Photosensitive resin composition, photosensitive element, printed wiring board, and method for producing printed wiring board
A photosensitive resin composition with specific components addresses the need for improved resolution and resistance in printed circuit boards by forming a permanent resist with enhanced fine pattern formation, heat resistance, and thermal shock resistance, suitable for advanced printed circuit board manufacturing.
Patent Information
- Application Number
- CN202380035615.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-06
- Filing Date
- 2023-04-27
- Publication Date
- 2024-12-03
AI Technical Summary
Printed circuit boards require resists with improved fine pattern formation, heat resistance, and thermal shock resistance as they become more dense, and existing methods struggle to balance these characteristics effectively.
A photosensitive resin composition containing an acid-modified vinyl resin, a thermosetting resin with a bisphenol-type epoxy compound, a photopolymerization initiator, a photopolymerizable compound, and an acrylic elastomer, which is used to form a photosensitive element and printed wiring board with enhanced resolution and resistance properties.
The composition enables the formation of a permanent resist with excellent resolution, heat resistance, and thermal shock resistance, suitable for advanced printed circuit board manufacturing processes.
Smart Images

Figure CN119072656A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a photosensitive resin composition, a photosensitive element, a printed circuit board and a method for manufacturing the printed circuit board. Background Art
[0002] In the field of printed wiring boards, a process of forming a permanent resist on a printed wiring board is performed. The permanent resist has the function of preventing corrosion of a conductor layer or maintaining electrical insulation between conductor layers when the printed wiring board is used. In recent years, the permanent resist also has the function of preventing solder from adhering to unnecessary parts of the conductor layer of the printed wiring board during the process of flip chip mounting or wire bonding mounting of semiconductor elements on the printed wiring board via solder, as a solder resist film.
[0003] Conventionally, permanent resists are produced by a method of screen printing using a thermosetting resin composition using a photographic method of a photosensitive resin composition. For example, in a flexible wiring board using a mounting method such as FC (Flip Chip), TAB (Tape Automated Bonding), COF (Chip On Film), in addition to IC chips, electronic parts or LCD (Liquid Crystal Display) panels and connection wiring pattern portions, a thermosetting resin paste is screen printed and thermally cured to form a permanent resist (for example, refer to Patent Document 1).
[0004] In semiconductor package substrates such as BGA (Ball Grid Array) and CSP (Chip Size Package) mounted on electronic parts, it is necessary to remove the permanent resist at the bonding portion (1) in order to flip-chip mount the semiconductor element on the semiconductor package substrate via solder, (2) in order to wire-bond the semiconductor element to the semiconductor package substrate, or (3) in order to solder the semiconductor package substrate to the motherboard substrate. In the image formation of the permanent resist, a photographic method is used in which a photosensitive resin composition is applied and dried, then selectively irradiated with active light such as ultraviolet rays to cure it, and only the unirradiated portion is removed by development to form an image. Photolithography is suitable for mass production because of its good workability, and is therefore widely used in the electronic materials industry for image formation of photosensitive materials.
[0005] (For example, refer to Patent Document 2).
[0006] Previous technical literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2003-198105
[0009] Patent Document 2: Japanese Patent Application Publication No. 2011-133851 Summary of the invention
[0010] Technical issues to be solved by the invention
[0011] As printed circuit boards become more dense, permanent resists (solder resists) are also required to have higher performance. In particular, the requirements for fine pattern formation, heat resistance, and thermal shock resistance are increasing year by year, and it is important to achieve a high balance between these characteristics.
[0012] An object of the present invention is to provide a photosensitive resin composition capable of forming a permanent resist having excellent resolution and pattern forming properties and excellent heat resistance and thermal shock resistance, a photosensitive element using the photosensitive resin composition, a printed wiring board, and a method for producing a printed wiring board.
[0013] Means for solving technical problems
[0014] One aspect of the present invention relates to a photosensitive resin composition, which contains (A) an acid-modified vinyl resin, (B) a thermosetting resin, (C) a photopolymerization initiator, (D) a photopolymerizable compound and (E) an elastomer, wherein the (B) thermosetting resin includes a bisphenol-type epoxy compound having an average molecular weight of less than 360, and the (E) elastomer includes an acrylic elastomer.
[0015] Another aspect of the present invention relates to a photosensitive element comprising a support film and a photosensitive layer formed on the support film, wherein the photosensitive layer comprises the photosensitive resin composition.
[0016] Another aspect of the present invention relates to a printed wiring board comprising a permanent resist comprising a cured product of the photosensitive resin composition.
[0017] Another aspect of the present invention relates to a method for manufacturing a printed wiring board, which comprises the steps of forming a photosensitive layer on a substrate using the above-mentioned photosensitive resin composition or photosensitive element, exposing and developing the photosensitive layer to form a resist pattern, and curing the resist pattern to form a permanent resist.
[0018] Effects of the Invention
[0019] According to the present invention, there can be provided a photosensitive resin composition capable of forming a permanent resist having excellent resolution and pattern forming properties and excellent heat resistance and thermal shock resistance, a photosensitive element using the photosensitive resin composition, a printed wiring board, and a method for producing a printed wiring board. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a cross-sectional view schematically showing the photosensitive element of this embodiment. DETAILED DESCRIPTION
[0021] One aspect of the present invention relates to the following photosensitive resin composition, photosensitive element, printed wiring board, and method for producing the printed wiring board.
[0022] [1] A photosensitive resin composition comprising (A) an acid-modified vinyl-containing resin, (B) a thermosetting resin, (C) a photopolymerization initiator, (D) a photopolymerizable compound, and (E) an elastomer, wherein the thermosetting resin comprises a bisphenol-type epoxy compound having an average molecular weight of 360 or less, and the elastomer comprises an acrylic elastomer.
[0023] [2] The photosensitive resin composition according to [1] above, wherein
[0024] The content of the thermosetting resin is 5 to 25% by mass based on the total solid content of the photosensitive resin composition.
[0025] [3] The photosensitive resin composition according to [1] or [2] above, wherein
[0026] The acrylic elastomer has a carboxyl group.
[0027] [4] The photosensitive resin composition according to [3] above, wherein
[0028] The acrylic elastomer further has an n-butyl group.
[0029] [5] The photosensitive resin composition according to any one of [1] to [4] above, wherein
[0030] The weight average molecular weight of the acrylic elastomer is 5,000 to 20,000.
[0031] [6] The photosensitive resin composition according to any one of [1] to [5], further comprising (I) a silane coupling agent.
[0032] [7] The photosensitive resin composition according to any one of [1] to [6] above, further comprising (F) an inorganic filler.
[0033] [8] A photosensitive element comprising a support film and a photosensitive layer formed on the support film, wherein the photosensitive layer comprises the photosensitive resin composition according to any one of [1] to [7] above.
[0034] [9] A printed wiring board comprising a permanent resist comprising a cured product of the photosensitive resin composition according to any one of [1] to [7] above.
[0035]
[10] A method for manufacturing a printed circuit board, comprising:
[0036] The process of forming a photosensitive layer on a substrate using the photosensitive resin composition described in any one of [1] to [7] above; exposing and developing the photosensitive layer to form a resist pattern; and curing the resist pattern to form a permanent resist.
[0037]
[11] A method for manufacturing a printed circuit board, comprising:
[0038] The process of forming a photosensitive layer on a substrate using the photosensitive element described in [8] above; the process of exposing and developing the photosensitive layer to form a resist pattern; and the process of curing the resist pattern to form a permanent resist.
[0039] Hereinafter, the present invention will be described in detail. In this specification, the term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes as long as the expected effect of the process is achieved. Regarding the term "layer", when observed in a plan view, in addition to the structure of the shape formed on the entire surface, it also includes a structure of the shape formed on a part. The numerical range represented by "~" indicates a range in which the numerical values recorded before and after "~" are included as the minimum and maximum values, respectively. Within the numerical range recorded in stages in this specification, the upper limit or lower limit of the numerical range of any stage can also be replaced by the upper limit or lower limit of the numerical range of other stages. Within the numerical range recorded in this specification, the upper limit or lower limit of its numerical range can be replaced by the value shown in the embodiment.
[0040] In the present specification, when the amount of each component in a composition is mentioned, or when a plurality of substances corresponding to each component are present in a composition, unless otherwise specified, the amount refers to the total amount of the plurality of substances present in the composition.
[0041] In this specification, the so-called "(meth)acrylate" refers to at least one of "acrylate" and its corresponding "methacrylate", and the same applies to other similar expressions such as (meth)acrylic acid, (meth)acryloyl, etc. In this specification, "solid content" refers to non-volatile components other than volatile substances (water, solvent, etc.) contained in the photosensitive resin composition, and also includes components that are liquid, syrupy, or waxy at room temperature (about 25°C).
[0042] [Photosensitive resin composition]
[0043] The photosensitive resin composition of the present embodiment contains (A) an acid-modified vinyl-containing resin, (B) a thermosetting resin, (C) a photopolymerization initiator, (D) a photopolymerizable compound, and (E) an elastomer as essential components. The photosensitive resin composition of the present embodiment is a negative photosensitive resin composition, and a cured film of the photosensitive resin composition can be suitably used as a permanent resist. The following is a more detailed description of each component used in the photosensitive resin composition of the present embodiment.
