Positive electrode active material, and positive electrode and lithium secondary battery comprising same
By using lithium manganese-based oxyhalides with disordered rock salt structure in the positive electrode active material of lithium secondary batteries and doping elements and halogen, the problem of poor rate performance and life characteristics of lithium secondary batteries is solved, and the further development is achieved High energy density and stability.
Patent Information
- Application Number
- CN202380035661.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-22
- Filing Date
- 2023-04-20
- Publication Date
- 2024-12-03
AI Technical Summary
The positive electrode active materials of existing lithium secondary batteries have low rate performance and poor service life characteristics due to structural characteristics, and the use of expensive transition metals increases costs, making it difficult to meet the needs of high energy density and price competitiveness.
Li-manganese-based oxyhalides with disordered rock salt structure are used as the positive electrode active material. By doping elements such as titanium and nickel, structural characteristics are controlled to alleviate the Jahn-Teller effect, and partial oxygen atoms are replaced by halogen to improve oxygen oxidation. Reduction reversibility and stability.
The life characteristics and rate performance of lithium secondary batteries are significantly improved, the oxidation number of transition metals is reduced, the stable oxidation/reduction amount of transition metals is increased, and the energy density and cycle characteristics are improved.
Smart Images

Figure CN119072796A_ABST
Abstract
Description
Technical Field
[0001] This application claims priority from Korean Patent Application No. 10-2022-0050421, filed on April 22, 2022, the disclosure of which is incorporated herein by reference.
[0002] The present invention relates to a positive electrode active material, a positive electrode containing the positive electrode active material and a lithium secondary battery, and more particularly to a manganese-based positive electrode active material having a disordered rock salt structure, and a positive electrode and a lithium secondary battery containing the same. Background Art
[0003] In recent years, interest in energy storage technology has grown as its applications have expanded to include powering mobile phones, cameras, laptops, and even electric vehicles, and research and development of electrochemical devices has gradually become more concrete.
[0004] Among these electrochemical devices, interest has been aroused in the development of rechargeable secondary batteries, and in particular, lithium secondary batteries developed in the early 1990s have attracted much attention because of their advantages of higher operating voltage and significantly higher energy density.
[0005] Lithium secondary batteries are typically manufactured by placing a separator between a positive electrode containing a positive electrode active material formed from a lithium-containing transition metal oxide and a negative electrode containing a negative electrode active material capable of storing lithium ions, thereby forming an electrode assembly. The electrode assembly is then inserted into a battery casing, into which a non-aqueous electrolyte, which acts as a lithium ion transport medium, is injected, and the battery casing is then sealed. The non-aqueous electrolyte is typically composed of a lithium salt and an organic solvent capable of dissolving the lithium salt.
[0006] Recently, with the increasing demand for high energy density secondary batteries (such as batteries for electric vehicles), lithium composite transition metal oxides (such as lithium nickel cobalt manganese aluminum oxide or layered structure lithium nickel cobalt manganese oxide with high energy density) are mainly used as positive electrode active materials. However, with the rapid growth in demand for secondary batteries, the prices of transition metals such as nickel and cobalt have also soared, thereby reducing price competitiveness. In addition, the increase in energy density of secondary batteries using conventional lithium composite transition metal oxides has reached its limit. Therefore, attempts have been made to develop positive electrode active materials based on manganese (Mn) with excellent price competitiveness.
[0007] As Mn-based cathode active materials that have been actively studied in recent years, there are over-lithiated manganese-rich cathode active materials (e.g., Li2MnO3 rock salt structure mixed with LiMO2 layered structure) 1.2 Ni 0.13 Mn 0.54 Co 0.13 O2), or cathode active materials with a partially spinel-disordered rock salt structure (e.g., Li1.68 Mn 1.6 O 3.7 F 0.3 Overlithiated manganese-rich cathode active materials have excellent capacity characteristics, but their structural characteristics lead to low rate performance, which limits their application. In addition, there is also the problem of reduced life characteristics due to irreversible oxygen redox reactions. For cathode active materials with partial spinel-disordered rock salt structures, they have excellent rate performance and capacity characteristics, but still have the problem of exhibiting low life characteristics. Summary of the Invention
[0008] [Technical Issues]
[0009] One aspect of the present invention provides a novel cathode active material based on relatively inexpensive manganese, which has excellent capacity characteristics, rate capability, and lifespan characteristics by including a disordered rock salt structure.
[0010] [Technical solution]
[0011] According to one aspect of the present invention, a positive electrode active material is provided, which includes a lithium manganese-based oxyhalide having a composition represented by [Formula 1] and having a disordered rock salt structure.
[0012] [Formula 1]
[0013] Li 0.5+a Mn b M c O d X e
[0014] In [Formula 1], M is selected from at least one of titanium (Ti), nickel (Ni), zirconium (Zr), vanadium (V), cobalt (Co), tin (Sn), iron (Fe), iridium (Ir), chromium (Cr), lead (Pb) and ruthenium (Ru), preferably Ti, X is a halogen element, preferably fluorine (F), 0<a≤0.7, 0.5≤b<1, 0<c≤b / 2, 1.5≤d≤1.9, 0.1≤e≤0.5, d+e≤2.
[0015] The atomic ratio of the cationic element to the anionic element in the lithium manganese-based oxyhalide may be 0.75:1 to 1:1.
[0016] The primary particle size of the lithium manganese-based oxyhalide may be 50 nm to 300 nm.
[0017] According to one embodiment, the lithium manganese-based oxyhalide may have a composition represented by [Formula 1-1].
