Non-noble metal alloy catalyst for preparing methyl glycolate through dimethyl oxalate hydrogenation as well as preparation method and application of non-noble metal alloy catalyst

By using a silica-supported nickel-cobalt alloy catalyst in the hydrogenation reaction of dimethyl oxalate, the problems of high temperature energy consumption and high cost of existing catalysts are solved, and low-temperature and efficient preparation of methyl glycolate is achieved, with good industrial Application value.

CN119075990AActive Publication Date: 2024-12-06XI AN JIAOTONG UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411202608.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The existing catalysts have problems such as high-temperature energy consumption, high cost, short catalyst life and poor stability in the preparation of methyl glycolate during the hydrogenation of dimethyl oxalate. Especially the complex preparation of precious metal catalysts and difficult recycling, and the high temperature of heterogeneous catalysts , Cu-based catalysts have a strong ability to activate hydrogen, resulting in low yield.

Method used

A non-precious metal alloy catalyst with nickel-cobalt alloy nanoparticles supported by silica support was prepared by equal volume impregnation method, and a stable bimetal structure was formed by using the similarity of nickel and cobalt, combining the thermal stability and pore characteristics of silica. Regulate metal active sites to achieve low-temperature and efficient hydrogenation reaction.

Benefits of technology

High methyl glycolate selectivity and hydrogenation reaction conversion rate are achieved at lower temperatures, reducing catalyst costs, improving the stability and universality of the catalyst, and suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075990A_ABST
    Figure CN119075990A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of catalyst preparation technology and performance application, and discloses a non-noble metal alloy catalyst for preparing methyl glycolate through dimethyl oxalate hydrogenation as well as a preparation method and application of the non-noble metal alloy catalyst. Wherein the active component is NixCoy alloy nanoparticles, the value range of x is 1-5, and the value range of y is 1-2; and the content of Ni is 15% of the mass of the non-noble metal alloy catalyst for preparing methyl glycolate through dimethyl oxalate hydrogenation. The preparation method comprises the following steps: adding a precursor solution into a silicon dioxide carrier, and standing, so that the silicon dioxide carrier adsorbs the precursor solution to obtain a catalyst precursor; and drying, roasting, reducing and passivating the catalyst precursor, so that the nano-particles of the active component are loaded on the silicon dioxide carrier, and the NixCoy alloy catalyst is obtained. The catalyst provided by the invention is relatively low in cost and catalysis temperature, and has relatively high methyl glycolate selectivity and hydrogenation reaction conversion rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalyst preparation technology and performance application, and specifically relates to a non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate, and a preparation method and application thereof. Background Art

[0002] MG (methyl glycolate) can undergo a variety of chemical reactions because it has both hydroxyl and ester functional groups: methyl glyoxylate obtained by oxidative dehydrogenation of MG contains both aldehyde and ester functional groups, and can be used as an important raw material for the synthesis of products such as vanillin, sunscreen coatings and pharmaceutical intermediates; ethylene glycol obtained by hydrogenation of MG can be used as an antifreeze and coolant, and is also an important additive for the production of polyesters, plasticizers and lubricants; glycine obtained by aminolysis of MG is a very important chemical intermediate, widely used in antiviral drugs, daily chemical production and food processing; methyl malonate obtained by carbonylation of MG is widely used in the synthesis of organic reagents, liquid crystal material manufacturing and pesticide production; glycolic acid obtained by hydrolysis of MG is a precursor of PGA (polyglycolic acid) degradable materials, widely used in chemical cleaning, cosmetics and pharmaceutical production.

[0003] Due to the large-scale production and use of plastic products, a large amount of difficult-to-degrade waste plastics are exposed to natural environments such as the ocean and soil, causing environmental pollution that seriously harms human life and health. Since PGA has good biodegradability and biocompatibility, the development of PGA degradable materials is of great significance to environmental governance and economic and social development, especially the process of preparing MG by catalytic hydrogenation using DMO (i.e. dimethyl oxalate) as raw material meets the requirements of environmental protection and coal resource utilization. DMO hydrogenation to MG is an especially important part of coal-based syngas to PGA. At present, the catalytic system used for DMO hydrogenation to MG is mainly represented by heterogeneous catalysts represented by supported Cu and Ag and homogeneous catalysts represented by precious metal Ru complexes. Among them, the homogeneous Ru complex catalyst is complex to prepare and has a short lifespan. The use of precious metals increases the catalyst cost and is difficult to recover, making it difficult to apply to large-scale industrial production; Cu-based catalysts are too strong in Cu activating hydrogen, and DMO is prone to over-hydrogenation, resulting in low MG yield and poor stability, while the loading amount of Ag-based catalysts is too large, making the cost high, which is not conducive to large-scale industrial application. Secondly, the current heterogeneous catalytic hydrogenation reaction temperature of DMO is greater than 200°C, and its energy consumption is relatively high. Therefore, the design and preparation of a low-temperature and efficient DMO hydrogenation non-precious metal catalyst will not only provide a strong guarantee for the low-cost large-scale production and terminal market supply of PGA, but will also make a positive contribution to the technological innovation of the coal chemical industry. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the purpose of the present invention is to provide a non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate, and a preparation method and application thereof. The catalyst of the present invention has relatively low cost and catalytic temperature, and has high methyl glycolate selectivity and hydrogenation reaction conversion rate.