[0044] ((A) ingredient: acid-modified vinyl-containing resin)
[0045] The photosensitive resin composition of the present embodiment contains an acid-modified vinyl-containing resin as the component (A). The acid-modified vinyl-containing resin is not particularly limited as long as it has a vinyl bond as a photopolymerizable ethylenically unsaturated bond and an alkali-soluble acidic group.
[0046] As the group having the ethylenic unsaturated bond possessed by the (A) component, for example, vinyl, allyl, propargyl, butenyl, ethynyl, phenylethynyl, maleimide, naphthalene diimide and (meth) acryloyl can be mentioned. Among them, from the viewpoint of reactivity and resolution, (meth) acryloyl is preferred. As the acidic group possessed by the (A) component, for example, carboxyl, sulfo group and phenolic hydroxyl can be mentioned. Among them, from the viewpoint of resolution, carboxyl is preferred.
[0047] The component (A) is preferably an acid-modified vinyl-containing epoxy derivative obtained by reacting (a) an epoxy resin (hereinafter, sometimes referred to as "component (a)"), (b) an organic acid containing an ethylenically unsaturated group (hereinafter, sometimes referred to as "component (b)") to obtain a resin (A'), and (c) a polyacid anhydride containing a saturated or unsaturated group (hereinafter, sometimes referred to as "component (c)").
[0048] Examples of acid-modified vinyl-containing epoxy derivatives include acid-modified epoxy (meth) acrylates. Acid-modified epoxy (meth) acrylates are resins obtained by acid-modifying epoxy (meth) acrylates, which are the reaction products of components (a) and (b), with component (c). Examples of acid-modified epoxy (meth) acrylates include addition reaction products obtained by adding saturated or unsaturated polybasic acid anhydrides to esters obtained by reacting epoxy resins with monocarboxylic acids containing vinyl groups.
[0049] As the component (A), for example, there can be mentioned an acid-modified vinyl-containing resin (A1) (hereinafter sometimes referred to as “component (A1)”) obtained by using a bisphenol novolac epoxy resin (a1) (hereinafter sometimes referred to as “epoxy resin (a1)”) as the component (a) and an acid-modified vinyl-containing resin (A2) (hereinafter sometimes referred to as “component (A2)”) obtained by using an epoxy resin (a2) other than the epoxy resin (a1) (hereinafter sometimes referred to as “epoxy resin (a2)”).
[0050] Examples of the epoxy resin (a1) include epoxy resins having a structural unit represented by the following formula (I) or (II).
[0051]
[0052] In formula (I), R 11 Represents a hydrogen atom or a methyl group, plural R 11 Can be the same or different. 1 and Y 2 Each independently represents a hydrogen atom or a glycidyl group, Y 1 and Y 2 From the viewpoint of suppressing the generation of undercuts and improving the linearity and resolution of the resist pattern profile, R is preferably 11 is a hydrogen atom. From the viewpoint of further improving the thermal shock resistance, Y 1 and Y 2 It is epoxypropyl.
[0053] The number of structural units represented by formula (I) in the epoxy resin (a1) is 1 or more, and can be 10 to 100, 12 to 80 or 15 to 70. If the number of structural units is within the above range, it is easy to improve the linearity of the resist pattern profile, the adhesion to the copper substrate, the heat resistance and the electrical insulation. Here, the number of structural units of the structural unit represents an integer value in a single molecule, and represents an average value, i.e., a rational number, in an aggregate of multiple molecules. Hereinafter, the number of structural units of the structural unit is also the same.
[0054]
[0055] In formula (II), R 12 Represents a hydrogen atom or a methyl group, plural R 12 Can be the same or different. 3 and Y 4 Each independently represents a hydrogen atom or a glycidyl group, Y 3 and Y 4 From the viewpoint of suppressing the generation of undercuts and improving the linearity and resolution of the resist pattern profile, R is preferably12 is a hydrogen atom. From the viewpoint of further improving the thermal shock resistance, Y 3 and Y 4 It is epoxypropyl.
[0056] The number of structural units represented by formula (II) in the epoxy resin (a1) is 1 or more, and may be 10 to 100, 12 to 80, or 15 to 70. When the number of structural units is within the above range, the linearity of the resist pattern profile, the adhesion to the copper substrate, and the heat resistance are easily improved.
[0057] In formula (II), R 12 is a hydrogen atom, Y 3 and Y 4 The epoxy resin having a glycidyl group is commercially available as EXA-7376 series (manufactured by DIC Corporation, product name), and R 12 is methyl and Y 3 and Y 4 The epoxy resin having a glycidyl group is commercially available as EPON SU8 series (manufactured by Mitsubishi Chemical Corporation, product name).
[0058] The epoxy resin (a2) is not particularly limited as long as it is an epoxy resin different from the epoxy resin (a1). From the viewpoint of suppressing the generation of undercuts and improving the linearity of the resist pattern profile, the adhesion to the copper substrate, and the resolution, it is preferably at least one selected from the group consisting of a novolac type epoxy resin, a bisphenol A type epoxy resin, a bisphenol F type epoxy resin, a trisphenol methane type epoxy resin, and a biphenyl type epoxy resin.
[0059] As a novolac type epoxy resin, for example, an epoxy resin having a structural unit represented by the following formula (III) can be cited. As a bisphenol A type epoxy resin or a bisphenol F type epoxy resin, for example, an epoxy resin having a structural unit represented by the following formula (IV) can be cited. As a trisphenol methane type epoxy resin, for example, an epoxy resin having a structural unit represented by the following formula (V) can be cited. As a biphenyl type epoxy resin, an epoxy resin having a structural unit represented by the following formula (VI) can be cited.
[0060] As the epoxy resin (a2), a novolac epoxy resin having a structural unit represented by the following formula (III) is preferred. Examples of the novolac epoxy resin having such a structural unit include a novolac epoxy resin represented by the following formula (III').
[0061]
[0062] In formula (III) and (III'), R 13 represents a hydrogen atom or a methyl group, Y 5 represents a hydrogen atom or an epoxypropyl group, Y 5 In formula (III'), n1 is a number greater than 1, and the plurality of R 13 and Y 5 From the viewpoint of suppressing the generation of undercuts and improving the linearity and resolution of the resist pattern profile, R 13 A hydrogen atom is preferred.
[0063] From the viewpoint of suppressing the generation of undercuts and improving the linearity and resolution of the resist pattern profile, in formula (III'), Y as a hydrogen atom is 5 With Y as epoxypropyl 5 The molar ratio of may be 0 / 100 to 30 / 70 or 0 / 100 to 10 / 90. n1 is 1 or more, but may be 10 to 200, 20 to 150, or 30 to 100. When n1 is within the above range, the linearity of the resist pattern profile, the adhesion to the copper substrate, and the heat resistance are easily improved.
[0064] Examples of the novolac epoxy resin represented by formula (III') include phenol novolac epoxy resins and cresol novolac epoxy resins. These novolac epoxy resins can be obtained by, for example, reacting phenol novolac resins or cresol novolac resins with epichlorohydrin by a known method.
[0065] As the phenol novolac type epoxy resin or cresol novolac type epoxy resin represented by formula (III'), for example, YDCN-701, YDCN-702, YDCN-703, YDCN-704, YDCN-704L, YDPN-638, YDPN-602 (these are product names manufactured by NIPPON STEEL Chemical & Material Co., Ltd.), DEN-431, DEN-439 (these are product names manufactured by The Dow Chemical Company), EOCN-120, EOCN-102S, EOCN-103S, EOCN-104S, EOCN-1012, EOCN-1025, EOCN-1027, BREN (these are product names manufactured by Nippon Kayaku Co., Ltd., product name), EPN-1138, EPN-1235, EPN-1299 (all manufactured by BASF, product name), N-730, N-770, N-865, N-665, N-673, VH-4150, VH-4240 (all manufactured by DIC Corporation, product name), etc.
[0066] As the epoxy resin (a2), preferably, bisphenol A epoxy resin or bisphenol F epoxy resin having a structural unit represented by the following formula (IV) can be mentioned. As the epoxy resin having such a structural unit, for example, bisphenol A epoxy resin or bisphenol F epoxy resin represented by the following formula (IV') can be mentioned.
[0067]
[0068] In formula (IV) and (IV'), R 14 Represents a hydrogen atom or a methyl group, and there are multiple R 14 Can be the same or different, Y 6 In formula (IV'), n2 represents a number greater than 1. When n2 is greater than 2, the plurality of Y 6 Can be the same or different, at least one Y 6 It is epoxypropyl.
[0069] From the viewpoint of suppressing the generation of undercut and improving the linearity and resolution of the resist pattern profile, R 14 is a hydrogen atom. From the viewpoint of further improving the thermal shock resistance, Y 6 n2 represents 1 or more, but may be 10 to 100, 12 to 80, or 15 to 60. When n2 is within the above range, the linearity of the resist pattern profile, the adhesion to the copper substrate, and the heat resistance are easily improved.
[0070] Y in formula (IV) 6 For example, a bisphenol A epoxy resin or a bisphenol F epoxy resin which is a glycidyl group can be obtained by making Y in formula (IV) 6 The hydroxyl group of bisphenol A epoxy resin or bisphenol F epoxy resin is a hydrogen atom (-OY 6 ) is obtained by reaction with epichlorohydrin.
