Method for forming electromagnetic wave shield, method for manufacturing structure, and structure

By forming a conductive layer with multiple openings on the surface and side of the electromagnetic wave shielding layer and covering the insulating layer, the problem of side interference leakage and insufficient durability of the electromagnetic wave shielding layer in the prior art is solved, and better shielding performance and durability are achieved sex.

CN119073010APending Publication Date: 2024-12-03RICOH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380025877.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-11-30
Filing Date
2023-03-13
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing electromagnetic wave shielding layer has problems with side interference leakage and durability, resulting in poor shielding effect and insufficient adhesive strength, especially in thinner situations.

Method used

By forming a conductive layer with multiple openings on the surface and sides of the object and covering the insulating layer, a continuous shielding layer is formed, reducing the risk of peeling and cracking, and improving adhesive strength and shielding performance.

Benefits of technology

Enhanced shielding performance and durability of electromagnetic wave shielding, reduce noise leakage, improve physical durability, and save resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119073010A_ABST
    Figure CN119073010A_ABST
Patent Text Reader

Abstract

A method of forming an electromagnetic wave shield includes forming a conductive layer and forming an insulating layer. The formation of the conductive layer means that a conductive layer having a plurality of openings is formed on the upper surface and the side surface of the surface of the object. And forming an insulating layer which is continuously formed from the surface of the conductive layer to the surface of the object through the plurality of openings, and which is adhered to the surface of the object.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method of forming an electromagnetic wave shield, a method of manufacturing a structure, and the structure. Background Art

[0002] Patent document 1 (PTL 1) describes a semiconductor integrated circuit which is mounted on a printed circuit board having a wiring pattern formed thereon and is connected to the wiring pattern through a plurality of terminals. The semiconductor integrated circuit includes a shielding portion for shielding electromagnetic wave interference, the shielding portion being provided to cover a surface of the semiconductor integrated circuit on a side opposite to the printed circuit board, and a ground for connecting the shielding portion and the printed circuit board.

[0003] Patent Document 2 (PTL 2) describes an electromagnetic interference (EMI) shield having a conductive layer including inkjet printing.

[0004] Patent document 3 (PTL 3) describes an electromagnetic wave shielding material 1, which includes a (polyethylene terephthalate) PET substrate layer, a primer layer, an ink receiving layer 6 and a grid-like electromagnetic wave shielding mesh layer. The primer layer and the ink receiving layer are arranged on one surface of the PET substrate layer. A grid-like electromagnetic wave shielding mesh layer formed by screen printing and firing a conductive paste-like ink is arranged on the ink receiving layer.

[0005] Citation List

[0006] Patent Literature

[0007] [PTL 1]

[0008] Japanese Unexamined Patent Application No. 2001-127211

[0009] [PTL 2]

[0010] USA9282630

[0011] [PTL 3]

[0012] Japanese Patent No. 5703050 Summary of the invention

[0013] Technical issues

[0014] An object of the present invention is to enhance the shielding performance and durability of electromagnetic wave shielding.

[0015] Solutions to the problem

[0016] According to an embodiment of the present invention, a method for forming an electromagnetic wave shield includes forming a conductive layer and forming an insulating layer. Forming a conductive layer means forming a conductive layer having a plurality of openings on the upper surface and the side surface of an object. Forming an insulating layer, the insulating layer is continuously formed from the surface of the conductive layer through the plurality of openings to the surface of the object, and is bonded to the surface of the object.

[0017] Effects of the Invention

[0018] According to the embodiments of the present invention, the shielding performance and durability of the electromagnetic wave shield can be enhanced. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] A more complete understanding of embodiments of the present invention and many of its attendant advantages and features may be readily obtained and appreciated by the following detailed description taken in conjunction with the accompanying drawings.

[0020] Figures 1A to 1C It is an explanatory diagram of an electronic device involved in an embodiment of the present invention.

[0021] Figure 2A and 2B It is an explanatory diagram of another electronic device involved in the embodiment of the present invention.

[0022] Figure 3A and 3B It is an explanatory diagram of a method of forming an electromagnetic wave shield according to an embodiment of the present invention.

[0023] Figure 4A and 4B It is a cross-sectional view of an electromagnetic shield according to an embodiment of the present invention.

[0024] Figure 5A and 5B This is a flowchart showing an example of a process of forming an electromagnetic shield according to an embodiment of the present invention.

[0025] Fig. 6A and 6B These are diagrams respectively showing the printed pattern A and the printed pattern B of Table 4 in the electromagnetic shield according to the example of the present invention.

[0026] Figure 7 It is a figure which shows the printing pattern C of Table 4 in the electromagnetic shield which concerns on Example of this invention.

[0027] Figure 8 This is a diagram showing an example of the printed pattern D of Table 4 in the electromagnetic shield according to the embodiment of the present invention.

[0028] Fig. 9 It is a diagram showing another example of the printed pattern D of Table 4 in the electromagnetic shield according to the embodiment of the present invention.

[0029] Fig.10 It is a diagram showing a method of evaluating the electromagnetic shielding effect according to an embodiment of the present invention.

[0030] The accompanying drawings are intended to illustrate embodiments of the present invention and should not be interpreted as limiting the scope thereof. Unless otherwise explicitly stated, the accompanying drawings should not be considered to be drawn to scale. Moreover, in multiple views, the same or similar reference numerals represent the same or similar components. DETAILED DESCRIPTION

[0031] In describing the embodiments shown in the drawings, specific terms are used for clarity. However, the disclosure of this specification is not intended to be limited to the specific terms selected, and it should be understood that each specific element includes all technical equivalents having similar functions, operating in a similar manner and achieving similar results.

[0032] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. As used herein, the singular forms "a", "an" and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise.

[0033] As is known, high reliability is required for a printed wiring board (PWB) without electronic components used for the fifth generation (5G) of high-speed communication or automatic operation, a printed circuit board (PCB) in a working state as an electronic circuit on which electronic components are soldered, and a technology for controlling electromagnetic waves generated from such electronic components or wiring. In addition, as is known, with the miniaturization and lightness of products, thinning and lightness of PCBs and the like, as well as a technology for shielding electromagnetic waves from PCBs and electronic components used on the PCBs, are also required.