[0005] The technical solution adopted by the present invention is as follows:

[0006] A non-noble metal alloy catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate, comprising a silicon dioxide carrier and an active component supported on the silicon dioxide carrier;

[0007] Among them, the active component is Ni x Co y The alloy nanoparticles have a value range of x of 1 to 5 and a value range of y of 1 to 2; the content of Ni is 15% of the mass of the non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenation of dimethyl oxalate.

[0008] The present invention also provides a method for preparing the non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenation of dimethyl oxalate, comprising the following steps:

[0009] Adding a precursor solution to a silica carrier and allowing the silica carrier to stand, so that the silica carrier absorbs the precursor solution, to obtain a catalyst precursor; the precursor solution is an aqueous solution of a nickel source and a cobalt source;

[0010] The catalyst precursor is dried, calcined, reduced and passivated to load the active component Ni on the silica carrier. x Co y Alloy nanoparticles are prepared to obtain the non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate.

[0011] Preferably, the nickel source is nickel nitrate, and the cobalt source is cobalt nitrate.

[0012] Preferably, the process of calcining, reducing and passivating the dried catalyst precursor is as follows:

[0013] The dried catalyst precursor is calcined at 345-355°C in an air atmosphere to convert the nickel source and the cobalt source into nickel oxide, cobalt oxide and nickel-cobalt oxide, and then reduced at 395-405°C in a reducing atmosphere to react the nickel oxide, cobalt oxide and nickel-cobalt oxide to form a nickel-cobalt alloy phase, and then cooled to 20-30°C and passivated in a mixed gas of oxygen and nitrogen to form a passivation layer on the surface of the nickel-cobalt alloy phase.

[0014] Preferably, the reducing atmosphere is hydrogen, and the volume content of oxygen in the mixed gas of oxygen and nitrogen is 1% to 3%.

[0015] Preferably, the water content in the precursor solution is equal to the saturated water absorption capacity of the silica carrier.

[0016] Preferably, when the precursor solution is added to the silica carrier: the precursor solution is added to the silica carrier at a rate of 3 to 5 s / drop.

[0017] Preferably, the preparation process of the silica carrier includes:

[0018] The silica gel with CAS number 112926-00-8 is washed and dried, and then calcined at 545-555° C. to remove the template agent remaining in the silica gel during the preparation process, thereby obtaining the silica carrier.

[0019] The present invention also provides the use of the non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenation of dimethyl oxalate as described above, comprising:

[0020] When dimethyl oxalate is hydrogenated to prepare methyl glycolate, the temperature is 170-220°C, the pressure is 1.0-3.0 MPa, and the liquid hourly space velocity is 0.0625-1.0 h -1 The hydrogenation reaction of dimethyl oxalate was carried out under the conditions of .

[0021] Preferably, the application further comprises an activation process:

[0022] The non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate is activated in a hydrogen atmosphere at 395-405° C. to remove the passivation layer, and the activated catalyst is used for preparing methyl glycolate by hydrogenating dimethyl oxalate.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention uses a non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate, adopts a silicon dioxide carrier, fully utilizes the characteristics of silicon dioxide, such as good thermal stability and chemical stability, rich pores and suitable specific surface area, rationally constructs a nickel-cobalt bimetallic alloy catalyst with synergistic effect to regulate the structure and morphology of the metal active site, thereby achieving higher methyl glycolate selectivity and hydrogenation reaction conversion rate at a lower temperature. The active component in the present invention is Ni x Co yAlloy nanoparticles, by doping Co element to construct a highly dispersed nickel-cobalt bimetallic catalyst, combined with relevant characterization, it is found that there is an elemental interaction between Ni and Co to form an alloy phase, which leads to changes in the electronic and surface properties of the bimetallic catalyst, and has better catalytic hydrogenation performance than Ni or Co single metal. The active components in the present invention are non-precious metal Ni and Co, so the cost is relatively low. According to experiments, the catalyst of the present invention can achieve a conversion rate of 87% for dimethyl oxalate and a selectivity of 85% for methyl glycolate under relatively mild conditions (180°C, 2.5MPa), and has good universality and industrial application value. In summary, the cost and catalytic temperature of the catalyst of the present invention are relatively low, and it has high selectivity for methyl glycolate and hydrogenation reaction conversion rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 (a1) is a physical adsorption curve diagram of the Ni1Co0 catalyst in Comparative Example 1 of the present invention; Figure 1 (a2) is a particle size distribution diagram of the Ni1Co0 catalyst in Comparative Example 1 of the present invention; Figure 1 (b1) is a physical adsorption curve diagram of the Ni5Co1 catalyst in Example 1 of the present invention; Figure 1 (b2) is a particle size distribution diagram of the Ni5Co1 catalyst in Example 1 of the present invention; Figure 1 (c1) is a physical adsorption curve diagram of the Ni3Co1 catalyst in Example 2 of the present invention; Figure 1 (c2) is a particle size distribution diagram of the Ni3Co1 catalyst in Example 2 of the present invention; Figure 1 (d1) is a physical adsorption curve diagram of the Ni3Co2 catalyst in Example 3 of the present invention; Figure 1 (d2) is a particle size distribution diagram of the Ni3Co2 catalyst in Example 3 of the present invention; Figure 1 (e1) is a physical adsorption curve diagram of the Ni1Co1 catalyst in Example 4 of the present invention; Figure 1 (e2) is a particle size distribution diagram of the Ni1Co1 catalyst in Example 4 of the present invention; Figure 1 (f1) is a physical adsorption curve diagram of the Ni0Co1 catalyst in Comparative Example 2 of the present invention; Figure 1 (f2) is a particle size distribution diagram of the Ni0Co1 catalyst in Comparative Example 2 of the present invention;