[0071] In order to promote the reaction of hydroxyl and epichlorohydrin, the reaction is preferably carried out in a polar organic solvent such as dimethylformamide, dimethylacetamide, dimethyl sulfoxide, etc. at a reaction temperature of 50 to 120° C. in the presence of an alkali metal hydroxide. If the reaction temperature is within the above range, the reaction will not become too slow and side reactions can be suppressed.
[0072] As the bisphenol A type epoxy resin or bisphenol F type epoxy resin represented by formula (IV'), for example, jER807, jER815, jER825, jER827, jER828, jER834, jER1001, jER1004, jER1007 and jER1009 (these are product names manufactured by Mitsubishi Chemical Corporation), DER-330, DER-301, DER-361 (these are product names manufactured by The Dow Chemical Company), YD-8125, YDF-170, YDF-175S, YDF-2001, YDF-2004, YDF-8170 (these are product names manufactured by NIPPON STEEL Chemical & Material Co., Ltd.), etc. are commercially available.
[0073] As the epoxy resin (a2), preferably, a trisphenol methane type epoxy resin having a structural unit represented by the following formula (V) is used. As the trisphenol methane type epoxy resin having such a structural unit, for example, a trisphenol methane type epoxy resin represented by the following formula (V') is used.
[0074]
[0075] In formula (V) and (V'), Y 7 represents a hydrogen atom or an epoxypropyl group, plural Y 7 Can be the same or different, at least one Y 7 In the formula (V'), n3 represents a number of 1 or more.
[0076] From the perspective of suppressing the generation of undercuts and upper defects and improving the linearity and resolution of the resist pattern profile, Y 7 Y as a hydrogen atom in7 With Y as epoxypropyl 7 The molar ratio of Y can be 0 / 100 to 30 / 70. 7 At least one of n3 is a glycidyl group. n3 is 1 or more, but may be 10 to 100, 12 to 80, or 15 to 70. When n3 is within the above range, the linearity of the resist pattern profile, the adhesion to the copper substrate, and the heat resistance are easily improved.
[0077] As the trisphenol methane type epoxy resin represented by the formula (V′), for example, FAE-2500, EPPN-501H, EPPN-502H (above, manufactured by Nippon Kayaku Co., Ltd., product names) and the like are commercially available.
[0078] As the epoxy resin (a2), preferably, a biphenyl type epoxy resin having a structural unit represented by the following formula (VI) is used. As the biphenyl type epoxy resin having such a structural unit, for example, a biphenyl type epoxy resin represented by the following formula (VI') is used.
[0079]
[0080] In formula (VI) and (VI'), Y 8 represents a hydrogen atom or an epoxypropyl group, plural Y 8 Can be the same or different, at least one Y 8 In the formula (VI'), n4 represents a number of 1 or more.
[0081] Examples of the biphenyl type epoxy resin represented by formula (VI') include NC-3000, NC-3000-L, NC-3000-H, NC-3000-FH-75M, NC-3100, and CER-3000-L (all manufactured by Nippon Kayaku Co., Ltd., product names) which are commercially available.
[0082] As the epoxy resin (a2), at least one selected from the group consisting of a novolac type epoxy resin having a structural unit represented by formula (III), a bisphenol A type epoxy resin having a structural unit represented by formula (IV) and a bisphenol F type epoxy resin having a structural unit represented by formula (IV) is preferred, and a bisphenol F type epoxy resin having a structural unit represented by formula (IV) is more preferred.
[0083] From the viewpoint of further improving heat shock resistance, warpage reduction and resolution, a bisphenol novolac type epoxy resin having a structural unit represented by formula (II) can be used as the (A1) component of the epoxy resin (a1) and a bisphenol A type epoxy resin or a bisphenol F type epoxy resin having a structural unit represented by formula (IV) can be used in combination as the (A2) component of the epoxy resin (a2).
[0084] As the component (b), for example, there can be mentioned acrylic acid, acrylic acid dimer, methacrylic acid, β-furfuryl acrylic acid, β-styryl acrylic acid, cinnamic acid, crotonic acid, α-cyanocinnamic acid and other acrylic acid derivatives; reaction products of hydroxyl-containing (meth) acrylic acid ester and dibasic acid anhydride, i.e., half ester compounds; and reaction products of vinyl-containing monoglycidyl ether or vinyl-containing monoglycidyl ester and dibasic acid anhydride, i.e., half ester compounds. The component (b) can be used alone or in combination of two or more.
[0085] The half ester compound is obtained by, for example, reacting a hydroxyl group-containing (meth)acrylate, a vinyl group-containing monoglycidyl ether, or a vinyl group-containing monoglycidyl ester with a dibasic acid anhydride.
[0086] Examples of the hydroxyl group-containing (meth)acrylate, vinyl group-containing monoglycidyl ether and vinyl group-containing monoglycidyl ester include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate and glycidyl (meth)acrylate.
[0087] Examples of the dibasic acid anhydride include succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, and itaconic anhydride.
[0088] In the reaction of component (a) and component (b), the epoxy group of component (a) is preferably reacted at a ratio of 0.6 to 1.05 equivalents of component (b) relative to 1 equivalent, and more preferably at a ratio of 0.8 to 1.0 equivalents. By reacting at such a ratio, there is a tendency that the photosensitivity becomes greater and the linearity of the resist pattern profile is excellent.
[0089] Component (a) and component (b) can be dissolved in an organic solvent and reacted. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as methyl celulose, butyl celulose, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, butyl celulose acetate, and carbitol acetate; aliphatic hydrocarbons such as octane and decane; petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent petroleum naphtha. The organic solvent may be used alone or in combination of two or more.
[0090] A catalyst for promoting the reaction of component (a) and component (b) may be used. Examples of the catalyst include triethylamine, benzylmethylamine, methyltriethylammonium chloride, benzyltrimethylammonium chloride, benzyltrimethylammonium bromide, benzyltrimethylammonium iodide, and triphenylphosphine. The catalyst may be used alone or in combination of two or more.
[0091] From the viewpoint of promoting the reaction between components (a) and (b), the amount of the catalyst used may be 0.01 to 10 parts by mass, 0.05 to 2 parts by mass, or 0.1 to 1 part by mass based on 100 parts by mass of the total of components (a) and (b).
[0092] In the reaction between the components (a) and (b), a polymerization inhibitor may be used to prevent polymerization during the reaction. Examples of the polymerization inhibitor include hydroquinone, methylhydroquinone, hydroquinone monomethyl ether, catechol, and gallol. The polymerization inhibitor may be used alone or in combination of two or more.
[0093] From the viewpoint of improving stability, the amount of the polymerization inhibitor used may be 0.01 to 1 part by mass, 0.02 to 0.8 part by mass, or 0.04 to 0.5 part by mass based on 100 parts by mass of the total of the components (a) and (b).
[0094] From the viewpoint of productivity, the reaction temperature of the component (a) and the component (b) may be 60 to 150°C, 80 to 120°C, or 90 to 110°C.
[0095] The component (A') obtained by reacting the components (a) and (b) has a hydroxyl group formed by a ring-opening addition reaction between the epoxy group of the component (a) and the carboxyl group of the component (b). By further reacting the component (c) with the component (A'), an acid-modified vinyl-containing resin can be obtained in which the hydroxyl group of the component (A') (including the hydroxyl group originally present in the component (a)) and the acid anhydride group of the component (c) are half-esterified.
[0096] As the (c) component, for example, succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride and itaconic anhydride can be mentioned. Among them, tetrahydrophthalic anhydride is preferred from the viewpoint of resolution. (c) component can be used alone or in combination of two or more.
[0097] In the reaction of the components (A') and (c), for example, the acid value of the component (A) can be adjusted by reacting 0.1 to 1.0 equivalent of the component (c) per 1 equivalent of the hydroxyl group in the component (A').
[0098] The reaction temperature of the component (A') and the component (c) may be 50 to 150°C, 60 to 120°C, or 70 to 100°C from the viewpoint of productivity.
[0099] If necessary, as the component (a), a part of a hydrogenated bisphenol A epoxy resin may be used in combination, and a part of a styrene-maleic acid resin such as a hydroxyethyl (meth)acrylate-modified product of a styrene-maleic anhydride copolymer may be used in combination.
[0100] From the viewpoint of suppressing the generation of undercuts and further improving the adhesion to the copper substrate, the heat shock resistance and the resolution, it is preferred that the component (A) contains the component (A1). In particular, from the viewpoint of improving the adhesion strength, it is more preferred that the component (A1) and the component (A2) are contained.
[0101] When the components (A1) and (A2) are used in combination as the component (A), the mass ratio of (A1) / (A2) is not particularly limited, but can be 20 / 80 to 90 / 10, 30 / 70 to 80 / 20, 40 / 60 to 75 / 25, or 50 / 50 to 70 / 30 from the viewpoint of improving the linearity of the resist pattern profile, resistance to electroless plating, and heat resistance.
[0102] The acid value of component (A) is not particularly limited. From the viewpoint of improving the solubility of the unexposed portion in an alkaline aqueous solution, the acid value of component (A) may be 30 mgKOH / g or more, 40 mgKOH / g or more, or 50 mgKOH / g or more. From the viewpoint of improving the electrical properties of the cured film, the acid value of component (A) may be 150 mgKOH / g or less, 120 mgKOH / g or less, or 100 mgKOH / g or less.
[0103] The weight average molecular weight (Mw) of component (A) is not particularly limited. From the perspective of improving the adhesion of the cured film, the Mw of component (A) may be 3000 or more, 4000 or more, or 5000 or more. From the perspective of improving the resolution of the photosensitive layer, the Mw of component (A) may be 30000 or less, 25000 or less, or 18000 or less.