[0034] That is, the structure serving as an electromagnetic wave shield includes electronic components such as integrated circuit (IC) chips, capacitors, resistors, diodes or solenoids, or semiconductor packages that house electronic components in electronic devices, and these electronic components, semiconductor packages or structures are covered with conductors such as shielding films, metal covers, conductive coating materials, or electromagnetic wave absorbers.

[0035] Figures 1A to 1C It is an explanatory diagram of an electronic device involved in an embodiment of the present invention.

[0036] like Figure 1A As shown, the electronic device 1 includes a semiconductor package 110 having an outer peripheral surface 100, a shielding layer 200 and a protective layer 300. The shielding layer 200 and the protective layer 300 are arranged on the outer peripheral surface 100. The shielding layer 200 is electrically connected to the ground 100G included in the semiconductor package 110. The protective layer 300 can be omitted, or can be formed integrally with the shielding layer 200.

[0037] like Figure 1B As shown, Figure 1A The shielding layer 200 in the embodiment includes a conductive layer 210 formed in a predetermined pattern on the upper surface and side surfaces of the outer peripheral surface 100 of the target semiconductor package 110 , and an insulating layer 230 covering the conductive layer 210 .

[0038] exist Figure 1B In the structure of Figure 1C As shown, a horizontally arranged inkjet head 400 and an inkjet head 401 and an inkjet head 402 arranged tilted to the left and right relative to an object respectively discharge ink 500, ink 501 and ink 502 each containing a conductive material onto the upper and side surfaces of the peripheral surface 100 of the semiconductor package 110, thereby forming a shielding layer 200 on the upper and side surfaces of the peripheral surface 100.

[0039] Here, inks 500, 501, and 502 are each an exemplary liquid composition containing a conductive material, and inkjet heads 400, 401, and 402 are each an exemplary applicator for applicating the corresponding liquid composition. Shielding layer 200 is an exemplary conductive layer.

[0040] Figure 2A and 2B It is an explanatory diagram of another electronic device involved in this embodiment.

[0041] like Figure 2A As shown, the electronic device 1 includes an electronic component 120 and a substrate 130. The electronic component 120 is provided with a connector 125, and a wiring 135 is provided on the substrate 130. The electronic component 120 is attached to the substrate 130 so that the connector 125 and the wiring 135 are electrically connected.

[0042] The electronic component 120 has an outer peripheral surface 100, on which a shielding layer 200 is provided. The shielding layer 200 is connected to the ground 100G of the electronic component 120. The electronic component 120 is attached to the substrate 130 so that the wiring 145 provided on the substrate 130 and the ground 100G provided on the electronic component 120 are electrically connected through the connector 155. The electronic component 120 is an exemplary electronic module. Alternatively, the shielding layer 200 may also be provided separately from the electronic component 120. In this case, the structure includes the electronic component 120 and the shielding layer 200.

[0043] like Figure 2B As shown, in this embodiment, the inkjet head 400, the inkjet head 401 and the inkjet head 402 respectively discharge ink 500, ink 501 and ink 502 each containing a conductive material onto the upper and side surfaces of the peripheral surface 100 of the electronic component 120, thereby forming a shielding layer 200 on the upper and side surfaces of the peripheral surface 100.

[0044] Here, in order to save space, reduce weight, and improve productivity, it is known to directly coat a conductive material on an electronic component by an inkjet technique to form an electromagnetic wave shield.

[0045] The specification of US Pat. No. 9,282,630 describes an EMI shielding in which the conductive layer includes inkjet printing. However, there is no mention of shielding ineffectiveness due to interference leakage from the sides of the shielding layer, or no description of the side coating of the shielding layer 200 and the peeling or cracking of the side coating.

[0046] The smaller the volume resistivity of the shielding layer 200 is, the better the shielding effect is, and the film thickness of the shielding layer 200 can be made thinner. In order to form the shielding layer 200 with a small volume resistivity, for example, coating and heating are required.

[0047] Here, there is a disadvantage that the stress generated by the thermal expansion difference between the upper and lower bonding surfaces of the shielding layer 200 due to the heat generated when the shielding layer 200 is formed or when the electronic device 1 is used may cause damage to the shielding layer 200 such as peeling or cracking, and the bonding strength of the shielding layer 200 itself is insufficient, resulting in poor durability when the film is thinned.

[0048] The purpose of this embodiment is to reduce the leakage of noise from the sides of the shielding layer 200 and the peeling and cracking of the sides of the shielding layer 200. More specifically, the purpose of this embodiment is to improve the shielding effect of the conductive layer as an electromagnetic wave shielding layer directly formed on the electronic component by inkjet technology, to improve the physical durability of the shielding layer by improving the adhesive strength, to reduce the weight by thinning the conductive layer, and to save resources by pattern coating of the conductive layer.

[0049] Figure 3A and 3B It is an explanatory diagram of the method of forming an electromagnetic wave shield according to the present embodiment.

[0050] like Figure 3A As shown, the inkjet head 400 is arranged to discharge ink 500 in the normal direction of the upper surface 102 of the outer peripheral surface 100 of the substrate, and the inkjet heads 401 and 402 are arranged on the left and right of the figure with the inkjet head 400 as the center, and are inclined relative to the inkjet head 400, so as to discharge ink 501 and 502 in the direction intersecting the upper surface 102 and the side surface 104 of the outer peripheral surface 100. Here, because the position on the outer peripheral surface 100 changes depending on the environment such as temperature and airflow, the inkjet heads 401 and 402 may not be arranged symmetrically with respect to the figure with the inkjet head 400 as the center.

[0051] When the carrier 600 moves in the direction of the arrow in the figure, the inkjet heads 400, 401 and 402 apply ink 500, 501 and 502 to the outer peripheral surface 100 placed on the carrier 600, thereby forming a shielding layer 250 on the upper surface 102 of the outer peripheral surface 100 and forming a shielding layer 260 on the side surface 104 of the outer peripheral surface.

[0052] Figure 3B This is a diagram of an object placed on the mounting table 600 as viewed from above. The object is placed so as to form a rhombus 100H with respect to the mounting table 600 .