[0018] [Formula 1-1]
[0019] Li1+a1 Mn b1 M c1 O 2-e1 X e1
[0020] In [Formula 1-1], M is at least one selected from Ti, Ni, Zr, V, Co, Sn, Fe, Ir, Cr, Pb and Ru, preferably Ti, X is a halogen element, preferably F, 0 <a1≤0.2,0.5≤b1<1,0<c1≤b1 / 2,0.1≤e1≤0.5。
[0021] The lithium manganese-based oxyhalide represented by [Formula 1-1] may have a single-phase structure of a disordered rock salt structure.
[0022] According to another embodiment, the lithium manganese-based oxyhalide may have a composition represented by [Formula 1-2].
[0023] [Formula 1-2]
[0024] Li 0.5+a2 Mn b2 M c2 O 2-e2 X e2
[0025] In [Formula 1-2], M is at least one selected from Ti, Ni, Zr, V, Co, Sn, Fe, Ir, Cr, Pb and Ru, preferably Ti, X is a halogen element, preferably F, 0 <a2<0.5,0.5≤b2<1,0<c2≤b2 / 2,0.1≤e2≤0.5。
[0026] The lithium manganese-based oxyhalide having a composition represented by [Formula 1-2] may have a multiphase structure in which a disordered rock salt structure, a layered rock salt structure, and a spinel structure are mixed. In this case, the proportion of the spinel phase in the lithium manganese-based oxyhalide is less than 75%, preferably 25% to 75%.
[0027] In addition, I(400) of the lithium manganese-based oxyhalide represented by [Formula 1-2] R / I(111) S , that is, the peak intensity of the (400) surface I(400) R Peak intensity I(111) with (111) surface S The ratio can be greater than 1.
[0028] According to another aspect of the present invention, a positive electrode including the positive electrode active material of the present invention and a lithium secondary battery including the positive electrode are provided.
[0029] [Beneficial Effects]
[0030] The positive electrode active material of the present invention comprises a lithium manganese-based oxyhalide having a disordered rock salt structure and doped with an element M (wherein M is at least one selected from titanium (Ti), nickel (Ni), zirconium (Zr), vanadium (V), cobalt (Co), tin (Sn), iron (Fe), iridium (Ir), chromium (Cr), lead (Pb) and ruthenium (Ru)). In the present invention, when the lithium manganese-based oxyhalide having a disordered rock salt structure is doped with the element M, the structural characteristics are controlled to alleviate the Mn 3+ The Jahn-Teller effect (Jahn-Teller distortion) caused by the reaction and the improvement of the oxygen redox reversibility during the charge and discharge process, thus significantly improving the life characteristics.
[0031] In addition, since some of the oxygen atoms in the lithium manganese-based oxyhalides are replaced by halogens, the presence of larger halogen elements (F - ), which can reduce the oxidation number of the transition metal and thus increase the oxidation / reduction amount of the stable transition metal, thereby obtaining better rate performance and cycle characteristics than conventional over-lithiated manganese-based oxides. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is a scanning electron microscope (SEM) image of the lithium manganese-based oxyhalide synthesized in Example 1.
[0033] Figure 2 is a SEM image of the lithium manganese-based oxyhalide synthesized in Example 2.
[0034] Figure 3 is a SEM image of the lithium manganese-based oxyhalide synthesized in Comparative Example 2.
[0035] Figure 4 is a SEM image of the lithium manganese-based oxyhalide synthesized in Example 3.
[0036] Figure 5 is a SEM image of the lithium manganese-based oxyhalide synthesized in Example 4.
[0037] Figure 6 : is a graph showing the life characteristics of lithium secondary batteries using the lithium manganese-based oxyhalides synthesized in Examples 1 and 2.
[0038] Figure 7 : is a graph showing the life characteristics of lithium secondary batteries using the lithium manganese-based oxyhalides synthesized in Comparative Example and Examples 3 and 4.
[0039] Figure 8 (A) is a high-resolution transmission electron microscopy (HR-TEM) image of the lithium manganese-based oxyhalide synthesized in Example 4, Figure 8(B) is the result of the selected area electron diffraction (SAED) spectrum of the lithium manganese-based halide oxide synthesized in Example 4.
[0040] Figure 9 The X-ray diffraction (XRD) data of the lithium manganese-based oxyhalide synthesized in the comparative example.
[0041] Figure 10 This is the XRD data of the lithium manganese-based oxyhalide synthesized in Example 3.
[0042] Figure 11 This is the XRD data of the lithium manganese-based oxyhalide synthesized in Example 4. DETAILED DESCRIPTION
[0043] Hereinafter, the present invention will be described in more detail.
[0044] positive electrode active material
[0045] The positive electrode active material of the present invention comprises a lithium manganese-based oxyhalide having a disordered rock salt structure and doped with an element M (wherein M is at least one selected from the group consisting of titanium (Ti), nickel (Ni), zirconium (Zr), vanadium (V), cobalt (Co), tin (Sn), iron (Fe), iridium (Ir), chromium (Cr), lead (Pb) and ruthenium (Ru)).
[0046] The crystal structure of conventionally used positive electrode active materials is generally composed of an ordered layered structure (in which the lithium layer and the transition metal layer are separated) or an ordered spinel structure. However, the problem with these conventional positive electrode active materials is that expensive transition metals (such as nickel or cobalt) must be used, and since phase transition occurs when lithium is deintercalated from the lithium layer, the improvement in energy density is limited. In contrast, for the positive electrode active material with a disordered rock salt structure in the present invention, since there is no separate lithium layer, the phase transition caused by the deintercalation of lithium occurs less, so there is an advantage of obtaining a higher energy density, and since the volume change caused by charging and discharging is small, the conductive network loss caused by the increase in the volume of the positive electrode active material can be minimized.
[0047] Specifically, the lithium manganese-based oxyhalide of the present invention may have a composition represented by the following [Formula 1].
