Copper alloy bonded body

By using aging hardened copper alloy with low beryllium content in the precooler for hydrogen refueling station for finishing and diffusion bonding, combined with solid solution treatment and aging treatment, the strength and thermal conductivity of the copper alloy joint in a high-pressure hydrogen environment are solved. Due to the shortage, a copper alloy joint with high strength and hydrogen embrittlement resistance has been realized.

CN119072550APending Publication Date: 2024-12-03NGK INSULATORS LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380035686.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-06
Filing Date
2023-07-03
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the heat exchanger of the precooler used in the existing hydrogen refueling station, it is difficult to achieve the same structure and strength as the base material, and the joint breakage is likely to occur in the solid solution treatment and time-efficiency treatment.

Method used

Aging hardened copper alloy with a beryllium content of less than 0.7% by weight is used to finish the bonding surface, remove the oxidation coating, and perform diffusion bonding and homogenization treatment. Combined with solid solution treatment and aging treatment, it has extremely high bonding strength. copper alloy joint.

Benefits of technology

It realizes extremely high bonding strength and hydrogen embrittlement resistance of the copper alloy joint, can maintain high strength and thermal conductivity in a high-pressure hydrogen environment, and is suitable for high-pressure hydrogen heat exchangers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072550A_ABST
    Figure CN119072550A_ABST
Patent Text Reader

Abstract

Provided is a bonded body of an age-hardening copper alloy that achieves extremely high bonding strength. The copper alloy bonded body is composed of a plurality of age-hardening copper alloy members which are diffusion bonded to each other, and the bonding interface of the plurality of members remains. The beryllium content of the age-hardening copper alloy of the copper alloy bonded body is 0.7 wt% or less, and the ratio of the total length of line segments corresponding to the discontinuous region to the total length of bonding interface lines defined along the bonding interface and the original position of the bonding interface in a laser microscope image of a cross section including the bonding interface is 3.5% or more. The discontinuous region is defined as a region in which three or more perpendicular lines adjacent to each other do not intersect the remaining bonding interface when a plurality of perpendicular lines are drawn at a pitch of 5 [mu] m with respect to the bonding interface line.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a copper alloy joined body. Background Art

[0002] In a hydrogen filling station for supplying hydrogen to a fuel cell vehicle, a precooler is provided to enable rapid supply of high-pressure hydrogen cooled to about -45°C. That is, if hydrogen is rapidly filled into the tank of a fuel cell vehicle, the tank temperature rises due to adiabatic compression, which is dangerous. Therefore, by cooling the hydrogen using a precooler during supply, high-pressure hydrogen can be safely and rapidly supplied to the fuel cell vehicle, etc. Therefore, in the heat exchanger, which is the main component of the precooler for a hydrogen filling station, hydrogen embrittlement cannot be exhibited, and it is also preferred to use a material with tensile strength that can withstand high pressure and thermal conductivity that can be efficiently cooled. At present, in the heat exchanger of the precooler for a hydrogen filling station, high-pressure hydrogen stainless steel such as SUS316L (Ni equivalent material) is used from the requirement of not causing hydrogen embrittlement, but there is room for improvement from the perspective of tensile strength and thermal conductivity.

[0003] Beryllium copper, which is known as a material with high tensile strength and thermal conductivity, is suitable as a raw material for heat exchangers, and it has been confirmed that it will not cause hydrogen embrittlement even under high-pressure hydrogen. For example, in Patent Document 1 (Japanese Patent Publication No. 9-87780), although it is not used for hydrogen refueling stations, a beryllium copper alloy for heat exchangers is disclosed, in which the Be content is 1.0-2.5%, the total content of Ni and Co is 0.2-0.6%, and the balance is composed of Cu and inevitable impurities. In addition, Patent Document 2 (Japanese Patent Publication No. 2017-145472) discloses a beryllium copper alloy with a Be content of 0.20-2.70 weight%, a total content of Co, Ni and Fe of 0.20-2.50 weight%, and a total content of Cu, Be, Co, Ni and Fe of more than 99 weight%, which has excellent hydrogen embrittlement resistance, tensile strength and thermal conductivity. In addition to not showing hydrogen embrittlement (i.e., being resistant to hydrogen embrittlement), beryllium copper alloy also has a higher tensile strength than high-pressure hydrogen stainless steel (e.g., about 1.5 to 2.5 times) and a higher thermal conductivity than stainless steel (e.g., about 7 to 16 times). Therefore, it can make the size of a high-pressure hydrogen heat exchanger that cannot be achieved with low-purity copper and low-strength copper alloys significantly smaller than a stainless steel high-pressure hydrogen heat exchanger (e.g., about one-quarter).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 9-87780

[0007] Patent Document 2: Japanese Patent Application Publication No. 2017-145472 Summary of the invention

[0008] The heat exchanger of the precooler for hydrogen refueling stations has a structure in which metal plates with slits or grooves are joined in multiple layers in order to form a flow path for hydrogen and refrigerant to pass through. As a currently used method for joining stainless steel for high-pressure hydrogen, it is widely known that the surface oxide film is sublimated and removed during the process of reducing pressure and heating to the joining temperature, and a bonding pressure is applied to the joint at a high temperature below the melting point to join the stainless steel plates to each other. However, for copper alloys, (i) there is a strong oxide film that is difficult to remove by simply reducing pressure and heating, and / or (ii) even if the oxide film is removed before joining, it is easy to form an oxide film on the joining surface (closely fitting surface) during the heating under high vacuum in the joining process (and, even when the temperature reaches near the joining temperature, the oxide film is difficult to sublime). When the copper alloy is diffusion-bonded by the same process, although a certain bonding strength can be ensured, it is difficult to obtain a structure and strength equivalent to that of the parent material. In particular, in order to realize the extremely high strength copper alloy parts required for the above-mentioned high-pressure heat exchanger application, it is necessary to perform solid solution treatment and aging treatment on the age-hardening copper alloy. However, the diffusion bonded body of the age-hardening copper alloy without sufficient bonding strength cannot withstand the severe thermal shock and dimensional changes accompanying the solid solution treatment and aging treatment, and there is a problem of fracture at the bonding part.

[0009] The inventors have obtained the following insight: by selectively using an age-hardenable copper alloy having a beryllium content of 0.7 wt% or less, after finishing the joining surfaces to a specified flatness and removing the oxide film, diffusion bonding is performed (and homogenization treatment is performed as required). In this case, solution treatment and aging treatment can be performed so that the ratio of the total length of the discontinuous areas in the cross-sectional observation image to the total length of the joining interface line is 3.5% or more, thereby providing a copper alloy joint body with extremely high joining strength.

[0010] Therefore, an object of the present invention is to provide a joined body of an age-hardenable copper alloy that achieves extremely high joining strength.

[0011] According to the present invention, the following aspects are provided.

[0012] [Aspect 1] A copper alloy joint body comprising a plurality of age-hardenable copper alloy parts that are diffusion-bonded to one another, wherein a bonding interface of the plurality of parts remains;

[0013] The age-hardenable copper alloy has a beryllium content of 0.7 wt % or less, and in a laser microscope image of a cross section including the joint interface, a ratio of a total length of line segments corresponding to discontinuous regions to a total length of a joint interface line defined along the joint interface and a position that was originally the joint interface is 3.5% or more;

[0014] The discontinuous region is defined as a region where, when a plurality of perpendicular lines are drawn at a pitch of 5 μm to the bonding interface line, three or more adjacent perpendicular lines do not intersect with the remaining bonding interface.

[0015] [Mode 2] The copper alloy bonded body according to Mode 1, wherein the copper alloy bonded body has been subjected to a solution treatment and an aging treatment.

[0016] [Aspect 3] The copper alloy joined body according to aspect 1 or 2, wherein the strength of the joined portion of the copper alloy joined body is 70% or more of the strength of a base material of the copper alloy joined body.

[0017] [Aspect 4] The copper alloy joined body according to any one of aspects 1 to 3, wherein the strength of a joined portion of the copper alloy joined body is 85% or more of the strength of a base material of the copper alloy joined body.

