Method for preparing antibacterial'oil-water diode 'film by atmospheric pressure plasma jet direct dry method

The antibacterial "oil-water diode" membrane is prepared by direct dry method of atmospheric pressure plasma jet, which solves the problems of complex equipment and biological pollution, and achieves efficient and environmentally friendly oil-water separation and sterilization effects, which are suitable for a variety of application scenarios.

CN119075385APending Publication Date: 2024-12-06WUHU TECH & INNOVATION RES INST AHUT +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411134878.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, when preparing antibacterial "oil-water diode" membranes, the equipment is complex and the process is cumbersome, and it is impossible to effectively remove bacterial and virus biological contamination in the water. The commonly used methods are inefficient and have a lot of pollution, and the equipment is expensive.

Method used

The content of the precursor hexamethyldisiloxane and the gas flow rate of the nano-silver dispersion are adjusted by atomizing cups to achieve controllable adjustment of the polyester fabric and the surface of the base fiber. Deposit nano-silver particles to achieve oil-water separation and disinfection and sterilization.

Benefits of technology

It realizes the simple, environmentally friendly and low-cost preparation of antibacterial "oil-water diode" membrane at room temperature and atmospheric pressure, improves the efficiency of oil-water separation, and has sterilization and disinfection functions. It is easy to operate and is suitable for medical and offshore oil spill treatment and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075385A_ABST
    Figure CN119075385A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing an antibacterial'oil-water diode 'membrane by an atmospheric pressure plasma jet direct dry method, and belongs to the technical field of membrane material preparation. Excitation gas such as argon / helium is used as pressure gas of the atomizing cup, and liquid can reach the plasma jet generator along with the excitation gas to react after being atomized. The flux of the precursor atomizing cup is controlled, so that the plasma jet flow can be converted between pure jet flow and deposition jet flow, when the flux is zero, the polyester fabric can be subjected to hydrophilization treatment, and when the flux is not zero, the polyester fabric can be subjected to hydrophobization treatment. The hydrophilic and hydrophobic degree of the polyester fabric can be controlled by controlling the treatment time. And the atomization flux of the pressure gas in the other path of nano-silver dispersion liquid atomizing cup is controlled, so that nano-silver particles with sterilization and disinfection functions can be attached to the fiber surface of the polyester fabric. The method is simple and high in efficiency, direct use of a chemical solution on the polyester fabric is not involved in the whole process, and the hydrophilic and hydrophobic degree of the film can be adjusted in real time while the film has the antibacterial property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of membrane material preparation, and in particular to a method for preparing an antibacterial "oil-water diode" membrane by direct dry method using atmospheric pressure plasma jet. Background Art

[0002] With the rapid development of industry and economy, the discharge of oily wastewater from the petroleum, pharmaceutical, metallurgical industries has increased dramatically, and frequent oil spills at sea have seriously affected human life and the ecological environment. In order to deal with the above problems, artificial intervention and separation of oil-water mixtures and recycling of water resources are an effective means of treating oily wastewater. Commonly used methods for treating oil-water mixtures can be divided into three categories: physical, chemical, and biochemical, including gravity method, suspension method, filtration method, sedimentation method, centrifugation method, in-situ combustion, anaerobic treatment technology, etc. Although the above methods can separate oil and water, they have low efficiency, pollution, expensive equipment, and cannot eliminate biological contamination such as bacteria and viruses in the water. In recent years, the "oil-water diode" membrane has attracted widespread attention for its unique charm in oil-water separation. The "oil-water diode" membrane is a material with different wettability on both sides, that is, one side is hydrophilic and oleophobic, and the other side is hydrophobic and oleophilic. When the oil-water mixture is on the hydrophobic side, the membrane allows oil to pass through while retaining water on the surface, thus playing a role in removing oil and retaining water; on the hydrophilic side, it allows water to pass through while retaining oil on the surface, thus playing a role in removing water and retaining oil. Therefore, it is similar to the "diode" effect in semiconductors.

