Double-electret polylactic acid nanofiber filter membrane and preparation method thereof
A dual-electret polylactic acid nanofiber filter membrane, prepared with ZIF-8 nanoparticles and electrospinning, addresses the limitations of traditional materials by enhancing dielectric properties and charge storage, achieving high filtration efficiency and biodegradability.
Patent Information
- Application Number
- CN202411473182.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-22
- Publication Date
- 2024-12-06
AI Technical Summary
Traditional polymer fiber filter materials face issues such as short charge life, rapid attenuation in filtration performance, and high plastic pollution due to low dielectric constant and charge storage capacity, while existing water electret processes are complex and inefficient, and difficult to improve dielectric properties of polylactic acid fibers.
A dual-electret polylactic acid nanofiber filter membrane is prepared by mixing ZIF-8 nanoparticles with polylactic acid using microwave-assisted aqueous dispersion and electrospinning technology, enhancing dielectric properties and charge storage capacity.
The membrane achieves high filtration efficiency, good biocompatibility, and degradability with a large specific surface area, dielectric constant, and stable electrostatic potential, reducing plastic pollution.
Smart Images

Figure CN119075711A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fully degradable filter fiber membranes, and in particular to a dual-electret polylactic acid nanofiber filter membrane and a preparation method thereof. Background Art
[0002] As a focal issue affecting public health, ecological environment and economic development worldwide, fine particulate matter (PM2.5) in polluted air is easily inhaled into the lungs due to its small size, complex composition and strong penetrability. After entering the heart, liver, kidneys and almost all human organs through the blood, it can even cross the blood-brain barrier and enter the brain, seriously endangering human health. According to statistics, only 0.18% of the world's land area (corresponding to 0.001% of the population) has an annual average PM2.5 concentration that does not exceed the health limit recommended by the World Health Organization (≤5μg / m 3 ). In order to cut off PM2.5 pollution and virus aerosol transmission, polymer fiber air filter materials are currently widely used for air purification.
[0003] Traditional polymer fiber filter materials often use non-degradable melt-blown polypropylene or polyvinylidene fluoride, and are combined with electret treatment to obtain electrostatic adsorption, but most of them are low-level shallow trap charges, which are easily dissipated in hot and humid environments and haze environments, resulting in short charge life, rapid attenuation of filtration performance, and short effective protection period. Frequent replacement produces a large amount of plastic pollution and microplastic hazards. Although polylactic acid (PLA) has become the most promising fiber filter material due to its good biodegradability, high mechanical strength and easy processing, it is difficult to meet its application in the field of air filtration due to its low dielectric constant, poor polarization effect, and low charge storage capacity. In order to improve this defect, the polylactic acid fiber membrane is usually modified by improving the electret method and adding various inorganic and organic materials.
[0004] In recent years, water electret treatment technology has received widespread attention due to its excellent charge storage stability. Currently, the water electret process on the market is mostly used to treat meltblown nonwoven fabrics, which has the following problems: (1) The existing water electret process is complex, costly, and inefficient; (2) The fiber diameter of meltblown nonwoven fabrics is in the micron range, which is not easy to intercept fine particles; (3) It is difficult to effectively improve the dielectric properties and charge storage capacity of fiber materials by water electret alone.
[0005] Metal-organic frameworks (MOFs) composed of metal ions and organic ligands are an emerging porous crystalline material with extremely high specific surface area, controllable pore size, excellent biocompatibility and biodegradability. Among them, zeolitic imidazolate framework-8 (ZIF-8) is a special type of MOFs material with strong adsorption, large porosity and specific surface area, adjustable pore size, high thermal stability, etc. In addition, it also has high zeta potential and polar functional groups, which provides the possibility for ZIF-8 to be used as an electret to improve the dielectric properties of fibers. Summary of the invention
[0006] Purpose of the invention: The technical problem to be solved by the present invention is to provide a dual-electret polylactic acid nanofiber filter membrane and a preparation method thereof in view of the deficiencies of the prior art. This filter membrane not only has a series of advantages such as large specific surface area, good dielectric properties, high surface potential, and excellent filtration performance, but also has good biocompatibility and degradability, and the preparation process is simple and the conditions are mild. It is a high-performance air filtration material with broad application prospects.
[0007] The invention provides a bi-electret polylactic acid nanofiber filter membrane, wherein the filter membrane is prepared by electrostatic spinning of ZIF-8 / water dispersion, polylactic acid and an organic solvent, and the specific surface area of the filter membrane is 274-550 m 2 / g, dielectric constant is 2.5~3.4F / m, surface potential is 8~12kV, PM2.5 filtration efficiency is 95.6~99.9%, and air resistance is less than 90Pa.
