the process of the invention, the precursor may be mixed with at least one lithium source, for example at least one compound selected from Li2O, LiOH and Li2CO3, and preferably the lithium source is Li2CO3. The amounts of the precursor and the lithium compound are selected to obtain the stoichiometry in formula (I).
[0038] The mixing in step (ii) can be carried out at ambient temperature and 1atm. In certain embodiments, the mixing is carried out in a mixer, such as a paddle mixer, a ploughshare mixer, a free-fall mixer, a roller mill or a high-shear mixer. And a ploughshare mixer is preferred. Mixing can be implemented at a speed in the range of 5rpm to 500rpm, preferably 5rpm to 60rpm. When a free-fall mixer is applied, a speed preferably in the range of 5rpm to 25rpm and more preferably 5rpm to 10rpm. When a ploughshare mixer is applied, a speed preferably in the range of 50rpm to 400rpm and more preferably 100rpm to 250rpm. When a high-shear mixer is applied, the speed of the preferred agitator is in the range of 100rpm to 950rpm, and the speed of the chopper is in the range of 100rpm to 3750rpm.
[0039] In order to carry out step (iii) of the method of the present invention, the mixture of the precursor and the lithium compound is calcined in multiple steps. The multiple steps include a step A of heating at a temperature in the range of 300°C to 600°C and preferably 400°C to 600°C and a step B of heating at a temperature in the range of 750°C to 900°C and preferably 750°C to 850°C after step A. The step A has a time period of 1 hour to 7 hours and preferably 3 hours to 5 hours. And the step B has a time period of 6 hours to 16 hours and preferably 8 hours to 14 hours. From step A to step B, a heating rate of 1K / min to 10K / min, preferably 2K / min to 5K / min, can be applied. During step A, the heating temperature remains stable within a fluctuation of ±5°C.
[0040] The step (iii) of the inventive method can be carried out in a furnace, such as a rotary tube furnace, a muffle furnace, a swing furnace, a roller hearth furnace, a straight furnace and a combination thereof. In certain embodiments, step (iii) is carried out in an oxygen-containing atmosphere. Examples of oxygen-containing atmospheres include air, pure oxygen, a mixture of oxygen and air, and air diluted with an inert gas such as nitrogen. Preferably, oxygen or an oxygen atmosphere diluted with air or nitrogen is used, and the minimum content of oxygen is 21% by volume. In some other embodiments, step (iii) is carried out in an atmosphere with reduced CO2 content, for example, a carbon dioxide content in the range of 0.01ppm to 500ppm by weight, preferably 0.1ppm to 50ppm by weight. CO2 content can be determined by, for example, an optical method using infrared light. More preferably, step (iii) is implemented in an atmosphere where the carbon dioxide content is lower than the lower limit detectable by an optical method using infrared light.
[0041] Step B includes transient thermal treatment (TTT). "Transient thermal treatment (TTT)" as used herein means that during step B of step (iii), the temperature is increased by 100°C to 450°C and maintained for a short time compared to the baseline temperature of step B. The temperature of TTT may be in the range of 1000°C to 1400°C, preferably 1000°C to 1200°C, such as 1000°C to 1100°C. The duration of TTT may be 1 min to 1 hour, preferably 1 min to 30 min, more preferably 5 min to 20 min. During step B, except for the time period of TTT, the heating temperature remains stable within a fluctuation of ±5°C.
[0042] TTT is carried out in an oxygen-containing atmosphere. Examples of oxygen-containing atmospheres include air, pure oxygen, a mixture of oxygen and air, and air diluted with an inert gas such as nitrogen. In TTT, it is preferred to use oxygen or an oxygen atmosphere diluted with air or nitrogen, and the minimum content of oxygen is 21% by volume.
[0043] During the temperature change from the base temperature of step B to the temperature of TTT, a heating rate of 1 K / min to 10 K / min and preferably 2 K / min to 5 K / min can be applied. During the temperature change from the temperature of TTT back to the base temperature of step B, the same cooling rate can be applied.
[0044] TTT may be performed from the beginning to the end of step B, at any stage in step B. Preferably, TTT may be started at a time point of 1 / 10 to 9 / 10, more preferably 1 / 5 to 4 / 5, and even more preferably 2 / 5 to 4 / 5 of the duration of step B.
[0045] Surprisingly, it has been found that by adding TTT during the duration of step B, single crystalline NCM with a uniform octahedral shape is obtained. In addition, the pressing density and electronic conductivity of the single crystalline NCM are shown to be at least 3.257 g / mL and at least 0.022 S / m, respectively, which are approximately 7.0% and 1.5 times higher than the average level on the market (3.046 g / mL; 0.00873 S / m). As is known in the art, the pressing density is associated with the energy density in the battery, and the greater the pressing density, the greater the energy density in the battery will be. On the other hand, the conductivity of the material is associated with the charging and discharging rate of the battery. This comparison shows that the potential of standard SCM as a cathode active material is considerable. In addition, the high simplicity of the TTT procedure significantly overcomes the technical barriers to product scale-up, making it more suitable for industrial production than the prior art.
[0046] Another aspect of the invention relates to electrodes comprising single-crystalline NCM obtained by the method of the invention. They are particularly useful for lithium-ion batteries. Lithium-ion batteries comprising at least one electrode of the invention exhibit very good charge / discharge and high capacity. Electrodes comprising single-crystalline NCM obtained by the method of the invention are also referred to hereinafter as electrodes of the invention or electrodes according to the invention, or as cathodes of the invention.
[0047] In some embodiments of the present invention, the electrode of the present invention is in the form of a thin film electrode. The thin film electrode comprises the electrode active material of the present invention. Physical or chemical vapor deposition techniques can be used to produce the thin film. The electrode film has a thickness in the range of 10 nm to 10,000 nm, preferably 100 nm to 5,000 nm.