[0048] [Formula 1]Li 0.5+a Mn b M c O d X e
[0049] In [Formula 1], M can be at least one selected from Ti, Ni, Zr, V, Co, Sn, Fe, Ir, Cr, Pb, and Ru, and preferably Ti. In the present invention, when an element M is doped in a lithium manganese-based oxyhalide having a disordered rock salt structure, due to Mn 3+ The Jahn-Teller effect (Jahn-Teller distortion) caused is alleviated, and the oxygen redox reversibility during charge and discharge can be improved by structural control, so that the effect of improving the life characteristics can be obtained.
[0050] X can be a halogen element, preferably fluorine (F), chlorine (Cl), bromine (Br), and / or iodine (I), more preferably F. When part of the oxygen atoms are replaced by a halogen, since the electronegativity of the halogen element is higher than that of the oxygen element, even when the addition amount of lithium exceeds the stoichiometry, the charge balance between cations and anions can be achieved, so that better rate performance and cycle characteristics than conventional over-lithiated manganese-based oxides can be obtained.
[0051] 0.5 + a represents the atomic ratio of lithium (Li) in the lithium manganese-based oxyhalide, where a can satisfy 0 < a ≤ 0.7, 0.02 ≤ a ≤ 0.7, 0.02 ≤ a ≤ 0.5, 0 < a ≤ 0.2, 0.02 ≤ a ≤ 0.2, or 0.2 ≤ a ≤ 0.7. Preferably, the positive electrode active material of the present invention contains lithium in excess of the stoichiometric ratio. When the content of lithium is greater than the stoichiometric ratio, the high-capacity characteristics are improved, and since the amount of lithium having 0 (0-TM) or 1 (1-TM) transition metals based on 4 tetrahedral faces increases, the effect of improving the rate performance is more significant. However, since excessive lithium may deteriorate the overall conduction characteristics by reducing the conductivity of the material, the atomic ratio of lithium in the lithium manganese-based oxyhalide is preferably 1.2 or less.
[0052] b represents the atomic ratio of manganese (Mn) in the lithium manganese-based oxyhalide, where b can satisfy 0.5 ≤ b < 1, 0.5 ≤ b ≤ 0.9, 0.6 ≤ b ≤ 0.8, 0.5 ≤ b < 1, or 0.5 ≤ b ≤ 0.9. When the atomic ratio of manganese satisfies the above range, excellent capacity characteristics can be obtained.
[0053] c represents the atomic ratio of the doped element M in the lithium manganese-based oxyhalide, where c can satisfy 0 < c ≤ b / 2, 0.05 ≤ c ≤ b / 2, or 0.1 ≤ c ≤ b / 2. When the atomic ratio of the doped element M satisfies the above range, a positive electrode active material having excellent capacity characteristics, rate performance, and life characteristics can be obtained. If the amount of the doped element M is excessively increased, the capacity and rate performance of the positive electrode active material may decrease; if the amount of the doped element M is too small, the effect of improving the life characteristics is not obvious.
[0054] d represents the atomic ratio of oxygen in the lithium manganese-based oxyhalide, where d can satisfy 1.5 ≤ d ≤ 1.9, 1.7 ≤ d ≤ 1.9, 1.5 ≤ d ≤ 1.7, or 1.75 ≤ d ≤ 1.85.
[0055] e represents the atomic ratio of the halogen element X in the lithium manganese-based oxyhalide, where e can satisfy 0.1 ≤ e ≤ 0.5, 0.1 ≤ e ≤ 0.4, or 0.1 ≤ e ≤ 0.3. When the atomic ratio of the halogen element X satisfies the above range, the charge balance between cations and anions can be appropriately maintained, thereby achieving excellent rate performance and cycling characteristics.
[0056] In Formula 1, d + e ≤ 2, and d + e is preferably 2.
[0057] In the lithium manganese-based oxyhalide, the atomic ratio of the cationic elements (i.e., lithium, manganese, and element M) to the anionic elements (i.e., oxygen and halogen) can be 0.75:1 to 1:1. When the atomic ratio of the cationic elements to the anionic elements satisfies the above range, a disordered rock salt structure can be successfully formed.
[0058] The lithium manganese-based oxyhalide can be in the form of primary particles and / or secondary particles formed by aggregation of multiple primary particles. In this case, the particle size of the primary particles can be 50 nm to 300 nm, preferably 50 nm to 250 nm. When the particle size of the primary particles satisfies the above range, the disadvantage of low ionic conductivity of the material can be overcome by increasing the surface-to-volume ratio.
[0059] According to one embodiment, the lithium manganese-based oxyhalide can have a composition represented by [Formula 1-1].
[0060] [Formula 1-1] Li 1+a1 Mn b1 M c1 O 2-e1 X e1
[0061] In [Formula -1], M and X are the same as defined in Formula 1. That is, M can be at least one selected from the group consisting of Ti, Ni, Zr, V, Co, Sn, Fe, Ir, Cr, Pb, and Ru, preferably Ti, and X can be a halogen element, preferably F.
[0062] 1 + a1 represents the atomic ratio of lithium in the lithium manganese-based oxyhalide, where a1 can satisfy 0 < a1 ≤ 0.2, 0.02 ≤ a1 < 0.2, or 0.02 ≤ a1 ≤ 0.15.
[0063] b1 represents the atomic ratio of Mn in the lithium manganese-based oxyhalide, where b1 can satisfy 0.5 ≤ b1 < 1, 0.6 ≤ b1 < 1, or 0.6 ≤ b1 ≤ 0.9.
[0064] c1 represents the atomic ratio of the doping element M in the lithium manganese-based oxyhalide, where c1 can satisfy 0 < c1 ≤ b1 / 2, 0.05 ≤ c1 ≤ b1 / 2, or 0.1 ≤ c1 ≤ b1 / 2.