[0008] The present invention also provides a method for preparing a dual-electret polylactic acid nanofiber filter membrane, comprising the following steps:
[0009] Step 1, preparing an aqueous dispersion containing ZIF-8 nanoparticles: dissolving zinc salt and 2-methylimidazole in deionized water to obtain a zinc salt solution and a 2-methylimidazole solution;
[0010] The zinc salt solution and the 2-methylimidazole solution are mixed and placed in a microwave reactor to prepare an aqueous dispersion containing ZIF-8 nanoparticles;
[0011] Step 2, preparing an electrospinning mixed solution: dissolving polylactic acid in an organic solvent to prepare a polylactic acid spinning stock solution, and adding an aqueous dispersion containing ZIF-8 nanoparticles into the polylactic acid spinning stock solution to prepare an electrospinning mixed solution;
[0012] Step 3, preparing a bi-electret polylactic acid nanofiber filter membrane: using electrospinning technology to prepare an electrospinning mixed solution into a bi-electret polylactic acid nanofiber filter membrane with high dielectric properties.
[0013] In step 1, the zinc salt is at least one of zinc nitrate, zinc chloride, zinc sulfate and zinc acetate.
[0014] In step 1, the concentration of the zinc salt is 0.02 to 2 mol / L.
[0015] In step 1, the molar ratio of 2-methylimidazole to zinc salt is 20:1 to 4:1.
[0016] In step 1, the output power of the microwave reactor is 500-6000W, the reaction temperature is 80-200°C, and the reaction time is 1-40 minutes.
[0017] In step 2, the organic solvent is at least one of chloroform, acetone, ethyl acetate, dimethylformamide, ethanol, dichloromethane, and chloroform.
[0018] In step 2, the concentration of polylactic acid in the polylactic acid spinning solution is 0.5 to 30 wt%.
[0019] In step 2, the volume ratio of the polylactic acid spinning solution to the aqueous dispersion containing ZIF-8 nanoparticles is 50:1 to 2:1.
[0020] In step 3, the electrospinning technology is used, including: the electrospinning voltage is 12 to 40 kV, the spinning solution consumption rate is 0.5 to 8 mL / h, the receiving distance is 12 to 24 cm, the temperature is 0 to 40°C, the relative humidity is 30 to 90%, and the average diameter of the obtained bipolar polylactic acid nanofibers is 10 to 400 nm, and the thickness of the bipolar polylactic acid nanofiber filter membrane is 20 to 180 μm.
[0021] Beneficial effects:
[0022] In order to meet the demand for high-efficiency air filtration materials, the present invention adopts microwave-assisted preparation of an aqueous dispersion containing ZIF-8 nanoparticles, mixes it with a polylactic acid spinning stock solution, and prepares a double-electret polylactic acid fiber air filtration membrane with high dielectric properties and high surface potential through electrospinning technology. The filtration membrane not only has a series of advantages such as large specific surface area, good dielectric properties, high surface potential, and excellent filtration performance, but also has good biocompatibility and degradability. The preparation process is simple and the conditions are mild. It is a high-performance air filtration material with broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.
[0024] Figure 1 It is a flow chart of the method of the present invention.
[0025] Figure 23 is a scanning electron microscope image of the dual-electret polylactic acid nanofiber membrane in Example 1. DETAILED DESCRIPTION
[0026] In Example 1 of the present invention, a dual-electret polylactic acid nanofiber filter membrane and a preparation method thereof are provided, comprising the following steps:
[0027] Step 1, preparing an aqueous dispersion containing ZIF-8 nanoparticles: zinc acetate (0.05 mol / L) and 2-methylimidazole (the molar ratio of 2-methylimidazole to zinc acetate is 10:1) are respectively dissolved in deionized water, and the zinc salt solution and the 2-methylimidazole solution are mixed and placed in a microwave reactor (140° C., 10 min) to prepare an aqueous dispersion containing ZIF-8 nanoparticles;
[0028] Step 2, preparing an electrospinning mixed solution: polylactic acid is dissolved in dichloromethane / dimethylformamide (mass ratio 7:3) to prepare a polylactic acid spinning solution, the concentration of polylactic acid in the solution is 10wt%, and the ZIF-8 aqueous dispersion prepared in step 1 (the volume ratio of polylactic acid spinning solution to ZIF-8 aqueous dispersion is 10:1) is added to the spinning solution to prepare an electrospinning mixed solution;
[0029] Step 3, preparation of bipolar polylactic acid nanofiber membrane: the mixed solution prepared in step 2 is used to prepare a bipolar polylactic acid nanofiber membrane with high dielectric properties through electrospinning technology (voltage 25 kV, solution consumption rate 1 mL / h, receiving distance 18 cm, temperature 27°C, relative humidity 50%), and the average diameter of the obtained fiber is 150 nm, and the fiber membrane thickness is 90 μm.