[0003] Polyester fabric, as a ubiquitous, low-cost, soft and elastic material, is considered to be one of the effective candidates for the preparation of superhydrophobic material substrates for "oil-water diodes". There are generally two methods for preparing superhydrophobic fabrics on fabrics: wet chemical method and dry physical method. Wet chemical method is usually accompanied by problems such as volatilization of solution, waste liquid treatment and environmental pollution, while dry physical method generally includes chemical vapor deposition (CVD), plasma etching processing, atomic layer deposition (ALD). Most of these methods have process problems such as complex equipment and cumbersome manufacturing process. Therefore, there is an urgent application demand for seeking a simple, environmentally friendly and low-cost method to prepare antibacterial "oil-water diode" membranes. Summary of the invention

[0004] In view of the deficiencies of the above-mentioned prior art, the present invention aims to provide a method for preparing an antibacterial "oil-water diode" film by a direct dry process using an atmospheric pressure plasma jet. The method can be operated at room temperature and atmospheric pressure. By adjusting the content of the precursor hexamethyldisiloxane through the atomizing cup, the atmospheric pressure plasma jet can be seamlessly switched between a jet containing the precursor and a jet not containing the precursor, thereby achieving controllable hydrophilicity and hydrophobicity of the base polyester fabric. In addition, by placing a nanosilver dispersion in another atomizing cup and adjusting the flow rate of the gas introduced into the atomizing cup, the generated atmospheric pressure plasma jet can contain nanosilver particles that can kill viruses and disinfect and be deposited on the surface of the base polyester fiber, thereby achieving a disinfecting and disinfecting effect while achieving oil-water separation.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing an antibacterial "oil-water diode" membrane by direct dry method using atmospheric pressure plasma jet, the specific steps are as follows:

[0007] Step 1: Take a piece of polyester fabric, wash it with anhydrous ethanol and deionized water for 5 minutes, and then dry it at 40°C for later use;

[0008] Step 2: Prepare a nanosilver dispersion, mix the nanosilver particles with deionized water in a certain ratio, and stir in a magnetic stirrer until the suspension is complete for later use;

[0009] Step 3: Take hexamethyldisiloxane into the first atomizing cup, and take the prepared nanosilver dispersion into the second atomizing cup;

[0010] Step 4: setting the gas flux in the first atomizing cup filled with hexamethyldisiloxane in step 3 to zero, the gas flux in the second atomizing cup filled with nanosilver dispersion to non-zero, and the flux in the mixing passage of plasma excitation gas and oxygen to non-zero;

[0011] Step 5: Place the clean polyester fabric that has been pretreated in step 1 flat on the center of the three-axis platform;

[0012] Step 6: According to the settings of step 4, plasma excitation gas and oxygen are introduced to obtain a low-temperature plasma jet at atmospheric pressure, and the jet contains nanosilver particles to perform hydrophilic treatment on one side of the polyester fabric placed in step 5;

[0013] Step 7: The host computer controls the three-axis platform to dynamically process the surface of the polyester fabric according to the set route;

[0014] Step 8: After step 7 is completed, turn the treated polyester fabric over and place it in the center of the three-axis platform;

[0015] Step 9: setting the gas flux in the first atomizing cup filled with hexamethyldisiloxane in step 4 to be non-zero, the gas flux in the second atomizing cup filled with nanosilver dispersion to be non-zero, and the flux in the mixing passage of plasma excitation gas and oxygen to be non-zero;

[0016] Step 10: According to the settings of step 9, plasma excitation gas and oxygen are introduced to obtain an atmospheric pressure low-temperature plasma jet. Hexamethyldisiloxane is decomposed and recombined in the jet to generate SiO x The particulate matter, while the jet contains nano silver particles, performs a hydrophobic treatment on one side of the polyester fabric placed in step eight;

[0017] Step 11: The host computer controls the three-axis platform to dynamically process the surface of the polyester fabric according to the set route.

[0018] Furthermore, in step 1, the polyester fabric is 50 mm long, 50 mm wide, and 0.4 mm thick. In actual applications, if necessary, the size can be modified according to demand.