[0104] Mw can be measured by gel permeation chromatography (GPC). Mw is measured, for example, under the following GPC conditions, and the value converted using the calibration curve of standard polystyrene can be set to Mw. The preparation of the calibration curve can use 5 sample groups ("PStQuick MP-H" and "PStQuick B", Tosoh Corporation) as standard polystyrene.
[0105] GPC apparatus: High-speed GPC apparatus "HCL-8320GPC" (manufactured by Tosoh Corporation)
[0106] Detector: Differential refractometer or UV detector (manufactured by Tosoh Corporation)
[0107] Column: TSKgel SuperMultipore HZ-H column (column length: 15 cm, column inner diameter: 4.6 mm) (manufactured by Tosoh Corporation)
[0108] Eluent: Tetrahydrofuran (THF)
[0109] Measurement temperature: 40℃
[0110] Flow rate: 0.35mL / min
[0111] Sample concentration: 10mg / THF5mL
[0112] Injection volume: 20 μL
[0113] From the viewpoint of improving the heat resistance, electrical properties and chemical resistance of the permanent resist, the content of the component (A) in the photosensitive resin composition may be 20 to 70 mass %, 25 to 60 mass %, or 30 to 50 mass % based on the total solid content of the photosensitive resin composition.
[0114] ((B) component: thermosetting resin)
[0115] The photosensitive resin composition of the present embodiment contains a thermosetting resin as the component (B), and the component (B) contains a bisphenol epoxy compound having an average molecular weight of 360 or less (hereinafter, sometimes referred to as "component (B1)"). The photosensitive resin composition of the present embodiment contains the component (B1), so that good resolution can be maintained and the heat resistance and thermal shock resistance of the cured film (permanent resist) formed from the photosensitive resin composition can be improved.
[0116] The component (B1) is an epoxy compound synthesized by a condensation reaction between a bisphenol compound and epichlorohydrin. Examples of the bisphenol compound include bisphenol A, bisphenol F, and bisphenol S. The component (B1) contains as a main component a diglycidyl ether having a bisphenol skeleton (a diglycidyl ether represented by the following formula (1)) in which 2 moles of epichlorohydrin are bonded to 1 mole of the bisphenol compound.
[0117]
[0118] In formula (1), X represents a methylene group (CH2), an ethylene group (CH2CH2), an ethylene group (CH(CH3)), a 1-methylethylene group (C(CH3)2), or a sulfone group. From the viewpoint of improving developability, X is preferably a methylene group or a 1-methylethylene group.
[0119] General bisphenol-type epoxy compounds include polymers of bisphenol compounds and epichlorohydrin (e.g., oligomer components such as dimers and trimers). In contrast, the content of oligomer components in component (B1) is small. From the viewpoint of further improving developability and heat shock resistance, the content of diglycidyl ether represented by formula (1) in component (B1) may be 94% by mass or more, 96% by mass or more, or 98% by mass or more.
[0120] From the viewpoint of further improving heat resistance and heat shock resistance, the average molecular weight of the component (B1) may be 310 to 360, 315 to 359, 320 to 358, 325 to 357, or 330 to 356. The average molecular weight can be calculated, for example, by the GPC method (see Reports of the Central Customs Laboratory, No. 21, 1980, pp. 85 to 90, "Determination of the degree of polymerization of epoxy oligomers by GPC, NMR, etc.").
[0121] From the viewpoint of further improving heat resistance and thermal shock resistance, the epoxy equivalent of component (B1) may be 150 to 182 g / eq, 154 to 181 g / eq, 160 to 180 g / eq, 162 to 179 g / eq, or 166 to 178 g / eq. The epoxy equivalent can be measured in accordance with JIS K 7236.
[0122] (B) component may include other thermosetting resins except (B1) component. As other thermosetting resins, for example, epoxy resins, phenolic resins, unsaturated imide resins, cyanate resins, isocyanate resins, benzoxazine resins, cyclohexane resins, amino resins, unsaturated polyester resins, allyl resins, dicyclopentadiene resins, silicone resins, triazine resins and melamine resins without bisphenol skeletons can be cited. Among them, from the viewpoint of further improving the heat resistance of the cured film, it is preferred that the epoxy resin does not have a bisphenol skeleton. As the epoxy resin without a bisphenol skeleton, for example, novolac type epoxy resins, dicyclopentadiene type epoxy resins, hydrogenated bisphenol A type epoxy resins, biphenyl type epoxy resins, hydantoin type epoxy resins, triglycidyl isocyanate and dimethylol type epoxy resins can be cited.
[0123] The content of the component (B1) in the component (B) may be 30% by mass or more, 50% by mass or more, or 60% by mass or more based on the total amount of the component (B). When the content is 30% by mass or more, there is a tendency to obtain better thermal shock resistance.
[0124] The content of the component (B) in the photosensitive resin composition can be 2 to 30 mass %, 5 to 25 mass %, 8 to 20 mass %, or 10 to 18 mass % based on the total solid content of the photosensitive resin composition. When the content of the component (B) is within the above range, the adhesion and heat resistance of the formed cured film can be further improved while maintaining good developability.
[0125] (Component (C): photopolymerization initiator)
[0126] The photopolymerization initiator as the component (C) is not particularly limited as long as it can polymerize the components (A) and (D). The component (C) may be used alone or in combination of two or more.
[0127] Examples of the component (C) include benzoin compounds such as benzoin, benzoin methyl ether, and benzoin isopropyl ether; acetophenone compounds such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexylphenyl ketone, 2-benzyl-2-dimethylamino-1-(4-(methylthio)phenyl)-butanone-1,2-methyl-[4-(methylthio)phenyl]-2-(methylthio)-1-propane, and N,N-dimethylaminoacetophenone; and 2-methylanthraquinone, 2-ethylanthraquinone, 2 -tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, 2-aminoanthraquinone and other anthraquinone compounds; 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-diisopropylthioxanthone and other thioxanthone compounds; acetophenone dimethyl ketal, benzyl dimethyl ketal and other ketal compounds; benzophenone, methyl benzophenone, 4,4'-dichlorobenzophenone, 4,4'-bis(diethylamino)benzophenone, michler's ketone, 4-benzoyl-4'-methyldiphenyl sulfide and other benzophenone compounds; 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer imidazole compounds such as 2-(o-chlorophenyl)-4,5-di(m-methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer, 2,4-di(p-methoxyphenyl)-5-phenylimidazole dimer, 2-(2,4-dimethoxyphenyl)-4,5-diphenylimidazole dimer; acridine compounds such as 9-phenylacridine and 1,7-bis(9,9'-acridinyl)heptane; 2,4,6- Acylphosphine oxide compounds such as trimethylbenzoyldiphenylphosphine oxide; oxime ester compounds such as 1,2-octanedione-1-[4-(phenylthio)phenyl]-2-(O-benzoyl oxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethanone 1-(O-acetyl oxime), and 1-phenyl-1,2-propanedione-2-[O-(ethoxycarbonyl)oxime]; and tertiary amine compounds such as N,N-dimethylaminobenzoic acid ethyl ester, N,N-dimethylaminobenzoic acid isopentyl ester, amyl-4-dimethylaminobenzoate, triethylamine, and triethanolamine.
[0128] The content of the component (C) in the photosensitive resin composition is not particularly limited, and may be 0.2 to 15% by mass, 0.4 to 5% by mass, or 0.6 to 1.5% by mass based on the total solid content of the photosensitive resin composition.
[0129] (Component (D): photopolymerizable compound)
[0130] From the viewpoint of improving the chemical resistance of the exposed portion and increasing the difference in developer resistance between the exposed portion and the unexposed portion, the photosensitive resin composition of the present embodiment contains a photopolymerizable compound as the (D) component. The (D) component is not particularly limited as long as it is a photopolymerizable compound having a photopolymerizable functional group and not having an acidic group. As the photopolymerizable functional group, for example, groups having ethylenically unsaturated bonds such as vinyl, allyl, propargyl, butenyl, ethynyl, phenylethynyl, maleimide, naphthalene diimide, and (meth)acryloyl can be cited.
[0131] (D) As a component, the photopolymerizable compound which has one ethylenically unsaturated bond, the photopolymerizable compound which has two ethylenically unsaturated bonds, and the photopolymerizable compound which has three or more ethylenically unsaturated bonds are mentioned, for example.
[0132] Examples of the photopolymerizable compound having one ethylenically unsaturated bond include (meth)acrylic acid and alkyl (meth)acrylates. Examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and hydroxyethyl (meth)acrylate.
[0133] Examples of the photopolymerizable compound having two ethylenically unsaturated bond groups include polyethylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, polypropylene glycol di(meth)acrylate, 2,2-bis(4-(meth)acryloyloxypolyethoxypolypropoxyphenyl)propane, and bisphenol A diglycidyl ether di(meth)acrylate.
[0134] Examples of the photopolymerizable compound having three or more ethylenically unsaturated bonds include (meth)acrylate compounds having a skeleton derived from trimethylolpropane, such as trimethylolpropane tri(meth)acrylate; (meth)acrylate compounds having a skeleton derived from tetramethylolmethane, such as tetramethylolmethane tri(meth)acrylate and tetramethylolmethane tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from pentaerythritol, such as pentaerythritol tri(meth)acrylate and pentaerythritol tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from dipentaerythritol, such as dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate; (meth)acrylate compounds having a skeleton derived from ditrimethylolpropane, such as ditrimethylolpropane tetra(meth)acrylate; and (meth)acrylate compounds having a skeleton derived from diglycerol.
