Exosome-loaded PLA bioremediation material and preparation method thereof

By loading stem cell exosomes in the tympanic membrane repair material and combining PLA biofilm, the problem of lack of existing materials to promote angiogenesis and cell proliferation is solved, and the effect of significantly accelerating the healing of the tympanic membrane is achieved, providing a more efficient treatment plan.

CN119074998APending Publication Date: 2024-12-06THE 988TH HOSPITAL OF THE CHINESE PEOPLES LIBERATION ARMY JOINT LOGISTICS SUPPORT FORCE
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411212032.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing tympanic membrane repair materials lack the function of promoting angiogenesis and cell proliferation, resulting in weak neovascularization ability and weakened cell adhesion, affecting the healing effect of tympanic membranes. Traditional surgery has problems such as pain in incision, long surgery time and high infection risk.

Method used

PLA biofilm is prepared by electrospinning technology and loaded with stem cell exosomes that promote cell proliferation and migration. By mixing with methacrylic gelatin hydrogel, Exo-PLA biorepair material is formed, providing mechanical support and biological activity promotion. heal.

Benefits of technology

The surface area and strength of cell attachment, growth and proliferation were improved, and the healing time of the tympanic membrane was significantly accelerated. The perforation was reduced by 81.27% after 14 days, and the complete cure was achieved after 28 days, which was better than the therapeutic effect of traditional materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119074998A_ABST
    Figure CN119074998A_ABST
Patent Text Reader

Abstract

The invention provides an exosome-loaded PLA bioremediation membrane material and a preparation method thereof, and relates to the technical field of tympanic membrane remediation biomaterials. According to the invention, the PLA biological membrane is firstly prepared by an electrostatic spinning technology, and is loaded with the mesenchymal stem cell-derived exosome capable of promoting cell proliferation and migration, and finally the Exo-PLA bioremediation membrane material is obtained. The bioremediation membrane material disclosed by the invention has a relatively high aperture structure and relatively good mechanical strength, and can provide a relatively large surface area and relatively high strength for attachment, growth and proliferation of cells; meanwhile, excellent biocompatibility is achieved, cell viability can be improved, and a promoting effect on cell proliferation is achieved. The Exo-PLA bioremediation membrane material disclosed by the invention can accelerate the tympanic membrane healing time and improve the tympanic membrane healing efficiency, and has remarkable treatment advantages.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of tympanic membrane repair biomaterials, and in particular to an exosome-loaded PLA biorepair material and a preparation method thereof. Background Art

[0002] The tympanic membrane is located between the middle ear and the external auditory canal. It is a thin and flexible membrane with a thickness of less than 100 μm. Histologically, the tympanic membrane is composed of three layers. The outer layer is the epithelial layer, which is composed of keratinocytes; the inner layer is the mucosal layer, which is composed of non-keratinized mucosal epithelium; the middle layer is the elastic fiber layer, which is composed of collagen that is radial on the outside and circular on the inside. This special arrangement of collagen gives the tympanic membrane the ability to conduct hearing. Tympanic membrane perforation can be caused by palm strikes, collisions, artillery shocks, explosions, foreign body penetration, external auditory canal flushing, and hot foreign body splashes. This disease is a common disease in the otolaryngology department. Patients often experience discomfort such as hearing loss, and severe cases may even affect their lives, studies, and work.

[0003] Generally, tympanic membrane perforation can heal naturally. If the patient still cannot heal naturally after 3 months, further surgical treatment is required to prevent complications such as middle ear infection and cholesteatoma. Its treatment currently includes tympanic membrane patch repair, local medication and tympanoplasty. At present, traditional surgery mainly uses autologous temporalis fascia, perichondrium, etc. as repair materials. Although the healing rate of tympanic membrane is high, there are still many defects, such as pain and surgical scars at the donor site after surgery, long operation time and increased anesthesia risk, and the selection of autologous materials requires a second incision, which invisibly increases the chance of infection at the sampling site and increases the chance of repair failure. Therefore, we urgently need to find new non-autologous materials that are incision-free, highly safe and reasonably priced for alternative repair.

