Gas absorber, gas separation material, filter, and gas separation device
By combining polymer compound particles with amino groups and small particle size particles in the gas absorption material, the problem of high energy cost in the CCS process is solved, efficient gas absorption and diffusion is achieved, and process costs are reduced.
Patent Information
- Application Number
- CN202411209943.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-05-21
- Filing Date
- 2020-05-21
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, the energy cost is high during the carbon dioxide capture and storage (CCS), especially the carbon dioxide separation and recovery process occupies most of the energy cost, and the gas absorption/release performance of existing gas absorbing materials is not good at high temperatures.
The gas absorbing material containing polymer compound particles having an amino group and particles with a particle size of 1000 nm or less is used to form a composite material through dry mixing and pressurization forming to improve the absorption rate and diffusion rate of the gas, and to optimize the structure of the particles and Surface modifications are made to enhance gas reversible absorption properties.
It significantly improves the gas absorption rate and diffusion rate, reduces the energy cost of the gas separation and recovery process, and maintains excellent gas reversible absorption performance at high temperatures.
Smart Images

Figure CN119075936A_ABST
Abstract
Description
[0001] This application is a divisional application, and the Chinese national application number of the application to which it is directed is 202080036733.4, the application date is May 21, 2020, and the name of the invention is "Gas absorption material, gas absorber, gas separation material, filter and gas separation device". Technical Field
[0002] The present invention relates to a gas absorbent having excellent reversible absorption performance for gases such as carbon dioxide, a gas absorber using the gas absorbent, a gas separation material, a filter, and a gas separation device. Background Art
[0003] In recent years, global warming caused by carbon dioxide discharged from large facilities such as thermal power plants, steel mills, and cement plants, and environmental pollution caused by hydrogen sulfide and the like have become problems. In order to curb such climate change and environmental pollution and realize a low-carbon society, research has been conducted on a method (CCS; Carbon dioxide Capture and Storage) of separating and recovering acidic gases such as carbon dioxide and hydrogen sulfide from the exhaust gas containing a large amount of water vapor discharged from these large facilities and sealing them underground or under the sea. However, the energy cost associated with CCS has become very high with current technology, and a significant reduction in energy costs is required. In particular, the separation and recovery process of carbon dioxide accounts for about 60% of the energy cost under CCS, so in order to reduce the energy cost under CCS, the high efficiency and significant energy saving of the separation and recovery process of carbon dioxide are indispensable. Furthermore, in the field of energy supply, processes for separating and recovering carbon dioxide, acidic gases such as hydrogen sulfide, and water vapor from fuel gases such as natural gas with a high carbon dioxide concentration, coal gas generated in integrated coal gasification combined power generation (IGCC), and hydrogen used in fuel cells are being developed. Improving the efficiency and energy saving of separation and recovery processes for carbon dioxide and the like is also important in reducing energy costs in such fields.
[0004] Here, the separation and recovery of gas is specifically carried out by using a gas reversible absorption process of diffusion after temporarily absorbing the target gas for separation and recovery. Therefore, in order to achieve the above-mentioned reduction in energy costs, the development of gas absorbent materials that can effectively absorb / diffuse acidic gases such as carbon dioxide at low cost is actively carried out.
[0005] For example, Patent Documents 1 and 2 propose the use of gel particles of a polymer compound having an amino group as a gas absorbent. The gel particles exhibit the following gas absorption / release performance: at a temperature of about 30°C, the alkalinity is high and carbon dioxide is absorbed, but when heated to about 75°C, the alkalinity decreases and carbon dioxide is released. By utilizing such performance, a gas absorbent having excellent gas reversible absorption performance and low cost can be provided.
[0006] Previous technical literature
[0007] Patent Literature
[0008] Patent Document 1: International Publication No. 2016 / 024633
[0009] Patent Document 2: International Publication No. 2017 / 146231 Summary of the invention
[0010] Technical issues to be solved by the invention
[0011] As described above, it is known that gel particles of polymer compounds having amino groups have excellent gas absorption / release performance. The present inventors have confirmed that when evaluating the practicality of the gel particles, excellent gas absorption / release performance can be obtained by actually making the gel particles into a film or filling them into a column. On the other hand, if the gas absorption / release performance is to be further improved, it is limited by only making it into a film or filling it into a column, and it is judged that it is necessary to work on it from a new perspective.
[0012] Therefore, in order to solve such problems in the prior art, the present inventors conducted research with the purpose of providing a gas-absorbing material having a higher gas absorption / diffusion rate using polymer compound particles having an amino group.
[0013] Means for solving technical problems
[0014] As a result of intensive research to solve the above-mentioned problems, the inventors have obtained the following knowledge: if fine particles with a primary particle size of 1000 nm or less are added to a gas absorbent using polymer compound particles having an amino group, the gas absorption rate and diffusion rate can be significantly improved. The present invention is proposed based on such knowledge, and specifically has the following structure.
[0015] [1] A gas-absorbing material comprising polymer compound particles having an amino group and fine particles having a primary particle size of 1000 nm or less (excluding the polymer compound particles having an amino group).
[0016] [2] The gas-absorbing material according to [1], wherein
[0017] The microparticles are particles containing silicon dioxide or carbon.
[0018] [3] The gas-absorbing material according to [1] or [2], wherein
[0019] The water contact angle of the microparticles is 70° or more.
[0020] [4] The gas-absorbing material according to any one of [1] to [3], wherein
[0021] The fine particles are particles containing carbon black or fluororesin.
[0022] [5] The gas-absorbing material according to any one of [1] to [4], wherein
[0023] The fine particles include a substrate particle and a water-repellent coating formed on the surface of the substrate particle.
[0024] [6] The gas-absorbing material according to [5], wherein
[0025] The hydrophobic coating contains dialkyl polysiloxane.
[0026] [7] The gas-absorbing material according to any one of [1] to [4], wherein
[0027] The fine particles are fine particles in which the surface of the substrate particles is modified to impart water repellency.
[0028] [8] The gas-absorbing material according to [7], wherein
[0029] The surface modification is to introduce an alkyl group into the surface of the substrate particles.
[0030] [9] The gas-absorbing material according to any one of [5] to [8], wherein
[0031] The substrate particles are inorganic particles.
[0032]
[10] The gas-absorbing material according to any one of [5] to [9], wherein
[0033] The water contact angle of the substrate particles is 70° or more.
[0034]
[11] The gas-absorbing material according to any one of [1] to
[10] , wherein
[0035] The average primary particle size of the microparticles is 5 to 200 nm.
[0036]
[12] The gas-absorbing material according to any one of [1] to
[11] , wherein
[0037] The polymer compound particles having an amino group include a polymer of a monomer component including a substituted (meth)acrylamide monomer having an amino group.
[0038]
[13] The gas-absorbing material according to
[12] , wherein
[0039] The substituted (meth)acrylamide monomer having an amino group is N-(aminoalkyl) (meth)acrylamide.
[0040]
[14] The gas-absorbing material according to any one of [1] to
[13] , wherein
[0041] The median particle size of the polymer compound particles having an amino group in a dry state is 1 to 50 μm.
[0042]
[15] The gas-absorbing material according to any one of [1] to
[14] , wherein
[0043] The average primary particle size of the fine particles is smaller than the median particle size of the polymer compound particles having an amino group in a dry state.
[0044]
[16] The gas-absorbing material according to any one of [1] to
[15] , wherein
[0045] The content of the polymer compound particles having an amino group is greater than the content of the fine particles in terms of solid content.
[0046]
[17] A gas absorber comprising granulated particles of the gas absorbent according to any one of [1] to
[16] .
[0047]
[18] A gas absorber comprising a molded body comprising a mixture of the gas absorbent according to any one of [1] to
[16] and a thermoplastic resin.
[0048]
[19] The gas absorber according to
[16] , wherein
[0049] The mixture contains granulated particles of the gas-absorbent material as the gas-absorbent material.
[0050]
[20] A gas absorber comprising a powder compact of the gas absorber according to any one of [1] to
[16] .
[0051]
[21] The gas absorber according to any one of
[17] to
[20] , further comprising a filler.
[0052]
[22] The gas absorber according to
[21] , wherein
[0053] The filler is activated carbon or zeolite.
[0054]
[23] A method for producing a gas absorber, comprising the steps of placing a composite material obtained by dry-mixing polymer compound particles having an amino group and fine particles having a primary particle size of 1000 nm or less into a molding die and performing pressure molding.
[0055]
[24] A gas separation material comprising the gas absorption material according to any one of [1] to
[16] .
[0056]
[25] The gas separation material according to
[24] , wherein
[0057] Selectively separate acid gases from mixed gases.
[0058]
[26] The gas separation material according to
[25] , wherein
[0059] The acid gas is carbon dioxide.
[0060]
[27] A filter comprising the gas separation material according to any one of
[24] to
[26] .
[0061]
[28] A gas separation device comprising the gas separation material according to any one of
[24] to
[26] .
[0062] Effects of the Invention
[0063] The gas absorbing material and gas absorber of the present invention have fast gas absorption and diffusion speeds and show excellent gas reversible absorption performance. Therefore, by using the gas absorbing material and gas absorber of the present invention as a gas separation material, the time efficiency of the gas separation and recovery process is improved, and the cost associated with the process can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] Figure 1 is a scanning electron microscope photograph (SEM photograph) of the particles used in the examples, Figure 1 (a) is a SEM photograph of polymer particles 1 containing amino groups. Figure 1 (b) is a SEM photograph of a composite material of the amino group-containing polymer particles 1 and carbon black.
[0065] Figure 2 This is a SEM photograph showing the internal structure of a compact (gas absorber 1) obtained by compacting the composite material into a film shape.
[0066] Figure 3 is a transmission electron microscope photograph (TEM photograph) of the gas absorber 1. Figure 3 (a) is a TEM photograph of a thin slice cut from the gas absorber 1. Figure 3(b) is a TEM image of characteristic X-rays of nitrogen and carbon released by energy dispersive X-ray spectroscopy (EDX).
[0067] Figure 4 It is a graph showing the CO2 absorption amount during the absorption process of a gas absorber 1 comprising amino-containing polymer particles 1 and carbon black, a gas absorber 2 comprising amino-containing polymer particles 1 and hydrophobic carbon black, and a comparative gas absorber 1 comprising only amino-containing polymer particles 1.
[0068] Figure 5 It is a graph showing the CO2 diffusion amount during the diffusion process of a gas absorber 1 comprising amino-containing polymer particles 1 and carbon black, a gas absorber 2 comprising amino-containing polymer particles 1 and hydrophobic carbon black, and a comparative gas absorber 1 comprising only amino-containing polymer particles 1.
[0069] Figure 6 It is a graph showing the CO 2 absorption amount of the gas absorbers 1 and 3 to 6 including the amino group-containing polymer particles 1 and carbon black, RY200, R805, PTFE particles or hydrophilic silica 200 during the absorption process.
[0070] Figure 7 It is a graph showing the CO 2 diffusion amount in the diffusion process of the gas absorbers 1 and 3 to 6 including the amino group-containing polymer particles 1 and carbon black, RY200, R805, PTFE particles or hydrophilic silica 200 .
[0071] Figure 8 This is a graph showing the CO 2 absorption amount during the absorption process measured by the temperature swing absorption method for gas absorbers 3 and 6 including amino group-containing polymer particles 1 and RY200 or 200 and a comparative gas absorber 1 including only amino group-containing polymer particles 1.
[0072] Fig. 9 This is a graph showing the CO 2 diffusion amount in the diffusion process measured by the temperature swing absorption method for gas absorbers 3 and 6 including amino group-containing polymer particles 1 and RY200 or 200 and a comparative gas absorber 1 including only amino group-containing polymer particles 1.