[0019] Furthermore, the plasma excitation gas in step six and step ten can be selected from inert gases such as argon, helium, neon, etc., and is not limited to one excitation gas.

[0020] Furthermore, in step six and step nine, the oxygen flow rate is set to 10-30 sccm, the plasma excitation gas and oxygen mixing passage flow rate is set to 500-700 sccm, the plasma excitation gas flow rate in the hexamethyldisiloxane atomization cup is 500-800 sccm, and the plasma excitation gas flow rate in the nanosilver dispersion atomization cup is 300-500 sccm.

[0021] Furthermore, in order to obtain the best jet intensity, the power supply adopts an AC sinusoidal power supply, and a pulse modulator is used to modulate the power duty cycle. The specific parameter ranges are: voltage 10-13 kV, frequency 4-5 kHz, and duty cycle 50-70%.

[0022] To obtain a better treatment effect, in steps seven and eleven, according to the size of the polyester fabric in step one, the route for reciprocating treatment of the polyester fabric is set to a straight line treatment of 40 mm with an interval of 5 mm, and the moving speed is adjusted between 1 and 4 mm / s. In step seven, the fabric is moved back and forth five times, and in step eleven, the fabric is moved back and forth ten times. By adjusting the moving speed and the number of reciprocating times, the treatment time can be changed; finally, an antibacterial "oil-water diode" membrane is prepared.

[0023] Beneficial effects of the present invention:

[0024] The present invention uses an exciting gas such as argon / helium as a pressure gas for an atomizing cup. After the liquid is atomized in the atomizing cup, it can reach a plasma jet generator with the plasma exciting gas to react. By controlling the flux of the precursor atomizing cup, the plasma jet can be switched between a pure jet and a precursor-containing jet. When the flux is zero, the polyester fabric can be hydrophilized. When it is not zero, the polyester fabric can be hydrophobicized. By controlling the treatment time, the hydrophilicity and hydrophobicity of the polyester fabric can be controlled. By controlling the atomization flux of the pressure gas in another nanosilver dispersion atomizing cup, nanosilver particles with sterilization and disinfection can be attached to the surface of the polyester fabric fiber. Compared with the traditional solution immersion or spraying method, this technology is simpler, more efficient, and does not involve the direct use of chemical solutions on the polyester fabric throughout the process. At the same time, the hydrophilicity and hydrophobicity of the polyester fabric can be adjusted in real time by adjusting the pressure gas flux in the atomizing cup. Therefore, the present invention is easy to operate, environmentally friendly, a dry process throughout, low in price, and can be prepared on a large scale. It will have good application prospects in the fields of medical treatment, offshore oil spills, oily wastewater treatment, etc. in the future. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The present invention will be further described below in conjunction with the accompanying drawings.

[0026] Figure 1 It is a schematic diagram of the method of the present invention;

[0027] Figure 2 It is a schematic diagram of the connection between the plasma jet generator, the atomizing cup and the gas source;

[0028] Figure 3 A schematic diagram of the real-time processing path of the plasma jet;

[0029] Figure 4 This is a schematic diagram of the cross section of the polyester fabric after treatment;

[0030] Figure 5 Oil / water contact angle images of treated polyester fabric under oil / water;

[0031] Figure 6 Scanning electron microscope images of the hydrophilic and hydrophobic surfaces of the prepared "oil-water diode" membrane. DETAILED DESCRIPTION

[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] The related devices used in the present invention are as follows: Figure 1As shown, the polyester fabric 101 is placed on a three-axis platform 102 , and a plasma generator 201 is also disposed on the three-axis platform 102 , and the plasma generator 201 is disposed directly above the polyester fabric 101 .

[0034] like Figure 2 , which is a schematic diagram of the connection between the plasma generator 201 and the atomizing cup and the gas source. Specifically, the first atomizing cup 202 and the second atomizing cup 203 are connected to the plasma generator 201 through the atomizing pipe 206, and the plasma excitation gas pipe 204 and the oxygen pipe 205 are connected to the plasma generator 201 through the plasma excitation gas and oxygen mixing passage 207.