[0004] The emergence of tissue engineering materials can effectively avoid the above problems. Tissue engineering materials are scaffolds and templates for tissue regeneration. They are polymer materials that can induce tissue regeneration, regulate cell growth and functional differentiation in tissues. In recent years, many novel tympanic membrane repair materials have emerged, including patches, 3D printed scaffolds, etc. The repair of tympanic membrane perforation mainly relies on the proliferation and migration of epithelial cells. The tympanic membrane repair material acts as a scaffold, that is, it induces cells at the edge of the perforation to grow toward the center to repair the perforation. Although there are currently a variety of repair materials to choose from, most of them can only provide mechanical support, lack the function of promoting angiogenesis or cell proliferation, which will lead to weak angiogenesis and insufficient secretion of growth factors. In addition, the lack of extracellular matrix will cause the cell adhesion to the new membrane to be weakened, further affecting the effect of tympanic membrane repair. Therefore, the selection of a suitable scaffold material combined with a bioactive substance has also become a new research direction in recent years. The present invention aims to provide a new biological tympanic membrane repair material with good biocompatibility, no rejection reaction, and a biomechanical structure and vibration characteristics similar to the tympanic membrane. Summary of the invention

[0005] 1. Technical issues to be solved

[0006] In view of the shortcomings of the prior art, the present invention provides a PLA bioremediation material loaded with exosomes and a preparation method thereof. The bioremediation material is prepared by using PLA biofilm as a supporting scaffold material and loaded with stem cell exosomes that can promote cell proliferation and migration.

[0007] (II) Technical solution

[0008] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0009] First, the present invention provides a PLA bioremediation material loaded with exosomes, wherein the bioremediation material is prepared by using PLA as a supporting scaffold material and loaded with stem cell exosomes that can promote cell proliferation and migration.

[0010] The present invention also provides a method for preparing an exosome-loaded PLA bioremediation material, wherein the bioremediation material is prepared according to the following steps:

[0011] (1) Preparation of exosomes

[0012] Donated adipose-derived stem cells (ADSCs) (Sigma) were cultured to P3, and after the cells were passaged and adhered, the complete culture medium was replaced with a serum-free stem cell culture medium (Corning China); after 48 hours of continuous culture, the cell culture medium was collected and replaced with fresh serum-free stem cell culture medium; the cell culture medium was centrifuged and filtered to collect exosomes;

[0013] Specifically, the cell culture medium was centrifuged and exosomes were collected according to the following steps: using an ultracentrifuge to precipitate at 300×g for 10 min at 4°C, and then at 2000×g for 30 min to remove dead cells; the remaining purified culture medium was centrifuged at 10000×g for 30 min, and the supernatant was filtered through a 0.22 μm filter to remove excess protein; then, the supernatant was centrifuged at 100000×g for 70 min, the precipitate was washed with PBS, and the solution was transferred to a new tube and centrifuged again at 100000×g for 70 min to obtain exosomes for use;

[0014] (2) Preparation of spinning solution

[0015] Dissolving PLA in dichloromethane to prepare a spinning solution containing 2% by mass of PLA;

[0016] (3) Preparation of PLA biofilm

[0017] The PLA spinning solution obtained in step (2) is subjected to an electrospinning method to obtain a PLA biofilm; during electrospinning printing, a self-made bracket collector is used, the distance between the needle and the self-made bracket collector is 15 cm, the electrospinning solution extrusion speed is 1 mL / h, the voltage between the needle and the self-made bracket collector is 18 kV, and the collection time is 2 h; the PLA film is deposited on the self-made bracket collector, and then the PLA biofilm is obtained, and after being sterilized with ultraviolet light for 3 h, it is then washed with a PBS solution for more than 3 times, and then dried and cut into an elliptical PLA biofilm for standby use;

[0018] (4) Preparation of Exo-PLA bioremediation materials

[0019] Gelatin methacrylate (GelMA) is prepared into an aqueous solution with a mass fraction of 1-5% to obtain a GelMA hydrogel solution, and then the exosomes prepared in step (1) are added and fully mixed with the GelMA hydrogel solution to obtain a GelMA hydrogel solution containing exosomes; the above hydrogel solution is added to a mold with a PLA biofilm, and is irradiated with ultraviolet light for photocuring to obtain an Exo-PLA bioremediation material.