[0053] Figure 4A and 4B It is a cross-sectional view of the electromagnetic wave shield according to this embodiment.

[0054] The shielding layer 200 of this embodiment includes at least a conductive layer 210 for reflecting electromagnetic waves and an insulating layer 230 for protecting the conductive layer 210 and having insulating properties. The insulating layer 230 may be configured as Figures 1A to 2B The protective layer 300 shown in FIG. Figures 1A to 2B In the case where the target electronic circuit element has a conductor connected to an electronic circuit other than the ground 100G, a primer layer 150 made of an insulating resin is provided, and a conductive layer and an insulating layer are provided in order on the primer layer 150 to ensure insulation.

[0055] exist Figure 4A In the embodiment, the conductive layer 210 included in the shielding layer 200 is provided on the upper surface and the side surface of the outer peripheral surface 100 of the base material, and the conductive layer 210 has a plurality of openings 220 .

[0056] The insulating layer 230 included in the shielding layer 200 includes a covering portion 234 covering the columnar object 212 of the conductive layer 210 having multiple openings 220 and a filling portion 232 continuous with the covering portion 234, wherein the multiple openings 220 are filled with the filling portion 232, and the insulating layer 230 is bonded to the outer peripheral surface 100 through the filling portion 232.

[0057] exist Figure 4B In the embodiment, the outer peripheral surface 100 has an insulating primer layer 150 on the surface of the semiconductor package 110 or the electronic element 120 , the conductive layer 210 included in the shielding layer 200 is disposed on the surface of the primer layer 150 , and the conductive layer 210 has a plurality of openings 220 .

[0058] The insulating layer 230 included in the shielding layer 200 includes a covering portion 234 covering the column 212 of the conductive layer 210 having multiple openings 220 and a filling portion 232 continuous with the covering portion 234, wherein the multiple openings 220 are filled with the filling portion 232, and the insulating layer 230 is bonded to the surface of the base coating 150 through the filling portion 232.

[0059] As described above, in this embodiment, the shielding layer 200 can be prevented from peeling off and breaking by sandwiching the conductive layer 210 between the outer peripheral surface 100 of the base material or the surface of the primer layer 150 integral with the filling portion 232 and the covering portion 234 .

[0060] The thickness of the conductive layer 210 of the present embodiment is 10 μm or less. This is because the effect of electromagnetic shielding is sufficient at a thickness of 1 μm or less, and a greater thickness will increase the cost. In the inkjet coating method, the coating amount can be freely adjusted. Therefore, even if the peripheral surface 100 of the substrate (electronic substrate) has irregularities, the thickness of the conductive layer 210, the shielding layer 200 and the filling portion 232 hardly changes. Thus, sufficient shielding effect and adhesion can be maintained.

[0061] Furthermore, the solid content of each ink including the conductive material for forming the conductive layer 210 is 50% or less, which makes it difficult to form an inclined shape with a thin film thickness.

[0062] Figure 5A and 5B This is a flowchart for explaining the formation of the electromagnetic wave shield according to the present embodiment. Figure 5A Indicates the formation Figure 4A Method of shielding layer 200 in the embodiment of the present invention.

[0063] First, a substrate having an outer peripheral surface 100 is set as a workpiece in an inkjet device (step S1), and then the workpiece is cleaned (step S2). As a method for cleaning the workpiece, there is air purging cleaning using air pressure, but general organic solvents (e.g., alcohol), adhesive roller cleaning by bonding, plasma cleaning, etc. can also be used.

[0064] Next, an inkjet printing pattern is prepared for the conductive material (step S3). In the inkjet printing pattern generation, a continuous printing pattern of a conductive layer connected to the ground is generated correspondingly to the outer peripheral surface 100 of the substrate provided with electromagnetic wave shielding.

[0065] Then, if Figure 3A and Figure 3B As shown, the inkjet head 400 applies the ink 500 containing the conductive material to the upper surface 102 of the outer peripheral surface 100 of the substrate placed on the mounting table 600 (step S4), and then thermally cures the conductive material to form the conductive layer 210 (step S5).

[0066] Here, the application of ink 500 in step S4 is performed on the inkjet printing pattern generated in step S3. In step S5, the volume resistance of the conductive layer is reduced by heating.

[0067] In step S5, the substrate having the peripheral surface 100 may be heated before imparting, or may be subjected to a heating batch process after imparting. In order to obtain stability in the volume and speed of the droplets discharged during inkjet imparting, the inkjet head and the ink supply system may be heated to control the viscosity of the ink 500.

[0068] Next, the film state of the conductive layer 210, such as the coating position and film thickness, is inspected for appearance and film thickness (step S6).

[0069] Then, if Figure 3A and Figure 3B As shown, the inkjet head 400 applies the ink 500 containing the insulating material to the upper surface 102 of the outer peripheral surface 100 of the substrate placed on the mounting table 600 (step S7). The insulating material is cured by ultraviolet (UV) exposure (step S8), and then the insulating material is thermally cured to form the insulating layer 230 (step S9).

[0070] Finally, the film state of the insulating layer 230, such as the coating position and film thickness, is inspected for appearance and film thickness (step S10 ).

[0071] Here, in the case where the insulating layer 230 does not require a printed pattern, it may be imparted using another technique such as dispensing or spraying in step S7 .

[0072] In the case of imparting an insulating material containing a UV curable resin, UV light irradiation is performed immediately after imparting, thereby being able to suppress the fluidity of the ink and impart the ink at a desired position with a desired film thickness without waste. In the case of UV light irradiation, UV light irradiation can be performed in a batch process after imparting, or can be performed while inkjet printing is performed by an inkjet head including a UV lamp or a light emitting diode (LED).

[0073] By heating and curing the insulating material containing the thermosetting resin, an electromagnetic wave shield with better adhesion, toughness and durability can be formed. In the heating, the substrate having the outer peripheral surface 100 may be heated before the ink is applied, or the heating batch process may be performed after the ink is applied.

[0074] Figure 5B It means forming Figure 4B The shielding layer 200 is used as a method. Figure 5B Steps S11, S12 and S17 to S24 in are similar to Figure 5ASteps S1 to S10 in the flowchart are not described, and therefore they are not described, and steps S13 to S16 will be described below.