[0035] Example 1

[0036] A method for preparing an antibacterial "oil-water diode" membrane by direct dry method using atmospheric pressure plasma jet, such as Figure 1 As shown, the following steps are included:

[0037] Step 1: Take a piece of polyester fabric 101 (50 mm long, 50 mm wide, 0.4 mm thick), wash it with anhydrous ethanol and deionized water for 5 minutes, and then dry it at 40° for later use;

[0038] Step 2: Prepare a nanosilver dispersion by placing 1 gram of nanosilver particle powder and 100 mL of deionized water in a magnetic stirrer and stirring until completely dissolved to prepare a 1% concentration nanosilver dispersion for later use;

[0039] Step 3: Take 5 ml of hexamethyldisiloxane into the first atomizing cup 202, and take 5 ml of the prepared 1% concentration nanosilver dispersion into the second atomizing cup 203;

[0040] Step 4: Set the gas flux in the first atomizing cup 202 containing hexamethyldisiloxane in step 3 to zero, the gas flux in the second atomizing cup 203 containing the nanosilver dispersion to 300 sccm, argon passes through the plasma excitation gas tube 204, and oxygen passes through the oxygen tube 205 to mix and pass into the plasma excitation gas and oxygen mixing passage 207, wherein the argon flux is 300 sccm and the oxygen flux is 10 sccm (e.g., Figure 2 );

[0041] Step 5: Place the clean polyester fabric 101 pretreated in step 1 flat on the center of the three-axis platform 102 controlled by the host computer;

[0042] Step 6: According to the settings of step 4, argon and oxygen are introduced to obtain a low-temperature plasma jet at atmospheric pressure in the plasma generator 201, and the jet contains nanosilver particles to perform a hydrophilic treatment on one side of the polyester fabric 101 placed in step 5;

[0043] Step 7: The host computer controls the three-axis platform 102 to follow the set route (such as Figure 3 ), dynamically treat the surface of the polyester fabric 101 to obtain the hydrophilic side 401 of the polyester fabric (such as Figure 4 );

[0044] Step 8: After step 7 is completed, the treated polyester fabric 101 is turned over and placed at the center of the three-axis platform 102;

[0045] Step 9: Set the gas flux in the first atomizing cup 202 filled with hexamethyldisiloxane to 700 scm, the gas flux in the second atomizing cup 203 filled with nanosilver dispersion to 300 sccm, the argon flux in the plasma excitation gas and oxygen mixing passage 207 to 300 sccm, and the oxygen flux to 10 sccm;

[0046] Step 10: Argon and oxygen are introduced to obtain a low-temperature plasma jet at atmospheric pressure in the plasma generator 201, and hexamethyldisiloxane is decomposed and recombined in the jet to generate SiO x The particulate matter, while the jet contains nano silver particles, performs a hydrophobic treatment on one side of the polyester fabric 101 placed in step eight;

[0047] Step 11: The host computer controls the three-axis platform 102 to follow the set route (such as Figure 3 ), dynamically treat the surface of the polyester fabric 101 to obtain the hydrophobic side 402 of the polyester fabric ( Figure 4 ).

[0048] The power supply adopts AC sinusoidal power supply, and uses pulse modulator to modulate the power duty cycle. Its specific parameters are: voltage 12.8kV, frequency 4kHz, duty cycle 60%;

[0049] The route of the reciprocating treatment of the polyester fabric 101 is set to be 40 mm in a straight line with an interval of 5 mm, and the moving speed is adjusted to 3 mm / s. The reciprocating movement is performed five times in step 7 and ten times in step 11. Finally, an antibacterial "oil-water diode" membrane (such as Figure 4-Figure 6 ).

[0050] The above specific implementation method part specifically introduces the analytical method involved in the present invention. It should be noted that the above introduction is only to help those skilled in the art better understand the method and ideas of the present invention, rather than limiting the relevant content. Without departing from the principle of the present invention, those skilled in the art may also make appropriate adjustments or modifications to the present invention, and the above adjustments and modifications shall also fall within the scope of protection of the present invention.