[0026] FIG. 2( a ) is a graph showing the Ni in Comparative Example 1, Examples 1 to 4 and Comparative Example 2 of the present invention. x Co y The conversion rate test diagram of the catalyst; Figure 2 (b) is a graph showing the conversion rate of Ni in Comparative Example 1, Examples 1 to 4 and Comparative Example 2 of the present invention. x Co y Catalyst selectivity test graph;

[0027] FIG3(a) is a TEM morphology image of the Ni3Co2 catalyst in Example 3 of the present invention at a scale of 50 nm; FIG3(b) is a TEM morphology image of the Ni3Co2 catalyst in Example 3 of the present invention at a scale of 10 nm; FIG3(c) is an EDX element distribution image of the Ni3Co2 catalyst in Example 3 of the present invention at a scale of 50 nm;

[0028] Figure 4 The Ni in Comparative Example 1, Examples 1 to 4 and Comparative Example 2 of the present invention is x Co y XRD phase structure spectrum of the catalyst;

[0029] FIG. 5( a ) is a test diagram showing the conversion rate of the Ni3Co2 catalyst in Example 3 of the present invention as a function of the space velocity; FIG. 5( b ) is a test diagram showing the selectivity of the Ni3Co2 catalyst in Example 3 of the present invention as a function of the space velocity;

[0030] Figure 6 The Ni in Comparative Example 1, Examples 1 to 4 and Comparative Example 2 of the present invention is x Co y H2-TPR spectrum of the catalyst. DETAILED DESCRIPTION

[0031] The specific implementation of the embodiment of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0032] The present invention provides a non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate, and a preparation method and application thereof. The present invention selects non-precious metal nickel (Ni) and cobalt (Co) with excellent hydrogenation efficiency and low cost as active components. Based on the similar atomic sizes of the two, this is conducive to mixing and uniform distribution at the atomic level. In addition, the two have good similarity in chemical properties, which is conducive to forming a stable bimetallic structure; secondly, silicon dioxide (SiO2) with good thermal stability and mechanical stability and suitable specific surface area is selected as a carrier, and the DMO conversion rate and MG selectivity are comprehensively improved by means of the synergistic effect of the nickel (Ni) and cobalt (Co) bimetallic.

[0033] The non-precious metal alloy catalyst of the present invention uses nickel and cobalt as active components, and uses an equal volume impregnation method to load the active components on a silicon dioxide carrier, wherein the active component is Ni x Co y The alloy nanoparticles have a value range of x of 1 to 5 and a value range of y of 1 to 2; the content of Ni is 15% of the mass of the non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenation of dimethyl oxalate.

[0034] The preparation method of the non-precious metal alloy catalyst comprises the following steps:

[0035] Step 1: Wash and dry commercial SiO2 (i.e. commercial silica gel) to remove dust, organic matter and other soluble impurities adsorbed on the surface and pores of SiO2. Then place it in a muffle furnace and roast it at 550±5℃ for 6 hours to remove the template agent remaining in the preparation process of commercial SiO2, and improve its stability to obtain a pure and stable SiO2 carrier. Add a certain amount of deionized water to the prepared SiO2 carrier and calculate the water absorption rate of the SiO2 carrier.