[0075] After step S12, the inkjet head 400 imparts the ink 500 containing the insulating material to the surface of the semiconductor package 110 or the electronic component 120 placed on the mounting table 600 (step S13). The insulating material is cured by UV exposure (step S14), and then the insulating material is thermally cured to form the primer layer 150 (step S15).

[0076] Then, the film state of the primer layer 150, such as the coating position and film thickness, is inspected for appearance and film thickness (step S16).

[0077] In the case where the primer layer 150 does not require a printed pattern, it may be imparted using another technique such as dispensing or spraying in step S13.

[0078] In the case of imparting an insulating material containing a UV curing resin, UV light irradiation is performed immediately after imparting, thereby being able to suppress the fluidity of the ink, and being able to impart the ink at a desired position with a desired film thickness without waste. In the case of UV light irradiation, UV light irradiation can be performed in a batch process after imparting, or can be performed while inkjet printing is performed by an inkjet head including a UV lamp or a light emitting diode (LED). In this embodiment, regardless of the size and surface inconsistency of the object, the layer can be formed with high precision by inkjet printing and light irradiation. In addition, the shielding layer including the conductive layer can be partially modified in structure to have a variety of structures.

[0079] By heating the insulating material containing the thermosetting resin to cure it, an electromagnetic wave shield with better adhesion, toughness and durability can be formed. In the heating, the semiconductor package 110 or the electronic element 120 may be heated before the ink is applied, or the batch heating process may be performed after the ink is applied.

[0080] Embodiments of the conductive layer

[0081] The conductive layer 210 is formed by inkjet printing using metal nanoparticle ink (e.g., Smart Jet I manufactured by GenesInk, SR7000 manufactured by Bando, IJ100E manufactured by Future ink Corporation, and I40DM manufactured by Pvnancell) or organic metal ink (TC-IJ-010 manufactured by InkTec Co., Ltd.; and EI-1208 manufactured by Electronik). A pattern having a non-printing portion of a minimum size that is continuously connected in an area direction and serves as an electromagnetic wave shield is formed, and then inkjet printing is performed.

[0082] The major diameter of the non-printing opening in the inkjet printed pattern of the conductive layer 210 has a size of 1 to 2000 μm.

[0083] In the case of a larger opening, high-frequency electromagnetic waves cannot be shielded, and in the case of a smaller opening, the interlayer bonding effect of the insulating layer is weakened. Therefore, the durability of the shielding layer is deteriorated due to the thermal history, so that the long diameter of the opening is preferably 5 to 1500 μm, more preferably 10 to 1000 μm.

[0084] An electromagnetic wave shield having a semi-transparent mesh conductive layer with an opening area ratio of 40% or more can be used for touch panels and display screens. However, in this embodiment, an electromagnetic wave shield is formed on a component that generates electromagnetic waves. The purpose of this embodiment is to achieve a highly durable electromagnetic wave shield capable of shielding high-frequency electromagnetic waves by reducing the opening area ratio of the electromagnetic wave shield.

[0085] By forming a conductive layer in a continuous printing pattern and providing an insulating layer on the conductive layer having openings of any major diameter with an opening area ratio of less than 1 to 50%, more preferably less than 3 to 40%, a highly durable electromagnetic shielding layer corresponding to high frequencies can be realized.

[0086] As long as the inkjet printed pattern of the conductive layer is continuously connected in the area direction and like a ground, such as a grid structure or an error diffusion dither pattern, a pattern having any shape can be used to obtain a shielding effect and an increase in adhesion strength due to the interlayer between the insulating layer and the substrate.

[0087] Regarding shielding characteristics, a pattern having a jitter shape caused by error diffusion with a small periodicity has a smaller shielding leakage at a specific wavelength than a pattern having such a grid structure with a strong periodicity. Depending on the electromagnetic wave frequency to be shielded and the electromagnetic wave intensity, different conductive layer printing patterns can be combined in the same electromagnetic wave shield.

[0088] Any conductive layer printing pattern is preferably imparted to any position and portion having irregularities of 5 mm or less by inkjet printing.

[0089] After inkjet printing, the metal nanoparticle ink or organometallic ink is heated to a volume resistivity of 10e -3 Ω·cm or less, and becomes a conductive layer that fully reflects electromagnetic waves.

[0090] When the metal particles are reduced to 100nm or less, the melting point is lower than that of the metal body. Therefore, when the metal nanoparticle ink is heated, the ink solvent evaporates, causing the metal nanoparticles to concentrate. In addition, since the melting point is lowered due to the formation of nanoparticles, each surface of the metal nanoparticles melts and sintered at a temperature lower than the temperature of the body metal. As a result, a conductive bus is formed, and the volume resistivity of the conductive layer is reduced.

[0091] Since the metal nanoparticle ink reflects the concentrated state of the solvent volatilization after coating, it is fired. Therefore, it is preferable to uniformly coat the metal nanoparticle ink in a thin film to volatilize the solvent. For thin and uniform coating, the inkjet printing method that can make the ink particle size uniform is more excellent than the jet method with a wide ink particle distribution when coating.

[0092] The heating conditions after inkjet printing are 80 to 180°C and 10 to 60 minutes. When the volume resistivity of the conductive layer is further less than 10e -5 When the thickness is less than Ω·cm, electromagnetic waves are more easily reflected, so that the film thickness of the conductive layer can be reduced. As the metal nanoparticles, Au, Ag or Cu can be used. As the organic metal ink, metal salts such as Ag and Cu can be used.

[0093] When the conductive layer is made thicker, the conductive layer is easily broken during the film formation process. When the conductive layer is made too thin, the shielding performance deteriorates due to the skin effect caused by electromagnetic wave reflection. Therefore, the thickness of the conductive layer is preferably 0.01 to 20 μm, more preferably 0.05 to 10 μm. The thinning of the conductive layer leads to a weight reduction of the shielding layer and resource saving of metal materials.