[0065] e1 represents the atomic ratio of the halogen element X in the lithium manganese-based oxyhalide, where e1 can satisfy 0.1 ≤ e1 ≤ 0.5, 0.1 ≤ e1 ≤ 0.4, or 0.1 ≤ e1 ≤ 0.25.
[0066] The lithium manganese-based oxyhalide represented by [Formula 1-1] may have a disordered rock salt structure phase and may preferably be composed of a single phase of the disordered rock salt structure. For conventional over-lithiated manganese oxides, to enable lithium to move smoothly in the structure, a large excess of lithium is required, resulting in the formation of a large amount of transition metal-poor oxides. Transition metals are crucial for solving the structural instability of the positive electrode during the charging process (delithiation reaction), but transition metal-poor oxides (oxides with excessive lithium) increase the structural instability. Therefore, in the present invention, by reducing the amount of excess lithium (a1) to less than 0.2 at%, the phenomenon of transition metal depletion in the positive electrode is minimized, thereby achieving structural stability, and the structural stability can be further improved by doping with the element M. As described above, since the stability of the positive electrode structure is achieved through the low excess lithium and doping in the manganese-based oxyhalide, the structural change of the positive electrode active material during charge and discharge can be suppressed, and thus, the life characteristics can be significantly improved.
[0067] According to another embodiment, the lithium manganese-based oxyhalide may have a composition represented by [Formula 1-2].
[0068] [Formula 1-2] Li 0.5+a2 Mn b2 M c2 O 2-e2 X e2
[0069] In [Formula -2], M and X are the same as those defined in [Formula 1]. That is, M may be at least one selected from the group consisting of Ti, Ni, Zr, V, Co, Sn, Fe, Ir, Cr, Pb, and Ru, preferably Ti, and X may be a halogen element, preferably F.
[0070] 0.5 + a2 represents the atomic ratio of lithium in the lithium manganese-based oxyhalide, where a2 can satisfy 0 < a2 < 0.5, 0.1 ≤ a2 < 0.5, or 0.2 ≤ a2 ≤ 0.4.
[0071] b2 represents the atomic ratio of Mn in the lithium manganese-based oxyhalide, where b2 can satisfy 0.5 ≤ b2 < 1, 0.6 ≤ b2 < 1, or 0.65 ≤ b2 ≤ 0.95.
[0072] c2 represents the atomic ratio of the doping element M in the lithium manganese-based oxyhalide, where c2 can satisfy 0 < c2 ≤ b2 / 2, 0.05 ≤ c2 ≤ b2 / 2, or 0.1 ≤ c2 ≤ b2 / 2.
[0073] e1 represents the atomic ratio of the halogen element X in the lithium manganese-based oxyhalide, where e2 can satisfy 0.1 ≤ e2 ≤ 0.5, 0.1 ≤ e2 ≤ 0.4, or 0.1 ≤ e2 ≤ 0.25.
[0074] The lithium manganese-based oxyhalide having the composition represented by [Formula 1-2] can have a multiphase structure in which a disordered rock salt structure, a layered rock salt structure, and a spinel structure are mixed.
[0075] In the disordered rock salt structure, transition metals and lithium are randomly distributed and arranged at the 16c and 16d octahedral sites. Its rate performance is usually low because the limitation is that lithium can move only when the number of transition metals is 0 (0-TM) or 1 (1-TM) based on the 4 tetrahedral faces for lithium movement in the structure. On the contrary, in the ordered spinel structure, lithium diffuses easily because all transition metals (such as Mn) are located at the 16d octahedral sites and lithium is located at the 8a tetrahedral sites. Therefore, all lithium atoms have a lithium environment of 0-TM where transition metals are not located on all tetrahedral faces. In addition, it has the characteristic of high rate performance by forming a three-dimensional lithium network in the structure. Therefore, in the case where the lithium manganese-based oxyhalide has a multiphase structure in which a disordered rock salt structure and a spinel structure are mixed, as described above, compared with the case where the lithium manganese-based oxyhalide is composed of only a single phase of the disordered rock salt structure, the effect of improving the rate performance can be obtained.
[0076] In this case, the proportion of the spinel phase in the lithium manganese-based oxide can be 75% or less, preferably 25% to 75%. When the proportion of the spinel phase satisfies the above range and the proportion of the rock salt structure increases, due to the suppression of the structural change of the positive electrode active material during charge and discharge, the effect of significantly improving the life characteristics can be obtained.
[0077] In addition, in the X-ray diffraction (XRD) data of the lithium manganese-based oxyhalide represented by [Formula 1-2], I(400) R / I(111) S , that is, the peak intensity I(400) of the (400) plane R and the peak intensity I(111) of the (111) plane S ratio can be 1 or more, preferably 1 to 2, more preferably 1 to 1.5. When I(400) R / I(111) S satisfies the above range, the effect of improving the life characteristics is excellent.
[0078] The lithium manganese-based oxyhalide having a disordered rock salt structure can be synthesized by mechanochemically mixing a lithium source, a manganese source, a halogen source, and a doping element M source. For example, the lithium manganese-based oxyhalide of the present invention can be prepared by adding a lithium source, a manganese source, a halogen source, and a doping element M source to a high-energy ball mill and then ball milling and mixing.
[0079] As the lithium source, for example, Li2O, Li2O2, Li2MnO3, or a combination thereof can be used. As the manganese source, for example, Mn2O3, MnO2, Li2MnO3, or a combination thereof can be used, but the present invention is not limited thereto. As the halogen source, for example, LiF, MnF2, or a combination thereof can be used. As the doping element M source, an oxide of the element M, for example, TiO2, can be used, but the present invention is not limited thereto.