[0073] Fig.10 It is a graph showing the diffusion-absorption cycle characteristics measured by the temperature swing absorption method for gas absorbers 3 and 6 including the amino group-containing polymer particles 1 and RY200 or 200 and the comparative gas absorber 1 including only the amino group-containing polymer particles 1.
[0074] Fig.11The SEM photographs are of particles of a mixture of a composite material (gas absorber 7) of amino group-containing polymer particles 1 and carbon black and polyethylene, and particles of a mixture (comparative gas absorber 2) of amino group-containing polymer particles 1 and polyethylene.
[0075] Fig.12 It is a graph showing the CO2 absorption amount during the absorption process and the CO2 diffusion amount during the diffusion process of particles of a mixture obtained by mixing a composite material of amino-containing polymer particles 1 and carbon black (gas absorbing material) and polyethylene (gas absorber 7), and particles of a mixture obtained by mixing amino-containing polymer particles 1 and polyethylene (comparison gas absorber 2).
[0076] Fig.13 This is the particle size distribution of a mixture of various amino-containing polymer crushed products and RY300.
[0077] Fig.14 It is a graph showing the CO2 absorption amount in the absorption process and the CO2 diffusion amount in the diffusion process of the gas absorbent 8 comprising a 7-centimeter-mesh amino-containing polymer crushed material and RY300, and the comparative gas absorbent 3 comprising only a 7-centimeter-mesh amino-containing polymer crushed material.
[0078] Fig.15 It is a curve chart showing the CO2 absorption amount during the absorption process of the gas absorbent 8 comprising a polymer crushed material containing amino groups crushed at 7 centimeters and RY300, and a crushed material (gas absorbent 9) which is a mixture of a polymer crushed material containing amino groups crushed at 1.5 centimeters and RY300 crushed using a bead mill.
[0079] Fig.16 This is a graph showing the change in particle size during the process of granulating a mixture of a polymer powder containing amino groups and RY300 pulverized to 7 centimeters by spraying a binder. Fig.16 (a) is the particle size distribution before granulation, Fig.16 (b) is the particle size distribution after granulation. DETAILED DESCRIPTION
[0080] Hereinafter, the present invention will be described in detail. The description of the constituent elements described below is sometimes completed based on representative embodiments and specific examples, but the present invention is not limited to such embodiments. In this specification, the numerical range represented by "to" refers to a range that includes the numerical values described before and after "to" as the lower limit and upper limit. In addition, in this specification, "(meth)acrylamide" refers to "acrylamide" and "methacrylamide". In addition, room temperature refers to 20°C.
[0081] <Gas Absorbent>
[0082] The gas-absorbing material of the present invention comprises polymer compound particles having an amino group and fine particles having a primary particle size of 1000 nm or less (excluding the “polymer compound particles having an amino group”).
[0083] In the present invention, “microparticles having a primary particle size of 1000 nm or less (excluding “polymer compound particles having an amino group”)” means microparticles having a primary particle size of 1000 nm or less in addition to polymer compound particles having an amino group. In the following description, “microparticles having a primary particle size of 1000 nm or less (excluding “polymer compound particles having an amino group”)” may be referred to simply as “microparticles”.
[0084] The gas-absorbing material has a high gas absorption rate and diffusion rate, a large gas absorption / diffusion amount, and exhibits excellent gas reversible absorption performance. This is presumably based on the following mechanism.
[0085] That is, as shown in the examples described below, if a gas absorbent material comprising polymer compound particles having an amino group and microparticles having a primary particle size of 1000 nm or less is formed, continuous pores that are not observed in a gas absorbent material to which no microparticles are added are formed inside the material. It is believed that the continuous pores effectively function as a gas diffusion phase. Therefore, in the gas absorbent material, the introduced gas easily penetrates into the interior, and as a result of effectively reacting with the amino groups of the polymer compound particles, the gas is fully absorbed in a short period of time. Furthermore, when gas is released from the polymer compound particles as conditions such as temperature changes and gas partial pressure changes, the released gas easily diffuses to the outside through the above-mentioned gas diffusion phase. Through such a mechanism, it is speculated that the gas absorbent material of the present invention exhibits a large gas absorption rate and gas diffusion rate, and exhibits excellent gas reversible absorption performance.
[0086] In particular, when the microparticles are hydrophobic microparticles, the continuous pores thereof become hydrophobic, and water is less likely to exist in the pores. As a result, the pores function more effectively as gas diffusion phases, and a more excellent gas reversible absorption performance is exhibited. Here, the meaning of "hydrophobic microparticles" can be referred to the description of the column [microparticles having a primary particle size of 1000 or less] below.
[0087] Hereinafter, the polymer compound particles having an amino group, the fine particles having a primary particle size of 1000 nm or less, and other materials added as necessary contained in the gas-absorbent of the present invention will be described.
[0088] [Polymer compound particles having amino groups]
[0089] The "polymer compound particles having an amino group" used in the present invention are particles containing a polymer compound having an amino group, and are preferably composed only of a polymer compound having an amino group, but may also contain materials used in preparing the particles, such as particle size adjusting components such as surfactants, polymers of (meth)acrylamide derivatives, crosslinking agents, unreacted monomers, etc.
[0090] (Polymer compound having an amino group)
[0091] The amino group of the polymer compound having an amino group can be any one of a primary amino group, a secondary amino group, and a tertiary amino group, but it is preferably designed with an acid dissociation constant of a conjugate acid. In particular, in order to dissolve carbon dioxide, it is preferred that the acid dissociation constant of the amino group is equal to or larger than the acid dissociation constant of carbonic acid. Among them, it is preferably a secondary or tertiary amino group, and more preferably a tertiary amino group. More preferably, dialkylamino groups such as dimethylamino groups are used. In addition, the amino group of the polymer compound can be bonded to the main chain or to the side chain, but it is preferably bonded to the side chain.
[0092] Furthermore, the polymer compound having an amino group preferably has a hydrophobic group. Examples of the hydrophobic group introduced into the polymer compound include X H 2X or C X H 2X+1 The hydrocarbon group represented by is preferably a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a tert-butyl group, a pentyl group, a cyclopentyl group, an isopentyl group, a hexyl group, a cyclohexyl group, etc. Among them, isobutyl group and tert-butyl group are more preferred. Alternatively, it may be a group in which a hydroxyl group is bonded to the above-mentioned hydrophobic group, such as a hydroxyethyl group, a hydroxypropyl group, and a hydroxybutyl group.
[0093] The polymer compound having an amino group used in the particles is not particularly limited, but examples thereof include (meth)acrylamide polymers and derivatives thereof, polyethyleneimine and derivatives thereof, polyethyleneamine and derivatives thereof, polyvinyl alcohol and derivatives thereof, polyallylamine and derivatives thereof, and the like, preferably (meth)acrylamide polymers, and more preferably acrylamide polymers. Specific constituent monomers for introducing amino groups include N,N-dimethylaminopropyl methacrylamide, N,N-diethylaminopropyl methacrylamide, N,N-dimethylaminoethyl methacrylamide, N,N-diethylaminoethyl methacrylamide, N,N-dimethylaminopropyl methacrylate, N,N-diethylaminopropyl methacrylate, N,N-dimethylaminoethyl methacrylate, N,N-diethylaminoethyl methacrylate, N,N-dimethylaminopropyl methacrylate, N,N-diethylaminoethyl methacrylate, N,N-dimethylaminopropyl methacrylate, N,N-diethylaminopropyl methacrylate, N,N-dimethylaminopropyl methacrylate, N,N-diethylaminoethyl methacrylate, N,N-dimethylaminopropyl methacrylate, N,N-dimethylaminopropyl methacrylate, N,N-diethylaminopropyl ... Acrylamide, N,N-diethylaminopropyl acrylamide, N,N-dimethylaminoethyl acrylamide, N,N-diethylaminoethyl acrylamide, 3-aminopropyl methacrylamide hydrochloride, 3-aminopropyl acrylamide hydrochloride, N,N-dimethylaminopropyl acrylate, N,N-diethylaminopropyl acrylate, N,N-dimethylaminoethyl acrylate, N,N-diethylaminoethyl acrylate, 3-aminopropyl methacrylate hydrochloride, 3-aminopropyl acrylate hydrochloride, etc.
[0094] In the polymer compound having an amino group, the polymer density in the particles in a dispersed state after the polymer compound particles are swollen in water is preferably 0.3 to 90%, more preferably 1 to 80%.
[0095] (Gelling Properties of Polymer Compound Particles Having Amino Groups)
[0096] The polymer compound particles having amino groups used in the present invention are preferably gelling polymer particles having amino groups. Here, "gelling polymer particles" refer to polymer particles having the property of swelling in water or polar solvents to become gel-like microparticles. Preferred gelling polymer particles are particles whose water content in the particles becomes 20 to 99.7% after being dispersed in water at 30°C and fully swollen. Furthermore, another preferred gelling polymer particle is a particle whose fluid dynamic diameter becomes 20nm to 1000μm (for example, 20 to 2000nm) after being dispersed in water at 30°C and fully swollen. Furthermore, the gelling polymer particles preferably have the following reversibility: after swelling and gelling in water or a polar solvent, after removing the water and polar solvent and drying, they are restored to the original gel state by adding water and polar solvent.
[0097] (Particle size of polymer compound particles having amino groups)
[0098] The median particle size of the polymer compound particles having an amino group used in the present invention in a dry state is preferably 5 nm to 500 μm (e.g., 5 nm to 50 μm), and more preferably 1 to 200 μm (e.g., 1 to 20 μm). The median particle size of the polymer compound particles having an amino group in a dry state can be measured by a dry laser diffraction particle size distribution measuring device. The parameter is preferably 20 or more, and more preferably 50 or more.
[0099] The hydrodynamic particle size after swelling the polymer compound particles having an amino group in water is preferably 10 nm to 1000 μm (e.g., 10 nm to 100 μm) in terms of the hydrodynamic diameter in water measured by the dynamic light scattering method, more preferably 50 nm to 500 μm (e.g., 50 nm to 50 μm), further preferably 100 nm to 200 μm (e.g., 100 nm to 20 μm), and still further preferably 200 nm to 100 μm (e.g., 200 nm to 10 μm). The "particle size after swelling in water" of the polymer compound particles is the particle size after the dried polymer compound particles are immersed in water at 30° C. for 24 hours, and refers to the average particle size measured by the dynamic light scattering method.
[0100] It is considered that when the particle size of the polymer compound particles having an amino group is within the above range, the diffusion distance of the molecules (gas molecules, ions derived from gas molecules) in the gel particles is within an appropriate range, and the gas absorption rate and diffusion rate tend to be further improved.
[0101] (Preparation of Polymer Compound Particles Having Amino Groups)
[0102] The polymer compound particles having amino groups can be prepared using a solution containing monomer components (hereinafter referred to as "particle preparation solution"). In this specification, "monomer components" refer to all monomers used for the synthesis of polymers of the polymer compound particles having amino groups. There are no particular restrictions on the method for preparing the polymer compound particles, and conventionally known methods such as precipitation polymerization, pseudo-precipitation polymerization, emulsion polymerization, dispersion polymerization, suspension polymerization, seed polymerization, bulk polymerization, and block polymerization can be used.
[0103] The monomer component used in the preparation of particles at least includes a monomer with an amino group, preferably includes a monomer with an amino group and a monomer without an amino group. That is, the polymer compound with an amino group can be a homopolymer or copolymer of a monomer with an amino group, or a copolymer of a monomer with an amino group and a monomer without an amino group. Thus, by controlling the ratio of these monomers, the density of the amino group of the polymer compound particles can be adjusted within an appropriate range. The monomer with an amino group and the monomer without an amino group used as required are preferably substituted (methyl) acrylamide monomers, more preferably substituted methacrylamide monomers.