[0094] Insulation and base coating

[0095] As insulating ink for the insulating layer and the primer layer, UV-curing and / or heat-curing insulating ink can be used, such as PR-1258 (UV-curing and heat-curing type) manufactured by GOO CHEMICAL CO., LTD., IJSR4000 (UV-curing and heat-curing type) manufactured by TAIYO INK; PA-1210-35 (UV-curing type) manufactured by JNC Corporation.

[0096] Insulation layer

[0097] The insulating layer is formed by coating on the patterned conductive layer, and the insulating layer is bonded to the substrate, electronic component or primer through the opening of the conductive layer, and is bonded in a sandwich manner including the conductive layer, thereby improving the bonding strength of the conductive layer.

[0098] The insulating layer is formed on the conductive layer by a coating method such as inkjet printing, spraying or dispensing. When the opening of the conductive layer is very thin, it is disadvantageous that the opening is filled with the insulating layer. However, by inkjet printing, it is easy to fill the insulating layer at the opening with ink having excellent fluidity.

[0099] The insulating layer is preferably an insulating layer with good adhesion to the substrate or the primer layer, and is preferably a coating material having excellent mechanical strength and heat resistance and containing a UV curing or heat curing resin. In order to ensure adhesion to the substrate or the primer layer, the constituent component of the insulating layer is preferably a heat curing resin, more preferably a heat curing epoxy resin. In addition, such a constituent component of the insulating layer is preferably a UV curing resin to prevent wetting and diffusion of the coating material after coating the insulating layer.

[0100] When the insulating layer is composed of two components, a thermosetting resin and a UV-curing resin, UV irradiation and heating can prevent wetting diffusion and adhesion strength with the substrate or primer layer, and improve the durability of the shielding layer, thereby enabling precise alignment between the shielding layer and the electronic circuit components.

[0101] In the case where the insulating layer includes a thermosetting resin and a UV curing resin, the curing conditions include 100 to 2000 mJ / cm 2 of UV irradiation, heating at 130-180°C and for 10-60 minutes.

[0102] Base coating

[0103] In the case where the target electronic circuit constituent element has a conductor connected to the electronic circuit other than the ground connector, a primer layer made of an insulating resin is provided, and a conductive layer and an insulating layer are provided in order on the primer layer to ensure insulation.

[0104] The primer layer is formed on the electronic circuit constituent element by a coating method such as inkjet printing, spraying, or dispensing.

[0105] The primer layer needs to have adhesion to the electronic circuit components, the conductive layer and the insulating layer. Therefore, similar to the insulating layer, the primer layer preferably comprises a thermosetting resin, more preferably a thermosetting epoxy resin. In addition, in order to prevent the wetting and diffusion of the coating material after the primer layer is applied, the primer layer preferably comprises a UV curing resin.

[0106] When the primer layer is composed of two components, a thermosetting resin and a UV-curing resin, UV irradiation and heating can prevent wetting diffusion and the bonding strength with the substrate, the conductive layer and the insulating layer, and improve the durability of the shielding layer, thereby enabling precise alignment between the shielding layer and the electronic circuit components.

[0107] In the case where the insulating layer includes a thermosetting resin and a UV curing resin, the curing conditions include 100 to 2000 mJ / cm 2 of UV irradiation, heating at 130-180°C and for 10-60 minutes.

[0108] Table 1, including Table 1-1, Table 1-2 and Table 1-3, shows a substrate having an outer peripheral surface 100, a conductive layer, an insulating layer and Figure 4A Evaluation results of the electromagnetic wave shielding embodiments and comparative examples.

[0109] Table 1-1

[0110]

[0111] Table 1-2

[0112]

[0113] Table 1-3

[0114] Volume resistivity Adhesion Electromagnetic wave shielding effect Example 1 <![CDATA[10e -5 W,cm]]> very good good Example 2 <![CDATA[10e -5 W,cm]]> very good very good Example 3 <![CDATA[10e -5 W,cm]]> good very good Example 4 <![CDATA[10e -5 W,cm]]> very good good Example 5 <![CDATA[10e -5 W,cm]]> very good good Example 6 <![CDATA[10e -6 W,cm]]> very good very good Comparative Example 1 <![CDATA[10e -5 W,cm]]> Difference bad Comparative Example 2 <![CDATA[10e -2 W,cm]]> Difference bad Comparative Example 3 <![CDATA[10e -5 W,cm]]> Difference bad

[0115] Table 2 including Table 2-1 and Table 2-2 shows a substrate having an outer peripheral surface 100, a primer layer, a conductive layer, an insulating layer, and Figure 4B Evaluation results of the electromagnetic wave shielding embodiments and comparative examples.

[0116] Table 2-1

[0117]

[0118] Table 2-2

[0119] Conductive layer and protective layer Volume resistivity Adhesion Electromagnetic wave shielding effect Example 7 Example 1 <![CDATA[10e -5 W×cm]]> very good good Example 8 Example 1 <![CDATA[10e -5 W×cm]]> very good good Example 9 Example 1 <![CDATA[10e -5 W×cm]]> very good good Example 10 Example 1 <![CDATA[10e -5 W×cm]]> very good good Comparative Example 4 Comparative Example 1 <![CDATA[10e -5 W×cm]]> Difference bad Comparative Example 5 Comparative Example 1 <![CDATA[10e -5 W×cm]]> Difference bad Comparative Example 6 Comparative Example 1 <![CDATA[10e -5 W×cm]]> Difference bad Comparative Example 7 Comparative Example 1 <![CDATA[10e -5 W×cm]]> Difference bad

[0120] Table 3 shows the details of the substrate types A to E in Table 1 and Table 2.

[0121] Table 3

[0122]

[0123] Table 4 shows the details of the printing patterns A to E of the conductive layers in Table 1.

[0124] Table 4

[0125]

[0126] Fig. 6A and 6B The printed pattern A and the printed pattern B in Table 4 are respectively shown in the electromagnetic shield according to the present embodiment.

[0127] Fig. 6A and 6BThe mesh conductive layer 210 includes a connection Figure 4A and 4B The column 212 has a plurality of connecting rods 214 and a plurality of openings 220 surrounded by the plurality of connecting rods 214.