[0048] In some embodiments of the present invention, the electrode of the present invention comprises a current collector and
[0049] (A) a single-crystalline NCM obtained by the method of the present invention,
[0050] (B) carbon in an electrically conductive form,
[0051] (C) an adhesive, and
[0052] (D) Optionally, a solid electrolyte.
[0053] In some embodiments of the present invention, the electrode of the present invention comprises a current collector and
[0054] (A) 50% to 98.99% by weight of single-crystalline NCM obtained by the method of the present invention,
[0055] (B) 1 to 5% by weight of carbon in an electrically conductive form,
[0056] (C) 0.01% to 5% by weight of a binder, and,
[0057] (D) 0 to 50% by weight of a solid electrolyte, based on the total weight of components (A), (B), (C) and (D).
[0058] The current collector used in the electrode of the present invention may be, for example, but not limited to, aluminum foil.
[0059] The electrode according to the invention further contains carbon in an electrically conductive form, also referred to as carbon (B) for short. Carbon (B) can be selected from soot, activated carbon, carbon nanotubes, graphene and graphite. Carbon (B) can be added as is during the preparation of the electrode material according to the invention.
[0060] In some embodiments, the amount of carbon (B) relative to the electrode material of the present invention is in the range of 1% to 15% by weight, preferably at least 2% by weight, relative to the sum of components (A), (B), (C) and (D).
[0061] The electrode of the present invention may further comprise a binder (C). Suitable binders (C) are preferably selected from organic (co)polymers. Suitable (co)polymers, i.e. homopolymers or copolymers, may be selected from (co)polymers obtainable, for example, by anionic, catalytic or free radical (co)polymerization, in particular selected from polyethylene, polyacrylonitrile, polybutadiene, polystyrene, and copolymers of at least two comonomers selected from ethylene, propylene, styrene, (meth)acrylonitrile and 1,3-butadiene. Polypropylene is also suitable. In addition, polyisoprene and polyacrylate are also suitable. Polyacrylonitrile is particularly preferred.
[0062] In the context of the present invention, polyacrylonitrile is understood to mean not only polyacrylonitrile homopolymers but also copolymers of acrylonitrile with 1,3-butadiene or styrene. Polyacrylonitrile homopolymers are preferred.
[0063] In the context of the present invention, polyethylene is understood to mean not only homopolyethylene but also copolymers of ethylene, which comprise at least 50 mol % of copolymerized ethylene and up to 50 mol % of at least one further comonomer, for example α-olefins such as propylene, butene (1-butene), 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-pentene and also isobutene, vinylaromatic compounds such as styrene and also (meth)acrylic acid, vinyl acetate, vinyl propionate, C1-C12-hydroxyethyl esters of (meth)acrylic acid. 10 - Alkyl esters, in particular methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-butyl acrylate, 2-ethylhexyl acrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, and also maleic acid, maleic anhydride and itaconic anhydride. The polyethylene may be HDPE or LDPE.
[0064] In the context of the present invention, polypropylene is understood to mean not only homopolypropylene, but also copolymers of propylene, the copolymers comprising at least 50 mol% of copolymerized propylene and up to 50 mol% of at least one other comonomer, for example ethylene and α-olefins such as butene, 1-hexene, 1-octene, 1-decene, 1-dodecene and 1-pentene. The polypropylene is preferably isotactic or substantially isotactic polypropylene.
[0065] In the context of the present invention, polystyrene is understood to mean not only homopolymers of styrene but also C1-C12 copolymers with acrylonitrile, 1,3-butadiene, (meth)acrylic acid, (meth)acrylic acid, and the like. 10 - copolymers of alkyl esters, divinylbenzene, especially 1,3-divinylbenzene, 1,2-diphenylethylene and α-methylstyrene.
[0066] Another preferred binder (C) is polybutadiene.Other suitable binders (C) are selected from polyethylene oxide (PEO), cellulose, carboxymethylcellulose, polyimide and polyvinyl alcohol.
[0067] In some embodiments of the present invention, the binder (C) is selected from a group consisting of binders having an average molecular weight M in the range of 50,000 g / mol to 1,000,000 g / mol, preferably 50,000 g / mol to 500,000 g / mol. w Those (co)polymers.
[0068] Binder (C) can be crosslinked or non-crosslinked (co)polymer. In a particularly preferred embodiment of the present invention, binder (C) is selected from halogenated (co)polymers, especially fluorinated (co)polymers. Halogenated or fluorinated (co)polymers are understood to mean those (co)polymers of (co)monomers containing at least one halogen atom or at least one fluorine atom per molecule, more preferably at least two halogen atoms or at least two fluorine atoms per molecule. Examples are polyvinyl chloride, polyvinylidene chloride, polytetrafluoroethylene, polyvinylidene fluoride (PVdF), tetrafluoroethylene-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), vinylidene fluoride-tetrafluoroethylene copolymer, perfluoroalkyl vinyl ether copolymer, ethylene-tetrafluoroethylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer and ethylene-chlorofluoroethylene copolymer.
[0069] Suitable binders (C) are, in particular, polyvinyl alcohols and halogenated (co)polymers, for example polyvinyl chloride or polyvinylidene chloride, and in particular fluorinated (co)polymers, such as polyvinyl fluoride and in particular polyvinylidene fluoride and polytetrafluoroethylene.