[0018] [Aspect 5] The copper alloy joint according to any one of aspects 1 to 4, comprising: grains of the age-hardenable copper alloy grown beyond the joining interface or a position that was originally the joining interface.

[0019] [Mode 6] The copper alloy joint body according to any one of Modes 1 to 5, wherein no residual component derived from a material other than the age-hardenable copper alloy exists at the joint interface or at a position that was originally the joint interface.

[0020] [Aspect 7] The copper alloy joined body according to any one of aspects 1 to 6, wherein the strength of a base material and a joined portion of the copper alloy joined body is 520 MPa or more.

[0021] [Mode 8] The copper alloy bonded body according to Mode 7, wherein the strength of the base material and the bonded portion of the copper alloy bonded body is 690 MPa or more.

[0022] [Aspect 9] The copper alloy joined body according to any one of aspects 1 to 8, wherein a joined portion of the copper alloy joined body has a joining strength at a temperature of -196°C that is 85% or more of the strength of a base material of the copper alloy joined body.

[0023] [Mode 10] A copper alloy joint according to any one of Modes 1 to 9, wherein a joint portion of the copper alloy joint has a Charpy impact value of 15% or more of a Charpy impact value of a base material of the copper alloy joint at each temperature of 25°C and -196°C.

[0024] [Aspect 11] The copper alloy joined body according to any one of aspects 1 to 10, wherein a thermal conductivity of a base material including a joined portion of the copper alloy joined body is 209 W / mK or more.

[0025] [Aspect 12] The copper alloy joined body according to any one of aspects 1 to 11, wherein the electrical conductivity of a base material of a joined portion including the copper alloy joined body is 50 IACS% or more.

[0026] [Aspect 13] The copper alloy joint according to any one of aspects 1 to 12, wherein the age-hardenable copper alloy is at least one selected from the group consisting of the following alloys:

[0027] Beryllium copper 11 alloy (JIS alloy number C1751, EN material number CW110C and UNS alloy number C17510); Beryllium copper 10 alloy (EN material number CW104C and UNS alloy number C17500); Beryllium copper CuCo1Ni1Be (EN material number CW103C); Beryllium copper 14Z alloy (Be: 0.2-0.6 wt%, Ni: 1.4-2.4 wt% , Zr: 0-0.5 wt%, the balance is composed of Cu and inevitable impurities); Beryllium copper 50 alloy (Be: 0.2-0.6 wt%, Ni: 1.4-2.1 wt%, Ag: 0.1-0.3 wt%, Zr: 0-0.5 wt%, the balance is composed of Cu and inevitable impurities); Beryllium copper 10Zr alloy (Be: 0.4-0.7 wt%, Co: 2.0-2.8 wt%, Zr r: 0-0.3 wt%, the balance consisting of Cu and inevitable impurities); chromium copper (UNS alloy number C18200); chromium zirconium copper (UNS alloy number C18510 and EN material number CW106C); zirconium copper (UNS alloy number C15000, EN material number CW120C) and Corson copper (EN material number CW109C, CW111C, UNS alloy number C19010, C70250, AMPCO944 (Ni: 6.5-7.5 wt%, Si: 1.5-2.5 wt%, Cr: 0.5-1.5 wt%, the balance consisting of Cu and inevitable impurities) and AMPCO940 (Ni: 1.5-3.0 wt%, Si: 0.5-1.5 wt%, Cr: 0.3-1.5 wt%, the balance consisting of Cu and inevitable impurities)).

[0028] [Mode 14] The copper alloy joint according to Mode 13, wherein the age-hardenable copper alloy is beryllium copper 11 alloy (JIS alloy number C1751, EN material number CW110C, and UNS alloy number C17510).

[0029] [Aspect 15] The copper alloy bonded body according to any one of aspects 1 to 14, wherein the copper alloy bonded body includes a flow path space therein. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1A This is a diagram for explaining the flow of an experiment for elemental analysis of oxide films formed on the surfaces of various copper alloys during heat treatment in a high vacuum furnace. It conceptually shows the progress of oxidation and shows the positions of the open surface and the sealing surface in the furnace where the elemental analysis is performed, as well as the appearance of the sample.

[0031] Figure 1B is in accordance with Figure 1A The experimental flow shown is the result of elemental analysis of the oxide film formed on the surface (pickling surface, furnace open surface and / or close-fitting surface) of various copper alloys during heat treatment in a high vacuum furnace. Specifically, the XPS results of beryllium copper 25 alloy, beryllium copper 165 alloy, beryllium copper 11 alloy, beryllium copper 10Zr alloy, beryllium copper 50 alloy and chromium copper alloy are shown.

[0032] Figure 1C is in accordance with Figure 1A The experimental flow shown shows the results of elemental analysis of oxide films formed on the surfaces (pickling surfaces, furnace open surfaces and / or close-fitting surfaces) of various copper alloys during heat treatment in a high vacuum furnace. Specifically, the XPS results of Corson copper AMPCO940 and Corson copper AMPCO944 are shown.

[0033] Figure 2A This is a diagram for explaining one embodiment of a discontinuous region in a bonding interface.

[0034] Figure 2B This is a diagram for explaining another aspect of the discontinuous region in the bonding interface.

[0035] Figure 3 Laser microscope images of cross sections including the bonding interfaces of the copper alloy joints produced by solution treatment and aging treatment in Examples 1a to 1d are shown.

[0036] Figure 4 Laser microscope images of cross sections including the bonding interfaces of the copper alloy joints produced by solution treatment and aging treatment in Examples 2a to 2f are shown.

[0037] Figure 5 Laser microscope images of cross sections including the bonding interface of the copper alloy bonded bodies produced by solution treatment and aging treatment in Examples 3 to 7b are shown.

[0038] Fig. 6A This is a diagram illustrating the first half of a series of procedures for calculating discontinuous region flows by performing image processing on laser microscope images using the image analysis software ImageJ.

[0039] Figure 6BThis is a diagram illustrating the second half of a series of procedures for calculating discontinuous region flows by performing image processing on laser microscope images using the image analysis software ImageJ. DETAILED DESCRIPTION

[0040] Copper alloy joint

[0041] The copper alloy joint body of the present invention is composed of a plurality of age-hardening copper alloy parts that are diffusion-bonded to each other, and is typically a copper alloy joint body that has been subjected to a solution treatment and an aging treatment. The joint interfaces of a plurality of parts remain in the copper alloy joint body. The beryllium content of the age-hardening copper alloy is 0.7% by weight or less. Moreover, in a laser microscope image of a cross section including a joint interface, the ratio of the total length of the line segments corresponding to the discontinuous region to the total length of the joint interface line delineated along the joint interface and the position originally at the joint interface is 3.5% or more. The discontinuous region is defined as a region where, when a plurality of perpendicular lines are drawn to the joint interface line at a spacing of 5 μm, three or more perpendicular lines adjacent to each other do not intersect with the remaining joint interface. In this way, when an age-hardenable copper alloy having a beryllium content of less than 0.7 weight % is selectively used, solution treatment and aging treatment are performed (after homogenization treatment as needed) so that the total length of the discontinuous regions is greater than 3.5% of the total length of the bonding interface line in the cross-sectional observation image, thereby providing a copper alloy joint having extremely high bonding strength.

[0042] As described above, when copper alloys (i) having a strong oxide film that is difficult to remove by simple decompression and temperature increase and / or (ii) that re-form an oxide film even under high vacuum are diffusion-bonded in the same process, a certain bonding strength can be ensured, but it is difficult to obtain a structure and strength equivalent to that of the parent material. In particular, in order to realize the extremely high-strength copper alloy parts required for the above-mentioned heat exchanger applications, it is necessary to perform solid solution treatment and aging treatment on the age-hardening copper alloy, but the diffusion-bonded body of the age-hardening copper alloy cannot withstand the severe thermal shock and dimensional changes associated with the solid solution treatment and aging treatment, and there is a problem of fracture at the joint.