[0104] For the description and preferred range of the amino group of the monomer having an amino group, reference can be made to the description in the column (polymer compound having an amino group). The number of amino groups possessed by the monomer is not particularly limited, and may be 1 or more than 2. When the monomer has more than 2 amino groups, each amino group may be the same or different.
[0105] The monomer having an amino group is not particularly limited, but N-(aminoalkyl)acrylamide, N-(aminoalkyl)methacrylamide, etc. can be cited, preferably N-(aminoalkyl)methacrylamide. For specific examples of monomers having an amino group, reference can be made to the description of "Specific constituent monomers" in the column about (polymer compounds having an amino group).
[0106] The monomer component preferably includes a monomer having an amino group and a monomer having a hydrophobic group. For the description and preferred range of the hydrophobic group of the monomer having a hydrophobic group, reference can be made to the description in the column (polymer compound having an amino group). The hydrophobic group is preferably present on the side chain. The monomer having a hydrophobic group may or may not have an amino group. By introducing a monomer having a hydrophobic group, the environment around the amino group can be made hydrophobic to appropriately adjust the acidity of the conjugate acid of the amino group.
[0107] The monomer having a hydrophobic group is not particularly limited, but examples thereof include N-alkyl acrylamide, N-alkyl methacrylamide, N-alkyl acrylate, N-alkyl methacrylate, N,N-dialkyl acrylamide, N-(hydroxyalkyl)methacrylamide, N,N-dialkyl acrylate, N-(hydroxyalkyl)methacrylate, N,N-dialkylmethacrylamide, N-(hydroxyalkyl)acrylamide, N,N-dialkyl methacrylate, N-(hydroxyalkyl)acrylamide, N,N-dialkyl methacrylate, and N-(hydroxyalkyl)acrylate. N-alkyl acrylamide is preferred.
[0108] As a preferred combination of a monomer having an amino group and a monomer having a hydrophobic group, a combination of N-(aminoalkyl)(meth)acrylamide and N-alkyl(meth)acrylamide can be mentioned, and a combination of N-(aminoalkyl)methacrylamide and N-alkylacrylamide is preferred. In particles containing a copolymer of N-(aminoalkyl)(meth)acrylamide and N-alkyl(meth)acrylamide, hydrophobic alkyl groups and hydrogen-bonding amides are uniformly distributed in the molecule in a balanced manner.
[0109] The ratio of the monomer having an amino group in the monomer component is preferably 1 to 95 mol%, more preferably 5 to 95 mol%, further preferably 30 to 85 mol%, for example, 30 to 60 mol%, relative to the total molar number of the monomer component. In addition, when the monomer component contains a monomer having a hydrophobic group, the molar ratio of the monomer having an amino group to the monomer having a hydrophobic group is preferably 95:5 to 5:95, more preferably 2:1 to 1:2. In addition, monomers having both an amino group and a hydrophobic group are classified as monomers having an amino group.
[0110] And, the monomer component can be set to the composition not containing the monomer without amino group (the monomer with amino group is 100 mol % composition), and the amount of the monomer without amino group can be set to a small amount (for example, less than 5 mol %). In these cases, the acid dissociation constant of the conjugate acid of amino group can be appropriately adjusted by increasing the crosslinking density or increasing the monomer concentration during polymerization.
[0111] The particle preparation liquid may contain only monomer components or other components. As other components, surfactants, cross-linking agents, polymerization initiators, pKa regulators, etc. can be cited. By adjusting the type and concentration of the surfactant added to the particle preparation liquid, the particle size of the obtained polymer compound particles can be controlled. In addition, by using a cross-linking agent, the swelling property of the particles can be controlled to avoid excessive swelling due to the formation of a cross-linked structure in the polymer compound within the particles. In addition, in the case where a cross-linking agent is used more or the monomer concentration during polymerization is set to a higher level, a cross-linked structure can also be formed between the particles. Thus, a relatively large continuous void structure can be formed between the composite particles connected by the cross-linked structure. In addition, the pKa regulator is used to adjust the pKa of the obtained polymer compound particles to a desired value, thereby enabling the absorption of the acidic gas in the target partial pressure region to change significantly with changes in temperature and partial pressure.
[0112] As the surfactant, a cationic surfactant such as cetyltrimethylammonium bromide or the like can be used.
[0113] As for the crosslinking agent, any crosslinking structure can be formed between the monomers used, and N,N'-alkylenebisacrylamide can be preferably used. The carbon number of the alkylene group of N,N'-alkylenebisacrylamide is not particularly limited, but is preferably 1 to 12, more preferably 1 to 4, and further preferably 1 to 2. Instead of the alkylene group, oligoethylene imine and oligoethylene glycol can be crosslinking agents that function as crosslinking agent chains.
[0114] As the pKa regulator, a substance that can protonate or deprotonate the amino group of the monomer can be used, and an acid such as hydrochloric acid or a base such as sodium hydroxide can be used by appropriately adjusting the concentration according to the desired pKa. In addition, the pKa of the polymer compound particles can also be controlled by the crosslinking ratio based on the crosslinking agent, so the crosslinking agent can also be used as a pKa regulator.
[0115] The solvent of the particle preparation solution is not particularly limited, but polar solvents such as water, methanol, ethanol, isopropanol, acetonitrile, N,N-dimethylformamide, and dimethyl sulfoxide can be cited, and a mixed solvent obtained by combining two or more of these polar solvents can also be used. Among them, water or a mixed solvent obtained by mixing water and other polar solvents is preferably used.
[0116] The polymer compound particles having an amino group can be supplied to the manufacture of the gas absorbent as dry particles (solid particles), or as gel particles obtained by swelling with a liquid, but can also be supplied to the manufacture of the gas absorbent as dry particles. The dry particles can be obtained, for example, by drying a suspension containing polymer compound particles having an amino group using a spray drying method or the like. Furthermore, a pulverized product obtained by pulverizing a gel that is an aggregate of gel particles can also be preferably used as the polymer compound particles having an amino group. The pulverization of the gel can be performed, for example, using a meat chopper.
[0117] [Microparticles with a primary particle size of 1000 nm or less]
[0118] In the present invention, fine particles having a primary particle size of 1000 nm or less are used in combination with polymer compound particles having an amino group (except for "polymer compound particles having an amino group").
[0119] The "primary particle size" of "fine particles having a primary particle size of 1000 nm or less" used in the present invention can be measured by transmission electron microscope observation. The "fine particles having a primary particle size of 1000 nm or less" used in the present invention preferably only contain fine particles having a primary particle size of 1000 nm or less.
[0120] The particle size of the microparticles used in the present invention is preferably 0.1nm to 1000nm, more preferably 0.3nm to 500nm, further preferably 0.5nm to 300nm, further preferably 1nm to 200nm, particularly preferably 1.5nm to 100nm, particularly preferably 2nm to 50nm, and most preferably 2.5nm to 25nm, in terms of average primary particle size. As a result, a gas diffusion phase is more reliably formed in the molded body of the gas absorbent material, and the absorption rate and diffusion rate of the gas tend to be further improved. The microparticles may be microparticles agglomerated from primary particles. The agglomerates are preferably 100nm to 200μm, more preferably 500nm to 100μm, and most preferably 2.5μm to 50μm.
[0121] The microparticles may be composed of inorganic materials, organic materials, or a combination of organic and inorganic materials. They may contain silicon dioxide or carbon, for example, carbon black or fumed silica. Furthermore, the microparticles may be hydrophobic microparticles or hydrophilic microparticles. Hydrophobic microparticles are particularly preferred when used in an environment where water vapor is easily condensed or condensed. As described above, when the microparticles are hydrophobic microparticles, the pores formed by the microparticles function more effectively as a gas diffusion phase.
[0122] Here, "hydrophobic particles" refer to particles having a primary particle size of 1000 nm or less and a water contact angle of 70° or more. The "water contact angle" of a particle refers to the contact angle with water measured on the surface of a particle deposition film formed by the particle. The water contact angle on the surface of the particle deposition film can be measured by static water contact angle measurement.
[0123] The water contact angle of the hydrophobic fine particles is preferably 80° or more, more preferably 100° or more, further preferably 110° or more, further preferably 120° or more, particularly preferably 130° or more, and most preferably 140° or more.
[0124] Hereinafter, constituent materials of water-repellent particles and other particles that can be used as particles of the gas-adsorbing material will be described.
[0125] (Hydrophobic particles)
[0126] The hydrophobic particles may be particles that have hydrophobicity themselves, or particles that have been imparted with hydrophobicity on the surface of particles that serve as a substrate (substrate particles). Examples of particles that have been imparted with hydrophobicity on the surface of substrate particles include coated particles that have formed a hydrophobic film on the surface of the substrate, and surface-modified particles that have been subjected to surface modification to impart hydrophobicity to substrate particles.
[0127] First, carbon black can be cited as the fine particles having water repellency in themselves. Examples of carbon black include acetylene black, furnace black, channel black, thermal black, lamp black, and Ketjen black, among which acetylene black is preferred.
[0128] Other water-repellent fine particles include fine particles made of CNovel (porous carbon, manufactured by Toyo Tanso Co., Ltd.), titanium oxide, mesoporous silica, and the like.
[0129] Furthermore, as the fine particles which have water repellency themselves, fine particles formed of a water repellent organic material can also be used. Examples of the water repellent organic material which can be used to form the particles include those composed of -(CA 1 A 2 -CA 3 A 4 )-represented by a fluororesin (wherein A 1 ~A 4 represents a hydrogen atom, a fluorine atom, a chlorine atom or a perfluoroalkyl group, A 1 ~A 4 At least one of the above is a fluorine atom). Specific examples of fluororesins include polytetrafluoroethylene (PTFE), copolymers of tetrafluoroethylene and other monomers, polychlorotrifluoroethylene (PCTFE), copolymers of chlorotrifluoroethylene and other monomers, polyvinylidene fluoride (PVDF), polyvinyl fluoride (PVF), polytetrafluoropropylene (HEP), etc. As copolymers of tetrafluoroethylene and other monomers, perfluoroalkoxyalkane (PFA: copolymer of tetrafluoroethylene and perfluoroalkyl vinyl ether), perfluoroethylene propylene copolymer (FEP: copolymer of tetrafluoroethylene and hexafluoropropylene), ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-perfluorodifuran copolymer (TFE / PDD), etc. can be mentioned. In addition, as copolymers of chlorotrifluoroethylene and other monomers, ethylene-chlorotrifluoroethylene copolymer (ECTFE) can be mentioned.
[0130] These water-repellent organic materials may be used alone or in combination of two or more.
[0131] The substrate particles of the coated particles and surface-modified particles may be inorganic particles or organic particles, but are preferably inorganic particles. Furthermore, if the particles themselves are hydrophobic, and a hydrophobic coating is applied to the particles to impart hydrophobic surface modification, the gas absorption / diffusion amount can be increased along with the gas absorption rate and diffusion rate.
[0132] As inorganic particles, known inorganic particles can be used, and carbon blacks such as acetylene black, furnace black, channel black, thermal black, lamp black, Ketjen black, etc., oxides of metal elements or semi-metal elements, hydroxides, nitrides, halides, carbonates, sulfates, acetates, phosphates, etc., particles of inorganic compounds, natural mineral particles, etc. can be cited. As inorganic compounds of metal elements or semi-metal elements, lithium fluoride, calcium carbonate, calcium phosphate, calcium sulfate, calcium fluoride, barium sulfate, titanium dioxide (t itania), zirconium dioxide (zirconium oxide), aluminum oxide (alumina), aluminum silicate (alumina silicate, kaolin, kaolinite), silicon oxide (silicon dioxide, silica gel), etc. can be cited, and as natural minerals, talc, clay, etc. can be cited. Among these, particles containing carbon black and silicon oxide are preferred.