[0020] Wherein, the GelMA hydrogel solution contains 0.1-0.5% of photoinitiator;

[0021] Wherein, the concentration of exosomes in the GelMA hydrogel solution is 200 μg / mL-500 ug / mL; preferably, the concentration of exosomes in the GelMA hydrogel solution is 350 ug / mL.

[0022] (III) Beneficial effects

[0023] The present invention first prepares a PLA biofilm using electrospinning technology, and loads exosomes derived from mesenchymal stem cells that promote cell proliferation and migration, and finally obtains an Exo-PLA bioremediation membrane material. The Exo-PLA bioremediation membrane material prepared by the present invention has a relatively high pore size structure and good mechanical strength, and can provide a large surface area and high strength for cell attachment, growth and proliferation; at the same time, it has excellent biocompatibility, can increase cell activity, and has a promoting effect on cell proliferation.

[0024] The Exo-PLA biorepair membrane material of the present invention can achieve a therapeutic effect of reducing the size of the perforation by 81.27% after treating rats with tympanic membrane perforation for 14 days, which is much higher than the 18.73% reduction in the hole size of the tympanic membrane; after treating rats with tympanic membrane perforation for 28 days, it can achieve a therapeutic effect of reducing the size of the perforation by 97.46%, and can achieve a complete cure effect on rats with tympanic membrane perforation.

[0025] The Exo-PLA bioremediation membrane material of the present invention can accelerate the time of tympanic membrane healing and improve the tympanic membrane healing efficiency, and has significant therapeutic advantages over the tympanic membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The results of CCK-8 method detection of the proliferation effect of different concentrations of stem cell-derived exosomes on tympanic membrane cells; compared with the blank control group, *P<0.05, **P<0.01, ***P<0.001, ****P<0.0001.

[0027] Figure 2 The cell scratch assay was used to detect the migration effect of different concentrations of stem cell-derived exosomes on tympanic membrane cells.

[0028] Figure 3 The results of the Transwell experiment were used to detect the migration effect of different concentrations of stem cell-derived exosomes on tympanic membrane cells.

[0029] Figure 4 This is the result of cell live-dead staining of material A.

[0030] Figure 5 The healing results of tympanic membrane perforations in each group of rats were observed by otoendoscopy before implantation of repair materials, 14 days after implantation, and 28 days after implantation. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] A method for preparing an exosome-loaded PLA bioremediation membrane, wherein the bioremediation membrane is prepared according to the following steps:

[0034] (1) Preparation of exosomes

[0035] Donated adipose-derived stem cells (ADSCs) (Sigma) were cultured to P3, and after the cells were passaged and adhered, the complete culture medium was replaced with a serum-free stem cell culture medium (Corning China); after 48 hours of continuous culture, the cell culture medium was collected and replaced with fresh serum-free stem cell culture medium; the cell culture medium was centrifuged and filtered to collect exosomes;

[0036] Specifically, the cell culture medium was centrifuged and exosomes were collected according to the following steps: using an ultracentrifuge to precipitate at 300×g for 10 min at 4°C, and then at 2000×g for 30 min to remove dead cells; the remaining purified culture medium was centrifuged at 10000×g for 30 min, and the supernatant was filtered through a 0.22 μm filter to remove excess protein; then, the supernatant was centrifuged at 100000×g for 70 min, the precipitate was washed with PBS, and the solution was transferred to a new tube and centrifuged again at 100000×g for 70 min to obtain exosomes for use;

[0037] (2) Preparation of spinning solution

[0038] Dissolving PLA in dichloromethane to prepare a spinning solution containing 2% by mass of PLA;