[0043] In this regard, according to the above-mentioned structure of the present invention, such problems can be well eliminated, and a copper alloy joint body with extremely high joint strength can be provided. The reason is as follows, as clearly stated in the confirmation test of the inventor described later. That is, an age-hardening copper alloy with a beryllium content of less than 0.7% by weight is selectively used, and the flatness and surface roughness of the joint surface are adjusted to be suitable for diffusion bonding. On this basis, the oxide film on the joint surface is removed, and the joint interface of the copper alloy parts is made to be close to each other and pressurized and heated to perform diffusion bonding. In this case, the proportion of discontinuous areas (areas where the joint interface is interrupted) in the joint interface (or the position originally used as the joint interface) formed in the age-hardening copper alloy with a beryllium content exceeding 0.7% by weight increases, so the residual joint interface is reduced, and as a result, high-quality diffusion bonding that can fully withstand solid solution treatment and aging treatment is achieved. That is, it is believed that the existence of discontinuous areas reduces the proportion of oxides in the interface, which helps to improve the joint strength.

[0044] However, it is known that stainless steel, pure copper, etc. can be bonded with high reliability by diffusion bonding. In the case of stainless steel, the dense chromium oxide film formed on the surface under the atmosphere becomes a protective film with strong weather resistance, but the oxide film will sublime when heated at a temperature exceeding 700°C under high vacuum. Therefore, it is naturally removed during the temperature increase of diffusion bonding, and an active stainless steel surface without an oxide film on the surface can be easily obtained. Therefore, only by pressurizing at the bonding temperature, a good bonding without residual oxides and other foreign matter at the bonding interface can be performed. In addition, pure copper has a copper oxide (CuO) film on the surface, but during the period when the diffusion bonding temperature is maintained, the oxide will decompose and oxygen will diffuse into the copper matrix. Therefore, like stainless steel, a good bonding without residual oxides and other foreign matter at the bonding interface can be performed.

[0045] The inventors of the present invention have confirmed that in tests before the completion of the present invention, a certain bonding strength can be obtained when the age-hardening copper alloy is subjected to the previously known diffusion bonding, but when the obtained bonded body is subjected to a solid solution aging treatment, the bonding strength deteriorates and often breaks. This phenomenon is particularly prominent in the case of beryllium copper 25 alloy (JIS C1720), which is known to be able to obtain the highest strength among age-hardening copper alloys. The inventors of the present invention presume that the reason for this is the oxide film remaining on the bonding surface that cannot be confirmed in stainless steel and pure copper. In order to clarify the mechanism of the oxide film remaining, the following was carried out: Figure 1A The following experiment is shown. Figure 1B and 1CEach alloy shown was processed into a plate of 15 mm × 15 mm × 5 mm in size, and the upper and lower surfaces of the obtained test piece 10 of 15 mm × 15 mm were polished and flattened to a flatness of less than 0.1 mm and a surface roughness Rzjis of less than 0.8 μm. Then, it was cleaned with 30% nitric acid immediately before the test to remove the oxide film. Three test pieces 10 were made for each alloy. Figure 1A As shown, one of the test pieces 10 is placed in contact with the vacuum atmosphere in the furnace, and the remaining two test pieces 10 are placed in a stacked (like the bonding surface in diffusion bonding) and in a close contact state, respectively, in the bonding furnace. In the bonding furnace, the same heat treatment as in the bonding is performed under various reduced pressure conditions, and then taken out. The former is subjected to argon etching on the surface in contact with the atmosphere in the furnace (hereinafter referred to as the furnace open surface), and the latter is subjected to argon etching on the surface of the samples that are in close contact with each other (hereinafter referred to as the close contact surface), and at the same time, the elemental analysis of the surface oxide film 12 is performed using an X-ray photoelectron spectroscopy device (XPS, product name: Quantera SXM, manufactured by ULVAC-PHI).

[0046] Figure 1B and 1C The results of the measurement of the oxide film of each alloy after pickling, heat treatment of the open surface in the furnace, and / or heat treatment of the close contact surface are shown. From these results, it can be seen that the oxide film of any alloy tested was completely removed by pickling, and the open surface in the furnace was completely removed even at 5×10 -5 A very thick oxide film will also be formed under a high vacuum of 100 Torr. The extent of oxide film formation on the bonding surface that is a problem in bonding has been confirmed to be:

[0047] i) Alloys (beryllium copper 11 alloy, beryllium copper 50 alloy, beryllium copper 10Zr alloy, chromium copper alloy, Corson copper AMPCO940 and Corson copper AMPCO944) with a beryllium content of 0.7 wt % or less were heated to 5×10 -5 When the process is carried out at the bonding temperature under a high vacuum of 0.1 Torr (the vacuum degree achieved by continuous exhaust with a diffusion pump), no oxide film is formed or only a very slight oxide film is formed.

[0048] ii) Even for alloys with a beryllium content of 0.7 wt% or less, -1 Even at a vacuum of about 1000 Torr, an oxide film may be formed due to oxygen intruding into the sealing surface, and

[0049] iii) Alloys with a beryllium content exceeding 0.7 wt. % (beryllium copper 25 alloy and beryllium copper 165 alloy) have a high beryllium content even at 5×10 - 5The above results show that beryllium has a very high affinity with oxygen. Therefore, when the beryllium concentration is above a certain level, even if the closeness of the parts is improved under high vacuum, it is difficult to suppress the formation of the oxide film caused by the oxygen invading the joint surface. In order to avoid the oxide film remaining on the joint surface, the beryllium content must be considered when selecting the raw materials.

[0050] The age-hardening copper alloy used in the copper alloy joint body of the present invention is not particularly limited as long as the beryllium content is less than 0.7 weight %, and may not contain beryllium (i.e., the beryllium content is 0 weight %). A joint body using a beryllium copper alloy with a high Be content exceeding 0.7 weight % (e.g., beryllium copper 25 alloy (JIS alloy number C1720)) has a significant oxide film remaining on the joint surface, cannot withstand solution treatment and aging treatment, and will break at the joint after solution treatment or aging treatment. However, by selectively using an age-hardening copper alloy with a low Be content of less than 0.7 weight % for diffusion bonding, a copper alloy joint body that can withstand solution treatment and aging treatment and has extremely high bonding strength can be achieved. Examples of such age-hardening copper alloys include beryllium copper 11 alloy (JIS alloy number C1751, EN material number CW110C, and UNS alloy number C17510), beryllium copper 10 alloy (EN material number CW104C and UNS alloy number C17500), beryllium copper CuCo1Ni1Be (EN material number CW103C), beryllium copper 14Z alloy, beryllium copper 50 alloy, beryllium copper 10Zr alloy, chromium copper (UNS alloy number C18200), chrome zirconium copper (UNS alloy number C18510 and EN material number CW106C), zirconium copper (UNS alloy number C15000, EN material number CW120C) and Corson copper (EN material number CW109C, CW111C, UNS alloy number C19010, C70250, AMPCO944 and AMPCO940), more preferably beryllium copper 11 alloy. These preferred age-hardening alloys can not only achieve extremely high bonding strength after solution aging, but also have excellent hydrogen embrittlement resistance and thermal conductivity, and are particularly advantageous as materials for heat exchangers of precoolers for hydrogen refueling stations. The compositions of the above-mentioned various copper alloys are shown in Table 1 below.

[0051] [Table 1]

[0052]

[0053] As described above, the copper alloy joint of the present invention has a plurality of joint interfaces remaining. The disappearance or remaining of the joint interface can be determined by observing the cross section of the copper alloy joint including the joint portion at a magnification of 200 to 1000 times using a laser microscope (for example, see the following). Figures 3 to 5 ). The disappearance / remaining of the joining interface is determined by whether traces of the joining surface of the copper alloy parts before joining remain. In addition, in the laser microscope image of the cross-section including the joining interface, the copper alloy joint of the present invention has a ratio of the total length of the line segments corresponding to the discontinuous area to the total length of the joining interface line drawn along the joining interface and the position where the joining interface was originally located, which is 3.5% or more. The cross-section including the joining interface is preferably set as a rectangular cross-section with a long side of 1200μm and a short side of 200μm (wherein the long side is parallel to the joining interface and the short side is perpendicular to the joining interface). The term "joining interface line" in this specification is a boundary line drawn along the joining interface and the position where the joining interface was originally located in a laser microscope image (expected to be an image deeply synthesized by a laser microscope) (cross-sectional observation image), and is a continuous line composed of a residual line segment determined based on the remaining joining interface and an imaginary line segment determined by extrapolating the residual line segment to the region where the joining interface disappears. That is, the bonding interface line can be defined by connecting the remaining line segments of the bonding interface and extrapolating these remaining line segments to the part where the bonding interface disappears to form a continuous line. Therefore, in this specification, the term "bonding interface line" and the term "bonding interface" are used separately.