[0135] Among them, from the viewpoint of improving the chemical resistance of the exposed portion and increasing the difference in developer resistance between the exposed portion and the unexposed portion, a (meth)acrylate compound having a skeleton derived from dipentaerythritol is preferred, and dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate are more preferred.
[0136] (D) The content of the component may be 1 to 20% by mass, 2 to 15% by mass, or 3 to 10% by mass based on the total solid content of the photosensitive resin composition.
[0137] ((E) component: elastomer)
[0138] The photosensitive resin composition of this embodiment contains an elastomer as the (E) component, which can suppress the reduction of flexibility and adhesive strength caused by the deformation (internal stress) inside the resin caused by the curing shrinkage of the (A) component. The (E) component contains an acrylic elastomer, thereby improving the heat resistance and impact resistance of the cured film formed by the photosensitive resin composition.
[0139] The acrylic elastomer can be synthesized by polymerizing a (meth)acrylic compound. Examples of the (meth)acrylic compound include (meth)acrylic acid, (meth)acrylic acid esters, and acrylonitrile.
[0140] Examples of the (meth)acrylate include methyl (meth)acrylate, (meth)acrylic acid, n-butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, and 2-ethoxyethyl (meth)acrylate.
[0141] From the viewpoint of further improving the developability, the acrylic elastomer preferably has a carboxyl group. The carboxyl group can be introduced by polymerizing (meth) acrylic acid. The content of the structural unit based on (meth) acrylic acid in the acrylic resin can be 2 to 50 mass %, 5 to 30 mass %, 8 to 25 mass %, or 10 to 20 mass %. If the content of the structural unit based on (meth) acrylic acid is within the above range, there is a tendency to improve developability and resolution.
[0142] From the viewpoint of further improving impact resistance, the acrylic elastomer preferably has an n-butyl group. The n-butyl group can be introduced by polymerizing n-butyl (meth)acrylate. The content of the structural unit based on n-butyl (meth)acrylate in the acrylic elastomer can be 30 to 90 mass %, 40 to 85 mass %, 45 to 80 mass %, or 50 to 75 mass %. If the content of the structural unit based on n-butyl (meth)acrylate is within the above range, there is a tendency to improve resolution and impact resistance.
[0143] The weight average molecular weight (Mw) of the acrylic elastomer may be 1000 to 50000, 2000 to 40000, 3000 to 30000, 5000 to 20000, or 8000 to 18000. When the Mw of the acrylic elastomer is within the above range, the compatibility with the component (A) and the developability of the unexposed portion are excellent and the resolution tends to be more excellent. The Mw of the acrylic elastomer can be measured by the above GPC method.
[0144] The component (E) may contain an elastomer other than the acrylic elastomer. Examples of the component (E) other than the acrylic elastomer include styrene elastomers, olefin elastomers, polyurethane elastomers, polyester elastomers, polyamide elastomers, and silicone elastomers.
[0145] Examples of the styrene-based elastomer include styrene-butadiene-styrene blocked copolymers, styrene-isoprene-styrene blocked copolymers, styrene-ethylene-butylene-styrene blocked copolymers, and styrene-ethylene-propylene-styrene blocked copolymers. As components constituting the styrene-based elastomer, in addition to styrene, styrene derivatives such as α-methylstyrene, 3-methylstyrene, 4-propylstyrene, and 4-cyclohexylstyrene can be used.
[0146] Examples of the olefin-based elastomer include ethylene-propylene copolymers, ethylene-α-olefin copolymers, ethylene-α-olefin-non-conjugated diene copolymers, propylene-α-olefin copolymers, butene-α-olefin copolymers, ethylene-propylene-diene copolymers, copolymers of non-conjugated dienes such as dicyclopentadiene, 1,4-hexadiene, cyclooctadiene, methylene norbornene, ethylidene norbornene, butadiene, and isoprene with α-olefins, epoxy-modified polybutadiene, and carboxylic acid-modified butadiene-acrylonitrile copolymers.
[0147] The epoxy-modified polybutadiene preferably has a hydroxyl group at a molecular terminal, more preferably has a hydroxyl group at both molecular terminals, and further preferably has a hydroxyl group only at both molecular terminals. The number of hydroxyl groups in the epoxy-modified polybutadiene may be 1 or more, preferably 1 to 5, more preferably 1 or 2, and further preferably 2.
[0148] As the polyurethane elastomer, a compound composed of a hard segment containing a low molecular weight (short chain) diol and a diisocyanate and a soft segment containing a high molecular weight (long chain) diol and a diisocyanate can be used.
[0149] Examples of the short-chain diol include ethylene glycol, propylene glycol, 1,4-butanediol, and bisphenol A. The number average molecular weight of the short-chain diol is preferably 48 to 500.
[0150] Examples of the long-chain diol include polypropylene glycol, polytetramethylene oxide, poly(1,4-butylene adipate), poly(ethylene-1,4-butylene adipate), polycaprolactone, poly(1,6-hexamethylene carbonate), and poly(1,6-adipate neopentanoic acid). The number average molecular weight of the long-chain diol is preferably 500 to 10,000.
[0151] As the polyester-based elastomer, a compound obtained by polycondensing a dicarboxylic acid or a derivative thereof and a diol compound or a derivative thereof can be used.
[0152] Examples of dicarboxylic acids include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, and naphthalene dicarboxylic acid; aliphatic dicarboxylic acids having 2 to 20 carbon atoms such as adipic acid, sebacic acid, and dodecanedicarboxylic acid; and alicyclic dicarboxylic acids such as cyclohexane dicarboxylic acid. The dicarboxylic acids may be used alone or in combination of two or more.
[0153] Examples of the diol compound include aliphatic diols such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, and 1,10-decanediol; alicyclic diols such as 1,4-cyclohexanediol; and aromatic diols such as bisphenol A, bis-(4-hydroxyphenyl)methane, bis-(4-hydroxy-3-methylphenyl)propane, and resorcinol.
[0154] As the polyester elastomer, a multi-block copolymer having an aromatic polyester (e.g., polybutylene terephthalate) as a hard segment component and an aliphatic polyester (e.g., polytetramethylene glycol) as a soft segment component can be used. There are different grades of polyester elastomers depending on the type, ratio, and molecular weight of the hard segment and the soft segment.
[0155] Polyamide elastomers are roughly divided into two types: polyether blocked amide type and polyether ester blocked amide type, which use polyamide in the hard segment and polyether or polyester in the soft segment. Examples of polyamide include polyamide-6, polyamide-11, and polyamide-12. Examples of polyether include polyoxyethylene glycol, polyoxypropylene glycol, and polytetramethylene glycol.
[0156] Silicone elastomers are compounds containing organopolysiloxane as a main component. Examples of organopolysiloxanes include polydimethylsiloxane, polymethylphenylsiloxane, and polydiphenylsiloxane. Silicone elastomers may be compounds obtained by modifying a portion of organopolysiloxane with a vinyl group, an alkoxy group, or the like.
[0157] The content of the component (E) may be 1 to 40 parts by mass, 2 to 35 parts by mass, 3 to 30 parts by mass, or 4 to 15 parts by mass relative to 100 parts by mass of the component (A). The content of the component (E) may be 5 parts by mass or more, 8 parts by mass or more, or 10 parts by mass or more, or may be 40 parts by mass or less, 35 parts by mass or less, 30 parts by mass or less, or 25 parts by mass or less relative to 100 parts by mass of the component (A). If the content of the component (E) is within the above range, the elastic modulus of the cured film in the high temperature region becomes lower, and the unexposed portion is more easily dissolved in the developer.
[0158] ((F) ingredient: inorganic filler)
[0159] The photosensitive resin composition of the present embodiment may further contain an inorganic filler as the component (F). By containing the component (F), the adhesive strength and hardness of the permanent resist can be improved. The component (F) may be used alone or in combination of two or more.
[0160] Examples of the inorganic filler include silica, alumina, titanium dioxide, tantalum oxide, zirconium oxide, silicon nitride, barium titanate, barium carbonate, magnesium carbonate, aluminum hydroxide, magnesium hydroxide, lead titanate, lead zirconate titanate, lead lanthanum zirconate titanate, gallium oxide, spinel, mullite, cordierite, talc, aluminum titanate, zirconium oxide containing yttrium oxide, barium silicate, boron nitride, calcium carbonate, barium sulfate, calcium sulfate, zinc oxide, magnesium titanate, hydrotalcite, mica, calcined kaolin and carbon.
[0161] From the perspective of improving the heat resistance of the permanent resist, the component (F) may contain silicon dioxide, from the perspective of improving the heat resistance and adhesive strength of the permanent resist, it may contain barium sulfate, or it may contain silicon dioxide and barium sulfate. From the perspective of improving the dispersibility of the inorganic filler, an inorganic filler that has been surface-treated in advance with aluminum oxide or an organic silane compound may be used.
[0162] From the viewpoint of resolution, the average particle size of the inorganic filler may be 0.01 to 5.0 μm, 0.05 to 3.0 μm, 0.1 to 2.0 μm, or 0.15 to 1.0 μm.