[0133] As the organic particles, known organic particles can be used, and examples thereof include particles containing styrene-based, acrylic-based, melamine-based, benzoguanamine-based, and silicone-based polymers. In this case, a filler may be used in combination, and for example, activated carbon or zeolite can be preferably used as the filler.
[0134] In the hydrophobic film formed on the substrate particles, in addition to the above-mentioned hydrophobic organic materials exemplified as hydrophobic materials that can be used for the formation of microparticles, films of organopolysiloxane and organohydrogenpolysiloxane can also be used. As organopolysiloxane, dialkylpolysiloxane and alkylphenylpolysiloxane can be mentioned, and as organohydrogenpolysiloxane, alkylhydrogenpolysiloxane can be mentioned. The alkyl group in dialkylpolysiloxane, alkylphenylpolysiloxane and alkylhydrogenpolysiloxane can be any of linear, branched and cyclic, but is preferably linear. The number of carbon atoms in the alkyl group is preferably 1 to 20, more preferably 1 to 10, and further preferably 1 to 6. Here, the two alkyl groups bonded to the silicon atom may be the same as each other or different from each other. As specific examples of organopolysiloxane, dimethylpolysiloxane, methylphenylpolysiloxane, etc. can be mentioned, and as specific examples of organohydrogenpolysiloxane, methylhydrogenpolysiloxane, etc. can be mentioned.
[0135] As a surface modification method for substrate particles, there can be cited a method of introducing a hydrophobic group such as an alkyl group or a fluorinated alkyl group into the surface of the substrate particles. The alkyl group or the fluorinated alkyl group introduced into the substrate particles may be any of a linear, branched, or cyclic type, but is preferably a linear type. The number of carbon atoms of the alkyl group or the fluorinated alkyl group is preferably 1 to 20, more preferably 1 to 15, and further preferably 1 to 10. Furthermore, the fluorinated alkyl group may be a partially fluorinated alkyl group in which a part of the hydrogen atoms of the alkyl group are replaced by fluorine atoms, or may be a perfluoroalkyl group in which all the hydrogen atoms are replaced by fluorine atoms.
[0136] The surface modification of the substrate particles by introducing these hydrophobic groups can be carried out using a silane coupling agent, a silane compound such as silazane, etc. Examples of the silane coupling agent include compounds represented by the following general formula (1).
[0137] General formula (1)
[0138] R 1 n SiX (4-n)
[0139] (In the general formula (1), X represents a hydrolyzable group that generates a silanol group by hydrolysis, and R 1 represents a group containing a hydrophobic group. n is an integer of 1 to 3. )
[0140] In the silane coupling agent represented by the general formula (1), the silanol group or silyl group generated by the hydrolysis of X reacts with the functional group on the surface of the substrate particle, thereby introducing a hydrophobic group into the substrate particle.
[0141] In the general formula, examples of the "hydrolyzable group that generates a silanol group" represented by X include alkoxy groups such as a methoxy group and an ethoxy group, and halogen groups.
[0142] As R 1 The hydrophobic group in can include alkyl, fluorinated alkyl, dimethylsiloxane, etc. For the description and preferred range of alkyl and fluorinated alkyl, reference can be made to the description and preferred range of the hydrophobic group that can be introduced into the surface of the substrate particles. The hydrophobic group can be directly bonded to Si or bonded via a linking group.
[0143] n is an integer of 1 to 3, preferably 1 or 2. When n is 2 or more, a plurality of R 1 When n is 2 or less, a plurality of Xs may be the same as or different from each other.
[0144] Examples of the silane coupling agent represented by the general formula (1) include triethoxyalkylsilane, diethoxydialkylsilane, ethoxytrialkylsilane, trimethoxyalkylsilane, dimethoxydialkylsilane, methoxytrialkylsilane, trichloroalkylsilane, etc. Specific examples of the silane coupling agent include triethoxyoctylsilane (triethoxy-n-octylsilane), octadecyltrichlorosilane, etc.
[0145] The formation of the water-repellent film on the substrate particles and the surface modification treatment can be performed according to a conventional method.
[0146] Examples of commercially available hydrophobic fine particles include Microdispers-200 (manufactured by Techno Chemical Corporation), AEROSIL RY200, AEROSIL RY300, and AEROSIL R805 (all manufactured by Evonik), and Ketjen Black (manufactured by Lion Specialty Chemicals Co., Ltd.).
[0147] The above-mentioned water-repellent fine particles may be used alone or in combination of two or more.
[0148] (Other particles)
[0149] The microparticles with a primary particle size of 1000 nm or less used in the present invention are not limited to hydrophobic microparticles, and may be microparticles other than hydrophobic microparticles, that is, microparticles with a water contact angle of less than 70°. In addition, hydrophobic microparticles and microparticles with a water contact angle of less than 70° may be used in combination. Among the microparticles with a water contact angle of less than 70°, the water contact angle may be less than 50°, less than 30°, or less than 10°. The lower limit of the water contact angle of the microparticles is 0°.
[0150] As particles other than hydrophobic particles, particles of inorganic compounds containing metal elements and semi-metallic elements and organic particles described as examples of substrate particles of coated particles and surface-modified particles in the above column (hydrophobic particles) can be cited, and silicon oxide particles are preferably used. In addition, these inorganic particles and organic particles may have a coating of an organic compound formed on their surface, or may have an organic functional group introduced therein.
[0151] As a commercially available product of fine particles other than the water-repellent fine particles, AEROSIL 200 (manufactured by Evonik) can be cited.
[0152] (Specific surface area of particles)
[0153] The specific surface area of the microparticles used in the present invention is preferably 1 to 3000 m 2 / g, more preferably 2.5 to 2750 m 2 / g, more preferably 5 to 2500 m 2 As a result, a gas diffusion phase is more reliably formed in the molded body of the gas-absorbent material, and the absorption rate and diffusion rate of the gas tend to be further improved.
[0154] The specific surface area of the fine particles can be measured by the BET method.
[0155] [Particle size ratio and amount ratio of polymer compound particles having an amino group and fine particles having a primary particle size of 1000 nm or less]
[0156] The average primary particle size of the microparticles having a primary particle size of 1000 nm or less is preferably smaller than the median particle size of the polymer compound particles having an amino group in a dry state. Specifically, the average primary particle size of the microparticles is preferably 1 / 3 to 1 / 100000 of the median particle size of the polymer compound particles having an amino group in a dry state, more preferably 1 / 10 to 1 / 100000, further preferably 1 / 20 to 1 / 50000, further preferably 1 / 25 to 1 / 1000, particularly preferably 1 / 50 to 1 / 900, and most preferably 1 / 100 to 1 / 800.
[0157] In order to effectively form a diffusion phase of gas, the amount of microparticles is preferably sufficient to cover the surface of the polymer microparticles having amino groups. In addition, in order not to reduce the gas absorption amount per unit weight of the gas absorbent material, the mixing ratio of microparticles is preferably as small as possible. That is, it is preferred to add the smallest microparticles required to cover the surface as thinly as possible. The larger the particle size of the polymer compound particles having amino groups, the smaller the surface area per unit weight. Therefore, the preferred amount of microparticles varies greatly depending on the particle size of the polymer compound particles having amino groups. If the particle size of the polymer compound particles having amino groups is less than 10 μm, the mixing ratio of the polymer compound particles having amino groups to the microparticles by weight of the solid content (polymer compound particles having amino groups: microparticles) is preferably 95:5 to 5:95, more preferably 90:10 to 30:70, and further preferably 80:20 to 50:50. In addition, it is preferred that the content of the polymer compound particles having amino groups in the gas absorbent is greater than the content of the hydrophobic particles in terms of solid content. Furthermore, when the polymer compound particles having amino groups are gel particles, if fine particles are added to the gel or its gel crushed product, which is an aggregate of the gel particles, the volume becomes smaller (the filling amount becomes larger) compared to the case where no fine particles are added, and the gas reversible absorption performance is improved. When such an effect is effectively obtained, the particle size of the polymer compound particles having amino groups is relatively large, for example, 10 μm or more, so the required mixing ratio of fine particles is relatively small, and the volume ratio of gel or gel crushed product to fine particles (gel or gel crushed product: fine particles) is preferably 99.9:0.1 to 95:5, more preferably 99.75:0.25 to 98:2, and further preferably 99.5:0.5 to 98.5:1.5.
[0158] By setting the particle size ratio and amount ratio of the polymer compound particles having an amino group to the fine particles within the above ranges, the absorption rate and diffusion rate of the gas tend to be increased.
[0159] [Other ingredients]
[0160] The gas absorbent may be composed only of polymer compound particles having an amino group and fine particles having a primary particle size of 1000 nm, or may contain other components. Examples of other components include polymer compounds other than polymer compound particles having an amino group and additives.
[0161] (Polymer compounds other than polymer compound particles having an amino group)
[0162] In the present specification, the “polymer compound other than polymer compound particles having an amino group” includes polymer compound particles not having an amino group, polymer compounds having an amino group not forming particles, and polymer compounds not having an amino group not forming particles.
[0163] There is no particular restriction on the polymer compound except the polymer compound particles with amino group, but it is preferably a polymer compound that reacts to stimulations such as temperature changes. As the reaction to stimulation, the change of the acid dissociation constant of the functional group, the change of the three-dimensional structure, the change of the swelling degree, the change of hydrophilicity, the change of water content, the change of water absorption, the change of the dissolution amount of bicarbonate ions, the change of the dissolution amount of hydrogen sulfide ions, etc. can be enumerated. Or, preferably, there is an amino group with an acid dissociation constant designed with a conjugate acid. Especially, in order to dissolve carbon dioxide, it is preferred that the acid dissociation constant of the amino group is equal to or larger than the acid dissociation constant of carbonic acid. Wherein, it is preferably a secondary or tertiary amino group, and more preferably a tertiary amino group. More preferably, dialkylamino groups such as dimethylamino groups. And, the amino group of the polymer compound can be bonded to the main chain, and can also be bonded to the side chain, but is preferably bonded to the side chain.
[0164] (additive)
[0165] Examples of the additive include a membrane stabilizer, an absorption accelerator, a diffusion accelerator, a moisture absorbent, and an antioxidant.
[0166] Examples of the film stabilizer include polymer compounds, polymerizable molecules (polymerizable compounds), crosslinking agents such as titanium crosslinking agents, primary amines, secondary amines, tertiary amines, etc. Among them, as the polymer compound, polymer compounds having primary amino groups such as polyvinylamine, polymer compounds having secondary amino groups, polymer compounds having tertiary amino groups, compounds having quaternary ammonium groups, polymer compounds having multiple primary amino groups, secondary amino groups, tertiary amino groups, quaternary ammonium groups, polyvinyl alcohol, polyethylene, polyvinyl alcohol / polyethylene copolymers, etc. can be preferably used.
[0167] Furthermore, when a polymerizable molecule is used as a film stabilizer, the polymer compound generated by the polymerization reaction of the molecule in the film also acts as a film stabilizer. Thus, after the film is formed, after adding water or after gas absorption and diffusion, it will not swell excessively and will easily maintain a uniform film shape. As a polymerizable molecule, a monomer having a polymerizable group can be cited, for example, a (meth) acrylic acid monomer can be exemplified. Among them, (meth) acrylamide or (meth) acrylamide derivatives can be preferably used. For example, alkyl acrylamide, substituted or unsubstituted aminoalkyl (meth) acrylamide, acrylamide derivatives having two polymerizable groups, etc. can be cited, among which substituted aminoalkyl acrylamide and acrylamide derivatives having two polymerizable groups can be preferably used. Substituted aminoalkyl acrylamide and acrylamide derivatives having two polymerizable groups are preferably used in combination, and their molar fraction is preferably 60 to 99:40 to 1, more preferably 80 to 99:20 to 1, and further preferably 90 to 99:10 to 1. As a specific example of a monomer having a polymerizable group, N-isopropylacrylamide (NIPAM), tert-butylacrylamide (TBAM), N,N-dimethylaminopropylmethacrylamide (DMAPM), N,N'-methylenebisacrylamide (BIS), acrylamide, etc. can be cited. These polymerizable compounds can be used alone or in combination of two or more. When two or more are used in combination, for example, a combination of N,N-dimethylaminopropylmethacrylamide (DMAPM) and N,N'-methylenebisacrylamide (BIS) can be cited as a preferred example.