[0054] like Figure 2A and Figure 2B As schematically shown in FIG. 1 , the discontinuous region is defined as a region where three or more adjacent perpendicular lines do not intersect the remaining bonding interface when multiple perpendicular lines are drawn at 5 μm intervals on the bonding interface line. That is, the discontinuous region may be as follows: Figure 2A As shown in FIG. 1 , the bonding interface completely disappears, so that the region where three or more adjacent perpendicular lines do not intersect with the bonding interface may also be as shown in FIG. Figure 2B As shown in FIG. 1 , the bonding interface is discontinuously interrupted, so that more than three adjacent perpendicular lines do not intersect the bonding interface. In the former discontinuous area ( Figure 2A ) does not contain any debris or traces of the bonding interface, on the other hand, in the latter discontinuity region ( Figure 2B ) but it does not intersect with more than 3 perpendicular lines. Moreover, the presence of such a discontinuous area helps to achieve extremely high bonding strength. It is believed that the presence of the discontinuous area reduces the proportion of oxides in the interface, which helps to improve the bonding strength. Relative to the total length of the bonding interface line, the ratio of the total length of the line segments corresponding to the discontinuous area is 3.5% or more, preferably 4.5% or more, more preferably 7.5% or more, and further preferably 10% or more. The upper limit of the ratio of the total length of the line segments corresponding to the discontinuous area is not particularly limited, and is typically 80% or less, more typically 70% or less, further typically 50% or less, and particularly typically 30% or less.

[0055] Therefore, the copper alloy joint of the present invention has extremely high joint strength. That is, by making the ratio of the total length of the discontinuous area in the cross-sectional observation image to the total length of the joint interface line be 3.5% or more, the starting point of crack generation during the tensile test will be reduced or the crack propagation speed will be reduced, and as a result, extremely high joint strength can be achieved. Specifically, the strength of the joint portion of the copper alloy joint is preferably 70% or more of the strength of the parent material of the copper alloy joint, more preferably 85% or more, further preferably 90% or more, and particularly preferably 95%. This strength is assumed to be a value at 25°C, but from the perspective of being able to maintain the joint strength even in extremely low temperature conditions such as liquid hydrogen and liquid oxygen, it is preferred that the strength within the above range can be achieved at -196°C. Therefore, the joint portion of the copper alloy joint preferably has a joint strength of 85% or more of the strength of the parent material of the copper alloy joint at a temperature of -196°C, more preferably 90% or more, and further preferably 95% or more. The strength of the joint of the copper alloy joint body is as high as possible, so the upper limit is not particularly limited, and is typically less than 100% of the strength of the parent material of the copper alloy joint body. The above strength is typically the strength after solution aging treatment. The strength of the parent material and the joint of the copper alloy joint body can be measured as follows: a test piece according to ASTM E8M Specimen 3 is made in such a way that the joint becomes the center position of the test piece, and the test piece is subjected to a tensile test according to the process according to ASTM E8M, thereby measuring.

[0056] Furthermore, the joint of the copper alloy joint preferably has a Charpy impact value of 15% or more of the Charpy impact value of the parent material of the copper alloy joint at each temperature of 25°C and -196°C, more preferably 25% or more, and further preferably 60% or more. In this way, by having a Charpy impact value within the above range not only at room temperature but also at -196°C, the desired performance of the copper alloy joint can be maintained even in extremely low temperature conditions such as liquid hydrogen and liquid oxygen. The higher the Charpy impact value of the joint of the copper alloy joint, the better, so its upper limit is not particularly limited, and is typically 80% or less of the Charpy impact value of the parent material of the copper alloy joint, more typically 70% or less, and further typically 60% or less. The Charpy impact values ​​of the parent material and the joint of the copper alloy joint can be measured according to JIS Z2242:2018 and the process of the embodiment described later.

[0057] An oxide film may exist at the bonding interface of the copper alloy joint body of the present invention. The thickness of the oxide film is typically 0 nm or more and 5.0 nm or less, preferably 0 nm or more and 4.0 nm or less, more preferably 0 nm or more and 3.0 nm or less, further preferably 0 nm or more and 2.0 nm or less, particularly preferably 0 nm or more and 1.5 nm or less, and most preferably 0 nm or more and 1.0 nm or less. If it is such a thin oxide film, a copper alloy joint body that can withstand solid solution aging treatment and has extremely high bonding strength after aging treatment can be obtained, similarly to the case where the bonding interface disappears. The thickness of the oxide film at the bonding interface can be determined as follows: a cross section including the bonding interface is observed with a scanning transmission electron microscope (STEM), an elemental mapping image of the cross section is obtained by electron energy loss spectroscopy (EELS) / energy dispersive X-ray analysis (EDX), and the STEM image is compared with the EELS / EDX elemental mapping image, thereby determining the oxide film and determining its thickness. It should be noted that the oxide film present at the bonding interface is not limited to a layered film but may also be a particle-shaped film (ie, oxide particles). In this case, the height of the oxide particles is also included in the thickness of the oxide film.

[0058] The copper alloy joint body of the present invention may include grains of age-hardenable copper alloy that have grown beyond the joint interface or the position that was originally the joint interface (old joint interface). That is, the copper alloy joint body of the present invention has a structure at the joint interface or the old joint interface where the grains of the joint surface of the copper alloy parts before joining are reorganized and recrystallized after joining, and a state of the joint interface that is not the state of the joint interface at the beginning of joining can be observed. The copper alloy joint body has such a joint microstructure, so that the joint strength becomes more excellent.

[0059] From the viewpoint of ensuring high bonding strength equal to the strength of the base material and hydrogen resistance equal to the base material, the copper alloy joint body of the present invention preferably does not have residual components from materials other than the age-hardening copper alloy at the bonding interface or the position (old bonding interface) that was originally the bonding interface. Therefore, it is expected that the copper alloy joint body of the present invention does not contain bonding agents such as brazing filler metal in the bonding. That is, the copper alloy joint body of the present invention is preferably composed only of inclusions composed of age-hardening copper alloy and oxides, carbides and / or intermetallic compounds thereof.

[0060] The strength of the base material and the joint of the copper alloy joint body after solution aging treatment is preferably 520MPa or more, and more preferably 690MPa or more. The copper alloy joint body is such a strength that the benchmark required for high-strength uses represented by the use of heat exchangers as precoolers for hydrogen stations is fully met. Since the expected strength is high, its upper limit should not be limited, but the strength of the base material and the joint of the copper alloy joint body having a beryllium content of less than 0.7% by weight after solution aging treatment is typically less than 895MPa. The strength of the base material and the joint of the copper alloy joint body before and after solution aging treatment can be made according to ASTM E8M Specimen 3 by making the joint into the central position of the test piece, and the test piece is subjected to a tensile test according to the process of ASTM E8M to measure.

[0061] It is desirable that the thermal conductivity of the base material of the joint part including the copper alloy joint body is high. Thermal conduction, like electrical conduction, is based on the energy transfer of conduction electrons, so there is a correlation between the two called the Wiedemann-Franz law, and thermal conductivity can be converted to electrical conductivity that can be measured more easily. The thermal conductivity (and its converted electrical conductivity) of the base material of the joint part including the copper alloy joint body is preferably 209W / mK or more (converted electrical conductivity 50IACS% or more), more preferably 228W / mK or more (converted electrical conductivity 55IACS% or more), and further preferably 246W / mK or more (converted electrical conductivity 60IACS% or more). If it is such a high thermal conductivity, it is advantageous in that the heat exchange efficiency is extremely high when used in a heat exchanger (for example, the thermal conductivity of the SUS316LNi equivalent material currently used for the heat exchanger of the precooler is 16W / mK due to its excellent hydrogen properties, which is very low, and becomes a difficulty in operation in terms of poor heat exchange efficiency). Since the thermal conductivity is expected to be high, its upper limit should not be limited, but for the base material of the joint portion of the copper alloy joint body of the present invention having a beryllium content of 0.7 weight % or less, the thermal conductivity of the base material that can ensure that the base material and the joint strength are 520 MPa or more is typically 280 W / mK or less.