[0128] exist Fig. 6A In the case of the conductive layer 210 in FIG. 1 , the width of each of the plurality of tie bars 214 is 580 μm, each of the plurality of openings 220 is 1000 μm×1000 μm, and the opening area ratio is 40%.

[0129] exist Figure 6B In the case of the conductive layer 210 in FIG. 1 , the width of each of the plurality of tie bars 214 is 125 μm, each of the plurality of openings 220 is 100 μm×100 μm, and the opening area ratio is 20%.

[0130] Figure 7 The printed pattern C in Table 4 is shown in the electromagnetic shield according to the present embodiment.

[0131] Figure 7 The conductive layer 210 in the jitter shape has a plurality of openings 220 arranged in an uneven manner. Each of the plurality of openings 220 has a size of 10 μm×10 μm, a major diameter of 14 μm, and an opening area ratio of 2.8%.

[0132] In steps S3 and S17 of FIG. 5, Figure 7 The conductive layer 210 in the dither shape is set as a printed pattern of a combination of four pixels 240 having ink non-imparted areas at different positions, where 6×6 dots serve as one pixel and one dot in each pixel 240 serves as the ink non-imparted area.

[0133] Figure 8 The printed pattern D of Table 4 is shown in the electromagnetic shield according to the present embodiment.

[0134] Figure 8 The conductive layer 210 in the jitter shape has a plurality of openings 220 with inconsistent orientations. The major diameter of each of the plurality of openings 220 is 10 μm×100 μm, and the opening area ratio is 34.7%.

[0135] In steps S3 and S17 of FIG. 5, Figure 8 The conductive layer 210 in the dither shape is set as a printed pattern of a combination of four pixels 240 having ink non-imparted areas with different orientations, wherein 12×12 dots serve as one pixel and 10 dots×5 in each pixel 240 serve as the ink non-imparted area.

[0136] Fig. 9Another example of the printed pattern D in Table 4 in the electromagnetic shield according to the present embodiment is shown.

[0137] Fig. 9 The conductive layer 210 in the jitter shape has a plurality of openings 220 with inconsistent orientations. The major diameter of each of the plurality of openings 220 is 99 μm, and the opening area ratio is 34.7%.

[0138] In steps S3 and S17 of Figure 5, the conductive layer 210 of the jitter shape shown in Figure 9 is set as a printed pattern of a combination of four pixels 240 with ink non-applied areas of different orientations, where 12×12 dots serve as one pixel and 50 dots in each pixel 240 serve as ink non-applied areas.

[0139] In conjunction with the printing patterns A to D of Table 4, the conductive layer 210 may have a plurality of openings 220 that are not uniform in size and shape.

[0140] Evaluation of electromagnetic wave shielding effect

[0141] Fig.10 This is a method for evaluating the electromagnetic shielding effect according to this embodiment.

[0142] like Fig.10 As shown, two shielding rooms 310 and 320 are prepared, and the test samples 305 prepared in the embodiment and the comparative example are arranged in the shielding rooms 310 and 320. Here, the conductive layer of each test sample 305 is grounded.

[0143] In addition, the first shield room 310 is provided with a transmitting antenna 315, and the second shield room 320 is provided with a receiving antenna 325. The transmitting antenna 315 and the receiving antenna 325 are connected to a measuring instrument 330. The transmitting antenna 315 and the receiving antenna 325 use a double-ridged guide horn antenna manufactured by EMCO. The measuring instrument 330 uses a vector network analyzer (37147A) manufactured by Anritsu Corporation.

[0144] Electromagnetic waves are emitted from the transmitting antenna 315 to perform measurement at a frequency of 1 to 10 GHz. The measurement results are processed by a personal computer (PC) 340, and the effect of electromagnetic wave shielding is evaluated based on the attenuation rate of the electromagnetic waves.

[0145] Very good: The attenuation rate of electromagnetic waves is 30dB or more.

[0146] Good: The attenuation rate of electromagnetic waves is greater than 20 dB and less than 30 dB.

[0147] Bad: The attenuation rate of electromagnetic waves is greater than 10 dB and less than 20 dB.

[0148] Poor: The attenuation rate of electromagnetic waves is less than 10dB.

[0149] Evaluation of volume resistivity of conductive layer

[0150] The test samples prepared in Examples and Comparative Examples were respectively measured by a four-terminal method with Loresta GP (manufactured by Mitsubishi Chemical Analytical Tech Co., Ltd.).

[0151] Thermal cycle load assignment method

[0152] The test samples prepared in the embodiment and the comparative example were subjected to 10°C=>100°C and 100°C=>10°C (temperature increase and decrease at intervals of one hour) 50 times in a constant temperature bath, which can control the temperature of the test samples prepared in the embodiment and the comparative example.

[0153] Adhesion evaluation (cross-cut method)

[0154] The test samples prepared in the examples and comparative examples were scraped with a cutter to form 100 grids of 1 mm on each side. Each test sample was attached with an adhesive tape manufactured by NICHIBAN Co., Ltd. The tape was peeled off perpendicularly to the sample surface, and then the number of grids remaining in the sample was evaluated.

[0155] Very good: 75 or more meshes are retained in the sample.

[0156] Good: More than 50 and less than 75 grids remain in the sample.

[0157] Poor: More than 25 and less than 50 meshes remain in the sample.

[0158] Bad: There are less than 25 meshes left in the sample.

[0159] Preparation of Examples 1 to 6 and Comparative Examples 1 to 3

[0160] No primer

[0161] On each substrate measuring 40 mm on each side in Table 3, the conductive material was inkjet printed with the corresponding printing pattern in Table 4 and the corresponding film thickness in Table 1, and heat-treated to provide a conductive layer. The corresponding insulating layer ink in Table 1 was applied to the conductive layer with the corresponding film thickness and process (spin coating or inkjet printing) in Table 1, and UV-cured and / or heat-cured under the corresponding conditions in Table 1 to prepare each test sample in Examples 1 to 6 and Comparative Examples 1 to 3.

[0162] After applying thermal cycle load to each test specimen produced, the adhesion was evaluated (cross-hatch method). Fig.10 The electromagnetic shielding effect of each test sample in the embodiment and the comparative example was evaluated by the evaluation method in , and the results in Table 1 were obtained.