[0168] The content of the membrane stabilizer in the gas-absorbent of the present invention is preferably 1 to 89% by mass based on the total amount of the gas-absorbent.
[0169] An absorption enhancer is a compound having the function of promoting the absorption of acidic gas into the gas absorbent of the present invention. A diffusion enhancer is a compound having the function of promoting the diffusion of acidic gas from the gas absorbent. In the present invention, an absorption diffusion enhancer having both the functions of an absorption enhancer and a diffusion enhancer can be used. These absorption enhancers, diffusion enhancers, and absorption diffusion enhancers can each have the function of a membrane stabilizer. The total content of the absorption enhancer, diffusion enhancer, and absorption diffusion enhancer in the gas absorbent of the present invention is preferably 0.05 mL or more per 1 g of solid content, and more preferably 0.1 mL or more. Furthermore, the content of the absorption enhancer in the gas absorbent of the present invention is preferably 0.1 to 12 N, more preferably 1 to 10 N, and even more preferably 3 to 9 N, calculated in terms of amine concentration.
[0170] As an absorption enhancer, a diffusion enhancer, or an absorption-diffusion enhancer, a low molecular weight amine can be preferably used. The molecular weight of the low molecular weight amine is preferably 61 to 10,000, more preferably 75 to 1,000, and even more preferably 90 to 500. From the viewpoint of long-term use and practicality, the boiling point of the low molecular weight amine is preferably 80° C. or more, more preferably 120° C. or more, and even more preferably 150° C. or more. An amine-containing compound having a portion that forms a salt with a counter ion like an ionic liquid in order to increase the boiling point and that is liquid can be used.
[0171] The low molecular weight amine may contain any one of a primary amino group, a secondary amino group, a tertiary amino group, an ammonium group, and an imidazolium group, and may also contain multiple amino groups, ammonium groups, and imidazolium groups, preferably 1 to 3. In addition, the secondary amino group and the tertiary amino group may be cyclic amino groups. In addition, the low molecular weight amine may contain functional groups other than amino groups, ammonium groups, and imidazolium groups, for example, hydroxyl groups. The number of hydroxyl groups contained in the low molecular weight amine is preferably 0 to 2. As preferred low molecular weight amines, amines having amino groups and hydroxyl groups, amines having 3 amino groups, etc. can be exemplified, and as more preferred low molecular weight amines, amines having secondary amino groups and hydroxyl groups can be exemplified. From the viewpoint of being able to particularly dramatically increase the diffusion amount of acidic gas in high concentration areas and being suitable for repeated use, amines having secondary amino groups and hydroxyl groups with a boiling point of 150°C or above are particularly preferred.
[0172] As the low molecular weight amine, specific compounds represented by the following formula can be mentioned.
[0173] [Chemical formula 1]
[0174]
[0175] Among these, DMAE, IP AE, Bis(2DMAE)ER, 1-2HE-PRLD, 1-2HE-PP, TM-1,4-DAB, TMHAD, and PMDETA are particularly preferably used from the viewpoint of increasing the diffusion amount of acidic gas. Among them, IPAE, Bis(2DMAE)ER, 1-2HE-PP, TM-1,4-DAB, TMHAD, and PMDETA are more preferably used from the viewpoint of having a relatively high boiling point and being less likely to evaporate. IPAE, TM-1,4-DAB, TMHAD, and PMDETA are further preferably used from the viewpoint of significantly increasing the diffusion amount of acidic gas by increasing their concentrations. IPAE, TMHAD, and PMDETA are particularly preferably used from the viewpoint of being easily available.
[0176] As for the desiccating agent that can be used as an additive, it is preferred to use a desiccating agent that has a relative humidity of 90% or less at 25° C. when it is made into a saturated aqueous solution. Examples of such desiccating agents include ions such as bromide ions, chloride ions, acetate ions, carbonate ions, bicarbonate ions, lithium ions, potassium ions, calcium ions, magnesium ions, and sodium ions. In addition, examples of such desiccating agents include salts such as lithium bromide, lithium chloride, calcium chloride, potassium acetate, magnesium chloride, potassium carbonate, and sodium carbonate. When a desiccating agent is added, the amount thereof added is preferably 0.01 to 10% by mass relative to the total amount of the gas absorbent.
[0177] Regarding antioxidants that can be used as additives, oxidation can be inhibited or prevented by adding them. Examples of such antioxidants include vitamin C (ascorbic acid), vitamin E (tocopherol), BHT (butylated hydroxytoluene), BHA (butylated hydroxyanisole), sodium isoascorbate, propyl gallate, sodium sulfite, sulfur dioxide, hydroquinone and its derivatives. When an antioxidant is added, the amount thereof added is preferably 0.01 to 10% by mass relative to the total amount of the gas absorbent.
[0178] The additives described above may be used alone or in combination of two or more.
[0179] [How to use gas absorbent materials]
[0180] The gas absorbent of the present invention can be used by filling a container such as a column, or by forming into a desired shape by powder compaction, granulation, kneading, etc. For descriptions of powder compaction, granulation, and kneading, refer to the corresponding description of the following <Gas Absorber>.
[0181] Furthermore, the gas absorbent of the present invention can be used by being impregnated with a liquid. As a result, the polymer compound particles having an amino group swell and gel, and become a state that easily absorbs acidic gases. The method of impregnation with a liquid is not particularly limited, and the gas absorbent filled in the column can be impregnated by injecting the liquid into the gas absorbent, or by placing the gas absorbent or its molded body in an atmosphere that volatilizes the target substance to be impregnated. For example, when the target substance to be impregnated is water, the gas absorbent or its molded body can be impregnated with water by placing it in a high humidity environment.
[0182] The liquid with which the gas absorbent is impregnated is not particularly limited, but examples thereof include polar solvents such as water, methanol, ethanol, isopropanol, acetonitrile, N,N-dimethylformamide, and dimethyl sulfoxide, and a mixed solvent obtained by combining two or more of these polar solvents may be used. Among them, water or a mixed solvent obtained by mixing water and other polar solvents is preferably used. Thus, the polymer compound particles containing amino groups become hydrogel particles.
[0183] The water content in the hydrogel particles is preferably 0.05 mL or more, more preferably 0.1 mL or more per 1 g of solid content, and is preferably 20 mL or less, more preferably 10 mL or less per 1 g of solid content.
[0184] The target gas to be absorbed by the gas absorbent of the present invention can be any gas as long as the target gas or ions derived from the target gas interact with the amino group, and examples thereof include acidic gases such as carbon dioxide and hydrogen sulfide. In carbon dioxide, bicarbonate ions generated by the reaction with hydroxide ions react with the amino group and are absorbed by the polymer compound particles.
[0185] The switching between the absorption process and the diffusion process of the gas in the gas absorbent can be performed by temperature changes and changes in the partial pressure of the target gas. For example, the gas absorbent swollen by water becomes highly alkaline at 30 to 50°C and easily absorbs carbon dioxide. If the gas absorbent absorbs carbon dioxide at this temperature and is heated to 60 to 90°C, the alkalinity decreases, allowing the absorbed carbon dioxide to diffuse. Alternatively, carbon dioxide can also be diffused by introducing nitrogen gas that does not contain carbon dioxide after absorbing carbon dioxide at 5 to 50°C.
[0186] <Method for producing gas absorbent>
[0187] The gas absorbent of the present invention can be produced by mixing polymer compound particles having an amino group, microparticles having a primary particle size of 1000 nm or less, and other components added as needed. The mixing of these materials is preferably carried out by dry mixing of materials in a dry state. Thus, a gas absorbent capable of fully forming a gas diffusion phase can be obtained.
[0188] The dry mixing can be performed using, for example, an elliptical rotor type stirring device, a fluidized granulator, a planetary mill, a ball mill, or a stirring granulator.
[0189] <Gas absorber>
[0190] Next, the gas absorber of the present invention will be described.
[0191] The gas absorber of the present invention comprises a powder compact of the gas absorbent of the present invention. Furthermore, the gas absorber of the present invention comprises granulated particles of the gas absorbent of the present invention. Furthermore, the gas absorber of the present invention is composed of a compact comprising a mixture of the gas absorbent of the present invention and a thermoplastic resin. In the following description, these gas absorbers are referred to as the first gas absorber, the second gas absorber, and the third gas absorber in the order listed above. For the description of the gas absorbent of the present invention in the first to third gas absorbers, reference can be made to the description in the column <Gas absorbent>.
[0192] Hereinafter, the first to third gas absorbers will be described in order.
[0193] [First gas absorber]
[0194] The first gas absorber includes a powder compact of the gas absorbent of the present invention.
[0195] The compressed powder molded body of the gas absorbent material contains polymer compound particles having amino groups at high density, and a pore structure based on microparticles having a primary particle size of 1000 nm or less is formed between the polymer compound particles, and the pore structure effectively functions as a gas diffusion phase. Therefore, the gas absorption rate and diffusion rate are fast, and excellent gas reversible absorption performance is shown.
[0196] The powder compact of the gas-absorbent is preferably produced by a process in which a composite material obtained by dry-mixing polymer compound particles having an amino group and fine particles is placed in a molding die and pressure-molded.
[0197] The pressure for compacting the gas absorber is preferably 0.1 to 2000 kg / cm 2 , more preferably 1 to 1500 kg / cm 2 , more preferably 10 to 1000 kg / cm 2 .
[0198] Morphology and properties of compressed powder compacts of gas absorbent materials
[0199] The powder compact constituting the gas adsorbent preferably has the following morphology and properties.
[0200] (Density of Powder Compacted Body)
[0201] The density of the powder compact is preferably 0.01 to 10.0 g / cm 3 , more preferably 0.05 to 7.5 g / cm 3 , more preferably 0.1 to 5.0 g / cm 3 It is presumed that in the powder compact having a density within the above range, pores are formed at an appropriate occupancy rate, and the absorption rate and diffusion rate of the gas can be further increased.
[0202] The density of the powder compact can be measured by a dry automatic density meter.
[0203] (Thickness of Powder Compacted Body)
[0204] The length (thickness) of the powder compact in the compression direction is preferably 1 μm to 10,000 μm, more preferably 5 μm to 5,000 μm, and even more preferably 10 μm to 1,000 μm.
[0205] The thickness of the powder compact can be measured by observation with a micro caliper, a laser microscope, or a scanning electron microscope.
[0206] (Shape of Powder Compacted Body)
[0207] The shape of the powder compact is not particularly limited and can be appropriately selected according to the purpose. For example, as a shape that is easy to use, a film-like shape and a cylindrical shape can be cited. In addition, when the powder compact is a film-like shape, it can be a single-layer structure or a multilayer structure formed by stacking a plurality of films. In the case of a multilayer structure, it is preferred that at least the materials, proportions, thicknesses, etc. of the films that are in contact with each other are different from each other. In addition, it is preferred that each film constituting the multilayer structure is within the above-mentioned appropriate thickness range.