[0070] The electrode of the present invention may contain 0.01% to 5% by weight of one or more binders (C) relative to the sum of components (A), (B), (C) and (D). The solid electrolyte (D) is a lithium ion conductive material that is solid at a temperature of at least 30° C., preferably at least 50° C. Examples of the solid electrolyte (D) are preferably lithium ion conductive materials such as lithium ion conductive ceramics, sintered ceramics, glass ceramics, glasses and polymer compounds. Preferred solid electrolytes (D) exhibit a temperature of more than 10° C. at 25° C. - 7 S / cm, preferably at 1·10 at 25°C -6 S / cm-5·10 -2 Lithium ion conductivity in the range of S / cm. In particular, ceramic materials with perovskite, sodium superionic conductor, lithium zinc thiogermanate, argyrodite or garnet-related crystal structures provide good conductivity, but inorganic phosphorus and sulfur-containing materials are suitable. The polymer-based electrolyte contains at least one polymer from the following list: polyether, polyester, polyimide, polyketone, polycarbonate, polyamide, polysulfide, polysulfone, polyurethane, polyacrylate, polyolefin, styrene polymer, vinyl polymer, fluoropolymer, polyphosphazene, polysiloxane, polysilazane, boron polymer, liquid crystal polymer (LCP), polyacetylene, polyaniline, polyfuran, polyphenylene, polypyrrole, polythiophene or a blend of at least two of the above polymers.
[0071] Another aspect of the present invention is an electrochemical cell comprising
[0072] at least one electrode according to the invention as cathode,
[0073] at least one anode, and
[0074] At least one electrolyte.
[0075] Embodiments of cathodes have been described in detail above. Anode and electrolyte are those commonly used in the art. Anode may contain at least one anode active material commonly used in the art, such as carbon (graphite), lithium metal, TiO2, lithium titanium oxide, silicon or tin. Anode may additionally include a current collector, such as metal foil, such as copper foil. Electrolyte may include at least one non-aqueous solvent, at least one electrolyte salt and optionally an additive.
[0076] The nonaqueous solvent of the electrolyte may be liquid or solid at room temperature and is preferably selected from polymers, cyclic or acyclic ethers, cyclic or acyclic acetals, and cyclic or acyclic organic carbonates.
[0077] Examples of suitable polymers are in particular polyalkylene glycols, preferably poly-C1-C4-alkylene glycols, and in particular polyethylene glycols. Polyethylene glycols may account for up to 20% by mole of one or more C1-C4-alkylene glycols. Polyalkylene glycols are preferably polyalkylene glycols with two methyl or ethyl end caps.
[0078] The molecular weight M of suitable polyalkylene glycols and in particular suitable polyethylene glycols is w The molecular weight M of suitable polyalkylene glycols and in particular suitable polyethylene glycols may be at least 400 g / mol. w It can be up to 5,000,000 g / mol, preferably up to 2,000,000 g / mol. Examples of suitable acyclic ethers are, for example, diisopropyl ether, di-n-butyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, wherein 1,2-dimethoxyethane is preferred. Examples of suitable cyclic ethers are tetrahydrofuran and 1,4-dioxane. Examples of suitable acyclic acetals are, for example, dimethoxymethane, diethoxymethane, 1,1-dimethoxyethane and 1,1-diethoxyethane. Examples of suitable cyclic acetals are 1,3-dioxane and in particular 1,3-dioxolane. Examples of suitable acyclic organic carbonates are dimethyl carbonate, ethyl methyl carbonate and diethyl carbonate.
[0079] Examples of suitable cyclic organic carbonates are compounds of the general formula (III.1) and the general formula (III.2)
[0080]
[0081] Where R 1 , R 2 and R3 may be identical or different and are selected from hydrogen and C1-C4-alkyl, for example methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl, wherein R 2 and R 3 Preferably, not all are tert-butyl. In a particularly preferred embodiment, R 1 is methyl and R 2 and R 3 Each is hydrogen, or R 1 , R 2 and R 3 Each is hydrogen.
[0082] Another preferred cyclic organic carbonate is vinylene carbonate, formula (IV).
[0083]
[0084] The solvent or solvents are preferably used in anhydrous state, ie with a water content in the range from 1 ppm to 0.1% by weight, which can be determined, for example, by Karl-Fischer titration.
[0085] The electrolyte further comprises at least one electrolyte salt. Suitable electrolyte salts are in particular lithium salts. Examples of suitable lithium salts are LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC(C n F 2n+1 SO2)3, lithium imide such as LiN(C n F 2n+ 1SO2)2, wherein n is an integer in the range of 1 to 20, LiN(SO2F)2, Li2SiF6, LiSbF6, LiAlCl4 and n F 2n+1 SO2) t Salts of YLi, wherein n, t and Y are defined as follows:
[0086] When Y is selected from oxygen and sulfur, t=1,
[0087] When Y is selected from nitrogen and phosphorus, t=2
[0088] When Y is selected from carbon and silicon, t=3, and
[0089] n is an integer ranging from 1 to 20.
[0090] Preferred electrolyte salts are selected from LiC(CF3SO2)3, LiN(CF3SO2)2, LiPF6, LiBF4, LiClO4, among which LiPF6 and LiN(CF3SO2)2 are particularly preferred.
[0091] In some embodiments of the invention, the battery cell according to the invention comprises one or more separators by which the electrodes are mechanically separated. Suitable separators are polymer films, in particular porous polymer films, which are non-reactive to metallic lithium. Particularly suitable materials for separators are polyolefins, in particular film-forming porous polyethylene and film-forming porous polypropylene.
[0092] The membrane comprises polyolefin, in particular polyethylene or polypropylene, and may have a porosity in the range of 35% to 45%. Suitable pore sizes are, for example, in the range of 30 nm to 500 nm.
[0093] In some other embodiments of the present invention, the separator can be selected from a PET nonwoven material filled with inorganic particles. Such a separator can have a porosity in the range of 40% to 55%. Suitable pore sizes are, for example, in the range of 80nm to 750nm.