[0030] In Example 2 of the present invention, a dual-electret polylactic acid nanofiber filter membrane and a preparation method thereof are provided, comprising the following steps:
[0031] Step 1, preparing an aqueous dispersion containing ZIF-8 nanoparticles: zinc nitrate (0.1 mol / L) and 2-methylimidazole (the molar ratio of 2-methylimidazole to zinc acetate is 8:1) are respectively dissolved in deionized water, and the zinc salt solution and the 2-methylimidazole solution are mixed and placed in a microwave reactor (160° C., 8 min) to prepare an aqueous dispersion containing ZIF-8 nanoparticles;
[0032] Step 2, preparing an electrospinning mixed solution: polylactic acid is dissolved in dichloromethane / chloroform (mass ratio 5:5) to prepare a polylactic acid spinning solution, the concentration of polylactic acid in the solution is 12wt%, and the ZIF-8 aqueous dispersion prepared in step 1 (the volume ratio of polylactic acid spinning solution to ZIF-8 aqueous dispersion is 8:1) is added to the spinning solution to prepare an electrospinning mixed solution;
[0033] Step 3, preparing a bi-electret polylactic acid nanofiber membrane: The mixed solution prepared in step 2 is used to prepare a bi-electret polylactic acid nanofiber membrane with high dielectric properties through electrospinning technology (voltage 20 kV, solution consumption rate 0.6 mL / h, receiving distance 20 cm, temperature 30°C, relative humidity 40%). The average diameter of the obtained fiber is 250 nm and the fiber membrane thickness is 100 μm.
[0034] In Example 3 of the present invention, a dual-electret polylactic acid nanofiber filter membrane and a preparation method thereof are provided, comprising the following steps:
[0035] Step 1, preparing an aqueous dispersion containing ZIF-8 nanoparticles: zinc acetate (0.08 mol / L) and 2-methylimidazole (the molar ratio of 2-methylimidazole to zinc acetate is 15:1) are respectively dissolved in deionized water, and the zinc salt solution and the 2-methylimidazole solution are mixed and placed in a microwave reactor (120° C., 15 min) to prepare an aqueous dispersion containing ZIF-8 nanoparticles;
[0036] Step 2, preparing an electrospinning mixed solution: polylactic acid is dissolved in dichloromethane / dimethylformamide (mass ratio 8:2) to prepare a polylactic acid spinning solution, the concentration of polylactic acid in the solution is 8wt%, and the ZIF-8 aqueous dispersion prepared in step 1 (the volume ratio of polylactic acid spinning solution to ZIF-8 aqueous dispersion is 15:1) is added to the spinning solution to prepare an electrospinning mixed solution;
[0037] Step 3, preparing a bi-electret polylactic acid nanofiber membrane: The mixed solution prepared in step 2 is used to prepare a bi-electret polylactic acid nanofiber membrane with high dielectric properties through electrospinning technology (voltage 18 kV, solution consumption rate 1.5 mL / h, receiving distance 22 cm, temperature 24°C, relative humidity 30%). The average diameter of the obtained fiber is 170 nm and the fiber membrane thickness is 60 μm.
[0038] In Example 4 of the present invention, a dual-electret polylactic acid nanofiber filter membrane and a preparation method thereof are provided, comprising the following steps:
[0039] Step 1, preparing an aqueous dispersion containing ZIF-8 nanoparticles: zinc nitrate (0.15 mol / L) and 2-methylimidazole (the molar ratio of 2-methylimidazole to zinc acetate is 20:1) are respectively dissolved in deionized water, and the zinc salt solution and the 2-methylimidazole solution are mixed and placed in a microwave reactor (200° C., 5 min) to prepare an aqueous dispersion containing ZIF-8 nanoparticles;
[0040] Step 2, preparing an electrospinning mixed solution: polylactic acid is dissolved in dichloromethane / acetone (mass ratio 6:4) to prepare a polylactic acid spinning solution, the concentration of polylactic acid in the solution is 9wt%, and the ZIF-8 aqueous dispersion prepared in step 1 (the volume ratio of polylactic acid spinning solution to ZIF-8 aqueous dispersion is 20:1) is added to the spinning solution to prepare an electrospinning mixed solution;
[0041] Step 3, preparing a bi-electret polylactic acid nanofiber membrane: The mixed solution prepared in step 2 is used to prepare a bi-electret polylactic acid nanofiber membrane with high dielectric properties through electrospinning technology (voltage 23 kV, solution consumption rate 2 mL / h, receiving distance 17 cm, temperature 32°C, relative humidity 45%). The average diameter of the obtained fiber is 200 nm and the fiber membrane thickness is 80 μm.