[0208] (Nitrogen permeation flow rate of powder compact)
[0209] The nitrogen permeation flow rate of the powder compact is preferably 100 GPU or less, more preferably 10 GPU or less at 40° C. Furthermore, the carbon dioxide permeation flux of the powder compact is preferably 10 GPU or more, more preferably 100 GPU or more at 40° C. The powder compact having the nitrogen permeation flow rate and the carbon dioxide flux within the above ranges can selectively permeate carbon dioxide relative to nitrogen, and therefore, when used in the gas separation material described later, carbon dioxide can be selectively separated from a mixed gas such as air containing nitrogen and carbon dioxide and efficiently recovered.
[0210] The "permeation flux" in this specification is a value obtained by the following formula (1).
[0211] Q=L / A×ΔP……(1)
[0212] In formula (1), Q represents the permeation flux, L represents the permeation flow rate per unit time, A represents the membrane area, and ΔP represents the partial pressure difference on both sides of the monolayer membrane. The permeation flow rate L can be measured as the amount of gas permeating the membrane per unit time by gas chromatography or the like. The unit of the permeation flux L is GPU (1 GPU is 1.0×10 -6 (cm 3 (STP) / (s·cm 2 ·cmHg)). The partial pressure difference ΔP can be determined as the difference between the gas partial pressure on the gas supply surface side and the gas partial pressure on the permeation surface side measured by a pressure gauge, gas chromatography, or the like.
[0213] In addition, the "selectivity" in this specification refers to the permeation flux Q of the gas that selectively permeates. S As molecules, the permeation flux Q of other gases O The value of the ratio as the denominator Q S / QO .
[0214] [Second gas absorber]
[0215] The second gas absorber includes granulated particles of the gas absorbent of the present invention.
[0216] Here, the "granulated particles of the gas-absorbent material" refer to particles obtained by forming the gas-absorbent material of the present invention into particles using a granulator.
[0217] Granulation of the gas absorbent may be dry granulation or wet granulation, but dry granulation is preferred.
[0218] Furthermore, the object to be granulated may be only the gas absorbent material or a mixture of the gas absorbent material and other materials. As other materials, fillers can be exemplified. As fillers, known fillers can be used. For example, activated carbon, zeolite, silica, fumed silica, hydrophobic silica, hydrophobic fumed silica, hydrophobic silica, alumina, hydrophobic alumina, hydrophobic alumina, boehmite, diatomaceous earth, titanium oxide, iron oxide, zinc oxide, magnesium oxide, oxides such as metal ferrites, hydroxides such as aluminum hydroxide and magnesium hydroxide, calcium carbonate (light, heavy), magnesium carbonate, dolomite, carbonates such as dawsonite, calcium sulfate, sulfuric acid, etc. can be cited. Sulfates or sulfites such as barium, ammonium sulfate, calcium sulfite, talc, mica, clay, glass fiber, silicate such as calcium silicate, montmorillonite, bentonite, borate such as zinc borate, barium metaborate, aluminum borate, calcium borate, sodium borate, carbon black, hydrophobic carbon black, hydrophobic carbon black, graphite, carbon fiber, other iron powders, copper powder, aluminum powder, zinc white, molybdenum sulfide, boron fiber, potassium titanate, lead zirconate titanate, fluorinated resin powder, Teflon (registered trademark) powder, etc. Among them, it is preferred to use hydrophobic fillers. As other materials, hydrophobic materials such as carbon black, silica particles, mesoporous silica, PTFE (polytetrafluoroethylene) particles, metal / inorganic oxide particles, zeolite, activated carbon, low molecular weight amine compounds, amine-containing polymers can be cited. In particular, if low molecular weight amines and amine-containing polymers are used, performance is improved, so it is preferred.
[0219] Furthermore, the granulated particles of the gas absorbent may contain a binder. The binder is preferably sprayed onto the gas absorbent when the gas absorbent is granulated. This reduces the scattering of the gas absorbent and improves the operability. As the binder, in addition to the binder usually used for granulation, a polymer solution having an amino group can also be used.
[0220] As the granulator, a stirring mixing granulator, an extrusion granulator, a pan type granulator or the like can be used.
[0221] The average primary particle size of the granulated particles of the gas-absorbent material is preferably 0.1 μm to 10 mm, more preferably 0.25 μm to 7.5 mm, and even more preferably 0.5 μm to 5.0 mm.
[0222] The average primary particle size of the granulated particles can be measured using a laser diffraction particle size distribution analyzer or an optical microscope.
[0223] [Third gas absorber]
[0224] The third gas absorber is composed of a molded body containing a mixture of the gas absorbent of the present invention and a thermoplastic resin.
[0225] Here, the thermoplastic resin contained in the mixture is not particularly limited, and examples thereof include polyolefins such as polyethylene and polypropylene, polyamide, polystyrene, polyimide, acrylic resin, thermoplastic polyurethane, polyvinyl alcohol, polyvinyl pyrrolidone, polyethylene oxide, and the like.
[0226] The content of the thermoplastic resin in the mixture is preferably 1 vol% to 99 vol%, more preferably 5 vol% to 95 vol%, and further preferably 10 vol% to 90 vol%.
[0227] The mixture can be obtained by kneading the gas-absorbent material and the thermoplastic resin using a kneading machine. In this case, the gas-absorbent material may be kneaded directly or in the form of granulated particles.
[0228] For the description of the “granulated particles”, reference can be made to the description in the above-mentioned column of “Second gas absorber”.
[0229] The mixture may contain only the gas absorbent material of the present invention and the thermoplastic resin, or may contain other materials. As other materials, fillers can be exemplified, among which hydrophobic fillers are preferably used. As other materials, hydrophobic materials such as carbon black, silica particles, mesoporous silica, PTFE particles, metal / inorganic oxide particles, zeolite, activated carbon, low molecular weight amine compounds, and amine-containing polymers can be cited. In particular, if low molecular weight amines and amine-containing polymers are used, the performance is improved, so it is preferred.
[0230] As a kneading machine for kneading the mixture, a twin-screw kneading machine, a kneading extruder, a single-screw extruder, etc. can be used.
[0231] For the description of the thickness and shape of the compact, reference can be made to the description in the above columns (thickness of the pressed powder compact) and (shape of the pressed powder compact). In addition, the compact may be a particle. The average particle size of the particles is preferably 0.5 to 10 mm, more preferably 1 to 4.5 mm, and further preferably 1.5 to 3 mm. The average particle size of the particles is the value obtained by measuring the maximum diameter of each of more than 100 particles and dividing it by the number of particles measured.
[0232] [Total pore volume and average pore diameter of gas absorber]
[0233] In the first gas absorber and the third gas absorber, the total pore volume is preferably 0.01 to 10 cm 3 / g, more preferably 0.01 to 5 cm 3 / g, more preferably 0.01 to 2.5 cm 3 / g.
[0234] Furthermore, in the first gas absorber and the third gas absorber, the average pore diameter is preferably 0.1 to 500 nm, more preferably 0.1 to 300 nm, and even more preferably 0.1 to 150 nm.
[0235] The total pore volume of the gas absorber can be measured by the BET method, and the average pore diameter can be obtained by analysis based on the Kelvin equation.
[0236] When the total pore volume and the average pore diameter of the gas absorber are within the above ranges, gas diffusion can be efficiently performed inside the gas absorber, and gas absorption and diffusion can be efficiently performed.
[0237] [Other parts of gas absorber]
[0238] The gas absorber of the present invention may be composed only of a powder compact of a gas absorbent material, or may include other components.
[0239] As other components, a carrier for supporting the powder compact can be cited. Among the carriers, a thin plate and a porous body can be used. As the thin plate serving as the carrier, a resin film, a metal foil, a sheet made of a carbon material, a carbon sheet, etc. can be used, and as the porous body, a resin, a metal, a porous body formed of carbon, a fiber aggregate, etc. can be used.
[0240] <Gas separation materials>
[0241] Next, the gas separation material of the present invention will be described.
[0242] The gas separation material of the present invention is characterized by comprising the gas adsorbent of the present invention. The gas adsorbent contained in the gas separation material can constitute the gas absorber of the present invention.
[0243] For the description of the gas-absorbent material and the gas absorber of the present invention, reference can be made to the description in the columns <Gas-absorbent material> and <Gas absorber>.
[0244] Examples of mixed gases for gas separation using the gas separation material of the present invention include natural gas, biogas, landfill gas, post-combustion gas, fuel gas, and gas modified by water vapor. The gas separation material of the present invention can selectively separate, for example, carbon dioxide from these mixed gases in a short period of time, significantly reducing the concentration of carbon dioxide in the mixed gas.
[0245] Furthermore, the gas separation material of the present invention is not limited to gas, but can also allow water or water vapor to pass through, thereby, for example, being able to separate water or water vapor from water or water vapor containing gas, in other words, being able to remove gas from water or water vapor.
[0246] The conditions for gas separation vary depending on the gas adsorbent used for the gas separation material, the composition of the mixed gas to be separated, the gas to be separated from the mixed gas, etc., but are preferably 0 to 130° C., more preferably 0 to 95° C., and preferably gas separation is performed at a temperature of 10 to 60° C. Furthermore, the water content of the gas adsorbent during gas separation is preferably 1% by mass to 1000% by mass of the dry membrane weight.
[0247] <Filter and gas separation device>
[0248] The filter and gas separation device of the present invention are characterized by comprising the gas separation material of the present invention.
[0249] For the description, preferred range and specific examples of the gas separation material of the present invention, reference can be made to the contents described in the column <Gas Separation Material>.
[0250] The filter and gas separation device of the present invention can efficiently separate and recover a specific gas from a mixed gas by using the gas separation material of the present invention.
[0251] Example
[0252] Hereinafter, examples and comparative examples are given to further specifically describe the features of the present invention. As long as the materials, usage amounts, ratios, processing contents, processing steps, etc. shown in the following examples are not deviated from the main purpose of the present invention, they can be appropriately changed. Therefore, the scope of the present invention should not be interpreted restrictively by the specific examples shown below. In addition, the water contact angle and average primary particle size of each particle are measured by the method described in [microparticles with a primary particle size of less than 1000nm]. In addition, the specific surface area and total pore volume shown in the following table 2 are measured by the BET method, and the average pore diameter is obtained by the Kelvin formula.
[0253] (Synthesis Example 1) Synthesis of Amino Group-Containing Polymer Particles 1
[0254] The amino group-containing polymer particles 1 used in this example were synthesized in the following manner.
[0255] [Chemical formula 2]
[0256]
[0257] 1 liter of pure water was added to a 2-liter three-necked flask, heated to 70°C, and 2mM of surfactant (hexadecyl trimethyl ammonium bromide) and 3 monomers were dissolved to make the total monomer concentration 312mM. Among the 3 monomers, N-(dimethylaminopropyl) methacrylamide was 55mol%, N-tert-butyl acrylamide was 43mol%, and N,N'-methylenebisacrylamide was 2mol%. N-(dimethylaminopropyl) methacrylamide used a substance from which polymerization inhibitors were removed by an alumina column. N-tert-butyl acrylamide was pre-dissolved in a small amount of methanol, and a substance made into a solution of 0.68g / mL was added. While the mixture was kept at 70°C, it was stirred with a mechanical stirrer, and nitrogen was bubbled for 1 hour to remove oxygen inside the system. To the monomer solution thus obtained, a solution obtained by dissolving 700 mg of 2,2'-azobis(2-methylpropionamidine) dihydrochloride in 5 mL of pure water was added, and the reaction was carried out at 70°C for 3 hours under a nitrogen atmosphere. After the reaction, the precipitate was filtered out and dialyzed for 3 days using a dialysis membrane (MWCO12-14.000, width: 75 mm, volume / length: 18 mL / mL) [manufactured by SPECTRUM LABORATORIES, INC.] to remove unreacted monomers and surfactants, and then the counter anions were removed using a strong basic ion exchange resin. The suspension of the gel particles obtained by the above process was dried using a spray drying method to obtain polymer compound particles having amino groups (polymer particles 1 containing amino groups). The particle size of the polymer particles 1 containing amino groups in a dry state is 4 μm in terms of the median particle size measured using a laser diffraction particle size distribution measuring device. In addition, the water contact angle of the polymer particles containing amino groups is 66.2°.