[0094] The electrochemical cell according to the invention may further comprise a housing, which may have any shape, such as the shape of a cubic or cylindrical disk. In one variant, a metal foil configured as a pouch is used as the housing. The electrochemical cell according to the invention provides very good charge / discharge and high capacity.
[0095] The battery according to the invention may comprise two or more electrochemical cells combined with one another, which may be connected in series or in parallel, for example. Preferably they are connected in series. In the battery according to the invention, at least one of the electrochemical cells comprises at least one electrode according to the invention. Preferably, in the electrochemical cells according to the invention, the majority of the electrochemical cells comprise an electrode according to the invention. Even more preferably, in the battery according to the invention, all electrochemical cells comprise an electrode according to the invention.
[0096] The invention further provides for the use of a battery according to the invention in an apparatus, in particular in a mobile device. Examples of mobile devices are vehicles, such as cars, bicycles, aircraft or water vehicles (such as ships or vessels). Other examples of mobile devices are those that are moved manually, such as computers, in particular laptops, telephones or electric hand tools, such as in the construction industry, in particular drills, battery-powered screwdrivers or battery-powered staplers.
[0097] The present invention is further illustrated by working examples, but the present invention is not limited thereto. BRIEF DESCRIPTION OF THE DRAWINGS
[0098] Figure 1 :Calcination curve of TTT procedure in the synthesis of single crystal NCM Ni90
[0099] Figure 2 :Calcination curve of normal procedure in the synthesis of NCM Ni90
[0100] Figure 3(a): SEM image of a sample synthesized by normal procedure at 10kx magnification Figure 3(b): SEM image of a sample synthesized by normal procedure at 20kx magnification
[0101] Figure 3(c): SEM image of the sample synthesized by the TTT process at 10kx magnification
[0102] Figure 3(d): SEM image of the sample synthesized by TTT process at 20kx magnification
[0103] Figure 4 :XRD of single crystal NCM Ni90 synthesized by TTT procedure
[0104] Figure 5 : Calcination curves at different TTT temperatures (830℃ (no TTT), 900℃, 970℃ and 1040℃)
[0105] Figure 6(a): SEM image of the sample synthesized without TTT
[0106] Figure 6(b): SEM image of the sample synthesized at a TTT temperature of 900°C
[0107] Figure 6(c): SEM image of the sample synthesized at a TTT temperature of 970°C
[0108] Figure 6(d): SEM image of the sample synthesized at a TTT temperature of 1040°C
[0109] Figure 7 : Comparison of the pressed density of samples synthesized at different TTT temperatures (830°C (without TTT), 900°C, 970°C and 1040°C)
[0110] Figure 8 : Comparison of electrical conductivity of samples synthesized at different TTT temperatures (830°C (without TTT), 900°C, 970°C, and 1040°C)
[0111] Fig. 9 : Calcination curves at different time points for transient heat treatment
[0112] Figure 10(a): SEM image of the sample synthesized using step B, which consists of 15 min TTT and 10 h baseline heating (0 h / 15 min-TTT / 10 h)
[0113] Figure 10(b): SEM image of the sample synthesized using step B, which consists of 2 hours of baseline heating, 15 minutes of TTT, and 8 hours of baseline heating (2h / 15min-TTT / 8h)
[0114] Figure 10(c): SEM image of the sample synthesized using step B, which consists of 4 hours of baseline heating, 15 minutes of TTT, and 6 hours of baseline heating (4h / 15min-TTT / 6h)
[0115] Figure 10(d): SEM image of the sample synthesized using step B, which consists of 6 hours of baseline heating, 15 minutes of TTT, and 4 hours of baseline heating (6h / 15min-TTT / 4h)
[0116] Figure 10(e): SEM image of the sample synthesized using step B, which consists of 8 hours of baseline heating, 15 minutes of TTT, and 2 hours of baseline heating (8h / 15min-TTT / 2h)
[0117] Figure 10(f): SEM image of the sample synthesized using step B, which consists of 10 hours of baseline heating and 15 minutes of TTT (10h / 15min-TTT / 0h)
[0118] Fig.11 : Comparison of the compression density of samples with TTT applied at different time points (0h / 15min-TTT / 10h, 2h / 15min-TTT / 8h, 4h / 15min-TTT / 6h, 6h / 15min-TTT / 4h, 8h / 15min-TTT / 2h and 10h / 15min-TTT)
[0119] Fig.12 : Comparison of conductivity of samples with TTT applied at different time points (0h / 15min-TTT / 10h, 2h / 15min-TTT / 8h, 4h / 15min-TTT / 6h, 6h / 15min-TTT / 4h, 8h / 15min-TTT / 2h and 10h / 15min-TTT)
[0120] Example
[0121] Example 1
[0122] A method for preparing a cathode active material having formula (I), the method comprising the following steps
[0123] LiNi x Co y Mn z O2(I)
[0124] i) Preparing precursors of hydroxides or carbonates of Ni, Co and Mn;
[0125] ii). mixing the precursor obtained from step i) with a Li source; and
[0126] iii). calcining the mixture obtained from step ii), wherein said step iii) comprises a multi-step calcination, wherein x is in the range of 0.80 to 0.95 and preferably 0.80 to 0.92, y is in the range of 0.01 to 0.15 and preferably 0.01 to 0.12, and z is in the range of 0.01 to 0.15 and preferably 0.01 to 0.12, and the sum of x, y and z is 1.
[0127] Example 2
[0128] The method according to embodiment 1, wherein the multi-step calcination includes a step of transient heat treatment (TTT) to a temperature in the range of 1000°C to 1400°C, preferably 1000°C to 1200°C.