[0036] Step 2: Add the nickel source and the cobalt source to a beaker, then add deionized water to dissolve the nickel source and the cobalt source and ultrasonicate for 30 minutes, which helps to disperse the nickel source and the cobalt source more evenly in the solvent, and then obtain a precursor solution; slowly drop the precursor solution into the silica carrier to prevent the drop rate from being too fast and causing agglomeration, so as to obtain a catalyst precursor with a suitable particle size and uniform distribution; wherein, the amount of deionized water added when preparing the precursor solution is equal to the saturated water absorption of the silica carrier, in order to improve the loading efficiency of the active component on the carrier, and the saturated water absorption of the silica carrier is calculated by the water absorption rate of the silica carrier in step 1. When the precursor solution is slowly added to the silica carrier, the precursor solution is added to the silica carrier at a rate of 3 to 5 seconds per drop.

[0037] Step 3: The catalyst precursor is allowed to stand for 12 hours to allow the precursor solution to fully diffuse in the pores of the silica carrier, thereby increasing the loading rate of the active component; then it is dried at 80±5°C for 6 hours to remove moisture while fixing the active component precursor on the carrier to prevent the loss of active components during subsequent treatment or reaction; then it is calcined at 350±5°C for 2 hours in an air atmosphere in a tubular furnace to promote the thermal decomposition of the active component precursor to form nickel oxide, cobalt oxide and nickel-cobalt oxide; then it is reduced at 400±5°C for 4 hours in a hydrogen atmosphere to adjust the oxidation state of the metal elements in the catalyst precursor so that it reacts to form a nickel-cobalt alloy phase; then it is cooled to room temperature (25±5°C), and a mixed gas of oxygen / nitrogen (wherein the volume content of oxygen is 1% to 3%) is introduced for passivation for 15 minutes to form a passivation layer on the surface of the nickel-cobalt alloy phase to prevent the degradation of catalyst performance caused by environmental factors (such as humidity, oxygen, etc.); finally, Ni with different Ni / Co ratios is obtained. x Co y A series of catalysts are prepared to obtain the non-precious metal alloy catalyst of the present invention.

[0038] In the above scheme of the present invention, in each temperature condition, ±5°C is the normal deviation of the equipment, and the parameter before the ± sign is the set value of the equipment. In the experiment, the mixed gas of oxygen and nitrogen is mixed in real time with oxygen and nitrogen, and then introduced into the tube furnace together. Due to the change of the cylinder pressure, the volume fraction of oxygen and nitrogen will change. During the experiment, the volume content of oxygen is maintained between 1% and 3%, which meets the passivation requirements.

[0039] The above-mentioned catalytic reaction performance evaluation method of the present invention is as follows:

[0040] The catalytic hydrogenation of DMO to produce MG is carried out in a stainless steel fixed bed reactor (inner diameter 8.0mm; length 300mm) connected to a high-pressure feed pump, a condenser and a liquid storage tank. A certain amount of catalyst mixed with quartz sand is placed in the central constant temperature zone of the reactor, and quartz wool is filled in the upper and lower sections of the catalyst respectively. The catalyst is activated for 4 hours in a hydrogen atmosphere at 400°C. After the reactor temperature is cooled to the reaction temperature (170-220°C) and the reaction pressure (1.0-3.0MPa) is adjusted to the set value, the methanol solution containing DMO is transported by a high-pressure liquid pump and mixed with hydrogen in a specific proportion, and flows into the reactor from the top of the reactor at a liquid hourly space velocity of 0.0625 to 1.0h -1 The dimethyl oxalate hydrogenation reaction is carried out under the conditions of , and the conversion rate of dimethyl oxalate and the selectivity of methyl glycolate are both greater than 85%.

[0041] It should be noted that if the prepared catalyst is stored for a long time, the activity of the catalyst may be reduced. In this case, it is best to subject the catalyst to the above-mentioned activation process and then carry out the dimethyl oxalate hydrogenation reaction.

[0042] Although supported silver-based and copper-based catalysts have certain activity and selectivity in the hydrogenation reaction of dimethyl oxalate, they each have obvious shortcomings, such as: the silver-based catalyst is too expensive, has low intrinsic activity, and requires a higher reaction temperature; the copper-based catalyst has a low selectivity for methyl glycolate due to its strong hydrogenation ability, which seriously restricts large-scale industrial application. Compared with the prior art, the present invention has the following advantages:

[0043] (1) Taking full advantage of the good thermal and chemical stability, rich pores and suitable specific surface area of ​​silica, a nickel-cobalt bimetallic alloy catalyst with synergistic effects was rationally constructed to regulate the related structure of metal active sites, thereby achieving higher methyl glycolate selectivity and hydrogenation reaction conversion rate at lower temperatures.

[0044] (2) The nickel-cobalt bimetallic alloy catalyst was prepared by the equal volume impregnation method, which has the advantages of simple operation, low cost, good repeatability and uniform distribution of active components, reducing the energy consumption and cost of the catalyst preparation process and improving the metal utilization rate.

[0045] (3) Under relatively mild conditions (180°C, 2.5 MPa), the conversion rate of dimethyl oxalate was 87% and the selectivity of methyl glycolate was 85%, which has good universality and industrial application value.