[0163] The average particle size of the component (F) is the average particle size of the inorganic filler in a state dispersed in the photosensitive resin composition, and is a value measured as follows. First, the photosensitive resin composition is diluted 1000 times with methyl ethyl ketone, and then the particles dispersed in the solvent are measured using a submicron particle analyzer (manufactured by Beckman Coulter, Inc., product name: N5) based on the international standard ISO13321 and a refractive index of 1.38, and the particle size at the integrated value of 50% (volume basis) in the particle size distribution is set as the average particle size.
[0164] The content of the component (F) can be 10 to 70 mass %, 15 to 60 mass %, or 20 to 50 mass % based on the total solid content of the photosensitive resin composition. When the content of the component (E) is within the above range, the low thermal expansion coefficient, heat resistance, and film strength can be further improved.
[0165] When silicon dioxide is used as the component (F), the content of silicon dioxide can be 5 to 60 mass%, 10 to 40 mass%, or 15 to 30 mass% based on the total solid content of the photosensitive resin composition. When barium sulfate is used as the component (F), the content of barium sulfate can be 5 to 30 mass%, 8 to 25 mass%, or 10 to 20 mass% based on the total solid content of the photosensitive resin composition. If the content of silicon dioxide and barium sulfate is within the above range, there is a tendency to have a low thermal expansion coefficient, excellent solder heat resistance and excellent bonding strength.
[0166] ((G) ingredient: pigment)
[0167] From the viewpoint of improving the recognition or appearance of the manufacturing device, the photosensitive resin composition of the present embodiment may further contain a pigment as the (G) component. As the (G) component, a colorant that develops a desired color when hiding the wiring (conductor pattern) etc. can be used. The (G) component may be used alone or in combination of two or more.
[0168] (G) As a component, phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, carbon black, and naphthalene black are mentioned, for example.
[0169] From the viewpoint of making the manufacturing device easily recognizable and further hiding the wiring, the content of the component (G) may be 0.01 to 5.0 mass %, 0.03 to 3.0 mass %, or 0.05 to 2.0 mass % based on the total solid content in the photosensitive resin composition.
[0170] ((H) component: ion trapping agent)
[0171] From the viewpoint of improving the resist shape, adhesion, fluidity and reliability, the photosensitive resin composition of the present embodiment may further contain an ion trapping agent as the component (H). The component (H) is not particularly limited as long as it can trap ions in the ion trapping agent and has the function of trapping at least one of cations and anions.
[0172] In this embodiment, the captured ions are introduced into the composition which reacts and changes its solubility in the solvent by irradiation with light, electron beams, etc., such as sodium ions (Na + ), chloride ion (Cl - ), bromide ion (Br - ), copper ions (Cu+ , Cu 2+ ) plasma. By capturing these ions, electrical insulation, electrical corrosion resistance, etc. are improved.
[0173] The component (H) preferably contains at least one ion trapping agent selected from the group consisting of Zr (zirconium), Bi (bismuth), Mg (magnesium), and Al (aluminum). The component (H) may be used alone or in combination of two or more.
[0174] Examples of the component (H) include a cation trapping agent that traps cations, anion trapping agents that trap anions, and both ion trapping agents that trap cations and anions.
[0175] Examples of the cation scavenger include inorganic ion exchangers of metal oxides such as zirconium phosphate, zirconium tungstate, zirconium molybdate, zirconium tungstate, zirconium antimonate, zirconium selenate, zirconium tellurate, zirconium silicate, zirconium phosphosilicate, and zirconium polyphosphate.
[0176] Examples of the anion scavenger include inorganic ion exchangers such as bismuth oxide hydrate and hydrotalcites.
[0177] Examples of the two-ion scavenger include inorganic ion exchangers of metal hydrous oxides such as alumina hydrate and zirconium oxide hydrate. Examples of the two-ion scavenger include IXE-1320 (Mg, Al containing compound), IXE-600 (Bi containing compound), IXE-633 (Bi containing compound), IXE-680 (Bi containing compound), IXE-6107 (Zr, Bi containing compound), IXE-6136 (Zr, Bi containing compound), IXEPLAS-A1 (Zr, Mg, Al containing compound), IXEPLAS-A2 (Zr, Mg, Al containing compound), and IXEPLAS-B1 (Zr, Bi containing compound) manufactured by TOAGOSEI CO., LTD.
[0178] The component (H) can be used in a granular form. From the viewpoint of improving insulation properties, the average particle size of the component (H) may be 5 μm or less, 3 μm or less, or 2 μm or less, or may be 0.1 μm or more. The average particle size of the component (H) is the particle size of particles dispersed in the photosensitive resin composition, and can be measured by the same method as the method for measuring the average particle size of the component (F).
[0179] When the photosensitive resin composition contains component (H), its content is not particularly limited. From the viewpoint of improving electrical insulation and electrical corrosion resistance, it can be 0.05 to 10 mass %, 0.1 to 5 mass %, or 0.2 to 1 mass % based on the total solid content of the photosensitive resin composition.
[0180] ((I) component: silane coupling agent)
[0181] The photosensitive resin composition of the present embodiment may further include a silane coupling agent as component (I). As component (I), a known silane coupling agent can be used. Component (I) can improve the adhesion between electronic parts and substrates, and is particularly effective when the substrate is a silicon-containing substrate (e.g., a glass substrate, a silicon wafer, an epoxy resin-impregnated glass cloth substrate, etc.).
[0182] Examples of the silane coupling agent include alkoxysilanes such as methyltrimethoxysilane, methyltriethoxysilane, phenyltrimethoxysilane, and phenyltriethoxysilane; (meth)acryloxypropyltrimethoxysilane, (meth)acryloxypropylmethyldimethoxysilane, and other (meth)acrylyl group-containing alkoxysilanes; amine alkoxysilanes such as γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, and 3-triethoxysilyl-N-(1,3-dimethylbutylene)propylamine; γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, and γ-glycidoxypropyltriethoxysilane. Alkoxysilanes containing glycidoxy groups such as triethoxysilane, glycidoxypropylmethyldiethoxysilane, and glycidoxypropylmethyldiisopropenoxysilane; alkoxysilanes containing alicyclic epoxy groups such as 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; alkoxysilanes containing urea groups such as 3-ureapropyltriethoxysilane; alkoxysilanes containing mercapto groups such as 3-mercaptopropyltrimethoxysilane and 3-mercaptopropylmethyldimethoxysilane; alkoxysilanes containing carbamate groups such as triethoxysilylpropylethylcarbamate; alkoxysilanes containing polyacid anhydride groups such as 3-(triethoxysilyl)propylsuccinic anhydride. The silane coupling agent can be used alone or in combination of two or more.
[0183] From the viewpoint of further improving adhesion, component (I) preferably contains a silane coupling agent having a (meth)acryloyl group. By using a silane coupling agent having a (meth)acryloyl group, the heat resistance of the permanent resist can be maintained and oozing out from the composition can be suppressed. In this specification, a silane coupling agent having a (meth)acryloyl group is not included in component (D).
[0184] As a commercial item of the silane coupling agent which has a (meth)acryloyl group, KBM-502, KBM-503, KBE-502, KBE-503, and KBM-5103 (made by Shin-Etsu Chemical Co., Ltd.) are mentioned, for example.
[0185] The content of the component (I) may be 0.1 to 10 mass %, 0.5 to 5 mass %, or 1 to 3 mass % based on the total solid content of the photosensitive resin composition. If the content of the component (I) is within the above range, the adhesion to the silicon wafer and the resolution tend to be excellent.
[0186] (Curing agent)
[0187] The photosensitive resin composition of the present embodiment may contain a curing agent in order to further improve the properties of the cured film, such as heat resistance, adhesion, and chemical resistance. The curing agent may be used alone or in combination of two or more.
[0188] As a curing agent, for example, imidazole compounds, guanamine compounds, amine compounds and triazine compounds can be mentioned. As imidazole compounds, for example, 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 2-phenylimidazole and 2-phenyl-4-methyl-5-hydroxymethylimidazole can be mentioned. As guanamine compounds, for example, acetoguanamine and benzoguanamine can be mentioned. As amine compounds, for example, diaminodiphenylmethane, metaphenylenediamine, metaxylene diamine, diaminodiphenyl sulfone, dicyandiamide, urea, urea derivatives, melamine and polybasic hydrazides can be mentioned. As triazine compounds, for example, ethyldiamino-s-triazine, 2,4-diamino-s-triazine and 2,4-diamino-6-xylene-s-triazine can be mentioned.
[0189] From the viewpoint of improving the reliability of the cured film, the content of the curing agent may be 0.01 to 20% by mass, 0.05 to 10% by mass, or 0.1 to 5% by mass based on the total solid content of the photosensitive resin composition.
[0190] (Other ingredients)
[0191] The photosensitive resin composition of the present embodiment may further include various additives as required. Examples of additives include polymerization inhibitors such as hydroquinone, methyl hydroquinone, hydroquinone monomethyl ether, catechol, and gallol; thickeners such as organic clay and montmorillonite; silicone-based, fluorine-based, and vinyl resin-based defoamers; and flame retardants such as brominated epoxy compounds, acid-modified brominated epoxy compounds, antimony compounds, phosphate compounds, aromatic condensed phosphates, and halogen-containing condensed phosphates.