[0062] The copper alloy joint including the joint part is subjected to a strain rate of 5×10 -5 s -1 The following range (e.g. 5×10 -5 s -1), the tensile strength in hydrogen is preferably 520 MPa or more, more preferably 690 MPa or more. The copper alloy joint, including the joint, has excellent hydrogen embrittlement resistance and high tensile strength. The low strain rate tensile test is carried out in accordance with ASTM-G-142. In the low strain rate tensile test, for example, a shaped test piece (smooth test piece) can be used. Usually, in a smooth test piece, the relative tensile strength RTS and relative cross-sectional reduction rate RRA, which are obtained by dividing the tensile strength and cross-sectional reduction rate in hydrogen by the tensile strength and cross-sectional reduction rate in a reference gas that is not affected by hydrogen, are used to evaluate hydrogen sensitivity. In the low strain rate tensile test of a smooth test piece, for example, a strain rate of 5×10 -5 s -1 Carry out the measurement. Assuming a 70MPa-level FCV (fuel cell vehicle) and a hydrogen refueling station, the low strain rate tensile test is carried out under a hydrogen pressure of more than 95MPa. If the hydrogen pressure is higher, the amount of hydrogen intruding into the material becomes more, so the test piece is easily affected by hydrogen exposure, and hydrogen embrittlement can be evaluated more appropriately. In tests related to the present application, it is preferred to use a shaped test piece (smooth test piece) and use relative tensile strength RTS and relative cross-sectional reduction RRA to evaluate hydrogen properties. For example, a copper alloy joint is cut out, and a test piece according to ASTM E8M Specimen 4 is made in such a way that the joint portion becomes the center position of the test piece.

[0063] For the copper alloy joint body including the joint, in the above-mentioned low strain rate tensile test, when the tensile strength is 520MPa or more, preferably 690MPa or more, the relative reduction of area RRA is preferably 0.8 or more, more preferably 0.9 or more. In addition, the tensile strength RTS is preferably 0.8 or more, more preferably 0.9 or more. When the tensile strength of the copper alloy joint body including the joint is a value within the above range at room temperature or under a hydrogen pressure of 95MPa or more, and its RRA and RTS also meet the values ​​within the above range, it means that the copper alloy joint body is high in strength and has excellent hydrogen embrittlement resistance, and is therefore particularly suitable for use as a heat exchanger for a precooler for a hydrogen refueling station. Since the above-mentioned tensile strength is expected to be high, its upper limit should not be limited, but the tensile strength of the copper alloy joint body having a beryllium content of 0.7% by weight or less in the low strain rate tensile test at room temperature or under a hydrogen pressure of 95MPa or more is typically 895MPa or less.

[0064] The copper alloy joint body may also be provided with a flow path space therein. In this case, the flow path space can be used as an internal space for passing a medium such as hydrogen or a refrigerant. Therefore, the copper alloy joint body provided with a flow path space can be preferably used as a heat exchanger for a precooler for a hydrogenation station that is expected to have a plurality of flow paths for passing hydrogen and a refrigerant, respectively.

[0065] Manufacturing method

[0066] The copper alloy joint body of the present invention can be produced by sequentially subjecting a plurality of age-hardenable copper alloy parts to smoothing of the joint surface as required (optional step), removal of oxide film, hot compression bonding (diffusion bonding), homogenization treatment as required (optional step), solution treatment and aging treatment. The details are as follows.

[0067] (a) Preparation of copper alloy parts

[0068] First, a plurality of age-hardening copper alloy parts to be joined are prepared. The age-hardening copper alloy has a beryllium content of 0.7 wt% or less, and the above-mentioned materials can be used. The topmost material and the bottommost material of the stacked joint body manufactured as a heat exchanger are preferably rolled materials or forged materials, and the plurality of stacked materials other than the topmost and bottommost materials with or without cooling water channels inside are preferably rolled materials.

[0069] The copper alloy joint of the present invention preferably uses a copper alloy material that does not cause hydrogen degradation. Regarding copper alloy raw materials, it is known that when the Ni concentration in white copper (Cu-10% to 30%) is 20% or more, hydrogen property degradation becomes significant, and even tough copper (undeoxidized pure copper) will significantly cause hydrogen property degradation. Therefore, when selecting a copper alloy for the copper alloy joint of the present invention, it is desirable to conduct a low strain rate tensile test in each atmosphere in the air and under high pressure hydrogen (for example, in 95MPa hydrogen) (for example, according to ASTM-G-142, the displacement rate of the smooth test piece is 0.001mm / sec (strain rate 0.00005 / sec)), and by comparing the test results in the air with the test results under high pressure hydrogen, it is confirmed that the copper alloy material does not degrade under hydrogen. For example, the copper alloy joint of the present invention is preferably used at a strain rate of 5×10 -5 s -1 The copper alloy part is produced such that the RRA (relative reduction of area) in hydrogen measured in the low strain rate tensile test conducted below is 0.8 or more, and more preferably 0.9 or more.

[0070] Here, for a plurality of age-hardening copper alloy parts used for joining, the surface to be joined needs to have a flat surface with a flatness of less than 0.1 mm and an arithmetic mean roughness Ra of less than 3.0 μm. That is, as described above, even if the oxide film on the surface of the joining parts is removed, in order to suppress the reoxidation of the joining surface during hot pressing (diffusion bonding), it is necessary to ensure the tightness of the joining surface so that the oxygen atoms invading the joining surface are sufficiently reduced even in a high vacuum atmosphere. If the flatness and Ra are within the above range, the tightness can be ensured. In the case where the joined parts are rolled materials, most of them meet the flatness and Ra within the above range, so no special smoothing process is required. On the other hand, in the case where the flatness and Ra within the above range are not met, a flat surface with a flatness and Ra within the above range is formed by grinding, cutting and / or other methods. It should be noted that sometimes the plate has curling, etc., but as long as the plate thickness accuracy is well adjusted, when the necessary load is applied in the hot pressing bonding (diffusion bonding), the flatness becomes less than 0.1mm, and there is no problem in ensuring the tightness as the target. It should be noted that the arithmetic mean roughness Ra is the surface roughness specified in JIS B 0601-2001. The arithmetic mean roughness Ra of the flat surface is less than 3.0μm, preferably less than 1.0μm, more preferably 0.50~1.0μm, and further preferably 0.10~0.50μm. In addition, in this specification, flatness is defined as a parameter of "the size of the deviation from the geometrically correct plane (geometric plane) of the plane body" in JIS B 0621-1984, and refers to the value represented by its width when the object is clamped by a pair of planes.

[0071] As needed, preferably before the oxide film is removed in the next process, grooves that become flow path spaces after joining are formed on the surfaces to be joined of the multiple parts. The formation of the grooves can be carried out by various well-known methods such as etching, stamping, and machining. Thus, as described above, it can be used to manufacture a copper alloy joint body with a flow path space inside. For example, by alternately stacking and joining a grooved copper alloy plate and a grooveless copper alloy plate, a copper alloy laminate formed with multiple flow paths can be manufactured. A multilayer joint body of such a structure can be preferably used as a heat exchanger for a precooler for a hydrogen refueling station that is expected to have multiple flow path spaces for hydrogen supply and refrigerant to pass through respectively.