[0046] In the following embodiments and comparative examples of the present invention, nickel nitrate (Ni(NO3)2·6H2O, CAS: 13138-45-9) is used as a nickel source, cobalt nitrate (Co(NO3)2·6H2O, CAS: 10141-05-6) is used as a cobalt source, and commercial silica gel SiO2 adopts a silica gel reagent with CAS: 112926-00-8. The above nickel nitrate, cobalt nitrate and commercial silica gel are all purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0047] Example 1

[0048] The process of this embodiment is as follows:

[0049] First, 5 g of commercial silica gel was added to 20 g of deionized water at room temperature, and then ultrasonicated for 15 minutes at room temperature, and then filtered and washed three times with deionized water and ethanol. The washed sample was placed in an oven at 80 ° C for 12 hours, and then calcined at 550 ° C for 6 hours in a muffle furnace at a heating rate of 3 ° C / min. Finally, the SiO2 carrier was obtained and its water absorption was calculated to be 1.3 mL / g. The specific surface area was 483.43 m 2 / g, pore volume is 0.75cm 3 / g, pore diameter is 6.03nm, and its phase structure is shown in Figure 4 .

[0050] Next, 2.23g of nickel nitrate hexahydrate and 0.45g of cobalt nitrate hexahydrate were added to a beaker, and then 3.9mL of deionized water was added to dissolve the nickel nitrate hexahydrate and ultrasonicated for 30 minutes to obtain a precursor solution. The precursor solution was slowly added to 3g of SiO2 carrier to obtain Ni5Co1 catalyst precursor. The catalyst precursor was allowed to stand for 12 hours, and then placed in an 80°C oven for 12 hours, and then air was introduced into a tube furnace at 350°C for 2 hours at a heating rate of 3°C / min. After cooling to room temperature, hydrogen was introduced at a heating rate of 3°C / min at 400°C for 4 hours. After cooling to room temperature, an oxygen / nitrogen mixture (1% v / v of O2 / N2) was introduced to passivate the catalyst for 15 minutes, and finally a Ni5Co1 catalyst was obtained. The specific surface area of ​​the Ni5Co1 catalyst was 386.94m by nitrogen physical adsorption / desorption. 2 / g, pore volume is 0.55cm 3 / g, pore size is 5.69nm, the phase structure of Ni5Co1 catalyst is shown in Figure 4 The adsorption-desorption isotherm and pore distribution of the Ni5Co1 catalyst are shown in Figure 1(b1) and Figure 1(b2). It can be seen that there is a hysteresis loop between the relative pressure of 0.4 and 0.98, and there is a partial volume increment with the increase of relative pressure. According to the IUPAC classification, it conforms to the type IV adsorption isotherm and forms an obvious H4 type hysteresis loop with the desorption curve, indicating that it has abundant mesopores.

[0051] Finally, 0.4 g of the above Ni5Co1 catalyst was mixed with quartz sand and loaded into the central constant temperature zone of the fixed bed reactor, and the catalyst was activated for 4 hours in a hydrogen atmosphere at 400 ° C. After the reactor temperature was cooled to the reaction temperature, the reaction pressure was adjusted to 2.5 MPa, and finally the DMO methanol solution was fed into the reactor from the top of the reactor together with hydrogen by a high-pressure liquid feed pump to participate in the reaction. The DMO liquid hourly space velocity was 0.5 h -1 , the molar ratio of hydrogen to DMO is 140:1, and the reaction temperature is 180°C. Combining Figure 2(a) and Figure 2(b), it can be obtained that the conversion rate of dimethyl oxalate is 22%, the selectivity of methyl glycolate is 67%, the selectivity of ethylene glycol is 4%, the selectivity of ethanol is 10%, the selectivity of methyl formate is 10%, the selectivity of methyl acetate is 0, and the selectivity of other by-products is 9%.

[0052] Example 2

[0053] The difference between this embodiment and embodiment 1 is that the amount of cobalt nitrate hexahydrate added is 0.75 g, and the catalyst is named Ni3Co1. The specific surface area of ​​the catalyst is 428.06 m 2 / g, pore volume is 0.59cm 3 / g, pore size is 5.53nm, the phase structure of Ni3Co1 catalyst is shown in Figure 4 The adsorption-desorption isotherms and pore distribution of the Ni3Co1 catalyst are shown in Figures 1(c1) and 1(c2). It can be seen that with the doping of Co, the specific surface area and pore volume are significantly increased, indicating that Co can prevent Ni from agglomerating to form larger particles to block the pores. Under the same performance evaluation conditions as in Example 1, combined with Figures 2(a) and 2(b), it can be obtained that the conversion rate of dimethyl oxalate is 25%, the selectivity of methyl glycolate is 28%, the selectivity of ethylene glycol is 18%, the selectivity of ethanol is 40%, the selectivity of methyl formate is 12%, the selectivity of methyl acetate is 0, and the selectivity of other by-products is 2%.