[0129] Example 3
[0130] The method according to embodiment 2, wherein the temperature of the TTT is maintained for a period of 1 min to 1 hour, preferably 1 min to 30 min and more preferably 5 min to 20 min.
[0131] Example 4
[0132] The method according to any one of embodiments 1 to 3, wherein the multi-step calcination comprises step A of heating at a temperature in the range of 300°C to 600°C and preferably 400°C to 600°C.
[0133] Example 5
[0134] The method according to embodiment 4, wherein step A has a time period of 1 hour to 7 hours and preferably 3 hours to 5 hours.
[0135] Example 6
[0136] The method according to any one of embodiments 1 to 5, wherein the multi-step calcination includes a step B of heating after step A at a temperature in the range of 750°C to 900°C and preferably 750°C to 850°C.
[0137] Example 7
[0138] The method according to embodiment 6, wherein step B has a time period of 6 hours to 16 hours and preferably 8 hours to 14 hours.
[0139] Example 8
[0140] A method according to any one of embodiments 2 to 7, wherein the TTT is performed at any time from the beginning to the end of step B, preferably, the TTT starts at a time point of 1 / 10 to 9 / 10, more preferably 1 / 5 to 4 / 5 and even more preferably 2 / 5 to 4 / 5 of the entire cycle of step B.
[0141] Example 9
[0142] The method according to any one of embodiments 1 to 8, wherein the Li source is at least one compound selected from Li2O, LiOH and Li2CO3.
[0143] Example 10
[0144] A cathode active material produced by the method according to any one of Embodiments 1 to 9.
[0145] Embodiment 11
[0146] The cathode active material according to embodiment 10 comprises single crystals of octahedral structure, wherein the lattice parameters a, b, and c are and
[0147] Example 12
[0148] The cathode active material according to Embodiment 11, wherein the single crystal has an average particle size of 3.5 um to 4.5 um as measured by PSD (particle size distribution).
[0149] Example 13
[0150] The cathode active material according to any one of Embodiments 11 to 12, wherein the single crystal has a pressing density of 3.0 g / ml to 4.0 g / ml measured by a powder resistivity measurement unit MCP-PD51 provided by Mitsubishi Chemical Analytical Technology Co., Ltd.
[0151] Embodiment 14
[0152] The cathode active material according to any one of Embodiments 11 to 13, wherein the single crystal has an electrical conductivity of 0.004 S / m to 0.08 S / m according to JIS K7194 / JIS R 1637.
[0153] Embodiment 15
[0154] The cathode active material according to any one of embodiments 11 to 14, comprising at least one selected from the group consisting of: LiNi 0.80 Co 0.10 Mn 0.10 O2(Ni80),LiNi 0.83 Co 0.12 Mn 0.05 O2(Ni83),LiNi 0.88 Co 0.06 Mn 0.06 O2(Ni88),LiNi 0.90 Co 0.05 Mn 0.05 O2(Ni90) and LiNi 0.92 Co 0.04 Mn 0.04 O2(Ni92).
[0155] Example 16
[0156] A single crystal cathode active material having an octahedral structure and having formula (I)
[0157] LiNi x Co y Mn z O2(I)
[0158] wherein x is in the range of 0.80 to 0.95 and preferably 0.80 to 0.02, y is in the range of 0.01 to 0.15 and 0.01 to 0.12, and z is in the range of 0.01 to 0.15 and preferably 0.01 to 0.12, and the sum of a, b and c is 1; wherein the lattice parameters a, b, c are respectively and The single crystal has an average particle size of 3.5um to 4.5um measured according to PSD (particle size distribution), a pressing density of 3.0g / ml to 4.0g / ml measured by a powder resistivity measuring unit MCP-PD51 provided by Mitsubishi Chemical Analytical Technology Co., Ltd., and an electrical conductivity of 0.004S / m to 0.08S / m according to JIS K7194 / JIS R1637.
[0159] Embodiment 17
[0160] The cathode active material according to embodiment 16 comprises at least one selected from the group consisting of: LiNi 0.80 Co 0.10 Mn 0.10O2(Ni80),LiNi 0.83 Co 0.12 Mn 0.05 O2(Ni83),LiNi 0.88 Co 0.06 Mn 0.06 O2(Ni88),LiNi 0.90 Co 0.05 Mn 0.05 O2(Ni90) and LiNi 0.92 Co 0.04 Mn 0.04 O2(Ni92).
[0161] Embodiment 18
[0162] A cathode comprising
[0163] (A) 50% to 98.99% by weight of the cathode active material of any one of Embodiments 10 to 17,
[0164] (B) 1 to 5% by weight of carbon in an electrically conductive state,
[0165] (C) 0.01% to 5% by weight of a binder, and
[0166] (D) 0 to 50% by weight of a solid electrolyte, based on the total weight of components (A), (B), (C) and (D).
[0167] Embodiment 19
[0168] An electrochemical cell comprising a cathode according to embodiment 18, an anode, and an electrolyte.
[0169] Examples
[0170] In the following examples, the raw material used was a Ni90 precursor prepared by the method described in Comparative Example 1 of CN113373517A, and then the precursor was mixed with Li2CO3 in a plowshare mixer at a speed of 100 rpm for 5 min. The obtained product has LiNi 0.90 Co 0.05 Mn 0.05 O2 composition and is synthesized by co-precipitation and then dried without calcination. The Ni90 precursor contains some water or hydroxide anions.
[0171] I. The impact of the existence of TTT
[0172] Example 1
[0173] The calcination was carried out using a calcination curve similar to that of Comparative Example 1, the only difference being that TTT was used in step B, such as Figure 1 As shown. In detail, after 4 h of step B at 830 ° C, a ramp of 5 ° C / min was implemented to reach 1040 ° C, and it was kept at 1040 ° C for 15 min. Then, the temperature was reduced to 830 ° C with the same ramp, and it was kept at 830 ° C for another 6 h. Finally, a cooling ramp of 4.3 ° C / min was applied to reach 400 ° C, and then cooled to room temperature in a natural way.