[0080] The above sources may be mixed in amounts satisfying the atomic ratio of Li, Mn, M, and O in the lithium manganese-based oxyhalide to be finally prepared.
[0081] In addition, the ball mill mixing may be performed at a stirring speed of 300 to 600 rpm, preferably 400 to 500 rpm, for 25 to 50 hours, and may be performed by adding stainless steel balls of two different sizes.
[0082] positive electrode
[0083] Next, the positive electrode of the present invention will be described.
[0084] The positive electrode of the present invention includes a positive electrode active material layer containing the positive electrode active material of the present invention. Specifically, the positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector and containing the positive electrode active material.
[0085] In the positive electrode, the positive electrode current collector is not particularly limited as long as it is conductive and does not cause adverse chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, fired carbon, or aluminum or stainless steel whose surface has been treated with one of carbon, nickel, titanium, silver, etc. can be used. In addition, the thickness of the positive electrode current collector is generally 3μm to 500μm, and microscopic irregularities may be formed on the surface of the current collector to improve the adhesion of the positive electrode active material. For example, the positive electrode current collector can adopt various shapes, such as films, sheets, foils, meshes, porous bodies, foams, non-woven fabrics, etc.
[0086] In addition, the positive electrode active material layer may contain a conductive agent and a binder in addition to the above-mentioned positive electrode active material.
[0087] The conductive agent is used to provide conductivity to the electrode, wherein any conductive agent can be used without particular limitation, as long as the conductive agent has suitable electronic conductivity and does not cause adverse chemical changes in the battery. Specific examples of the conductive agent can be graphite, such as natural graphite or artificial graphite; carbon-based materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber and carbon nanotubes; metal powder or metal fiber, such as copper, nickel, aluminum and silver; conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium oxide; or conductive polymers, such as polyphenylene derivatives, any one of which or a mixture of two or more can be used. Based on the total weight of the positive electrode active material layer, the content of the conductive agent can generally be 1% by weight to 30% by weight, preferably 1% by weight to 20% by weight, and more preferably 1% by weight to 10% by weight.
[0088] The binder can improve the bonding force between the positive active material particles and the bonding force between the positive active material and the positive current collector. Specific examples of the binder can be polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber or its various copolymers, any one of which or a mixture of two or more can be used. Based on the gross weight of the positive active material layer, the content of the binder can be 1% by weight to 30% by weight, preferably 1% by weight to 20% by weight, more preferably 1% by weight to 10% by weight.
[0089] The positive electrode can be prepared according to a conventional method for preparing a positive electrode. For example, the positive electrode can be prepared by mixing a positive electrode active material, a binder, and / or a conductive agent in a solvent to prepare a positive electrode slurry, coating the slurry on a positive electrode current collector, and then drying and rolling the coated positive electrode current collector. In this case, the types and amounts of the positive electrode active material, binder, and conductive agent are the same as those described above.
[0090] The solvent may be a commonly used solvent in the art. The solvent may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone or water, any one of which or a mixture of two or more thereof may be used. Taking into account the coating thickness and manufacturing yield of the slurry, if the solvent can dissolve or disperse the positive electrode active material, the conductive agent and the binder, and can have a viscosity that can provide excellent thickness uniformity during the subsequent coating of the positive electrode, then the amount of the solvent is sufficient.
[0091] As another method, the positive electrode may be prepared by casting the positive electrode slurry on a separate support and then laminating the film peeled from the support on a positive electrode current collector.
[0092] lithium secondary batteries
[0093] Next, the lithium secondary battery of the present invention will be described.
[0094] The lithium secondary battery of the present invention comprises the positive electrode of the present invention. Specifically, the lithium secondary battery comprises a positive electrode, a negative electrode arranged to face the positive electrode, a separator arranged between the positive electrode and the negative electrode, and an electrolyte, and the positive electrode is the same as described above. In addition, the lithium secondary battery may optionally include a battery container for accommodating the electrode assembly of the positive electrode, the negative electrode and the separator, and a sealing member for sealing the battery container.
[0095] In a lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector.
[0096] The negative electrode current collector is not particularly limited, as long as it has high conductivity and does not cause adverse chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, or copper or stainless steel surface-treated with one of carbon, nickel, titanium, or silver, or aluminum-cadmium alloys, can be used. Furthermore, the negative electrode current collector typically has a thickness of 3 to 500 μm. Similar to the positive electrode current collector, microscopic irregularities may be formed on the current collector surface to improve adhesion of the negative electrode active material. For example, the negative electrode current collector can take various shapes, such as films, sheets, foils, meshes, porous bodies, foams, and non-woven fabrics.
[0097] The negative electrode active material layer optionally contains a binder and a conductive agent in addition to the negative electrode active material.
[0098] Compounds that can reversibly intercalate and deintercalate lithium can be used as negative electrode active materials. Specific examples of negative electrode active materials include: carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fibers, and amorphous carbon; metal substances that can be alloyed with lithium, such as silicon (Si), aluminum (Al), tin (Sn), lead (Pb), zinc (Zn), bismuth (Bi), indium (In), magnesium (Mg), gallium (Ga), cadmium (Cd), Si alloys, Sn alloys, or Al alloys; metal oxides that can be doped with and dedoped with lithium, such as SiO β (0<β<2), SnO2, vanadium oxide and lithium vanadium oxide; or a composite comprising a metal substance and a carbonaceous material, such as a Si-C composite or a Sn-C composite, and any one thereof or a mixture of two or more thereof may be used.
[0099] In addition, a metallic lithium thin film can be used as a negative electrode active material. In addition, low-crystalline carbon and high-crystalline carbon can be used as carbon materials. Typical examples of low-crystalline carbon can be soft carbon and hard carbon, and typical examples of high-crystalline carbon can be irregular, planar, flaky, spherical or fibrous natural graphite or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fibers, mesophase carbon microbeads, mesophase pitch and high-temperature sintered carbon, such as coke derived from petroleum or coal tar pitch.