[0054] Example 3

[0055] The difference between this embodiment and embodiment 1 is that the amount of cobalt nitrate hexahydrate added is 1.50 g, and the catalyst is named Ni3Co2. The specific surface area of ​​the catalyst is 362.84 m 2 / g, pore volume is 0.50cm 3 / g, pore size is 5.55nm, the phase structure of Ni3Co2 catalyst is shown in Figure 4 The adsorption-desorption isotherm and pore distribution of the Ni3Co2 catalyst are shown in Figure 1(d1) and Figure 1(d2). It can be seen that the particle size distribution curve is smooth without sharp turns, indicating that the pore size distribution of the Ni3Co2 catalyst has good uniformity. Under the same performance evaluation conditions as in Example 1, combined with Figure 2(a) and Figure 2(b), it can be obtained that the conversion rate of dimethyl oxalate is 51%, the selectivity of methyl glycolate is 91%, the selectivity of ethylene glycol is 4%, the selectivity of ethanol is 3%, the selectivity of methyl formate is 0, the selectivity of methyl acetate is 0, and the selectivity of other by-products is 2%. The nanoscale morphology of the Ni3Co2 catalyst obtained in this example is as follows: Figure 3(a)-Figure 3(c) As shown, TEM and EDX characterizations show that Ni and Co nanoparticles are uniformly dispersed on the SiO2 carrier, and Ni and Co elements are evenly distributed without obvious phase separation, verifying the formation of the alloy phase.

[0056] The performance of the Ni3Co2 catalyst obtained in this example varies with temperature and pressure as shown in Table 1:

[0057] Table 1

[0058]

[0059] Example 4

[0060] The difference between this embodiment and embodiment 1 is that the amount of cobalt nitrate hexahydrate added is 2.24 g, and the catalyst obtained is named Ni1Co1. The specific surface area of ​​the catalyst is 304.18 m 2 / g, pore volume is 0.45cm 3 / g, pore size is 5.91nm, the phase structure of Ni1Co1 catalyst is shown in Figure 4 The adsorption-desorption isotherms and pore distribution of the Ni1Co1 catalyst are shown in Figures 1(e1) and 1(e2). It can be seen that the specific surface area and pore volume of the catalyst are significantly reduced, indicating that too high a Co doping amount will cause the particle size of the nickel-cobalt alloy to become larger. Under the same performance evaluation conditions as in Example 1, combined with Figures 2(a) and 2(b), it can be obtained that the conversion rate of dimethyl oxalate is 32%, the selectivity of methyl glycolate is 84%, the selectivity of ethylene glycol is 4%, the selectivity of ethanol is 6%, the selectivity of methyl formate is 1%, the selectivity of methyl acetate is 0, and the selectivity of other by-products is 5%.

[0061] Comparative Example 1

[0062] The difference between this comparative example and Example 1 is that the amount of cobalt nitrate hexahydrate added is 0.00 g, and the catalyst is named Ni1Co0. The specific surface area of ​​the catalyst is 258.41 m 2 / g, pore volume is 0.41cm 3 / g, pore size is 6.12nm, the phase structure of Ni1Co0 catalyst is shown in Figure 4 , the adsorption-desorption isotherms and pore distribution of the Ni1Co0 catalyst are shown in Figures 1(a1) and 1(a2). By comparing the SiO2 carrier and the Ni1Co0 catalyst, it can be seen that the specific surface area and pore volume of the supported catalyst are significantly reduced, which may be due to the blocking of some pores by the supported Ni. Under the same performance evaluation conditions as in Example 1, combined with Figures 2(a) and 2(b), it can be obtained that the conversion rate of dimethyl oxalate is 17%, the selectivity of methyl glycolate is 84%, the selectivity of ethylene glycol is 3%, the selectivity of ethanol is 7%, the selectivity of methyl formate is 1%, the selectivity of methyl acetate is 0, and the selectivity of other by-products is 5%.

[0063] Comparative Example 2

[0064] The difference between this comparative example and Example 1 is that the amount of nickel nitrate hexahydrate added is 0.00 g, and the amount of cobalt nitrate hexahydrate added is 2.24 g, and the catalyst is named Ni0Co1. The specific surface area of ​​the catalyst is 315.18 m 2 / g, pore volume is 0.51cm 3 / g, pore size is 6.23nm, the phase structure of Ni0Co1 catalyst is shown in Figure 4 , the adsorption-desorption isotherms and pore distribution of Ni0Co1 catalyst are shown in Figure 1 (f1) and Figure 1 (f2). The specific surface area and pore volume of Ni0Co1 catalyst are significantly larger than those of Ni1Co0 catalyst, but smaller than those of Ni5Co1, Ni3Co1 and Ni3Co2. It can be seen that the particle size of cobalt in Ni0Co1 catalyst is smaller than that of nickel in Ni1Co0 catalyst, and the doping of Co element to construct a highly dispersed nickel-cobalt bimetallic alloy catalyst has more excellent physicochemical properties than Ni or Co single metal. Under the same performance evaluation conditions as Example 1, combined with Figure 2 (a) and Figure 2 (b), it can be obtained that the conversion rate of dimethyl oxalate is 20%, the selectivity of methyl glycolate is 85%, the selectivity of ethylene glycol is 6%, the selectivity of ethanol is 5%, the selectivity of methyl formate is 2%, the selectivity of methyl acetate is 0, and the selectivity of other by-products is 2%.