[0192] (Solvent)
[0193] The photosensitive resin composition of the present embodiment contains a solvent for dissolving and dispersing each component, and thus can be easily applied on a substrate to form a coating film having a uniform thickness.
[0194] Examples of the solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as methyl celulose, butyl celulose, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, butyl celulose acetate, and carbitol acetate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent petroleum naphtha. The solvent may be used alone or in combination of two or more.
[0195] The amount of the solvent to be blended is not particularly limited, and the ratio of the solvent in the photosensitive resin composition may be 10 to 50% by mass, 20 to 40% by mass, or 25 to 35% by mass.
[0196] The photosensitive resin composition of the present embodiment can be prepared by uniformly mixing the above-mentioned components using a roll mill, a bead mill, or the like.
[0197] [Photosensitive element]
[0198] The photosensitive element of the present embodiment includes a support film and a photosensitive layer containing the above-mentioned photosensitive resin composition. Figure 1 Schematic diagram of a cross-sectional view of a photosensitive element according to this embodiment. Figure 1 As shown, the photosensitive element 1 includes a support film 10 and a photosensitive layer 20 formed on the support film 10 .
[0199] The photosensitive element 1 can be produced by coating the photosensitive resin composition of the present embodiment on the support film 10 by a known method such as reverse roll coating, gravure roll coating, comma coating, curtain coating, and drying the coating to form the photosensitive layer 20 .
[0200] As the support film, for example, polyester films such as polyethylene terephthalate and polybutylene terephthalate, polyolefin films such as polypropylene and polyethylene can be cited. The thickness of the support film can be, for example, 5 to 100 μm. The thickness of the photosensitive layer can be, for example, 5 to 50 μm, 5 to 40 μm, or 10 to 30 μm. The surface roughness of the support film is not particularly limited, and the arithmetic mean roughness (Ra) can be less than 1000 nm, less than 500 nm, or less than 250 nm.
[0201] The coating film can be dried by hot air drying, far infrared ray drying or near infrared ray drying. The drying temperature may be 60 to 120° C., 70 to 110° C. or 80 to 100° C. The drying time may be 1 to 60 minutes, 2 to 30 minutes or 5 to 20 minutes.
[0202] The photosensitive layer 20 may further include a protective film 30 covering the photosensitive layer 20. The photosensitive element 1 may also have a protective film 30 laminated on the surface of the photosensitive layer 20 opposite to the surface in contact with the support film 10. As the protective film 30, for example, a polymer film such as polyethylene or polypropylene may be used.
[0203] [Printed circuit board]
[0204] The printed wiring board of the present embodiment includes a permanent resist composed of a cured product of the photosensitive resin composition of the present embodiment.
[0205] The method for manufacturing a printed wiring board of this embodiment comprises the steps of forming a photosensitive layer on a substrate using the above-mentioned photosensitive resin composition or photosensitive element, exposing and developing the photosensitive layer to form a resist pattern, and curing the resist pattern to form a permanent resist. An example of each step is described below.
[0206] First, a substrate such as a copper-clad laminate is prepared, and a photosensitive layer is formed on the substrate. The photosensitive layer can also be formed by coating a photosensitive resin composition on the substrate and drying it. As a method for coating the photosensitive resin composition, for example, screen printing, spraying, roller coating, curtain coating and electrostatic coating can be cited. The drying temperature can be 60 to 120°C, 70 to 110°C, or 80 to 100°C. The drying time can be 1 to 7 minutes, 1 to 6 minutes, or 2 to 5 minutes. The thickness of the photosensitive layer is preferably 5 μm or more, and can also be 10 to 200 μm, 15 to 150 μm, 20 to 100 μm, or 23 to 50 μm.
[0207] The photosensitive layer can also be formed by peeling off the protective film from the photosensitive element and laminating the photosensitive layer on the substrate. As a method for laminating the photosensitive layer, for example, a method of heat lamination using a laminator can be mentioned.
[0208] Then, the negative film is brought into direct contact with the photosensitive layer or through a supporting film, and exposed to active light. Examples of active light include electron beams, ultraviolet rays, and X-rays, preferably ultraviolet rays. As the light source, a low-pressure mercury lamp, a high-pressure mercury lamp, an ultrahigh-pressure mercury lamp, a halogen lamp, etc. can be used. The exposure amount can be 10 to 2000 mJ / cm 2 100~1500mJ / cm 2 , or 300~1000mJ / cm 2 .
[0209] After exposure, the unexposed portion is removed with a developer to form a resist pattern. As a developing method, for example, an immersion method and a spray method can be cited. As a developer, for example, an alkaline aqueous solution such as potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, and tetramethylammonium hydroxide can be used.
[0210] By performing at least one of post-exposure and post-heating on the resist pattern, a pattern cured film (permanent resist) can be formed. The exposure dose of the post-exposure can be 100 to 5000 mJ / cm 2 , 500~2000mJ / cm 2 , or 700~1500J / cm 2 The heating temperature of the post-heating may be 100 to 200° C., 120 to 180° C., or 135 to 165° C. The heating time of the post-heating may be 5 minutes to 12 hours, 10 minutes to 6 hours, or 30 minutes to 2 hours.
[0211] The permanent resist of this embodiment can be used as an interlayer insulating layer or surface protective layer of a semiconductor element. A semiconductor element having an interlayer insulating layer or surface protective layer formed by a cured film of the above-mentioned photosensitive resin composition, and an electronic device including the semiconductor element can be produced. The semiconductor element can be, for example, a memory, a package, etc. having a multi-layer wiring structure, a redistribution structure, etc. As electronic devices, for example, mobile phones, smart phones, tablet terminals, personal computers, and hard disk suspensions can be cited. A patterned cured film formed by the photosensitive resin composition of this embodiment can provide semiconductor elements and electronic devices with excellent reliability.
[0212] Example
[0213] Hereinafter, the present invention will be described in further detail by way of examples, but the present invention is not limited to these examples.
[0214] (Synthesis example 1)
[0215] A bisphenol F novolac epoxy resin (manufactured by DIC Corporation, product name "EXA-7376", wherein Y 3 and Y 4 is epoxypropyl, R 12 350 parts by mass of bisphenol F novolac-type epoxy resin having a structural unit of hydrogen atoms, epoxy equivalent: 186), 70 parts by mass of acrylic acid, 0.5 parts by mass of methylhydroquinone and 120 parts by mass of carbitol acetate were stirred and mixed at 90°C. The mixed solution was cooled to 60°C, 2 parts by mass of triphenylphosphine was added, and the mixture was reacted at 100°C until the acid value of the solution became 1 mgKOH / g or less. 98 parts by mass of tetrahydrophthalic anhydride (THPAC) and 85 parts by mass of carbitol acetate were added to the reaction solution, and the mixture was reacted at 80°C for 6 hours. Thereafter, the reaction solution was cooled to room temperature to obtain a solution of acid-modified epoxy acrylate (A-1) as component (A) (solid content concentration: 73% by mass).
[0216] (Synthesis example 2)
[0217] After adding 70g of ethyl lactate, 13.4g of methyl acrylate, 22.5g of n-butyl acrylate, 2.0g of acrylic acid and 3.0g of azobisisobutyronitrile to a 100mL three-necked flask equipped with a stirrer, a nitrogen inlet tube and a thermometer, the mixture was stirred at about 160rpm at room temperature, and nitrogen was flowed at a flow rate of 400mL / min for 30 minutes to remove the dissolved oxygen in the flask. Thereafter, the flow of nitrogen was stopped, the flask was sealed, and the temperature was raised to 65°C in a thermostatic water bath for about 25 minutes. The polymerization reaction was carried out at the same temperature for 10 hours to obtain an acrylic elastomer (E-1). The Mw of E-1 was about 10,000.
[0218] (Synthesis example 3)
[0219] Except for adding 70 g of ethyl lactate, 2.8 g of methyl acrylate, 13.3 g of n-butyl acrylate, 2.4 g of acrylic acid and 1.0 g of azobisisobutyronitrile, polymerization reaction was carried out in the same procedure as the synthesis of E-1 to obtain an acrylic elastomer (E-2). The Mw of E-2 was about 15,000.
[0220] The following materials were prepared as components (A) to (I).
[0221] A-1: Acid-modified epoxy acrylate of Synthesis Example 1 (A-1)
[0222] B-1: Bisphenol F type epoxy resin (manufactured by NIPPON STEEL Chemical & Material Co., Ltd., product name "YDF-8170C", average molecular weight: 310 to 330, epoxy equivalent: 155 to 165)
[0223] B-2: Bisphenol A type epoxy resin (manufactured by NIPPON STEEL Chemical & Material Co., Ltd., product name "YD-8125", average molecular weight: 336 to 356, epoxy equivalent: 168 to 178)
[0224] B-3: Bisphenol A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name "jER828", average molecular weight: 368 to 388, epoxy equivalent: 184 to 194)
[0225] B-4: Phenol novolac type epoxy resin (manufactured by Nippon Kayaku Co., Ltd., product name "RE-306", average molecular weight: 400, epoxy equivalent: 170 to 181)
[0226] C-1: 2-methyl-[4-(methylthio)phenyl]isopropyl-1-propanone (manufactured by IGM Resins BV, product name "Omirad 907")
[0227] C-2: 2,4-diethylthioxanthone (manufactured by Nippon Kayaku Co., Ltd., product name "DETX-S")
[0228] C-3: 4,4'-bis(diethylamino)benzophenone (EAB)
[0229] C-4: Ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(0-acetyl oxime) (manufactured by BASF JAPAN LTD., product name "Irgacure OXE02")
[0230] D-1: Dipentaerythritol hexaacrylate (manufactured by Nippon Kayaku Co., Ltd., product name "DPHA")
[0231] E-1: Acrylic elastomer of Synthesis Example 2 (E-1)
[0232] E-2: Acrylic elastomer of Synthesis Example 3 (E-2)
[0233] F-1: Silica (manufactured by Denka Company Limited, product name "SFP20M", average particle size: 0.3 μm)
[0234] F-2: barium sulfate (manufactured by Sakai Chemical Industry Co., Ltd., product name "B-34", average particle size: 0.3 μm)
[0235] G-1: Phthalocyanine pigment (manufactured by SANYO COLOR WORKS, Ltd.)