[0039] (3) Preparation of PLA biofilm

[0040] The PLA spinning solution obtained in step (2) is subjected to an electrospinning method to obtain a PLA biofilm; during electrospinning printing, a homemade bracket collector is used, the distance between the needle and the homemade bracket collector is 15 cm, the electrospinning solution extrusion speed is 1 mL / h, the voltage between the needle and the homemade bracket collector is 18 kV, and the collection time is 2 h; the PLA film is deposited on the homemade bracket collector, and then the PLA biofilm is obtained, and after being sterilized with ultraviolet light for 3 h, it is then washed with a PBS solution for more than 3 times, and then dried and cut into elliptical biofilms for standby use;

[0041] (4) Preparation of Exo-PLA bioremediation materials

[0042] Gelatin methacrylate (GelMA) is prepared into an aqueous solution with a mass fraction of 5% to obtain a GelMA hydrogel solution, and then the exosomes prepared in step (1) are added and fully mixed with the GelMA hydrogel solution to obtain a GelMA hydrogel solution containing exosomes; the above hydrogel solution is added to a mold with a PLA biofilm, and is irradiated with ultraviolet light for photocuring to obtain an Exo-PLA bioremediation material.

[0043] Among them, the GelMA hydrogel solution contained 0.35% of photoinitiator;

[0044] Among them, the concentration of exosomes in the GelMA hydrogel solution was 350ug / mL.

[0045] In order to further evaluate and verify the effectiveness and feasibility of the biorepair membrane of the present invention in treating tympanic membrane perforation, the following experiment is provided for illustration.

[0046] 1 Materials and methods

[0047] 1.1 Experimental Materials

[0048] A. Bioremediation membrane prepared in Example 1; B. Bioremediation membrane

[0049] 1.2 Construction of a rat model of traumatic tympanic membrane perforation

[0050] Forty male SD rats with no significant differences in body size and health were selected and placed in a room with a temperature of 22°C, a humidity of 50%, and an ambient noise of 40 dB. All animal experiments were conducted in accordance with the regulations of the ethics committee. A tympanic membrane perforation model was established in 30 rats. Rats were intraperitoneally injected with 4% chloral hydrate (10 mL / kg) for general anesthesia, and all rat ears were examined under a microscope, and ears with ear effusion were not included in the study; the ear canal was disinfected with povidone-iodine solution, and a sterile 23-gauge needle was used to manually create a tympanic membrane perforation model, involving the anterior and posterior aspects of the tympanic membrane to achieve tympanic membrane perforation (50% pars tensa) without damaging the ossicles; then, gelatin sponges were dipped in mitomycin C 0.4 mg / mL and hydrocortisone 10 mg / mL, respectively, and the edges of the tympanic membrane perforation were locally wet-applied for 10 minutes each, once a day, for 3 consecutive days; after surgery, 150 mg / kg of ampicillin was injected intramuscularly continuously to prevent infection; observation that the perforated tympanic membrane did not heal after 8 weeks indicated that the tympanic membrane perforation model was successfully modeled.

[0051] 1.3 Grouping and restorative material implantation treatment

[0052] The 30 rats with successful modeling were randomly divided into 3 groups, 10 in each group, namely the model group, experimental group A, and experimental group B, and another 10 healthy rats were used as the blank control group. The model group and the blank control group did not receive any special treatment; the experimental group A and group B were repaired with materials A and B, respectively, and the specific method was as follows: 4% chloral hydrate (10mL / kg) was injected intraperitoneally into the rats for general anesthesia, the ear canal was disinfected with povidone iodine solution, the tympanic cavity was first filled with gelatin sponge soaked in 1% chelidonin eye drops, and the tympanic cavity surface of the tympanic membrane residual edge was lined with the corresponding size of repair material from the perforation to the inner lining of the tympanic cavity, and the repair material completely covered the tympanic membrane perforation, and the external auditory canal was filled with the aforementioned antibiotic gelatin sponge, and 150mg / kg of ampicillin was injected intramuscularly after surgery for 5 consecutive days to prevent infection, and the healing of the tympanic membrane of each group of rats was observed.