[0072] (b) Removal of oxide film

[0073] As described above, there is an oxide film on the surface of the copper alloy part. Therefore, it is necessary to remove the oxide film on the surface to be joined of the copper alloy part. From the perspective of being able to effectively remove the oxide film, the removal of the oxide film is preferably carried out by cleaning the surface to be joined of the copper alloy part with an inorganic acid solution. Examples of inorganic acid solutions include nitric acid, sulfuric acid, chemical polishing liquid, hydrochloric acid, nitric acid-sulfuric acid mixed bath (キリンス bath), hydrofluoric acid, etc., and nitric acid is particularly preferred. It should be noted that the chemical polishing liquid is an acid in which hydrogen peroxide as an oxidant is added to sulfuric acid, and the nitric acid-sulfuric acid mixed bath is a mixed acid of sulfuric acid, nitric acid and hydrochloric acid, and sometimes a small amount of sodium hydroxide is added. As an example of a preferred mixing ratio in the nitric acid-sulfuric acid mixed bath, sulfuric acid: nitric acid: hydrochloric acid = 61:4:4, 81:1:0.02 or 11:1:0.02 can be cited. Alternatively, the removal of the oxide film can be carried out by mechanical grinding, or mechanical grinding and cleaning with an inorganic acid solution can be used in combination.

[0074] (c) Thermocompression bonding (diffusion bonding)

[0075] The intermediate joint body is made by joining a plurality of copper alloy parts by hot pressing. The joining can be carried out by a diffusion bonding method. For example, hot pressing is preferably carried out by bonding at a temperature of more than 1.0×10 -2 Torr vacuum (i.e. less than 1.0×10 -2 Torr pressure) in a furnace at 500°C to 1050°C for 30 minutes to 480 minutes and a pressure of 5.0 MPa or more (preferably 10 MPa or more). However, in the case of an age-hardening copper alloy that does not contain Be (such as Corson copper), hot pressing can be performed by placing the alloy in a furnace with a pressure of 1.0×10 -1 Torr or higher vacuum degree (i.e., 1.0×10 -1Torr or lower pressure), and apply a pressure of 5.0 MPa or more at a temperature of 500°C to 1050°C for 30 minutes to 480 minutes. In any case, the hot pressing is carried out in a manner that the length deformation in the pressurizing direction when joining the copper alloy parts is preferably 0.5% to 35%, more preferably 0.5% to 30%, further preferably 1% to 20%, and particularly preferably 2% to 8%. There is a suitable combination of hot pressing temperature and pressure, preferably 5.0 MPa to 20 MPa when it is above 840°C and below 1050°C, 2 MPa to 24 MPa when it is above 720°C and below 840°C, and 4 MPa to 50 MPa when it is above 600°C and below 720°C. The hot pressing time is preferably 15 minutes to 480 minutes, more preferably 30 minutes to 150 minutes, and further preferably 30 minutes to 60 minutes. It should be noted that from the viewpoint of suppressing the progress of oxidation, the degree of vacuum in the furnace during hot pressing is preferably less than 1.0×10 -3 Torr, more preferably less than 1.0×10 -4 Torr, more preferably less than 5.0×10 -5 Torr.

[0076] In particular, when grooves are formed on the surface of the copper alloy component so that the intermediate joint body has a flow path space, the hot pressing is preferably performed at a relatively low temperature and a relatively high pressure from the viewpoint of being able to control the flow path flattening caused by the stamping to be slight. Specifically, the hot pressing in this method is performed at a vacuum degree of more than 1.0×10 -2 Torr vacuum (i.e. less than 1.0×10 -2 Torr), and more preferably higher than 1.0×10 -4 Torr vacuum (i.e. less than 1.0×10 -4 Torr pressure) in a furnace:

[0077] (i) applying a pressure of 1 MPa to 4 MPa at a temperature exceeding 840° C. and not exceeding 930° C. for 30 to 480 minutes (preferably 30 to 60 minutes); or

[0078] (ii) applying a pressure of 2 MPa to 8 MPa at a temperature exceeding 720° C. and not more than 840° C. for 30 to 480 minutes (preferably 30 to 60 minutes); or

[0079] (iii) Applying a pressure of 4 MPa to 30 MPa at a temperature of 600° C. to 720° C. for 30 to 480 minutes (preferably 30 to 60 minutes).

[0080] (d) Homogenization (optional step)

[0081] When grooves are formed on the surface of the copper alloy part so that the intermediate joint body has a flow path space, when hot pressing is performed at the relatively low temperature and high pressure, it is preferred that the temperature be higher than 1.0×10 -1 Torr vacuum (i.e. less than 1.0×10 -1 The intermediate joint body is subjected to a homogenization treatment for 60 minutes to 480 minutes in a furnace in a (normal or reduced pressure) nitrogen or other non-oxidizing gas atmosphere (inactive atmosphere) at a temperature of 900°C to 1050°C. Homogenization treatment is also called homogenization annealing, but the term homogenization treatment is used in this specification. That is, when hot pressing is performed at a relatively low temperature and a relatively high pressure, the bonding interface is likely to remain, but by performing a homogenization treatment, the bonding interface can be reduced or eliminated, and by subsequent solution treatment and aging treatment, extremely high bonding strength can be achieved. That is, it is possible to achieve both suppression of flow path flattening and high bonding strength. In order to suppress the progress of oxidation, the homogenization treatment is preferably performed at a temperature below 1.0×10 -1 Torr, or atmospheric pressure or reduced pressure to less than 1.0×10 -1 The treatment is carried out in an inert atmosphere such as nitrogen at a pressure of 0.1 to 0.04 Torr. The homogenization treatment temperature is preferably 900°C to 1050°C, more preferably 930°C to 1000°C, and further preferably 960°C to 990°C. The holding time at the above homogenization treatment temperature is 60 minutes to 480 minutes, more preferably 60 minutes to 360 minutes, and further preferably 60 minutes to 240 minutes. Of course, it goes without saying that the above homogenization treatment can be carried out as needed even if grooves are not formed on the surface of the copper alloy part.

[0082] It should be noted that (c) hot compression bonding (diffusion bonding) and (d) homogenization treatment are preferably performed continuously by releasing the pressurization load and raising the temperature without lowering the temperature in the furnace. Thus, after hot compression bonding (diffusion bonding) under a temperature pressurization condition in which the flow path space is not excessively flattened, the homogenization treatment at a temperature effective for homogenizing the tissue can be performed as a series of continuous operations without pressurization to flatten the flow path space, which is advantageous not only from the perspective of improving the reliability of the bonded portion but also from the perspective of economic efficiency.

[0083] (e) Solution treatment

[0084] The intermediate joint body is subjected to a solution treatment. The solution treatment is preferably carried out by heating the intermediate joint body at a temperature of 700°C to 1100°C in an atmospheric furnace, a non-oxidizing atmosphere furnace, a salt bath furnace, etc. for 1 minute to 180 minutes and then cooling it with water. The copper alloy used in the present invention is an age-hardening alloy. After the bonding interface disappears or the thickness of the oxide film at the bonding interface is adjusted to a certain value or less, it undergoes a solution treatment and a subsequent aging treatment, thereby being able to present the desired tempering characteristics (such as high strength), especially extremely high bonding strength. The suitable range of the solution treatment temperature will vary slightly depending on the alloy composition, but is preferably 700°C to 1100°C, more preferably 800°C to 1050°C, and further preferably 900°C to 1000°C. The actual holding time of the above-mentioned solution treatment temperature is preferably 1 minute to 180 minutes, more preferably 5 minutes to 90 minutes, and further preferably 10 minutes to 60 minutes.

[0085] (f) Aging treatment

[0086] The intermediate joint body subjected to the solution treatment is subjected to an aging treatment. The suitable region for the aging treatment will slightly vary depending on the alloy composition, but it is preferably carried out by performing an aging treatment at 350°C to 550°C for 30 minutes to 480 minutes. As described above, age-hardening alloys such as beryllium copper alloys can exhibit desired tempering properties (such as high strength), especially extremely high joint strength, by undergoing solution treatment and aging treatment. The aging treatment temperature is preferably 350°C to 550°C, more preferably 400°C to 500°C, and further preferably 450°C to 480°C. The holding time at the above-mentioned aging treatment temperature is preferably 30 minutes to 480 minutes, more preferably 30 minutes to 300 minutes, further preferably 60 minutes to 240 minutes, and particularly preferably 90 minutes to 180 minutes. From the viewpoint of inhibiting oxidation, the aging treatment is preferably performed at a temperature higher than 1.0×10 -1 Torr vacuum (i.e. less than 1.0×10 -1 Torr pressure) or in a furnace with a non-oxidizing atmosphere such as nitrogen.