[0100] The conductive agent is used to provide conductivity to the electrode, wherein any conductive agent can be used without particular limitation, as long as the conductive agent has suitable electronic conductivity and does not cause adverse chemical changes in the battery. Specific examples of the conductive agent can be graphite, such as natural graphite or artificial graphite; carbon-based materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber and carbon nanotubes; metal powder or metal fiber, such as copper, nickel, aluminum and silver; conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium oxide; or conductive polymers, such as polyphenylene derivatives, any one of which or a mixture of two or more can be used. The content of the conductive agent can generally be 1% by weight to 30% by weight, preferably 1% by weight to 20% by weight, and more preferably 1% by weight to 10% by weight, based on the total weight of the negative electrode active material layer.
[0101] The binder can improve the bonding force between the negative electrode active material particles and the bonding force between the negative electrode active material and the negative electrode current collector. Specific examples of the binder can be polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber or its various copolymers, any one of which or a mixture of two or more can be used. Based on the total weight of the negative electrode active material layer, the content of the binder can be 1% by weight to 30% by weight, preferably 1% by weight to 20% by weight, and more preferably 1% by weight to 10% by weight.
[0102] For example, the negative electrode active material layer can be prepared by coating a negative electrode collector with a negative electrode slurry containing a negative electrode active material and optionally a binder and a conductive agent and drying it, or by casting the negative electrode slurry on a separate support and then laminating a film separated from the support on the negative electrode collector.
[0103] In lithium secondary batteries, the diaphragm separates the negative electrode from the positive electrode and provides a path for the movement of lithium ions, wherein, as long as it is a diaphragm commonly used in lithium secondary batteries, it can be used as a diaphragm, without particular limitation, in particular, any diaphragm having a high moisture retention capacity for electrolytes and low resistance to electrolyte ion transfer can be used. Specifically, a porous polymer film can be used, for example, a porous polymer film prepared by a polyolefin-based polymer, such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer and an ethylene / methacrylate copolymer, or a two-layer or multilayer laminated structure thereof. In addition, a commonly used porous non-woven fabric can also be used, such as a non-woven fabric formed by high melting point glass fiber or polyethylene terephthalate fiber. In addition, a coated diaphragm comprising a ceramic component or a polymer material can also be used to ensure heat resistance or mechanical strength, and a diaphragm with a single layer or multilayer structure can also be optionally used.
[0104] In addition, the electrolyte used in the present invention may include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel polymer electrolytes, inorganic solid electrolytes or molten inorganic electrolytes that can be used to prepare lithium secondary batteries, but the present invention is not limited thereto.
[0105] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0106] Any organic solvent can be used as the organic solvent without particular limitation, as long as it can be used as a medium through which ions participating in the electrochemical reaction of the battery can move. Specifically, as the organic solvent, ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC) and propylene carbonate (PC); alcohol solvents such as ethanol and isopropanol; nitriles such as R-CN (wherein R is a linear, branched or cyclic C2-C20 hydrocarbon group, and may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes. Among these solvents, carbonate solvents are preferred, and more preferred are mixtures of cyclic carbonates (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant and low viscosity linear carbonate compounds (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) which can improve the charge / discharge performance of the battery.
[0107] Lithium salts can be used without particular limitation, as long as they are compounds that can provide lithium ions for lithium secondary batteries. Specifically, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2 can be used as lithium salts. The concentration range of the lithium salt can be 0.1M to 5.0M, preferably 0.1M to 3.0M. If the concentration of the lithium salt is within the above range, since the electrolyte can have suitable conductivity and viscosity, excellent electrolyte performance can be obtained, and lithium ions can be efficiently moved.
[0108] In order to improve the life characteristics of the battery, suppress the reduction of the battery capacity, improve the discharge capacity of the battery, additives can be further added to the electrolyte. For example, as additives, halogenated alkylene carbonate compounds (such as difluoroethylene carbonate), pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexamethylphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N, N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrroles, 2-methoxyethanol or aluminum chloride can be used alone or in the form of their mixtures, but the present invention is not limited thereto. Based on the gross weight of the electrolyte, the content of the additive can be 0.1 weight % to 10 weight %, preferably 0.1 weight % to 5 weight %.
[0109] As described above, since the lithium secondary battery including the positive electrode active material of the present invention stably exhibits excellent capacity characteristics, output characteristics and life characteristics, the lithium secondary battery is suitable for portable devices such as mobile phones, notebook computers, digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0110] Therefore, according to another embodiment of the present invention, a battery pack including the above-mentioned lithium secondary battery as a unit cell and a battery pack including the battery pack are provided.
[0111] The battery pack or battery package can be used as a power source for at least one of the following large and medium-sized devices: power tools; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); and power storage systems.
[0112] Hereinafter, the embodiments of the present invention will be described in detail in a manner that a person skilled in the art can easily implement the present invention. However, the present invention can be implemented in many different forms and should not be construed as being limited to the embodiments set forth herein.
[0113] Example 1
[0114] Li2O, Li2O2, MnO, MnF2, and TiO2 were added to a PM200 high-energy instrument at a weight ratio of 0.0510:0.2050:0.6118:0.1012:0.0432, and then 10 5mm stainless steel balls and 5 10mm stainless steel balls were added per 1g batch, and dry milling was carried out at 450rpm for 33h to synthesize Li 1.05 Mn 0.90 Ti 0.05 O 1.8 F 0.2 .