[0163] For the samples prepared as follows, the volume resistivity of the conductive layer was measured respectively. Such a conductive layer was formed in a manner similar to that in the above-mentioned embodiment and comparative example, except that the conductive layer had the entire surface printed without openings on the glass substrate, instead of pattern printing with openings, and the volume resistivity was measured by the evaluation method described later. Table 1 shows the results.

[0164] In any of the test samples of Comparative Examples 1 to 3, the adhesion is poor. Due to the poor adhesion, a portion of the conductive layer is damaged or peeled off, and the function of the conductive layer is impaired. Therefore, the electromagnetic wave shielding effect is not good.

[0165] Preparation of Examples 7 to 10 and Comparative Examples 4 to 7

[0166] With base coating

[0167] Each primer ink in Table 2 was imparted to a corresponding substrate measuring 40 mm on each side in Table 3 with a corresponding film thickness and process (spin coating or inkjet printing) in Table 2, and UV-cured and / or thermally cured under the corresponding conditions in Table 2 to produce a primer. Each conductive layer and each insulating layer were formed on the corresponding primer in a manner similar to Example 1 and Comparative Example 1 in Table 1 to produce each test sample in Examples 7 to 8 and Comparative Examples 4 to 5.

[0168] After applying thermal cycle load to each fabricated test specimen, adhesion was evaluated (cross-hatch method).

[0169] In addition, for each of the test samples in the examples and comparative examples, the electromagnetic shielding effect was evaluated by the evaluation method described later. The results are shown in Table 2.

[0170] The volume resistivity of the conductive layer was measured for each sample prepared as follows. The conductive layer was formed in a manner similar to that in the above-mentioned embodiment and comparative example, except that the conductive layer had an entire surface printed without openings on the glass substrate, rather than pattern printing with openings, and the volume resistivity was measured by the evaluation method described later. The results are shown in Table 2.

[0171] In any of the test samples of Comparative Examples 4 to 7, the adhesion is poor. Due to the poor adhesion, a portion of the conductive layer is damaged or peeled off, and the function of the conductive layer is impaired. Therefore, the electromagnetic wave shielding effect is not good.

[0172] Aspect 1

[0173] As described above, the method for forming a shielding layer 200 involved in an embodiment of the present invention includes: forming a conductive layer 210 having a plurality of openings 220 on the upper surface 102 and the side surface 104 of the peripheral surface 100 of the substrate; and forming an insulating layer 230, which is continuously formed from the surface of the conductive layer 210 through the plurality of openings 220 to the peripheral surface 100 of the substrate, and is bonded to the peripheral surface 100 of the substrate.

[0174] Here, the shielding layer 200 is an example of an electromagnetic wave shield, the outer peripheral surface 100 of the base material is an example of a surface of an object, and the shielding layer is an example of the conductive layer 210 .

[0175] Therefore, the conductive layer 210 is sandwiched between the cover portion 234 and the outer peripheral surface 100 of the base material integrated by the filling portion 232 , thereby reducing peeling and cracking on the upper surface 102 and the side surface 104 of the shield layer 200 .

[0176] Aspect 2

[0177] According to aspect 1, forming a conductive layer includes: using inkjet head 400, inkjet head 401 and inkjet head 402 to discharge ink 500, ink 501 and ink 502, each containing a conductive material, onto the top 102 and side 104 of the outer peripheral surface 100 of the substrate to form a conductive layer 210 having multiple openings 220.

[0178] Here, the inkjet heads 400 , 401 , and 402 are each an example of an applicator, and the inks 500 , 501 , and 502 are each an example of a liquid composition.

[0179] Aspect 3

[0180] According to aspect 2, forming the conductive layer includes applying inks 501 and 502 in a direction intersecting upper surface 102 and side surface 104 of outer peripheral surface 100 of the substrate using inkjet heads 401 and 402. Thus, conductive layer 210 can be reliably formed on the entire side surface 104 of outer peripheral surface 100 of the substrate.

[0181] Aspect 4

[0182] According to any one of aspects 1 to 3, forming the conductive layer 210 includes forming a plurality of openings 220 that are not uniform in at least one of size, shape, orientation, and configuration. Thus, shielding leakage of a specific wavelength can be reduced.

[0183] Aspect 5

[0184] According to any one of aspects 1 to 4, the method further includes: discharging ink 500 with an inkjet head to form a pattern before forming the conductive layer 210. Therefore, the conductive layer 210 can be formed in any pattern.

[0185] Aspect 6

[0186] According to any one of aspects 1 to 5, the method further includes: heating the conductive layer 210 to reduce the volume resistivity of the conductive layer 210. Therefore, even if the conductive layer 210 is made thinner, the shielding effect of the shielding layer 200 can be improved.

[0187] Aspect 7

[0188] According to any one of aspects 1 to 6, the method also includes: forming an insulating primer layer 150 on the outer peripheral surface 100 of the substrate, wherein forming a conductive layer 210 includes: forming the conductive layer 210 on the surface of the primer layer 150, and forming an insulating layer 230 includes: continuously forming from the surface of the conductive layer 210 to the surface of the primer layer 150 via multiple openings 220.

[0189] Therefore, the conductive layer 210 is sandwiched between the cover portion 234 and the surface of the primer layer 150 integrated by the filling portion 232 , so that peeling and cracking of the shielding layer 200 can be reduced.

[0190] Aspect 8

[0191] According to any one of aspects 1 to 7, the method further includes curing at least one of the insulating layer 230 and the primer layer 150 by at least one of UV irradiation and heating.

[0192] Thus, the bonding strength between the insulating layer 230 and the outer peripheral surface 100 of the base material can be improved, so that the peeling and cracking of the shielding layer 200 can be further reduced.

[0193] Aspect 9

[0194] A method for manufacturing a structure composed of electronic components 120 includes the method according to any one of aspects 1 to 8 of the embodiments of the present invention.

[0195] Aspect 10

[0196] The structure involved in the embodiment of the present invention includes: a shielding layer 200, including: a conductive layer 210 having a plurality of openings 220, the conductive layer 210 being formed on the upper surface and the side surface of the outer peripheral surface 100 of the substrate by inkjet; and an insulating layer 230, including: a covering portion 234 covering the conductive layer 210; and a filling portion 232 continuous with the covering portion 234, the filling portion 232 filling the plurality of openings 220, the insulating layer 230 being bonded to the outer peripheral surface 100 of the substrate at the filling portion 232.