[0053] 1.4 Observation indicators

[0054] 1.4.1 Effects of stem cell exosomes on tympanic membrane cells

[0055] 1.4.1.1 Effect of stem cell exosomes on the proliferation of tympanic membrane cells

[0056] CCK-8 cell proliferation assay: P3-P5 tympanic fibroblasts were selected and inoculated into 96-well plates at a number of 2,000 cells per well after cell counting. After the cells adhered to the plate, the medium containing low (2.5 x 10 8 ), Medium(5x10 8 ), high (10x10 8 ) exosomes / mL) and a control group without exosomes were cultured with 100 μL of liquid per well. On days 1, 2, and 3, 10 μL of CCK-8 working solution was added to each well according to the manufacturer's instructions. After incubation at 37°C for 2 h, the absorbance of the liquid was detected using a microplate reader to evaluate the proliferation of cells.

[0057] 1.4.1.2 Effect of stem cell exosomes on the migration of tympanic membrane cells

[0058] Cell scratch test: chondrocytes were seeded in a six-well plate at a number of 5*10^6 / ml cells per well. After the cells adhered to the wall, the culture medium was aspirated and three scratches were made evenly in the well plate using a 200μL pipette tip to simulate wounds. Set the low (2.5x10 8 ), Medium(5x10 8 ), high (10x10 8 ) exosomes / mL measurement group and control group, and photographed the cells in each group at 0h and 48h to observe the cell migration.

[0059] Transwell experiment: 3 μm transwell cell chambers were purchased from Nest (Shanghai, China). Tympanic membrane cells were counted and 2×10 cells were placed in each well. 4 The number of cells was inoculated into the chamber, the upper chamber was cultured with serum-free cell culture medium, and the lower chamber was cultured with complete culture medium containing or not containing exosomes for 24 hours. After washing the chamber with PBS, the bottom of the chamber was fixed with 4% paraformaldehyde, the cells were stained with 0.1% crystal violet stain, and the migration of cells was photographed under a microscope.

[0060] 1.4.2 Porosity

[0061] Both A and B materials were cut into equal volumes (10mmx5mm), and the porosity was evaluated by using the liquid displacement method. The specific method is: the dry AC material is placed in a determined volume (V1) of ethanol for 10 minutes to completely fill the voids. The volume after the bracket is immersed is recorded as V2. After the bracket is removed, the remaining ethanol volume is recorded as V3. The porosity is calculated according to the following equation:

[0062] Porosity of the scaffold (%) = {(V1-V3) / (V2-V3)}×100

[0063] 1.4.3 Mechanical properties

[0064] Materials A and B were cut into small strips (10×40 mm) respectively; the tensile test was carried out using a tensile testing machine, and the stress-strain curve of the scaffold was recorded at a tensile speed of 0.5 mms-1. All values ​​were expressed as mean ± standard deviation.

[0065] 1.4.4 Live and dead cell staining

[0066] 1*10 6 The cells were seeded on 2cm*2cm sized A materials, and the A materials were co-cultured for 1, 2, 4, and 7 days. The Te staining solutions of AM and PI were added to the cell-laden composite scaffolds at 0.5 μL / ml using PBS solution until the working solution submerged the samples. The samples were incubated at 37°C for 30 minutes, and the samples were photographed and observed using a fluorescent inverted microscope.

[0067] 1.4.5 Otoendoscopy

[0068] 14 and 28 days after implantation of the repair material, the rats in each group were examined for TM morphology using a digital otoscope (MacroView; Welch Allyn), and the perforation size of each ear (perforation area / pars tensa area × 100 (%)) was calculated using ImageJ software. The healing rate was defined as the ratio of the number of completely closed tympanic membranes to the total number of perforated tympanic membranes in each group. For the healed tympanic membranes, the healing time of each group was calculated and compared.