[0087] Example

[0088] The present invention is further specifically described by the following examples.

[0089] Examples 1a to 7b

[0090] A copper alloy bonded body was produced according to the following procedure, and various evaluations were performed.

[0091] (1) Preparation of copper alloy

[0092] In each example, a plurality of copper alloy parts were prepared which were composed of the alloy types and compositions shown in Table 2 and had the following forms.

[0093] - 2 copper alloy round bars with a diameter of 80 mm and a length of 50 mm (Examples 1a to 1d and 6a to 7b)

[0094] - 2 forging materials (square bars or rectangular blocks) of 160mm x 280mm x length (thickness) 50mm (Examples 2a to 3)

[0095] - 2 forged materials (square bars or rectangular blocks) of 150mm×220mm×length (thickness) 25mm and 10 rolled materials (square plates) of 150mm×220mm×thickness 1.3mm (Examples 4a and 4b)

[0096] - 2 forged materials (square bars or rectangular blocks) of 50mm×50mm×length (thickness) 40mm and 4 rolled materials (square plates) of 50mm×50mm×thickness 1.3mm (Example 5)

[0097] The surfaces for joining of each copper alloy component (hereinafter referred to as joining surfaces) were processed by lathe processing, polishing and grinding, etc., and were made into flat surfaces with an arithmetic mean roughness Ra of less than 3.0 μm measured in accordance with JIS B 0601-2001 and a flatness of less than 0.1 mm measured in accordance with JIS B 0621-1984. The average values ​​of the arithmetic mean roughness Ra obtained by measuring the joining surfaces after surface treatment are shown in Table 2. It should be noted that, as representative values ​​of Ra shown in Table 2, in the case of two copper alloy round bars or two forged materials (Examples 1a to 3 and 6a to 7b), the average values ​​of Ra of the joining surface of the upper bar and Ra of the joining surface of the lower bar were used. In addition, in the case of two forged materials and 10 or 4 rolled materials (Examples 4a, 4b and 5), the average values ​​of Ra of the upper plate joining surface and Ra of the lower plate joining surface at one joining position of the 10 or 4 rolled materials were used as representative values.

[0098] (2) Removal of oxide film

[0099] The joining surfaces of the copper alloy parts were cleaned with 30% nitric acid to remove the oxide film present on the joining surfaces.

[0100] (3) Hot pressing

[0101] In Examples 1a to 3 and 6a to 7b, the joint surfaces of two copper alloy round bars or two forged materials cleaned with nitric acid are directly butted against each other (without brazing filler metal), and hot pressed in a vacuum furnace under the joining conditions shown in Table 2 to obtain a round bar or square bar intermediate joint body. In Examples 4a, 4b and 5, the joint surfaces of two copper alloy casting materials (square bars) cleaned with nitric acid are butted against each other with 10 sheets (Examples 4a and 4b) or 4 sheets (Example 5) of copper alloy rolled materials (square plates) (without brazing filler metal) between them, and hot pressed in a vacuum furnace under the joining conditions shown in Table 2 to obtain a square bar intermediate joint body. The cumulative length of the length of the copper alloy parts in the joining direction before joining is set as L0, and the length of the sample in the joining direction after joining is set as L1, and the deformation amount ΔL during joining at this time is calculated by the following formula:

[0102] ΔL=[(L0-L1) / L0]×100

[0103] The results are shown in Table 2. In order to perform various evaluations, a plurality of tensile test specimens were prepared for each example.

[0104] (4) Homogenization (only in Examples 1b-1d, 2b-2f, 6b and 7b)

[0105] In Examples 1b to 1d, 2b to 2f, 6b and 7b, the heated and pressed intermediate joint body was subjected to homogenization treatment (high temperature holding) at the temperature shown in Table 3 for 8 hours and furnace cooling before the subsequent solution treatment.

[0106] (5) Solution treatment

[0107] The intermediate bonded body obtained in (2) or (3) is subjected to a solution treatment by holding the copper alloy bonded body in a molten salt bath at 930° C. for 5 minutes and then cooling with water.

[0108] (6) Aging treatment

[0109] The intermediate joint body subjected to the solution treatment is subjected to an aging treatment. The aging treatment is performed by subjecting the copper alloy joint body to a temperature of 1×10 -1 The method is carried out by holding the copper alloy in a vacuum furnace at a vacuum degree of 100 torr at 450°C for 3 hours (Examples 1a to 5) or at 500°C for 2 hours (Examples 6a to 7b) and then cooling the copper alloy in the furnace. In this way, a round rod or square rod-shaped copper alloy joint body is obtained after being tempered by solution treatment and aging treatment (Examples 1a, 2a, 3 to 6a and 7a) or by homogenization treatment, solution treatment and aging treatment (Examples 1b to 1d, 2b to 2f, 6b and 7b).

[0110] (7) Evaluation

[0111] The following evaluations were performed on the intermediate joined body joined by the hot pressing and the copper alloy joined body obtained by the aging treatment (hereinafter, these are collectively referred to as joined body samples).

[0112] <Joint Strength>

[0113] Each joint sample was processed to produce a test piece according to ASTM E8M Specimen 3 in such a way that the joint portion was the center of the test piece. For the test piece, a tensile test was performed at 25°C and / or -196°C according to ASTM E8M, and the tensile strength (joint strength) was measured, and the fracture position was confirmed. The results are shown in Tables 3 and 4.

[0114] <Observation of the cross section of the joint using a laser microscope>

[0115] The cross section including the joint part of the joint sample that was further subjected to solution treatment and aging treatment after joining was cut out and ground. As an observation sample, a material that was adjacent to the part cut out from the tensile test piece as described above and had undergone the same joint heat treatment process was used. After the obtained cross section was etched with a mixture of 30-36% hydrogen peroxide water and 29% ammonia water, the microstructure of the joint was observed at a magnification of 500 times using a laser microscope (manufactured by KEYENCE, VK-X100) to confirm the residual joining interface. These images were processed using the automatic image connection function to obtain images for image analysis. At this time, a rectangular cross section with a long side of 1200μm × a short side of 200μm was included in the laser microscope image (the image obtained by deep synthesis using a laser microscope) (wherein the long side is parallel to the joining interface and the short side is perpendicular to the joining interface). Figure 3 to Figure 5 The cross-sectional photographs obtained in Examples 1a to 7b are shown.

[0116] <Ratio of discontinuous area in bonding interface line>

[0117] The laser microscope image obtained above was analyzed using the image analysis software ImageJ according to the following operation procedure to determine the ratio (%) of the total length of the line segments corresponding to the discontinuous regions to the total length of the bonding interface line.

[0118] (Operation process in ImageJ)

[0119] -Step 1: Import the laser microscope image into the image analysis software ImageJ (refer to Fig. 6A (a)).

[0120] - Step 2: A region of 1200 μm×200 μm including the bonding interface is cut out (this region is referred to as a “region of interest”).

[0121] -Step 3: Select the command in the order of "Image" → "Type" → "16-bit" to convert the image to "16-bit".

[0122] Step 4: Select the commands in the order of "Process" → "Filters" → "Gaussian Blur", and adjust the "Sigma (Radius)" value (for example, 0.1) through the Gaussian Blur function to reduce noise.

[0123] - Step 5: Select the command in the order of "Image" → "Adjust" → "Threshold" to adjust the threshold value and color the grain boundary and the bonding interface (refer to Figure 6B ). At this time, in the "Threshold" window, the threshold value is adjusted so that only the grain boundaries and the bonding interface are selectively colored red (the threshold value is set to a value greater than 140 in this analysis), and the region corresponding to the grain boundaries and the bonding interface is selected.

[0124] - Step 6: Select the "Apply" command in the "Threshold" window while the grain boundaries and the bonding interface are colored, and perform binarization on the area of ​​interest (see Fig. 6A (c)).

[0125] - Step 7: In the obtained binary processed image, numerous vertical lines are synthesized at 5 μm intervals on the bonding interface (refer to Figure 6B (d)). The synthesis of the vertical line can be performed in PowerPoint.