[0174] Comparative Example 2
[0175] Normal calcination is carried out in a conventional manner, i.e. in the absence of TTT. The calcination curve comprises two sections - pre-calcination and step B, such as Figure 2 As shown. First, the sample was heated from room temperature to 500°C at a ramp of 5°C / min, and kept at 500°C for 180min (3h) to complete pre-calcination. Afterwards, a ramp of 3.3°C / min was applied to reach 830°C as the temperature of step B, and kept at 830°C for 600min (10h). Then, the temperature was reduced to 400°C at a ramp of 4.3°C / min, and then cooled to room temperature in a natural manner.
[0176] The morphology of the samples synthesized by the normal procedure and the TTT procedure was studied by scanning electron microscopy (SEM) of JSM-7800 (5keV, working distance (WD) = 15-15.33mm). The morphological comparison of the samples synthesized by the normal procedure and the TTT procedure is shown in Figure 3, indicating that the spherical particles can be converted into octahedral particles by TTT. In addition, the crystal size also changes from about 1.5um to 2.2um. Therefore, it can be concluded that the direct effect of TTT is to form octahedrons and increase the particle size.
[0177] Figure 4 The XRD pattern of the TTT sample (measured by a Rigaku-600 X-ray diffractometer with Cu-Kα radiation in the range of 10° to 110°) is shown, showing peak characteristics close to those of the sample synthesized by the normal procedure. This indicates that although TTT produces an ordered morphology, the corresponding chemical composition in the bulk is not affected.
[0178] Pressed density is a key indicator affecting the energy density of CAM. Therefore, a comparison of samples of the TTT procedure and the normal procedure was conducted by a powder resistivity measurement unit MCP-PD51 from Mitsubishi Chemical Analytical Technology Co., Ltd., showing that TTT produced a pressed density of 3.725 g / ml, which is 18% higher than the normal procedure (3.151 g / ml). This improvement is conducive to increasing the energy density to further improve the performance. In addition, conductivity is crucial to reflect the electron transport of CAM.
[0179] The conductivity was measured by a powder resistivity measurement unit MCP-PD51 from Mitsubishi Chemical Analytical Technology Co., Ltd. according to 4-pin probe JIS K 7194 / JIS R 1637. TTT gave a sharp increase in conductivity of 0.149 S / m, which is unexpectedly 489% higher than the normal value (0.025 S / m). This means faster and stronger electron transport of the CAM generated by TTT.
[0180] Benefits beyond the octahedral morphology are the improvement in pressing density and conductivity, which means the potential for achieving higher energy density and faster electron transport of CAMs.
[0181] II. Effect of TTT temperature
[0182] Three TTT temperatures were applied to study the effect of TTT temperature on morphology, pressed density and electrical conductivity.
[0183] Comparative Example 3
[0184] For comparison, a calcination experiment including step B at 830 °C without TTT was also performed. Figure 5-8 The temperature is indicated as "830°C".
[0185] Comparative Example 4
[0186] like Figure 5 As shown in , a step experiment was performed on the TTT temperature. First, the sample was heated from room temperature to 500°C with a ramp of 5°C / min, and kept at 500°C for 180min (3h) to complete pre-calcination. Afterwards, a ramp of 3.3°C / min was applied to reach 830°C as the temperature of step B, and kept at 830°C for 600min (10h). Then, a ramp of 5°C / min was implemented to reach 900°C, and kept at 900°C for 15min. Finally, a cooling ramp of 4.3°C / min was applied to reach 400°C, and then cooled to room temperature in a natural manner.
[0187] Comparative Example 5
[0188] A step experiment on TTT temperature was conducted in the same manner as in Comparative Example 4, with the only difference being that the instantaneous treatment temperature was 970°C.
[0189] Example 6
[0190] A step experiment on TTT temperature was conducted in the same manner as in Comparative Example 4, with the only difference being that the instantaneous treatment temperature was 1040°C.
[0191] The morphology is compared in Figure 6, showing that when the instantaneous processing temperature reaches 1040°C, octahedrons can be observed from the SEM image. The average particle size is about 2.6um. In contrast, when the temperature drops to 970°C, the octahedrons disappear. Instead, normal spherical particles are formed. This means that 1040°C may be responsible for the formation of octahedrons, and the effect of temperatures below 1000°C on the morphology is negligible.
[0192] Figure 7 is the pressed density of the four samples, showing that the sample treated at 1040°C shows an increase of 8% compared to the sample in the normal procedure, with an absolute value of 3.415 g / ml. In addition, an upward trend can also be seen in the pressed density, which means a positive correlation between instantaneous treatment temperature and pressed density.
[0193] Figure 8 A comparison of the conductivity of the samples is shown in Figure 1. When 900°C is applied to the TTT treatment, an increase of 0.025 S / m can be observed, reaching 0.050 S / m. Then, it drops back to 0.022 S / m at 970°C. Finally, when the temperature reaches 1040°C, the conductivity reaches 0.061, which is an increase of 143% compared to the normal procedure.
[0194] It is concluded that 1040°C is an effective temperature for achieving octahedral morphology, where the pressing density and electrical conductivity increase significantly. Furthermore, the trend from 830°C to 1040°C shows that a positive correlation can be seen between temperature, morphology evolution, and pressing density. Furthermore, although a similar correlation is not seen for electrical conductivity, the highest value can be reached at 1040°C.