[0069] 2 Results

[0070] 2.1 Effects of stem cell exosomes on tympanic membrane cells

[0071] Figure 1 To show the proliferation effect of different concentrations of stem cell exosomes on CCK-8 cells, we used the CCK-8 method to perform a digital analysis of the cell proliferation effect of stem cell exosomes. On the third day of the experiment, the OD value of different concentrations of stem cell exosomes increased significantly compared with the blank control group, and the difference was extremely significant (P<0.01). This result shows that stem cell exosomes have a significant proliferation effect on tympanic membrane cells.

[0072] Figure 2 and Figure 3 The effects of stem cell exosomes on the migration ability of tympanic membrane cells were tested by cell scratch assay and transwell cell migration assay. The results showed that stem cell exosomes have a significant promoting effect on the migration of tympanic membrane cells.

[0073] 2.2 Porosity and mechanical properties

[0074] As shown in Table 1, the porosity and mechanical properties of the bioremediation membrane prepared by the present invention are comparable to those of the PLA biomembrane, with no significant difference (P>0.05). This result indicates that loading exosomes onto the PLA biomembrane does not affect the porosity and mechanical strength of the scaffold, and the bioremediation membrane provided by the present invention can provide a larger surface area and higher strength for cell attachment, growth and proliferation.

[0075] Table 1 Porosity and mechanical properties of the bioremediation membrane and the membrane of the present invention

[0076] project Porosity (%) Modulus (MPa) AMaterial 82.75±4.65 3.0±0.6 B Material 83.45±5.56 3.1±0.4

[0077] 2.3 Live and dead cell staining

[0078] Figure 4 The results of cell live-death staining of material A were obtained. We tested the cell survival on days 1, 2, 4, and 7. As the culture time increased, the number of cells in material A also increased, and after seven days of culture, the cell density on material A increased significantly compared to the first day. This result shows that the bioremediation membrane of the present invention has excellent biocompatibility, can increase cell activity, and has a promoting effect on cell proliferation.

[0079] 2.4 Otoendoscopy

[0080] like Figure 5 As shown in Table 2, there was no statistical difference in the diameter of the tympanic membrane perforation in each group of rats before implantation of the repair material. 14 days after implantation, compared with the model group, the diameter of the perforation in the rats in the experimental group A was significantly smaller, and the difference was extremely significant (P<0.01), and the diameter of the perforation in the rats in the experimental group B was significantly smaller, and the difference was significant (P<0.05); among them, the reduction degree of the perforation diameter in the rats in the experimental group A was 81.27% after 14 days, and the reduction degree of the perforation diameter in the rats in the experimental group B was 18.73% after 14 days. 28 days after implantation, the diameter of the perforation in the rats in the experimental group A and experimental group B was significantly smaller, and the difference was extremely significant (P<0.01). Among them, the reduction degree of the perforation diameter in the rats in the experimental group A was 97.46% after 28 days, and the reduction degree of the perforation diameter in the rats in the experimental group B was 43.93% after 28 days.

[0081] Table 2 Diameter of perforation in rats with tympanic membrane perforation before, 14 days after and 28 days after implantation of repair materials in each group

[0082] Grouping Before implantation (mm) 14 days after implantation (mm) 28 days after implantation (mm) Blank control group — — — Model Group 3.12±0.26 3.09±0.31 3.12±0.37 Experimental Group A 3.15±0.11 0.59±0.08** 0.08±0.05** Experimental Group B 3.05±0.17 2.46±0.21* 1.71±0.10**

[0083] Note: Compared with the model group, *P<0.05, **P<0.01.