[0197] Aspect 11

[0198] According to aspect 10 , the substrate having the outer peripheral surface 100 is the electronic component 120 or the semiconductor package 110 that houses the electronic component in the electronic device 1 .

[0199] Aspect 12

[0200] According to aspect 10 or aspect 11, the plurality of openings 220 are non-uniform in at least one of size, shape, orientation, and configuration.

[0201] Aspect 13

[0202] According to any one of aspects 10 to 12, the major diameter of each of the plurality of openings 220 is 10 to 1000 μm, and the area ratio is 3 to 40%. Therefore, inkjet is suitable for forming the non-uniform openings 220 or the fine openings 220. In addition, inkjet with ink having excellent fluidity is suitable because such fine openings 220 are filled with the filling portion 232.

[0203] Aspect 14

[0204] According to any one of aspects 10 to 13, primer layer 150 having insulating properties is provided on outer peripheral surface 100 of the substrate, conductive layer 210 is provided on the surface of primer layer 150 , and insulating layer 230 is bonded to the surface of the primer layer through the filling portion.

[0205] Aspect 15

[0206] In any one of aspects 10 to 14, the thickness of the conductive layer 210 is 0.05 to 10 μm.

[0207] Aspect 16

[0208] According to any one of aspects 10 to 15, the volume resistivity of the conductive layer 210 is 10e -6 ~10e -3 Therefore, inkjet is suitable for forming a thin conductive layer 210.

[0209] The above embodiments are illustrative and do not limit the present invention. Therefore, many additional modifications and variations are possible based on the above teachings. For example, within the scope of the present invention, the elements and / or features of different illustrative embodiments can be combined with each other and / or replaced with each other. Any of the above operations can be performed in various other ways, for example, in a different order than described above.

[0210] This patent application is based upon and claims the benefit of priority from Japanese Patent Application No. 2022-042254 filed with the Japan Patent Office on March 17, 2022, and No. 2022-191226 filed with the Japan Patent Office on November 30, 2022, the disclosures of which are incorporated herein in their entirety by reference.

[0211] Reference numerals list

[0212] 1 Electronic equipment

[0213] 100 Outer Surface

[0214] 100G Grounding

[0215] 110Semiconductor packaging

[0216] 120 electronic components

[0217] 125 Connector

[0218] 130 substrate

[0219] 135 Wiring

[0220] 150 Base Coating

[0221] 200 shielding layer

[0222] 210 conductive layer

[0223] 212 Column

[0224] 214 Connecting rod

[0225] 220 opening

[0226] 230 insulation layer

[0227] 232 Filling Department

[0228] 234 Covering

[0229] 240 pixels

[0230] 300 protection layers

[0231] 305 samples

[0232] 310 First Shielded Room

[0233] 315 Transmitting Antenna

[0234] 320 Second Shielding Room

[0235] 325 receiving antenna

[0236] 330 measuring instruments

[0237] 340PC

[0238] 400 inkjet head (an example of an inkjet applicator)

[0239] 500 ink (an example of a liquid composition)

[0240] 600 loading platform

Claims

1. A method for forming an electromagnetic wave shield, the method comprising: forming a conductive layer having a plurality of openings on the upper surface and side surfaces of a surface of an object; as well as An insulating layer is formed, the insulating layer being continuously formed from the surface of the conductive layer to the surface of the object through the plurality of openings and being bonded to the surface of the object.

2. The method according to claim 1, in, The forming of the conductive layer includes: discharging a liquid composition containing a conductive material onto the upper surface and the side surface of the surface of the object using an applicator to form the conductive layer having the plurality of openings.

3. The method according to claim 2, in, The forming of the conductive layer includes applying the liquid composition in a direction intersecting the upper surface and the side surfaces of the surface of the object using the applicator.

4. The method according to any one of claims 1 to 3, in, Forming the conductive layer includes forming the plurality of openings to be non-uniform in at least one of size, shape, orientation, and configuration. 5 . The method according to claim 1 , further comprising discharging a liquid composition with an applicator to form a pattern before forming the conductive layer.

6. The method according to any one of claims 1 to 5, further comprising heating the conductive layer to reduce the volume resistivity of the conductive layer.

7. The method according to any one of claims 1 to 6, further comprising forming a primer layer having insulating properties on the surface of the object, in, Forming the conductive layer includes forming the conductive layer on a surface of the primer layer, and forming the insulating layer includes continuously forming the insulating layer from the surface of the conductive layer to the surface of the primer layer via the plurality of openings. 8 . The method according to claim 7 , further comprising curing at least one of the insulating layer and the primer layer by at least one of UV irradiation and heating.

9. A method of manufacturing a structure comprising an electronic component, the method comprising the method according to any one of claims 1 to 8.

10. A structure comprising: a conductive layer having a plurality of openings, the conductive layer being formed on an upper surface and a side surface of a surface of an object; a covering portion covering the conductive layer; as well as The insulating layer has a filling portion continuous with the covering portion, the plurality of openings are filled with the filling portion, and the insulating layer is bonded to the surface of the object at the filling portion.

11. The structure according to claim 10, in, The object is an electronic component or a package that houses the electronic component.

12. The structure according to claim 10 or 11, in, The plurality of openings are not uniform in at least one of size, shape, orientation, and configuration.

13. The structure according to any one of claims 1 to 12, in, Each of the plurality of openings has a major diameter of 10 to 1000 μm, and an area ratio of 3 to 40%.

14. The structure according to any one of claims 1 to 13, in, A primer layer having insulating properties is provided on the surface of the object, the conductive layer is provided on the surface of the primer layer, and the insulating layer is bonded to the surface of the primer layer at the filling portion.

15. The structure according to any one of claims 1 to 14, The thickness of the conductive layer is 0.05-10 μm.

16. The structure according to any one of claims 1 to 15, The volume resistivity of the conductive layer is 10e -6 ~10e -3 Ω·cm.