[0195] III. The impact of TTT timing
[0196] like Fig. 9 As shown, a further stepwise investigation was conducted on the flexibility of 1040 °C as the TTT temperature for the Step B stage. Six time points were applied for 15 min TTT in 2 h increments from the start to the end of Step Bs. In addition, morphology, pressed density, and electrical conductivity were evaluated.
[0197] Example 7
[0198] First, the sample was heated from room temperature to 500°C at a ramp of 5°C / min, and kept at 500°C for 180min (3h) to complete pre-calcination. Afterwards, a ramp of 3.3°C / min was applied to reach 830°C as the temperature of step B. After reaching 830°C, a ramp of 5°C / min was applied to reach 1040°C as the temperature of TTT, and kept at 1040°C for 15min. Afterwards, the temperature was reduced to 830°C at a ramp of 5°C / min, and kept at 830°C for 600min (10h). Then, the temperature was reduced to 400°C at a ramp of 4.3°C / min, and then cooled to room temperature in a natural manner.
[0199] Example 8
[0200] The same procedure as in Example 7 was followed, with the only difference being that 15min-TTT was applied 2 hours after the start of step B.
[0201] First, the sample was heated from room temperature to 500°C at a ramp of 5°C / min, and kept at 500°C for 180min (3h) to complete pre-calcination. Afterwards, a ramp of 3.3°C / min was applied to reach 830°C as the temperature of step B, and kept at 830°C for 120min (2h). Afterwards, a ramp of 5°C / min was applied to reach 1040°C as the temperature of TTT, and kept at 1040°C for 15min. Afterwards, the temperature was reduced to 830°C at a ramp of 5°C / min, and kept at 830°C for another 480min (8h). Then, the temperature was reduced to 400°C at a ramp of 4.3°C / min, and then cooled to room temperature in a natural manner.
[0202] Example 9
[0203] The same procedure as in Example 7 was followed, with the only difference being that 15min-TTT was applied 4 hours after the start of step B.
[0204] First, the sample was heated from room temperature to 500°C at a ramp of 5°C / min, and kept at 500°C for 180min (3h) to complete pre-calcination. Afterwards, a ramp of 3.3°C / min was applied to reach 830°C as the temperature of step B, and kept at 830°C for 240min (4h). Afterwards, a ramp of 5°C / min was applied to reach 1040°C as the temperature of TTT, and kept at 1040°C for 15min. Afterwards, the temperature was reduced to 830°C at a ramp of 5°C / min, and kept at 830°C for another 360min (6h). Then, the temperature was reduced to 400°C at a ramp of 4.3°C / min, and then cooled to room temperature in a natural manner.
[0205] Example 10
[0206] The same procedure as in Example 7 was followed, with the only difference being that 15 min-TTT was applied 6 hours after the start of step B.
[0207] First, the sample was heated from room temperature to 500°C at a ramp of 5°C / min, and kept at 500°C for 180min (3h) to complete pre-calcination. Afterwards, a ramp of 3.3°C / min was applied to reach 830°C as the temperature of step B, and kept at 830°C for 360min (6h). Afterwards, a ramp of 5°C / min was applied to reach 1040°C as the temperature of TTT, and kept at 1040°C for 15min. Afterwards, the temperature was reduced to 830°C at a ramp of 5°C / min, and kept at 830°C for another 240min (4h). Then, the temperature was reduced to 400°C at a ramp of 4.3°C / min, and then cooled to room temperature in a natural manner.
[0208] Example 11
[0209] The same procedure as in Example 7 was followed, with the only difference being that 15 min-TTT was applied 8 hours after the start of step B.
[0210] First, the sample was heated from room temperature to 500°C at a ramp of 5°C / min, and kept at 500°C for 180min (3h) to complete pre-calcination. Afterwards, a ramp of 3.3°C / min was applied to reach 830°C as the temperature of step B, and kept at 830°C for 480min (8h). Afterwards, a ramp of 5°C / min was applied to reach 1040°C as the temperature of TTT, and kept at 1040°C for 15min. Afterwards, the temperature was reduced to 830°C at a ramp of 5°C / min, and kept at 830°C for another 120min (2h). Then, the temperature was reduced to 400°C at a ramp of 4.3°C / min, and then cooled to room temperature in a natural manner.
[0211] Example 12
[0212] The same procedure as in Example 7 was performed, with the only difference that 15 min-TTT was applied 10 hours after the start of step B (ie, at the end of step B).
[0213] First, the sample was heated from room temperature to 500°C at a ramp of 5°C / min, and kept at 500°C for 180min (3h) to complete pre-calcination. Afterwards, a ramp of 3.3°C / min was applied to reach 830°C as the temperature of step B, and kept at 830°C for 600min (10h). Afterwards, a ramp of 5°C / min was applied to reach 1040°C as the temperature of TTT, and kept at 1040°C for 15min. Afterwards, the temperature was reduced to 830°C at a ramp of 5°C / min. Then, the temperature was reduced to 400°C at a ramp of 4.3°C / min, and then cooled to room temperature in a natural manner.
[0214] Figure 10 is a collection of morphologies at different TTT time points, showing close octahedrons but different particle sizes. For samples treated with 15min-TTT / 10h, 2h / 15min-TTT / 8h, 8h / 15min-TTT / 2h and 10h / 15min-TTT, a size of about 3.5um can be seen, while for samples treated with 4h / 15min-TTT / 6h, 6h / 15min-TTT / 4h, a smaller size can be seen, especially the sample treated with 4h / 15min-TTT / 6h showed a size of about 2.0um.
[0215] Fig.11 The comparison of the compression density is shown in Figure 1, indicating that all samples have a higher compression density (>3.4 g / ml) than the normal value, which confirms the influence of TTT again. Among them, the samples treated with 4h / 15min-TTT / 6h and 8h / 15min-TTT / 2h gave the top two values of 3.725 and 3.818 g / ml.