[0258] (Synthesis Example 2) Synthesis of Amino Group-Containing Polymer Particles 2
[0259] Dimethylaminopropylacrylamide (DMAPAAm: 85 mol%) and BIS (15 mol%) were dissolved in MilliQ water at 60°C to prepare a total of 30 mL of an aqueous solution, and ethanol was further added so that the total monomer concentration of the reaction mixture to be reacted in the subsequent step became 2.3 mol / L, thereby preparing a mixture. After the mixture was heated to 70°C, nitrogen was bubbled for 30 to 60 minutes while stirring. A solution of AIBN (AIBN concentration in the reaction mixture: 2.58 mM, solvent: a mixed solvent of acetone and water) was added to the mixture to prepare a reaction mixture, and block polymerization was carried out at 70°C for 3 hours under a nitrogen flow, thereby obtaining a gel. It was crushed with a meat grinder (1.5 mesh), washed with water, and the washing liquid was removed by filtration to obtain amino-containing polymer particles 2. The moisture content of the amino-containing polymer particles 2 was 73.7% by weight.
[0260] [Chemical formula 3]
[0261]
[0262] (The primary particle size used in this example is 1000 nm or less)
[0263] Table 1 shows the microparticles used in this example, their structure, water contact angle and average primary particle size.
[0264] [Table 1]
[0265]
[0266] [1] Evaluation of CO2 reversible absorption performance
[0267] The evaluation of the CO 2 reversible absorption performance in this example was carried out using a pressure swing absorption method (PSA method) and a temperature swing absorption method (TSA method).
[0268] (Evaluation of CO2 reversible absorption performance based on pressure swing absorption method)
[0269] The evaluation of the reversible absorption performance of CO2 by the pressure swing absorption method was carried out by the following procedure.
[0270] First, the sample to be measured contained in the reactor was placed in a thermostatic bath at a temperature of 40°C and a relative humidity of more than 98% and fully humidified, and then the temperature was adjusted to 30°C. Next, a mixed gas of humidified CO2 and N2 (CO2 concentration: 10.03% by volume) was introduced into the sample to be measured at a flow rate of 200 mL / min, and the CO2 concentration (A) of the gas discharged from the sample to be measured was measured by a multi-gas analyzer (manufactured by HORIBA, Ltd.: VA-3000) (absorption process). Next, the gas introduced into the sample to be measured was replaced with humidified N2 gas and introduced into the sample to be measured at a flow rate of 200 mL / min, and the CO2 concentration (B) of the gas discharged from the sample to be measured was measured (diffusion process). The CO2 reversible absorption performance of the sample to be measured was evaluated by taking the cumulative value of the difference between the CO2 concentration of the introduced mixed gas and the CO2 concentration (A) measured during the absorption process as the CO2 absorption amount, and taking the cumulative value of the CO2 concentration (B) measured during the diffusion process as the CO2 diffusion amount. In addition, when the CO2 absorption amount measured in this way is shown in a graph, in order to distinguish it from the CO2 diffusion amount, the value A is sometimes marked with a "-" sign and shown on the negative side of the vertical axis.
[0271] (Example 1) Production of Gas Absorber 1 Using Amino-Containing Polymer Particles 1 and Carbon Black
[0272] The amino-containing polymer particles 1 and the carbon black shown in Table 1 were mixed at room temperature in a volume ratio of amino-containing polymer particles 1:carbon black=7:3, and mixed at 300 rpm for 10 minutes using a planetary grinding device equipped with 2 mm zirconia beads, thereby obtaining a composite material of amino-containing polymer particles 1 and carbon black (gas absorbent material 1).
[0273] The SEM photograph (magnification: 3700 times) of the amino group-containing polymer particles 1 before adding carbon black is shown in FIG. Figure 1 (a) A SEM photograph (magnification: 3700 times) of a composite material (gas absorbent material 1) obtained by mixing amino group-containing polymer particles 1 and carbon black is shown in FIG. Figure 1 (b) According to Figure 1 The SEM photograph of the composite material (b) shows that the surface of the amino group-containing polymer particle 1 is covered with small particles (carbon black).
[0274] Next, the gas absorbent material 1 was placed in a reactor (width×depth×height: 15 cm×8 cm×0.2 cm) and heated at 5000 kg / 120 cm 2 The powder was pressed to obtain a film-like gas absorber 1 having a film thickness of 300 μm.
[0275] The SEM photograph (magnification: 20000 times) of the internal structure of the gas absorber 1 is shown in Figure 2 A TEM photograph (magnification: 50,000 times) of a thin slice cut out from the gas absorber 1 is shown in FIG. Figure 3 (a) Energy dispersive X-ray spectroscopy (EDX) was performed on the thin slice, and a TEM photograph of characteristic X-rays of nitrogen and carbon was taken. Figure 3 (b) According to Figure 2 , Figure 3 The microscope photograph shown confirms that a pore-like structure is formed inside the film of the gas absorber 1 .
[0276] In addition, the specific surface area, total pore volume and average pore diameter of carbon black, gas absorbent material 1 (gas absorbent material 1 before powder compaction) and gas absorber 1 were measured. The results are shown in Table 2. It was confirmed that pores capable of diffusing the gas based on carbon black were maintained even after powder compaction. The capacity ratio of gas absorber 1 (amino group-containing polymer particles 1: carbon black: pores) was 0.433:0.429:0.138.
[0277] [Table 2]
[0278]
[0279] (Examples 2 to 6) Production of a gas absorber using amino-containing polymer particles 1 and hydrophobic carbon black, hydrophobic silica RY200, hydrophobic silica R805, PTFE particles or hydrophilic silica 200
[0280] Gas absorbers 2 to 6 were produced in the same manner as in Example 1 except that the fine particles shown in Table 3 were used instead of carbon black.
[0281] (Comparative Example 1) Production of Comparative Gas Absorber 1 Containing Amino Group-Containing Polymer Particles 1
[0282] A gas absorber (comparative gas absorber 1) was produced in the same manner as in Example 1 except that only the amino group-containing polymer particles 1 were powder-pressed into a film shape instead of the composite material of the amino group-containing polymer particles 1 and carbon black.
[0283] [Table 3]
[0284] Example No Gas absorber No particle Example 1 Gas absorber 1 Carbon Black Example 2 Gas absorber 2 Hydrophobic Carbon Black Example 3 Gas absorber 3 Hydrophobic Silica RY200 Example 4 Gas absorber 4 Hydrophobic Silica R805 Example 5 Gas absorber 5 PTFE particles Example 6 Gas absorber 6 Hydrophilic Silica 200 Comparative Example 1 Comparison of gas absorbers 1 none
[0285] The CO2 absorption amounts measured during the absorption process for the gas absorbers 1, 2 and the comparative gas absorber 1 are shown in FIG. Figure 4 , the CO2 diffusion amount in the diffusion process is shown in Figure 5 In addition, the CO2 absorption amount measured in the absorption process of the gas absorbers 1, 3 to 6 is shown in FIG. Figure 6 , the CO2 diffusion amount in the diffusion process is shown in Figure 7 In the attached drawings, "GP" indicates amino-containing polymer particles 1, "CB" indicates carbon black, "hydrophobic CB" indicates hydrophobized carbon black, "RY200" indicates hydrophobic silica RY200, "R805" indicates hydrophobic silica R805, "PTFE" indicates PTFE particles, and "200" indicates hydrophilic silica 200. Figures 8 to 10 , 12. Furthermore, the CO2 absorption amount or CO2 diffusion amount expressed in the units of "mL / g-GPs" or "mL / g" represents the CO2 absorption amount or CO2 diffusion amount per 1 g of the polymer particles containing the amino group.
[0286] like Figures 4 to 7 As shown in FIG. 1 , the CO2 absorption of gas absorbers 1 to 6 containing microparticles with a primary particle size of 1000 nm or less is saturated in a short time and ends the absorption compared to the comparative gas absorber 1 containing no microparticles. Figure 6 , Figure 7As shown in the figure, the absorption rate and diffusion rate are faster in the order of gas absorbers 3, 4, 6 using microparticles with an average primary particle size of 12nm (hydrophobic silica RY200, R805 and hydrophilic silica 200), gas absorber 1 using microparticles with an average primary particle size of 30nm (carbon black CB), and gas absorber 5 using microparticles with an average primary particle size of 200nm (PTFE particles). It is found that the smaller the average primary particle size of the microparticles, the better the absorption rate and diffusion rate. Moreover, as Figure 4 As shown, the gas absorber 2 using the hydrophobized carbon black (hydrophobic CB) exhibits a larger CO 2 absorption / diffusion amount than the gas absorber 1 in which the carbon black (CB) is not hydrophobized.
[0287] These results confirm that the gas absorption rate and diffusion rate are increased by using the polymer compound particles having an amino group and fine particles having a primary particle size of 1000 nm or less in combination, and that the gas reversible absorption performance is improved by further increasing the water repellency of the fine particles.
[0288] Furthermore, when polymer compound particles having amino groups were prepared by changing the median particle size within the range of 2 to 10 μm and the gas absorbers were prepared in the same manner using the particles, the same gas reversible absorption performance as that of the gas absorbers in the respective examples was obtained.
[0289] (Evaluation of CO2 reversible absorption performance based on temperature swing absorption method)
[0290] The evaluation of the CO 2 reversible absorption performance based on the temperature swing absorption method was carried out by the following procedure.
[0291] First, the reactor containing the sample to be measured was placed in a water bath adjusted to 30°C, and a mixed gas of CO2 and N2 (CO2 concentration: 10.0 volume %) humidified at 60°C was introduced into the reactor at a flow rate of 100 mL / min, and the sample to be measured was fully humidified (humidification process). Next, the reactor was quickly transferred to a water bath adjusted to 75°C, and the gas discharged from the sample to be measured was dehumidified, and its CO2 concentration (B) was measured by a multi-gas analyzer (HORIBA, Ltd. manufacturing: VA-3000) (diffusion process). After CO2 was fully diffused from the sample to be measured, the reactor was quickly transferred to a water bath at 30°C, and the mixed gas of CO2 and N2 humidified above was introduced into the reactor at a flow rate of 100 mL / min, and the gas discharged from the sample to be measured was dehumidified, and its CO2 concentration (A) was measured by a multi-gas analyzer (absorption process). Here, the diffusion process was performed for 300 seconds and the absorption process was performed for 500 seconds. Furthermore, the cumulative value of the difference between the CO2 concentration of the introduced mixed gas and the CO2 concentration (A) measured in the absorption process is taken as the CO2 absorption amount, and the cumulative value of the CO2 concentration (B) measured in the diffusion process is taken as the CO2 diffusion amount. Furthermore, the diffusion-absorption cycle in which the above diffusion process and absorption process are alternately repeated is performed to evaluate the cycle performance. In addition, when the CO2 absorption amount measured here is shown in a graph, in order to distinguish it from the CO2 diffusion amount, the value A is sometimes marked with a "-" sign and shown on the negative side of the vertical axis.
[0292] The CO2 absorption amounts of the gas absorbers 3 and 6 manufactured in the above-mentioned examples and the comparative gas absorber 1 during the absorption process measured by the temperature swing absorption method are shown in FIG. Figure 8 , the CO2 diffusion amount in the diffusion process is shown in Fig. 9 In addition, the CO2 diffusion amount and CO2 absorption amount when 5 cycles of diffusion-absorption cycle are performed are shown in Fig.10 .