[0065] Based on the above examples and comparative examples, the phase composition of the catalyst in the examples was analyzed by XRD, and the results are as follows: Figure 4 As shown, it can be seen that the X-ray diffraction peaks of the SiO2 carrier are attributed to the characteristic peaks of the (101) crystal plane of SiO2 according to the XRD standard spectrum (PDF#76-0940). The X-ray diffraction peaks of Ni1Co0 are attributed to the characteristic peaks of Ni(111), (200), and (220) crystal planes according to the XRD standard spectrum (PDF#70-1849), and there are weak NiO characteristic peaks; the X-ray diffraction peaks of Ni0Co1 are attributed to the characteristic peaks of CoO(111), (220), and (311) crystal planes according to the XRD standard spectrum (PDF#70-2856), and there are Co characteristic peaks. The main diffraction peaks of the nickel-cobalt bimetallic catalysts of Examples 1 to 4 are located between Ni and Co, and no new impurity peaks are generated, indicating that alloy structures are formed; as the Ni / Co ratio increases, the offset of the X-ray diffraction peak from Ni to Co increases, indicating that the interaction between the nickel-cobalt bimetallic is enhanced.

[0066] Based on the above examples and comparative examples, the catalyst reduction performance was analyzed by H2-TPR. Figure 6As shown, it can be seen that the reduction peak of Ni1Co0 at 358.5°C is the reduction of NiO to Ni, the reduction peak of Ni0Co1 at 315.6°C is the reduction of Co3O4 to CoO, and the reduction peak of 508.1 in the high temperature zone corresponds to the reduction of CoO to Co; this indicates that there are a small amount of Co3O4 and a large amount of CoO species in Ni0Co1, and NiO species in the Ni1Co0 catalyst, which is consistent with the XRD result analysis. In the nickel-cobalt bimetallic catalysts of Examples 1 to 4, as the Ni / Co ratio increases, the reduction peak shifts to the high temperature zone, which may be due to the change in the electron cloud density of the nickel-cobalt bimetallic, the stabilization effect is enhanced, and a higher reduction temperature is required, which further indicates that the nickel-cobalt bimetallic forms an alloy phase.

[0067] Example 5

[0068] The Ni3Co2 catalyst prepared in Example 3 with relatively high dimethyl oxalate conversion and methyl glycolate selectivity was comprehensively selected, and the performance was evaluated under the same conditions as in Example 3 within a temperature range of 170-220°C to explore the effect of temperature on the reactant conversion and product selectivity. Combining the results in Table 1, the following conclusions can be drawn: the conversion of dimethyl oxalate decreases with decreasing temperature and increases with increasing temperature, the selectivity of methyl glycolate decreases with increasing temperature, and the selectivity of ethylene glycol and ethanol increases with increasing temperature.

[0069] Example 6

[0070] The Ni3Co2 catalyst prepared in Example 3 with relatively high dimethyl oxalate conversion and methyl glycolate selectivity was comprehensively selected, and the performance was evaluated under the same conditions as in Example 3 within a pressure range of 1.0-3.0 MPa to explore the effect of pressure on reactant conversion and product selectivity. Combined with the results in Table 1, the following conclusions can be drawn: the conversion of dimethyl oxalate decreases with decreasing pressure, and the selectivity of methyl glycolate decreases with increasing pressure. When the pressure is within the range of 1.0-3.0 MPa, the product is still mainly methyl glycolate.

[0071] Example 7

[0072] Based on the experimental results of Example 5 and Example 6, the reaction conditions (180°C, 2.5 MPa) with relatively high conversion rate of dimethyl oxalate and selectivity of methyl glycolate were selected, and the reaction temperature was 0.0625-1.0 h. -1 In the range of air velocity, the performance evaluation was carried out under the same conditions as in Example 3 to explore the effect of air velocity on the conversion rate of reactants and the selectivity of products. Combining the result graphs of Figure 5(a) and Figure 5(b), the following conclusions can be drawn: the conversion rate of dimethyl oxalate increases with the decrease of air velocity, and the selectivity of methyl glycolate increases with the increase of air velocity. When the air velocity is between 0.0625-1.0h -1In the range of 0.125h -1 Under the conditions of , the conversion rate of dimethyl oxalate was 87% and the selectivity of methyl glycolate was 85%.