[0115] Synthetic Li 1.05 Mn 0.90 Ti 0.05 O 1.8 F 0.2 The differential scanning electron microscopy images of the powders are shown in Figure 2. Figure 1 As shown. Figure 1 It can be confirmed that the synthesized Li 1.05 Mn 0.90 Ti 0.05 O 1.8 F 0.2 It is in the form of secondary particles aggregated from primary particles with a particle size of 50 nm to 300 nm.
[0116] Example 2
[0117] Li2O, Li2O2, MnO, MnF2, and TiO2 were added to a PM200 high-energy instrument at a weight ratio of 0.0999:0.1302:0.5117:0.1026:0.1665, and then 10 5mm stainless steel balls and 5 10mm stainless steel balls were added per 1g batch, and dry milling was carried out at 450rpm for 33h to synthesize Li 1.05 Mn 0.76 Ti 0.19 O 1.8 F 0.2 .
[0118] Synthetic Li 1.05 Mn 0.76 Ti 0.19 O 1.8 F 0.2 The differential scanning electron microscopy images of the powders are shown in Figure 2. Figure 2 As shown. Figure 2 It can be confirmed that the synthesized Li 1.05 Mn 0.76 Ti 0.19 O 1.8 F0.2 It is in the form of secondary particles aggregated from primary particles with a particle size of 50 nm to 300 nm.
[0119] Comparative Example
[0120] Li2MnO3, Mn2O3, MnO2 and MnF2 were added to the PM200 high energy instrument at a weight ratio of 0.6029:0.2803:0.0392:0.0856, and then 10 5mm stainless steel balls and 5 10mm stainless steel balls were added per 1g batch, and dry milling was carried out at 450rpm for 33h to synthesize Li 0.89 Mn 0.80 O 1.85 F 0.15 .
[0121] Synthetic Li 0.89 Mn 0.80 O 1.85 F 0.15 The differential scanning electron microscopy images of the powders are shown in Figure 2. Figure 3 As shown. Figure 3 It can be confirmed that the synthesized Li 0.89 Mn 0.80 O 1.85 F 0.15 It is in the form of secondary particles aggregated from primary particles with a particle size of 50 nm to 300 nm.
[0122] Example 3
[0123] Li2MnO3, Mn2O3, MnO2, MnF2 and TiO2 were added to the PM200 high energy instrument at a weight ratio of 0.6068:0.0394:0.2023:0.0861:0.0736, and then 10 5mm stainless steel balls and 5 10mm stainless steel balls were added per 1g batch, and dry milling was carried out at 450rpm for 33h to synthesize Li 0.89 Mn 0.725 Ti 0.075 O 1.85 F 0.15 .
[0124] Synthetic Li 0.89 Mn 0.725 Ti 0.075 O 1.85 F 0.15 The differential scanning electron microscopy images of the powders are shown in Figure 2. Figure 4 As shown. Figure 4 It can be confirmed that the synthesized Li 0.89 Mn 0.725 Ti 0.075 O 1.85 F0.15 It is in the form of secondary particles aggregated from primary particles with a particle size of 50 nm to 300 nm.
[0125] Example 4
[0126] Li2MnO3, Mn2O3, MnO2, MnF2 and TiO2 were added to the PM200 high energy instrument at a weight ratio of 0.6107:0.0397:0.1232:0.0867:0.0148, and then 10 5mm stainless steel balls and 5 10mm stainless steel balls were added per 1g batch, and dry milling was carried out at 450rpm for 33h to synthesize Li 0.89 Mn 0.65 Ti 0.15 O 1.85 F 0.15 .
[0127] Synthetic Li 0.89 Mn 0.65 Ti 0.15 O 1.85 F 0.15 The differential scanning electron microscopy images of the powders are shown in Figure 2. Figure 5 As shown. Figure 5 It can be confirmed that the synthesized Li 0.89 Mn 0.65 Ti 0.15 O 1.85 F 0.15 It is in the form of secondary particles aggregated from primary particles with a particle size of 50 nm to 300 nm.
[0128] Experimental Example 1: Evaluation of Lifespan Characteristics
[0129] Each of the lithium manganese-based oxyhalides prepared in Examples 1 to 4 and Comparative Examples was added to a Premium Line 7 instrument of FRISTCH GmbH with SUPER P at a weight ratio of 7:2, and then mixed at 300 rpm for 30 minutes to allow SUPER P to coat the surface of the lithium manganese-based oxyhalide, thereby preparing a positive electrode active material.
[0130] The prepared positive electrode active material, conductive agent (SUPER P) and binder (PVDF 5120) were mixed in N-methylpyrrolidone (NMP) at a weight ratio of 7:2:1 to prepare a positive electrode material mixture, and then an aluminum current collector was coated with the positive electrode material mixture, dried, and then roll-pressed to prepare a positive electrode.
[0131] A lithium metal foil with a thickness of 0.2 mm was used as the negative electrode.
[0132] An electrode assembly was prepared by placing a separator between the positive electrode and the negative electrode prepared above, inserting the electrode assembly into a battery case, and then injecting an electrolyte to prepare a lithium secondary battery. The electrolyte was prepared by dissolving LiPF6 at a concentration of 1 M in a mixed organic solvent of ethylene carbonate (EC):dimethyl carbonate (DMC) in a volume ratio of 1:1.
[0133] Each lithium secondary battery prepared above was charged to 4.8V at 0.1C in constant current-constant voltage (CC-CV) mode at 25°C, and the CV mode was maintained until the charging current was below 0.05C. Each lithium secondary battery was discharged to 1.5V at a constant current of 0.1C. This process was set as one cycle. 30 or 50 charge and discharge cycles were performed, and the discharge capacity was measured to evaluate the life characteristics. Measurement results Figure 6 and Figure 7 shown.