[0042] Comparative Example 1 (addition of ZIF-8 nanoparticles)
[0043] The polylactic acid nanofiber filter membrane was prepared basically by the method of Example 1. The difference is that in this example, only ZIF-8 nanoparticles were added as electrets to be mixed with the polylactic acid spinning solution. Specifically, zinc acetate (0.05 mol / L) and 2-methylimidazole (the molar ratio of 2-methylimidazole to zinc acetate is 10:1) were respectively dissolved in deionized water, the zinc salt solution and the 2-methylimidazole solution were mixed and placed in a microwave reactor (140°C, 10 min) to prepare an aqueous dispersion containing ZIF-8 nanoparticles, the dispersion was centrifuged (7000 rpm, 10 min), washed three times with deionized water, and then dried in an oven at 60°C for 24 h to obtain ZIF-8 nanocrystals with a rhombic dodecahedral morphology and a particle size of 200 to 300 nm; polylactic acid was dissolved in A polylactic acid spinning solution was prepared in dichloromethane / dimethylformamide (mass ratio 7:3), wherein the concentration of polylactic acid in the solution was 10 wt %. The prepared ZIF-8 nanocrystals (the mass ratio of polylactic acid to ZIF-8 was 10:1) were added into the spinning solution to prepare an electrospinning mixed solution. The mixed solution was subjected to electrospinning technology (voltage 25 kV, solution consumption rate 1 mL / h, receiving distance 18 cm, temperature 27°C, relative humidity 50%) to prepare a ZIF-8 single electret polylactic acid nanofiber membrane, and the obtained fiber had an average diameter of 210 nm and a fiber membrane thickness of 120 μm.
[0044] Comparative Example 2 (adding aqueous dispersion containing ZIF-8 nanoparticles by electrospraying)
[0045] The bi-electret polylactic acid nanofiber filter membrane was prepared by basically adopting the method of Example 2. The difference is that in this example, the aqueous dispersion containing ZIF-8 nanoparticles was added into the polylactic acid nanofiber membrane by electrospraying. Specifically, zinc nitrate (0.1 mol / L) and 2-methylimidazole (the molar ratio of 2-methylimidazole to zinc acetate is 8:1) are respectively dissolved in deionized water, and the zinc salt solution and the 2-methylimidazole solution are mixed and placed in a microwave reactor (160°C, 8 min) to prepare an aqueous dispersion containing ZIF-8 nanoparticles; polylactic acid is dissolved in dichloromethane / chloroform (mass ratio 5:5) to prepare a polylactic acid spinning solution, and the concentration of polylactic acid in the solution is 12wt%; during the electrospinning process of the polylactic acid spinning solution (voltage 20kV, solution consumption rate 0.6mL / h, receiving distance 20cm, temperature 30°C, relative humidity 40%), the aqueous dispersion containing ZIF-8 nanoparticles is added to the polylactic acid nanofiber membrane by electrospraying to prepare a bi-electret polylactic acid nanofiber membrane with high dielectric properties, and the obtained fiber has an average diameter of 280nm and a fiber membrane thickness of 90μm.
[0046] Comparative Example 3 (without adding aqueous dispersion containing ZIF-8 nanoparticles)
[0047] The polylactic acid nanofiber membrane was prepared by the method of Example 3, except that the aqueous dispersion containing ZIF-8 nanoparticles was not added in this example. Specifically, polylactic acid was dissolved in dichloromethane / dimethylformamide (mass ratio 8:2) to prepare a polylactic acid spinning solution, the concentration of polylactic acid in the solution was 8wt%, and the polylactic acid nanofiber membrane was prepared by electrospinning technology (voltage 18kV, solution consumption rate 1.5mL / h, receiving distance 22cm, temperature 24°C, relative humidity 30%), and the average diameter of the obtained fiber was 300nm, and the fiber membrane thickness was 120μm.