[0084] 3 Conclusion

[0085] The present invention first prepares a PLA biofilm by electrospinning technology, and loads exosomes derived from mesenchymal stem cells that promote cell proliferation and migration, and finally obtains an Exo-PLA biorepair membrane material. The Exo-PLA biorepair membrane material prepared by the present invention has a relatively high pore size structure and good mechanical strength, and can provide a large surface area and high strength for cell attachment, growth and proliferation; at the same time, it has excellent biocompatibility, and can increase cell activity, and has a promoting effect on cell proliferation. The Exo-PLA biorepair membrane material of the present invention can achieve a therapeutic effect of reducing the perforation size by 81.27% after treating rats with tympanic membrane perforation for 14 days, which is much higher than the pore size reduction of 18.73% of the Rui membrane; after treating rats with tympanic membrane perforation for 28 days, it can achieve a therapeutic effect of reducing the perforation size by 97.46%, and can achieve a complete cure effect on rats with tympanic membrane perforation. The Exo-PLA biorepair membrane material of the present invention can accelerate the healing time of the tympanic membrane, improve the healing efficiency of the tympanic membrane, and has significant therapeutic advantages over the Rui membrane.

[0086] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A PLA bioremediation material loaded with exosomes, characterized in that: The biorepair material is prepared by using a PLA biofilm as a supporting scaffold material and loaded with stem cell exosomes that can promote cell proliferation and migration.

2. The method for preparing a PLA bioremediation material loaded with exosomes according to claim 1, characterized in that: The bioremediation material is prepared according to the following steps: (1) Preparation of exosomes Donated adipose-derived stem cells (ADSCs) (Sigma) were cultured to P3, and after the cells were passaged and adhered, the complete culture medium was replaced with a serum-free stem cell culture medium (Corning China); after 48 hours of continuous culture, the cell culture medium was collected and replaced with fresh serum-free stem cell culture medium; the cell culture medium was centrifuged and filtered to collect exosomes; Specifically, the cell culture medium was centrifuged and exosomes were collected according to the following steps: using an ultracentrifuge to precipitate at 300×g for 10 min at 4°C, and then at 2000×g for 30 min to remove dead cells; the remaining purified culture medium was centrifuged at 10000×g for 30 min, and the supernatant was filtered through a 0.22 μm filter to remove excess protein; then, the supernatant was centrifuged at 100000×g for 70 min, the precipitate was washed with PBS, and the solution was transferred to a new tube and centrifuged again at 100000×g for 70 min to obtain exosomes for use; (2) Preparation of spinning solution Dissolving PLA in dichloromethane to prepare a spinning solution containing 2% by mass of PLA; (3) Preparation of PLA biofilm The PLA spinning solution obtained in step (2) is subjected to an electrospinning method to obtain a PLA biofilm; during electrospinning printing, a self-made bracket collector is used, the distance between the needle and the self-made bracket collector is 15 cm, the electrospinning solution extrusion speed is 1 mL / h, the voltage between the needle and the self-made bracket collector is 18 kV, and the collection time is 2 h; the PLA film is deposited on the self-made bracket collector, and then the PLA biofilm is obtained, and after being sterilized with ultraviolet light for 3 h, it is then washed with a PBS solution for more than 3 times, and then dried and cut into an elliptical PLA biofilm for standby use; (4) Preparation of Exo-PLA Tympanic Membrane Biorepair Materials Gelatin methacrylate (GelMA) is prepared into an aqueous solution with a mass fraction of 1-5% to obtain a GelMA hydrogel solution, and then the exosomes prepared in step (1) are added and fully mixed with the GelMA hydrogel solution to obtain a GelMA hydrogel solution containing exosomes; the above hydrogel solution is added to a mold with a PLA biofilm, and is irradiated with ultraviolet light for photocuring to obtain the bioremediation material.

3. The method for preparing a PLA bioremediation material loaded with exosomes according to claim 2, characterized in that: The GelMA hydrogel solution contains 0.1-0.5% photoinitiator.

4. The method for preparing a PLA bioremediation material loaded with exosomes according to claim 2, characterized in that: The concentration of exosomes in the GelMA hydrogel solution was 200 μg / mL-500 ug / mL.

5. The method for preparing a PLA bioremediation material loaded with exosomes according to claim 2, characterized in that: The concentration of exosomes in the GelMA hydrogel solution was 350ug / mL.

Citation Information

Cited By

  • Preparation method of hypoxia-pretreated exosome-loaded photo-crosslinked collagen hydrogel