[0126] - Step 8: In the obtained composite image, the area where three or more adjacent vertical lines (with a pitch of 5 μm) (i.e., a width of 10 μm or more) do not intersect with the remaining bonding interface (refer to Figure 2A and 2B ) is determined as a discontinuous area.

[0127] -Step 9: Enlarge the image corresponding to the total length of the bonding interface line drawn along the bonding interface and the position that was originally the bonding interface (i.e., 1200 μm), and visually select the discontinuous area. The selection of the discontinuous area is performed by adding a length measuring line in the enlarged image according to each part determined to be a discontinuous area. Specifically, in ImageJ, select the commands in the order of "Edit" → "Add to Manager" → "ROI Manager" (or "Analyze" → "Tool" → "ROI Manager") to start the ROI Manager. Then, the so-called straight line (refer to Figure 6B A straight line (icon shown in (e)) is drawn parallel to the bonding interface line in an area containing three or more vertical lines with a spacing of 5 μm (overall width of 10 μm or more). Click "Add" in the ROI manager window to add a straight line (6B (e)). In this way, multiple straight lines can be drawn.

[0128] -Step 10: Click "Measure" in the ROI Manager window to automatically display the length of each straight line. Figure 6B (f)). In this way, the total length of the line segments corresponding to the discontinuous regions can be automatically calculated.

[0129] - Step 11: Calculate the ratio of the total value of the straight line length to the total length using Excel spreadsheet software. That is, by dividing the obtained total length by the total length of the bonding interface line (i.e., 1200 μm) and then multiplying by 100, the ratio (%) of the total length of the line segments corresponding to the discontinuous region to the total length of the bonding interface line (i.e., 1200 μm) is calculated.

[0130] <Charpy Shock Value>

[0131] In order to measure the Charpy impact value of the parent material and the joint of the joint sample, a Charpy impact test according to JIS Z2242:2018 was performed. The Charpy impact test was performed as follows: the joint sample was processed to make a V-notch test piece specified in JIS Z2242:2018 (length 55mm, square cross-section shape with one side of 10mm, V-notch at the center of the length, notch angle 45°, notch depth 2mm and notch bottom radius 0.25mm), and the Charpy impact value (absorbed energy) was measured at 25°C or -196°C using a Charpy impact tester (Tokyo Hyoki Testing Machinery Co., Ltd., automatic Charpy impact tester CI-500D). As a test piece for measuring the Charpy impact value of the parent material, a test piece with a V-notch formed on a parent material sample prepared separately using the raw material for making the joint was used. On the other hand, as a test piece for measuring the Charpy impact value of the joint, a test piece with a V-notch formed in a manner such that the front end of the V-notch is located at the joint interface position of the joint was used. The test piece with the tip of the V-notch at the bonding interface position was obtained by etching the bonded body sample with 30% nitric acid in advance to determine the position of the bonding interface, and then forming the V-notch so that the tip of the V-notch coincided with the bonding interface position.

[0132] <Measurement of electrical conductivity and conversion to thermal conductivity>

[0133] The conductivity (IACS%) of the bonded body sample was measured at room temperature using an eddy current conductivity meter (product name: Hocking Auto Sigma 3000DL, manufactured by GE Sensing & Inspection Technologies Inc.) The obtained conductivity was converted using a correlation equation based on the Wiedemann-Franz law to obtain thermal conductivity (W / mK).

[0134] [Table 2]

[0135]

[0136] [Table 3]

[0137]

[0138] [Table 4]

[0139]

Claims

1. A copper alloy joint body, comprising a plurality of age-hardening copper alloy parts that are diffusion-bonded to each other, wherein a bonding interface of the plurality of parts remains, The age-hardenable copper alloy has a beryllium content of 0.7 wt % or less, and in a laser microscope image of a cross section including the bonding interface, a ratio of a total length of line segments corresponding to discontinuous regions to a total length of a bonding interface line defined along the bonding interface and a position originally at the bonding interface is 3.5% or more, The discontinuous region is defined as a region where, when a plurality of perpendicular lines are drawn at a pitch of 5 μm to the bonding interface line, three or more adjacent perpendicular lines do not intersect with the remaining bonding interface.

2. The copper alloy joint body according to claim 1, in, The copper alloy joint body has been subjected to solution treatment and aging treatment.

3. The copper alloy joint according to claim 1 or 2, in, The strength of the joint portion of the copper alloy joint body is 70% or more of the strength of a base material of the copper alloy joint body.

4. The copper alloy joined body according to claim 1 or 2, in, The strength of the joint portion of the copper alloy joined body is 85% or more of the strength of a base material of the copper alloy joined body. 5 . The copper alloy joint body according to claim 1 , comprising: grains of the age-hardenable copper alloy grown beyond the joint interface or a position that was originally the joint interface.

6. The copper alloy joined body according to claim 1 or 2, in, No residual component derived from a material other than the age-hardenable copper alloy exists at the joint interface or at a position which was originally the joint interface.

7. The copper alloy joined body according to claim 1 or 2, in, The strength of the base material and the joint of the copper alloy joint body is 520 MPa or more.

8. The copper alloy joined body according to claim 5, in, The strength of the base material and the joint of the copper alloy joint body is 690 MPa or more.

9. The copper alloy joined body according to claim 1 or 2, in, The joined portion of the copper alloy joined body has a joining strength at a temperature of -196°C that is 85% or more of the strength of a base material of the copper alloy joined body.

10. The copper alloy joined body according to claim 1 or 2, in, The joined portion of the copper alloy joined body has a Charpy impact value of 15% or more of a Charpy impact value of a base material of the copper alloy joined body at each of 25° C. and −196° C.

11. The copper alloy joined body according to claim 1 or 2, in, The thermal conductivity of a base material of a joining portion including the copper alloy joined body is 209 W / mK or more.

12. The copper alloy joined body according to claim 1 or 2, in, The electrical conductivity of a base material of a joined portion including the copper alloy joined body is 50 IACS% or more.

13. The copper alloy joined body according to claim 1 or 2, in, The age-hardenable copper alloy is at least one selected from the group consisting of the following alloys: Beryllium copper 11 alloy, namely JIS alloy number C1751, EN material number CW110C and UNS alloy number C17510; Beryllium copper 10 alloy, EN material number CW104C and UNS alloy number C17500; Beryllium copper CuCo1Ni1Be, EN material number CW103C; Beryllium copper 14Z alloy, wherein Be: 0.2-0.6 wt %, Ni: 1.4-2.4 wt %, Zr: 0-0.5 wt %, and the balance is Cu and unavoidable impurities; Beryllium copper 50 alloy, wherein Be: 0.2-0.6 wt %, Ni: 1.4-2.1 wt %, Ag: 0.1-0.3 wt %, Zr: 0-0.5 wt %, and the balance is Cu and unavoidable impurities; Beryllium copper 10Zr alloy, wherein Be: 0.4-0.7 wt %, Co: 2.0-2.8 wt %, Zr: 0-0.3 wt %, and the balance is Cu and unavoidable impurities; Chromium copper, UNS alloy number C18200; Chrome zirconium copper, i.e. UNS alloy number C18510 and EN material number CW106C; Zirconium copper, UNS alloy number C15000, EN material number CW120C; and Corson copper, namely EN material number CW109C, CW111C, UNS alloy number C19010, C70250, AMPCO944 and AMPCO940, wherein, in AMPCO944, Ni: 6.5-7.5 weight%, Si: 1.5-2.5 weight%, Cr: 0.5-1.5 weight%, and the balance is composed of Cu and inevitable impurities; in AMPCO940, Ni: 1.5-3.0 weight%, Si: 0.5-1.5 weight%, Cr: 0.3-1.5 weight%, and the balance is composed of Cu and inevitable impurities.

14. The copper alloy joined body according to claim 13, in, The age-hardenable copper alloy is beryllium copper 11 alloy, namely JIS alloy number C1751, EN material number CW110C and UNS alloy number C17510.

15. The copper alloy joined body according to claim 1 or 2, in, The copper alloy bonded body includes a flow path space therein.

Citation Information

Patent Citations

  • Beryllium copper alloy for heat exchanger

    JP1997087780A

  • Hydrogen resistant member and application method of hydrogen resistant member

    JP2017145472A