[0293] like Figure 8 to Figure 10As shown, the gas absorbers 3 and 6 containing microparticles show a large CO2 absorption / diffusion amount compared to the comparative gas absorber 1 without microparticles. In particular, the gas absorber 3 using hydrophobic silica RY200 has a large CO2 absorption / diffusion amount compared to the gas absorber 6 using hydrophilic silica 200, and shows a stable diffusion-absorption cycle. It is believed that this is because, in the temperature-variable absorption method measured under high humidity, when the water condensed in the pores of the membrane greatly affects the gas diffusion, in the gas absorber 3, the hydrophobicity of the hydrophobic silica RY200 covering the polymer particles containing amino groups inhibits the condensed water from blocking the pores and effectively acts as a gas diffusion phase. Therefore, it is known that the gas absorber containing hydrophobic microparticles can be effectively used as a film for separating CO2 in a short time under high humidity, etc.
[0294] [2] Research on the granulation of gas absorbing materials
[0295] (Example 7) Production of Gas Absorber 7 Containing Pellets of a Mixture of Gas Absorbent and Polyethylene
[0296] A composite material (gas absorbent) of amino-containing polymer particles 1 and carbon black CB was obtained in the same manner as the preparation steps of the gas absorbent 1 of Example 1. The composite material and polyethylene (LDPE: Asahi Kasei Corporation. Suntech LD M6520) were kneaded at a weight ratio of composite material: polyethylene = 2:1 using a twin-screw kneading extruder (manufactured by Xplore Instruments: benchtop kneader MC6) to obtain a gas absorbent 7 containing particles with an average particle size of 3 mm.
[0297] (Comparative Example 2) Production of Comparative Gas Absorber 2 Containing Particles of a Mixture of Amino Group-Containing Polymer Particles 1 and Polyethylene
[0298] Pellets (comparative gas absorber 2) were produced in the same manner as in Example 7 except that a kneaded product of amino group-containing polymer particles 1 and polyethylene (LDPE: Asahi Kasei Corporation. Suntech LD M6520) was used at a weight ratio of amino group-containing polymer particles 1:polyethylene=4:1.
[0299] SEM photographs of the gas absorber 7 and the comparative gas absorber 2 are shown in FIG. Fig.11 .exist Fig.11In the figure, the upper photo is a SEM photo of the gas absorber 7, and from the left are SEM photos of the appearance of the particle, SEM photos of the internal structure of the particle at a magnification of 35 times, and SEM photos of the internal structure of the particle at a magnification of 5000 times. Fig.11 In the figure, the lower photo is an SEM photo of the comparison gas absorber 2, and from the left are an SEM photo of the appearance of the particle, an SEM photo of the internal structure of the particle at a magnification of 35 times, and an SEM photo of the internal structure of the particle at a magnification of 5000 times.
[0300] In addition, the CO 2 absorption amount in the absorption process and the CO 2 diffusion amount in the diffusion process measured by the temperature-variable absorption method for the gas absorber 7 and the comparative gas absorber 2 are shown in FIG. Fig.12 It was confirmed that the addition of carbon black CB accelerated the absorption and diffusion rates in the initial 30 minutes in both the absorption and diffusion processes.
[0301] [3] Research on the filling amount of gas absorbing materials
[0302] The gel (aggregate of gel particles) containing the amino-containing polymer particles 2 synthesized in Synthesis Example 2 was crushed with a meat grinder at 1.5 mesh (pore size 4.8 mm), 1.3 mesh (pore size 4.0 mm), 1 mesh (pore size 3.2 mm), 7 mesh (pore size 2.4 mm) and 3 mesh (pore size 1.1 mm) in sequence, thereby obtaining various amino-containing polymer crushed products (gel crushed products) with different crushing degrees. Hydrophobic silica RY300 was added to each crushed product in the proportion shown in Table 4 to prepare a mixture, and the mixture was placed in a 250 mL plastic container and shaken to mix, and then the surface was leveled and the height was measured. The results are shown in the bold frame of Table 4. In addition, the particle size distribution of the mixture in which the proportion of hydrophobic silica RY300 was set to 0.50 volume % is shown in Fig.13 The CO2 absorption amount in the absorption process and the CO2 diffusion amount in the diffusion process measured by the pressure swing absorption method for a mixture obtained by adding hydrophobic silica RY300 (0.50% by volume) to a polymer powder containing amino groups crushed at 7 centimeters (gas absorbent material 8) and a polymer powder containing amino groups crushed at 7 centimeters (comparative gas absorbent material 3) are shown in the figure. Fig.14 In addition, here, 10L of gas absorbing material was used as the measurement object sample, and the flow rate of the mixed gas of CO2 and N2 and the N2 gas was set to 1000mL / min. Fig.13 , Fig.14In the table, "3 centimeters GP" to "1.5 centimeters GP" respectively represent amino group-containing polymer powders crushed to 3 centimeters to 1.5 centimeters, and "RY300" represents hydrophobic silica RY300.
[0303]
[0304] As shown in Table 4, the volume (filling amount) of the mixture changes by changing the content of hydrophobic silica RY300, and the volume becomes the smallest (filling amount becomes the largest) when the mixing ratio is set to 0.50 volume %. Fig.14 As shown, the composite material (gas-absorbent material 8) having a large filling amount has a significantly improved CO 2 reversible absorption amount per unit mass and CO 2 absorption / diffusion rate compared to the comparative gas-absorbent material 3 not containing the hydrophobic silica RY300.
[0305] This shows that the addition of fine particles can increase the filling amount of the gas absorbent and thus increase the CO 2 reversible absorption amount and CO 2 absorption / diffusion rate.
[0306] The amino group-containing polymer pulverized products used in the following Examples 9 and 10 were also prepared by the same procedure as the amino group-containing polymer pulverized products prepared in this section.
[0307] [4] Research on the effect of pulverization of gas absorbent materials
[0308] (Example 9) Production of Gas-Absorbent Material 9 Comprising a Mixture of a Polymer Pulverized Material Containing Amino Group and Hydrophobic Silica RY300 Further Finely Grinded
[0309] A mixture was obtained by mixing a polymer pulverized material containing amino groups pulverized at 1.5 meshes with a meat grinder and hydrophobic silica RY300 at a volume ratio of polymer pulverized material containing amino groups: hydrophobic silica RY300 = 99.5:0.5. The mixture was pulverized at 230 rpm using a planetary ball mill (manufactured by Fritsch Japan Co., Ltd: P-5) using zirconium oxide beads with a diameter of 5 mm, thereby obtaining a gas absorbent material 9 containing the pulverized material. When the particle size distribution of the pulverized material was measured, it was confirmed that the particle size of most polymer particles was less than 100 μm. In addition, the moisture content of the pulverized material was 72.45%, and the moisture content of the polymer pulverized material containing amino groups was 73.17% by weight, which was slightly smaller than the moisture content (73.7%) of the polymer particles 2 containing amino groups used in the material.
[0310] The CO2 absorption amount during the absorption process measured by the pressure swing absorption method for the gas absorbent material 9 and the above-mentioned gas absorbent material 8 is shown in FIG. Fig.15 Here, 10 L of the gas absorbent was used as a sample to be measured, and the flow rate of the mixed gas of CO 2 and N 2 and the N 2 gas was set to 3000 mL / min for measurement.
[0311] according to Fig.15 It can be seen that the gas absorbent 9 pulverized by the bead mill has a significantly higher CO2 absorption rate than the gas absorbent 8 not pulverized by the bead mill. This shows that the CO2 reversible absorption performance of the gas absorbent can be further improved by increasing the degree of pulverization of the gas absorbent.
[0312] [5] Study on the effect of binder spraying and granulation on gas absorbent materials
[0313] (Example 10) Production of a gas absorber 10 comprising granulated particles obtained by granulating a mixture of an amino group-containing polymer powder and hydrophobic silica RY300 using a binder
[0314] The amino-containing polymer powder and hydrophobic silica RY300, which were ground into 7 cm mesh by a meat grinder, were put into a pan-type granulator (DPZ-01R manufactured by AS ONE Corporation) at a volume ratio of amino-containing polymer powder: hydrophobic silica RY300 = 99.8:0.2 (total amount of 1 kg) and mixed. The mixture in the granulator was granulated by heating and stirring while spraying a nanoparticle aqueous solution (400 mL) prepared by dissolving the amino-containing polymer particles 1 in water at a ratio of 20 g / mL, thereby obtaining a gas absorber 10 containing granulated particles.
[0315] The particle size distribution of the mixture before granulation is shown in Fig.16 In (a), the particle size distribution of the granulated particles (gas absorbent 11) is shown in Fig.16 (b) in.
[0316] according to Fig.16 (a) and Fig.16 Comparison with (b) shows that the scattering of the gas absorbent material decreases as the particle size increases during granulation.
[0317] Industrial Applicability
[0318] The gas absorbent material of the present invention can absorb / diffuse acidic gases such as carbon dioxide at a high speed and exhibits excellent gas reversible absorption performance. Therefore, by using the gas absorbent material of the present invention, the time efficiency of the gas separation and recovery process is improved and the cost can be reduced. Therefore, the industrial applicability of the present invention is high.
Claims
1. A gas absorber comprising a gas absorbent material and other materials, wherein: The gas absorbing material is composed of a composite material of polymer compound particles having an amino group and microparticles having a primary particle size of 1000 nm or less, wherein the microparticles do not include the polymer compound particles having an amino group and are particles different from the polymer compound particles. The average primary particle size of the microparticles is smaller than the median particle size of the polymer compound particles having an amino group in a dry state. The content of the polymer compound particles having an amino group is greater than the content of the microparticles in terms of solid content. The other materials are carbon black, silicon dioxide particles, mesoporous silicon oxide, polytetrafluoroethylene particles, metal oxide particles, inorganic oxide particles, zeolite, activated carbon, low molecular weight amine compounds, or amine-containing polymers.
2. The gas absorber according to claim 1, wherein: The microparticles are particles containing silicon dioxide or carbon.
3. The gas absorber according to claim 1, wherein: The water contact angle of the microparticles is 70° or more.
4. The gas absorber according to claim 1, wherein: The fine particles are fine particles containing carbon black or fluororesin.
5. The gas absorber according to any one of claims 1 to 4, wherein The fine particles include a substrate particle and a water-repellent coating formed on the surface of the substrate particle.
6. The gas absorber according to claim 5, wherein: The hydrophobic coating contains dialkyl polysiloxane.
7. The gas absorber according to any one of claims 1 to 4, wherein: The fine particles are fine particles in which the surface of the substrate particles is modified to impart water repellency.
8. The gas absorber according to claim 7, wherein: The surface modification is to introduce an alkyl group into the surface of the substrate particles.
9. The gas absorber according to claim 5, wherein: The substrate particles are inorganic particles.
10. The gas absorber according to claim 5, wherein: The water contact angle of the substrate particles is 70° or more.
11. The gas absorber according to any one of claims 1 to 4, wherein: The average primary particle size of the microparticles is 5 to 500 nm.
12. The gas absorber according to any one of claims 1 to 4, wherein: The substituted (meth)acrylamide monomer having an amino group is N-aminoalkyl (meth)acrylamide.
13. The gas absorber according to any one of claims 1 to 4, wherein: The median particle size of the polymer compound particles having an amino group in a dry state is 2 to 10 μm.
14. The gas absorber according to any one of claims 1 to 4, wherein: The gas absorbing material is granulated particles.
15. The gas absorber according to any one of claims 1 to 4, wherein: It further comprises a thermoplastic resin. 16 . A gas separation material comprising the gas absorber according to claim 1 .
17. The gas separation material according to claim 16, wherein Selectively separate acid gases from mixed gases.
18. The gas separation material according to claim 17, wherein The acid gas is carbon dioxide.
19. A filter comprising the gas separation material according to any one of claims 16 to 18. 20 . A gas separation device comprising the gas separation material according to claim 16 .