[0048] Structural characterization and performance testing:
[0049] Scanning electron microscope observation: The microstructure of the double-electret polylactic acid nanofiber membrane was observed by field emission scanning electron microscope (model JSM-7900F, Japan Electronics Co., Ltd.) Figure 2 ).
[0050] Specific surface area test: The nitrogen adsorption isotherm was measured at 77 K using a gas adsorption instrument (ASAP 2060, Micromeritics, USA).
[0051] Surface potential test: A non-contact electrostatic meter (VM54XQS, Quatek, USA) was used to test the surface potential of the nanofiber membrane. The test height was 2 cm, the temperature and humidity were constant at 25°C and 45%, and 20 data points were randomly collected for each sample and the average value was taken.
[0052] Dielectric constant test: The dielectric constant of the sample was tested using a dielectric tester (WK-6500B, Wayne Kerr Electronic Co., Ltd., UK).
[0053] Filtration performance test: The air filtration performance of the fiber membrane (area 113.04 cm2) was tested using an LZC-K automatic filter material tester (Suzhou Huada Instrument Equipment Co., Ltd.), with the gas flow rate set to 85 L / min and the particle size range of the NaCl atomized particles generated by the aerosol generator being 0.1 to 10 μm. At least three different positions were tested for each group of fiber membranes, and the average value of the results was taken.
[0054] Experimental results: Figure 2 As shown, the fiber membrane is prepared by mixing the aqueous dispersion containing ZIF-8 nanoparticles with the polylactic acid spinning solution, which can realize the in-situ electret of ZIF-8 and water on the surface of the polylactic acid fiber. In Example 1, the surface of the polylactic acid fiber has a porous structure, which is caused by the evaporation of water molecules after electret in the fiber, and the appearance of "bulges" in the fiber indicates that the ZIF-8 crystals are loaded in the polylactic acid fiber. The dual electret of water molecules and ZIF-8 crystals in the polylactic acid fiber greatly improves the specific surface area, dielectric properties and surface charge of the fiber membrane.
[0055] Table 1 compares the specific surface area, dielectric properties and filtration performance test results of the dual electret polylactic acid nanofiber membranes obtained in the examples and comparative examples. Examples 1-4 and comparative examples 1 and 2 have a higher specific surface area (274.4 m 2 / g-550.2m 2 / g), this is because ZIF-8 crystals have a high specific surface area. A large amount of ZIF-8 crystals loaded on the fiber greatly increases the specific surface area of the fiber membrane, thereby effectively improving the surface roughness of the fiber membrane; the specific surface area of comparative example 3 is only 26.3m 2 / g, which is due to the lack of ZIF-8 crystal loading on the fiber.
[0056] Table 1
[0057]
[0058] Examples 1 to 4 all exhibit extremely high dielectric constants (2.5F / m-3.4F / m) and surface potentials (7.9kV-12.3kV), and the surface potential hardly decays over time. The electrostatic electret effect is significant and stable, confirming that the dual electret effect of ZIF-8 crystals and water can give the fiber membrane an extremely high electrostatic potential and excellent charge storage capacity. In particular, the dielectric constant of Example 1 is as high as 3.4F / m, the initial value of the surface potential is as high as 12.3kV, and the surface potential remains at 11.8kV after 30 days; the dielectric properties of Comparative Example 1 are relatively low, because the polylactic acid fiber membrane is only loaded with ZIF-8 crystals, and its electret effect is significantly lower than the double electret of ZIF-8 and water; the dielectric properties of Comparative Example 2 are also poor, which may be because the aqueous dispersion containing ZIF-8 crystals is not completely loaded on the fiber membrane during the electrospraying process, making the electret effect of the polylactic acid fiber membrane not obvious; the dielectric constant of Comparative Example 3 is only 1.2F / m, and the surface potential is 2.3kV, because there is no electret on the polylactic acid fiber membrane.
[0059] The filtration performance of polylactic acid nanofiber membrane is closely related to the dielectric properties. Examples 1-4 with extremely high surface potential have a good effect on PM 0.3 and PM 2.5 The filtration efficiency of the nanofiber membranes is above 96%, and the air resistance is much lower than that of the traditional nanofiber membranes (all < 90Pa), which truly achieves high efficiency and low resistance. Among them, Example 1 with the highest surface potential performs best in the filtration test, PM 0.3 and PM 2.5 The filtration efficiencies of PM2.5 and PM3.5 were 97.8% and 99.9%, respectively, which were much higher than those of the comparative examples 1–3 (PM 0.3 and PM 2.5 The filtration efficiency is less than 94%).