[0236] H-1: Zwitterion scavenger containing Zr, Mg, and Al (manufactured by Toagosei Company, Limited, product name "IXEPLAS-A2", average particle size: 0.2 μm, content of Zr compound: 20 to 30% by mass)
[0237] I-1: 3-methacryloxypropyltriethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-503")
[0238] [Photosensitive resin composition]
[0239] Each component was blended in the amount (parts by mass, amount based on solid content) shown in Table 1 or Table 2 and kneaded using a three-roll mill. Then, carbitol acetate was added so that the solid content concentration became 70% by mass to prepare a photosensitive resin composition.
[0240] [Photosensitive element]
[0241] A polyethylene terephthalate film (manufactured by TOYOBO FILMSOLUTIONS, product name "G2-25") with a thickness of 25 μm was prepared as a support film. A solution obtained by adding methyl ethyl ketone to a photosensitive resin composition and diluting the solution was applied to the support film so that the thickness after drying became 25 μm, and the solution was dried at 75°C for 30 minutes using a hot air convection dryer to form a photosensitive layer. Then, a polyethylene film (manufactured by TAMAPOLY CO., LTD., product name "NF-15") was laminated as a protective film on the surface opposite to the side in contact with the support film of the photosensitive layer to obtain a photosensitive element.
[0242] (Resolution)
[0243] A copper-clad laminate substrate (Showa Denko Materials Co., Ltd., product name "MCL-E-67") with a thickness of 0.6 mm was prepared. The protective film was peeled off from the photosensitive element, and a photosensitive layer was laminated on the copper-clad laminate substrate using a pressing vacuum laminator (Meiki Co., Ltd., product name "MVLP-500") with a pressing pressure of 0.4 MPa, a pressing hot plate temperature of 80°C, a vacuuming time of 25 seconds, and a lamination pressing time of 25 seconds to obtain a laminate. Then, a negative mask having an opening pattern of a predetermined size (opening diameter size: 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 150, 200 μm) was brought into close contact with the support film of the above-mentioned laminate, and the photosensitive layer was exposed using an ultraviolet exposure device (manufactured by OAK Co., Ltd., product name "EXM-1201") at an exposure amount that resulted in 13 stages of complete curing in the number of grids (manufactured by Showa Denko Materials Co., Ltd.). Thereafter, the support film was peeled off from the photosensitive layer, and a 1 mass % sodium carbonate aqueous solution was used for 60 seconds at 1.765×10 5 The developed photosensitive layer was sprayed with a pressure of 2000 mJ / cm 2 After exposure with an exposure amount of 1000 nm, the substrate was heated at 170° C. for 1 hour to prepare a test piece having a cured film with an opening pattern of a predetermined size formed on the copper-clad laminate substrate. The test piece was observed using an optical microscope and evaluated based on the following criteria.
[0244] A: The minimum opening size is 30 μm or less.
[0245] B: The minimum opening diameter size is more than 30 μm and is 50 μm or less.
[0246] C: The minimum opening size exceeds 50 μm.
[0247] (Resist pattern shape)
[0248] The test piece was cast with an embedding resin (Mitsubishi Chemical Corporation's product name "jER828" as an epoxy resin and triethylenetetramine as a curing agent) and fully cured, then polished with a grinder (Refine Tech Co., Ltd. product name "Refine Polisher") to cut out the cross section of the opening pattern of the cured film. The cross section of the obtained opening pattern was observed using a metal microscope and evaluated according to the following criteria.
[0249] A: No undercut or missing of the resist upper portion was observed, and the linearity of the pattern profile was good.
[0250] B: Undercut or missing of the upper portion of the resist was confirmed, or the linearity of the pattern profile was poor.
[0251] (Thermal shock resistance)
[0252] The test pieces prepared for the evaluation of resolution were subjected to a temperature cycle test with 30 minutes at -65°C and 30 minutes at 150°C as one cycle. The test pieces were observed visually and under an optical microscope at 1000 and 2000 cycles and evaluated according to the following criteria.
[0253] A: No cracks were observed in 2000 cycles.
[0254] B: No cracks were observed in 1000 cycles, but cracks were observed in 2000 cycles.
[0255] C: Generation of cracks was observed in 1000 cycles.
[0256] (Heat resistance)
[0257] The test pieces produced in the evaluation of resolution were placed in an environment of 150° C., and after 1000 hours and 2000 hours, the test pieces were observed visually and under an optical microscope, and evaluated according to the following criteria.
[0258] A: No cracks were observed within 2000 hours.
[0259] B: No cracks were observed within 1000 hours, but cracks were observed within 2000 hours.
[0260] C: Generation of cracks was observed within 1000 hours.
[0261] (Adhesion)
[0262] A laminate having a photosensitive layer was prepared by the same procedure as the laminate prepared in the evaluation of resolution except that a 6-inch silicon wafer (manufactured by ELECTRONICS AND MATERIALS CORPORATION) was used instead of the copper-clad laminate substrate. The laminate was exposed to light at 500 mJ / cm using an i-ray exposure device (manufactured by USHIO INC., product name "UX-2240SM-XJ-01"). 2 Then, the support film was peeled off from the photosensitive layer and an ultraviolet exposure device was used to expose the entire surface at 2000 mJ / cm 2 After further exposing the photosensitive layer with an exposure amount of , the cured film of the photosensitive resin composition was formed on the silicon wafer by heating at 170°C for 1 hour. Thereafter, an Al-made pin with an epoxy adhesive (manufactured by PHOTOTECHNICA Co., Ltd., product name "P / N901106", adhesive portion diameter: 2.7 mm) was vertically set on the cured film, and heated at 150°C for 1 hour to obtain a test piece. The pin on the test piece was fixed to the chuck of a thin film adhesion strength measuring device (manufactured by PHOTOTECHNICA Co., Ltd.), and a force was applied vertically to the cured film. The adhesion of the cured film to the silicon wafer was evaluated according to the following criteria.
[0263] A: There is no peeling at the interface between the cured film and the silicon wafer, and the epoxy adhesive is destroyed by cohesion.
[0264] B: Peeling at the interface between the cured film and the silicon wafer.
[0265] [Table 1]
[0266]
[0267] [Table 2]
[0268]
[0269] Explanation of symbols
[0270] 1-photosensitive element, 10-support film, 20-photosensitive layer, 30-protective film.
Claims
1. A photosensitive resin composition comprising (A) an acid-modified vinyl-containing resin, (B) a thermosetting resin, (C) a photopolymerization initiator, (D) a photopolymerizable compound, and (E) an elastomer, The thermosetting resin comprises a bisphenol epoxy compound having an average molecular weight of 360 or less, The elastomer includes an acrylic elastomer.
2. The photosensitive resin composition according to claim 1, in, The content of the thermosetting resin is 5 to 25% by mass based on the total solid content of the photosensitive resin composition.
3. The photosensitive resin composition according to claim 1, in, The acrylic elastomer has a carboxyl group.
4. The photosensitive resin composition according to claim 3, in, The acrylic elastomer further has an n-butyl group.
5. The photosensitive resin composition according to claim 1, in, The weight average molecular weight of the acrylic elastomer is 5,000 to 20,000. The photosensitive resin composition according to claim 1 , further comprising (I) a silane coupling agent. 7 . The photosensitive resin composition according to claim 1 , further comprising (F) an inorganic filler.
8. A photosensitive element comprising a support film and a photosensitive layer formed on the support film, The photosensitive layer comprises the photosensitive resin composition according to any one of claims 1 to 7. 9 . A printed wiring board comprising a permanent resist comprising a cured product of the photosensitive resin composition according to claim 1 .
10. A method for manufacturing a printed circuit board, comprising: A step of forming a photosensitive layer on a substrate using the photosensitive resin composition according to any one of claims 1 to 7; A step of exposing and developing the photosensitive layer to form a resist pattern; and The process of curing the resist pattern to form a permanent resist.
11. A method for manufacturing a printed circuit board, comprising: A step of forming a photosensitive layer on a substrate using the photosensitive element according to claim 8; A step of exposing and developing the photosensitive layer to form a resist pattern; and The process of curing the resist pattern to form a permanent resist.
Citation Information
Patent Citations
Process for preparing butyl-p-benzoylbenzoates
EP0000502A1
Method for making lithographic printing plates
EP0001138A1
Device for distributing traction forces in traction elements made of materials bonded with oriented fibres
EP0001235A1
Resin paste and flexible wiring board using the same
JP2003198105A
Black matrix composition with high light-shielding property and improved adhesive force to substrate
JP2011133851A