[0216] When it comes to conductivity, Fig.12 As shown, from the beginning to the end of the TTT time point, these values first increased from 0.081 to 0.096 to 0.148 S / m, and then decreased to 0.124 to 0.031 S / m, and finally reached 0.066 S / m. The highest value (0.148 S / m) came from the sample treated with 4h / 15min-TTT / 6h.
Claims
1. A method for preparing a cathode active material having formula (I), the method comprising the following steps LiNi x Co y Mn z O2(I) i) Preparing precursors of hydroxides or carbonates of Ni, Co and Mn; ii). mixing the precursor obtained from step i) with a Li source; and iii). calcining the mixture obtained from step ii), wherein step iii) comprises a multi-step calcination, wherein x is in the range of 0.80 to 0.95 and preferably 0.80 to 0.92, y is in the range of 0.01 to 0.15 and preferably 0.01 to 0.12, and z is in the range of 0.01 to 0.15 and preferably 0.01 to 0.12, and the sum of x, y and z is 1.
2. The method according to claim 1, wherein: The multi-step calcination includes a step of transient heat treatment (TTT) to a temperature in the range of 1000°C to 1400°C, preferably 1000°C to 1200°C.
3. The method according to claim 2, wherein: The temperature of the TTT is maintained for a period of 1 min to 1 hour, preferably 1 min to 30 min and more preferably 5 min to 20 min.
4. The method according to any one of claims 1 to 3, wherein: The multi-step calcination includes step A of heating at a temperature ranging from 300°C to 600°C and preferably from 400°C to 600°C.
5. The method according to claim 4, wherein: The step A has a time period of 1 to 7 hours and preferably 3 to 5 hours.
6. The method according to any one of claims 1 to 5, wherein: The multi-step calcination includes step B of heating after step A at a temperature ranging from 750°C to 900°C and preferably from 750°C to 850°C.
7. The method according to claim 6, wherein: The step B has a time period of 6 to 16 hours and preferably 8 to 14 hours.
8. The method according to any one of claims 2 to 7, wherein: The TTT is performed at any time from the beginning to the end of step B. Preferably, the TTT starts at a time point of 1 / 10 to 9 / 10, more preferably 1 / 5 to 4 / 5, and even more preferably 2 / 5 to 4 / 5 of the entire cycle of step B.
9. The method according to any one of claims 1 to 8, wherein: The Li source is at least one compound selected from Li2O, LiOH and Li2CO3.
10. A cathode active material produced by the method according to any one of claims 1 to 9.
11. The cathode active material according to claim 10, comprising single crystals of octahedral structure, wherein lattice parameters a, b, c are and 12. The cathode active material according to claim 11, wherein The single crystal has an average particle size of 3.5 um to 4.5 um as measured by PSD (particle size distribution).
13. The cathode active material according to any one of claims 11 to 12, wherein The single crystal has a pressed density of 3.0 to 4.0 g / ml measured by a powder resistivity measuring unit MCP-PD51 provided by Mitsubishi Chemical Analytical Technology Co., Ltd.
14. The cathode active material according to any one of claims 11 to 13, wherein The single crystal has an electrical conductivity of 0.004 S / m to 0.08 S / m according to JIS K7194 / JIS R 1637.
15. The cathode active material according to any one of claims 11 to 14, comprising at least one selected from the group consisting of: LiNi 0.80 Co 0.10 Mn 0.10 O2(Ni80),LiNi 0.83 Co 0.12 Mn 0.05 O2(Ni83),LiNi 0.88 Co 0.06 Mn 0.06 O2(Ni88),LiNi 0.90 Co 0.05 Mn 0.05 O2(Ni90) and LiNi 0.92 Co 0.04 Mn 0.04 O2(Ni92).
16. A single crystal cathode active material having an octahedral structure and having the formula (I) LiNi x Co y Mn z O2(I) wherein x is in the range of 0.80 to 0.95 and preferably 0.80 to 0.02, y is in the range of 0.01 to 0.15 and 0.01 to 0.12, and z is in the range of 0.01 to 0.15 and preferably 0.01 to 0.12, and the sum of a, b and c is 1; wherein the lattice parameters a, b, c are respectively and The single crystal has an average particle size of 3.5um to 4.5um measured according to PSD (particle size distribution), a pressing density of 3.0g / ml to 4.0g / ml measured by a powder resistivity measuring unit MCP-PD51 provided by Mitsubishi Chemical Analytical Technology Co., Ltd., and an electrical conductivity of 0.004S / m to 0.08S / m according to JIS K7194 / JIS R1637.
17. The cathode active material according to claim 16, comprising at least one selected from the group consisting of: LiNi 0.80 Co 0.10 Mn 0.10 O2(Ni80),LiNi 0.83 Co 0.12 Mn 0.05 O2(Ni83),LiNi 0.88 Co 0.06 Mn 0.06O2(Ni88),LiNi 0.90 Co 0.05 Mn 0.05 O2(Ni90) and LiNi 0.92 Co 0.04 Mn 0.04 O2(Ni92).
18. A cathode comprising (A) 90% to 98.99% by weight of a cathode active material according to any one of claims 10 to 17, (B) 1 to 5% by weight of carbon in an electrically conductive state, (C) 0.01% to 5% by weight of a binder, and (D) 0 to 50% by weight of a solid electrolyte, based on the total weight of components (A), (B), (C) and (D).
19. An electrochemical cell comprising a cathode according to claim 18, an anode and an electrolyte.
Citation Information
Patent Citations
High-nickel single-crystal small-particle ternary precursor and continuous preparation method thereof
CN113373517A