[0060] This shows that the technical solution proposed in the present invention enables the dual-electret polylactic acid nanofiber filter membrane to have a high specific surface area, high dielectric properties and high filtration performance, which is likely due to: (1) the ZIF-8 crystals obtained by the microwave-assisted method have better structural regularity and are uniformly dispersed in water; (2) the two electrets, ZIF-8 and water molecules, synergistically improve the dielectric properties of the polylactic acid fiber membrane, so that it has a significant and stable electrostatic electret effect, which can effectively filter fine particles; (3) the loading of ZIF-8 crystals on the fiber and the pore structure formed by the evaporation of water molecules greatly increase the specific surface area of the polylactic acid fiber membrane and increase the probability of particle deposition on the fiber; (4) the "bulge + mesh" fiber structure formed by the dual electret of ZIF-8 crystals and water molecules makes the polylactic acid fiber membrane have a lower pressure drop.
[0061] The present invention provides a dual-electret polylactic acid nanofiber filter membrane and a preparation method thereof. There are many methods and approaches to specifically implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention. All components not specified in this embodiment can be implemented using existing technologies.
Claims
1. A dual-electret polylactic acid nanofiber filter membrane, characterized in that: The filter membrane is prepared by electrospinning ZIF-8 / water dispersion, polylactic acid and organic solvent, and the specific surface area of the filter membrane is 274-550m 2 / g, dielectric constant is 2.5~3.4F / m, surface potential is 8~12kV, PM2.5 filtration efficiency is 95.6~99.9%, and air resistance is less than 90Pa.
2. A method for preparing a dual-electret polylactic acid nanofiber filter membrane as claimed in claim 1, characterized in that: The steps include: Step 1, preparing an aqueous dispersion containing ZIF-8 nanoparticles: dissolving zinc salt and 2-methylimidazole in deionized water to obtain a zinc salt solution and a 2-methylimidazole solution; The zinc salt solution and the 2-methylimidazole solution are mixed and placed in a microwave reactor to prepare an aqueous dispersion containing ZIF-8 nanoparticles; Step 2, preparing an electrospinning mixed solution: dissolving polylactic acid in an organic solvent to prepare a polylactic acid spinning stock solution, and adding an aqueous dispersion containing ZIF-8 nanoparticles into the polylactic acid spinning stock solution to prepare an electrospinning mixed solution; Step 3, preparing a bi-electret polylactic acid nanofiber filter membrane: using electrospinning technology to prepare an electrospinning mixed solution into a bi-electret polylactic acid nanofiber filter membrane with high dielectric properties.
3. The method according to claim 2, characterized in that In step 1, the zinc salt is at least one of zinc nitrate, zinc chloride, zinc sulfate and zinc acetate.
4. The method according to claim 2, characterized in that: In step 1, the concentration of the zinc salt is 0.02 to 2 mol / L.
5. The method according to claim 2, characterized in that: In step 1, the molar ratio of 2-methylimidazole to zinc salt is 20:1 to 4:
1.
6. The method according to claim 2, characterized in that In step 1, the output power of the microwave reactor is 500-6000W, the reaction temperature is 80-200°C, and the reaction time is 1-40 minutes.
7. The method according to claim 2, characterized in that In step 2, the organic solvent is at least one of chloroform, acetone, ethyl acetate, dimethylformamide, ethanol, dichloromethane, and chloroform.
8. The method according to claim 2, characterized in that: In step 2, the concentration of polylactic acid in the polylactic acid spinning solution is 0.5 to 30 wt%.
9. The method according to claim 2, characterized in that: In step 2, the volume ratio of the polylactic acid spinning solution to the aqueous dispersion containing ZIF-8 nanoparticles is 50:1 to 2:
1.
10. The method according to any one of claims 2 to 9, characterized in that: In step 3, the electrospinning technology is used, including: the electrospinning voltage is 12 to 40 kV, the spinning solution consumption rate is 0.5 to 8 mL / h, the receiving distance is 12 to 24 cm, the temperature is 0 to 40°C, the relative humidity is 30 to 90%, and the average diameter of the obtained bipolar polylactic acid nanofibers is 10 to 400 nm, and the thickness of the bipolar polylactic acid nanofiber filter membrane is 20 to 180 μm.
Citation Information
Cited By
Multi-micropore refined low-resistance-consumption fiber membrane as well as preparation method and application thereof
CN120174544A