[0134] Figure 6 is a graph showing the life characteristics of lithium secondary batteries using the lithium manganese-based oxyhalides synthesized in Examples 1 and 2, Figure 7 : is a graph showing the life characteristics of lithium secondary batteries using the lithium manganese-based oxyhalides synthesized in Comparative Example and Examples 3 and 4.
[0135] like Figure 6 and Figure 7 As shown, the lithium secondary batteries using the Ti-doped lithium manganese-based oxyhalides of Examples 1 to 4 have better lifespan characteristics than the lithium secondary battery using the undoped lithium manganese-based oxyhalides of the comparative example.
[0136] Experimental Example 2
[0137] The crystal structure of the lithium manganese-based oxyhalide synthesized in Example 4 was measured by high-resolution transmission electron microscopy (HR-TEM) analysis and selected area electron diffraction (SAED) analysis.
[0138] The measurement results are as follows Figure 8 shown. Figure 8 (A) is a high-resolution transmission electron microscopy (HR-TEM) image of the lithium manganese-based oxyhalide synthesized in Example 4, Figure 8 (B) is the measurement result of the SAED spectrum of the lithium manganese-based halide oxide synthesized in Example 4.
[0139] refer to Figure 8 , it can be confirmed that the lithium manganese-based oxyhalide in Example 4 has a multiphase mixed with a disordered rock salt structure (DRX), a layered rock salt structure, and a spinel structure.
[0140] Experimental Example 3
[0141] The X-ray diffraction patterns of the lithium manganese-based oxyhalides synthesized in Comparative Example and Examples 3 to 4 were measured. Figures 9 to 11 shown. Figure 9 is the X-ray diffraction data of the comparative example, Figure 10 is the X-ray diffraction data of Example 3, Figure 11 This is the X-ray diffraction data of Example 4.
[0142] Reference Figures 9 to 11 , it can be confirmed that for the Ti-doped lithium manganese-based oxyhalides of Examples 3 and 4, (400) R Peak ratio (111) S The peak is more significant, but for the comparative example of undoped Ti lithium manganese-based oxyhalide, (400) R Fenghe(111) S The peak intensities are similar. Specifically, I(400) of Example 3 R / I(111) S The ratio is 1.95, and I(400) of Example 4 R / I(111) S The ratio is 1.15, and the I(400) of Comparative Example 2 R / I(111) S The ratio is 0.95.
[0143] In addition, the ratio of spinel phase to rock salt phase (disordered rock salt phase + layered rock salt phase) was measured by XRD data analysis. The results showed that the ratio of spinel phase in Example 3 was 72.6%, the ratio of spinel phase in Example 4 was 60.5%, and the ratio of spinel phase in the comparative example was 76.4%. It can be confirmed that when titanium is doped, the ratio of spinel phase decreases.
Claims
1. A positive electrode active material comprising a lithium manganese-based oxyhalide having a composition represented by Formula 1 and having a disordered rock salt structure, [Formula 1] Li 0.5+a Mn b M c O d X e in, In formula 1, M is at least one selected from titanium (Ti), nickel (Ni), zirconium (Zr), vanadium (V), cobalt (Co), tin (Sn), iron (Fe), iridium (Ir), chromium (Cr), lead (Pb) and ruthenium (Ru), X is a halogen element, 0 <a≤0.7,0.5≤b<1,0<c≤b / 2,1.5≤d≤1.9,0.1≤e≤0.5,d+e≤2。 2. The positive electrode active material according to claim 1, wherein The molar ratio of the cationic element to the anionic element in the lithium manganese-based oxyhalide is 0.75:1 to 1:
1.
3. The positive electrode active material according to claim 1, wherein In Formula 1, M is Ti and X is F.
4. The positive electrode active material according to claim 1, wherein The primary particle size of the lithium manganese-based oxyhalide is 50 nm to 300 nm.
5. The positive electrode active material according to claim 1, wherein The lithium manganese-based oxyhalide has a composition represented by Formula 1-1, [Formula 1-1] Li 1+a1 Mn b1 M c1 O 2-e1 X e1 Among them, in formula 1-1: M is at least one selected from Ti, Ni, Zr, V, Co, Sn, Fe, Ir, Cr, Pb and Ru, X is a halogen element, 0 <a1≤0.2,0.5≤b1<1,0<c1≤b1 / 2,0.1≤e1≤1。 6. The positive electrode active material according to claim 5, wherein The lithium manganese-based oxyhalide has a single-phase structure with a disordered rock salt structure.
7. The positive electrode active material according to claim 1, wherein The lithium manganese-based oxyhalide has a composition represented by Formula 1-2, [Formula 1-2] Li 0.5+a2 Mn b2 M c2 O 2-e2 X e2 Wherein, in Formula-1-2, M is at least one selected from Ti, Ni, Zr, V, Co, Sn, Fe, Ir, Cr, Pb and Ru, X is a halogen element, 0 <a2<0.5,0.5≤b2<1,0<c2≤b2 / 2,0.1≤e2≤0.5。 8. The positive electrode active material according to claim 7, wherein The lithium manganese-based oxyhalide has a multiphase structure in which a disordered rock salt structure, a layered rock salt structure and a spinel structure are mixed.
9. The positive electrode active material according to claim 8, wherein The proportion of the spinel structure in the lithium manganese-based oxyhalide is less than 75%.
10. The positive electrode active material according to claim 7, wherein I(400) of the lithium manganese-based oxyhalide R / I(111) S , that is, the peak intensity of the (400) plane I(400) R The peak intensity of the (111) surface is I(111) S The ratio is greater than 1. 11 . A positive electrode comprising the positive electrode active material according to claim 1 .
12. A lithium secondary battery comprising the positive electrode according to claim 11.
Citation Information
Patent Citations
Apparatus for preventing from bridge falling accident
KR1020220050421A