Claims

1. A method for preparing an antibacterial "oil-water diode" membrane by direct dry method using atmospheric pressure plasma jet, characterized in that: The specific steps are as follows: Step 1: Pre-treat the polyester fabric; Step 2: Prepare a nanosilver dispersion, mix the nanosilver particles with deionized water in a certain ratio, and stir in a magnetic stirrer until the suspension is complete for later use; Step 3: Take hexamethyldisiloxane into the first atomizing cup, and take the prepared nanosilver dispersion into the second atomizing cup; Step 4: setting the gas flux in the first atomizing cup filled with hexamethyldisiloxane in step 3 to zero, the gas flux in the second atomizing cup filled with nanosilver dispersion to non-zero, and the flux in the mixing passage of plasma excitation gas and oxygen to non-zero; Step 5: Place the clean polyester fabric that has been pretreated in step 1 flat on the center of the three-axis platform; Step 6: According to the settings of step 4, plasma excitation gas and oxygen are introduced to obtain a low-temperature plasma jet at atmospheric pressure, and the jet contains nanosilver particles to perform hydrophilic treatment on one side of the polyester fabric placed in step 5; Step 7: The host computer controls the three-axis platform to dynamically process the surface of the polyester fabric according to the set route; Step 8: After step 7 is completed, turn the treated polyester fabric over and place it in the center of the three-axis platform; Step 9: setting the gas flux in the first atomizing cup filled with hexamethyldisiloxane in step 4 to be non-zero, the gas flux in the second atomizing cup filled with nanosilver dispersion to be non-zero, and the flux in the mixing passage of plasma excitation gas and oxygen to be non-zero; Step 10: According to the settings of step 9, plasma excitation gas and oxygen are introduced to obtain an atmospheric pressure low-temperature plasma jet. Hexamethyldisiloxane is decomposed and recombined in the jet to generate SiO x The particulate matter, while the jet contains nano silver particles, performs a hydrophobic treatment on one side of the polyester fabric placed in step eight; Step 11: The host computer controls the three-axis platform to dynamically process the surface of the polyester fabric according to the set route.

2. The method for preparing an antibacterial "oil-water diode" membrane by direct dry method of atmospheric pressure plasma jet according to claim 1, characterized in that: The specific operation of step one is: take a piece of polyester cloth, wash it with anhydrous ethanol and deionized water for 5 minutes, and then dry it at 40°C for later use.

3. The method for preparing an antibacterial "oil-water diode" membrane by direct dry method using atmospheric pressure plasma jet according to claim 1, characterized in that: The plasma excitation gas in step six and step ten is an inert gas.

4. The method for preparing an antibacterial "oil-water diode" membrane by direct dry method using atmospheric pressure plasma jet according to claim 1, characterized in that: In step six and step nine, the oxygen flow rate is set to 10-30 sccm, the plasma excitation gas and oxygen mixing passage flow rate is set to 500-700 sccm, the plasma excitation gas flow rate in the hexamethyldisiloxane atomization cup is 500-800 sccm, and the plasma excitation gas flow rate in the nanosilver dispersion atomization cup is 300-500 sccm.

5. The method for preparing an antibacterial "oil-water diode" membrane by direct dry method using atmospheric pressure plasma jet according to claim 1, characterized in that: The power supply adopts an AC sinusoidal power supply and uses a pulse modulator to modulate the power supply duty cycle. The specific parameter ranges are: voltage 10-13kV, frequency 4-5kHz, and duty cycle 50-70%.

6. The method for preparing an antibacterial "oil-water diode" membrane by direct dry method using atmospheric pressure plasma jet according to claim 1, characterized in that: In step 7 and step 11, according to the size of the polyester fabric in step 1, the route for reciprocating processing of the polyester fabric is set to process 40mm in a straight line with an interval of 5mm, and the moving speed is adjusted between 1 and 4mm / s. In step 7, the fabric is moved back and forth five times, and in step 11, the fabric is moved back and forth ten times. The processing time is changed by adjusting the moving speed and the number of reciprocating times.