[0073] It can be seen from the above scheme that the present invention constructs a highly dispersed nickel-cobalt bimetallic alloy catalyst by doping Co element, which has better catalytic hydrogenation performance than Ni or Co single metal; Ni and Co interact to form an alloy phase, resulting in changes in the coordination environment, particle size and surface properties of the bimetallic catalyst, thereby enhancing the activation ability of the reactants and the product selectivity, thereby comprehensively improving the conversion rate of dimethyl oxalate and the yield of methyl glycolate.

[0074] The technical solution provided by the present invention demonstrates its unique technical route and application potential through the above-mentioned embodiments. However, the present invention is not limited to the embodiments described, but covers specific methods, material preparation and conclusions that conform to its technical essence. Any reasonable changes to the existing embodiments, or equivalent modifications based on the principles of the present invention, should not exceed the scope of protection of the present invention.

Claims

1. A non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenation of dimethyl oxalate, characterized in that: It includes a silicon dioxide carrier and an active component loaded on the silicon dioxide carrier; Among them, the active component is Ni x Co y The alloy nanoparticles have a value range of x of 1 to 5 and a value range of y of 1 to 2; the content of Ni is 15% of the mass of the non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenation of dimethyl oxalate.

2. The method for preparing the non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenation of dimethyl oxalate according to claim 1, characterized in that: The process includes the following: Adding a precursor solution to a silica carrier and allowing the silica carrier to stand to allow the precursor solution to be adsorbed by the silica carrier to obtain a catalyst precursor, wherein the precursor solution is an aqueous solution of a nickel source and a cobalt source; The catalyst precursor is dried, calcined, reduced and passivated to load the active component Ni on the silica carrier. x Co y Alloy nanoparticles are prepared to obtain the non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate.

3. The method for preparing a non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenation of dimethyl oxalate according to claim 2, characterized in that: The nickel source is nickel nitrate, and the cobalt source is cobalt nitrate.

4. The method for preparing a non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenation of dimethyl oxalate according to claim 2, characterized in that: The process of calcining, reducing and passivating the dried catalyst precursor is as follows: The dried catalyst precursor is calcined at 345-355° C. in an air atmosphere to convert the nickel source and the cobalt source into nickel oxide, cobalt oxide and nickel-cobalt oxide, and then reduced at 395-405° C. in a reducing atmosphere to react the nickel oxide, cobalt oxide and nickel-cobalt oxide to form a nickel-cobalt alloy phase, and then cooled to 20-30° C. and passivated in a mixed gas of oxygen and nitrogen to form a passivation layer on the surface of the nickel-cobalt alloy phase.

5. The method for preparing a non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenation of dimethyl oxalate according to claim 4, characterized in that: The reducing atmosphere is hydrogen, and the volume content of oxygen in the mixed gas of oxygen and nitrogen is 1% to 3%.

6. The method for preparing a non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenation of dimethyl oxalate according to claim 2, characterized in that: The water content in the precursor solution is equal to the saturated water absorption capacity of the silica carrier.

7. The method for preparing a non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenation of dimethyl oxalate according to claim 2, characterized in that: When adding the precursor solution to the silica carrier: add the precursor solution to the silica carrier at a rate of 3 to 5 s / drop.

8. The method for preparing a non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenation of dimethyl oxalate according to any one of claims 2 to 7, characterized in that: The preparation process of the silica carrier comprises: The silica gel with CAS number 112926-00-8 is washed and dried, and then calcined at 545-555° C. to remove the template agent remaining in the silica gel during the preparation process, thereby obtaining the silica carrier.

9. The use of the non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenation of dimethyl oxalate according to claim 1, characterized in that: include: When dimethyl oxalate is hydrogenated to prepare methyl glycolate, the temperature is 170-220°C, the pressure is 1.0-3.0 MPa, and the liquid hourly space velocity is 0.0625-1.0 h -1 The hydrogenation reaction of dimethyl oxalate was carried out under the conditions of .

10. The use of the non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenation of dimethyl oxalate according to claim 9, characterized in that: Also includes the activation process: The non-precious metal alloy catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate is activated in a hydrogen atmosphere at 395-405° C. to remove the passivation layer, and the activated catalyst is used for preparing methyl glycolate by hydrogenating dimethyl oxalate.

Citation Information

Patent Citations

  • Supported nickel-based alloy catalyst as well as preparation method and application thereof

    CN109675569A

  • Catalyst for producing ethyl alcohol through C2 acid ester hydrogenation, and preparation and application of catalyst

    CN110385131A

  • Preparation method and application of supported catalyst for catalyzing hydrogenation of dimethyl oxalate

    CN111774050A

  • Catalyst for preparing butanedioic anhydride through maleic anhydride liquid phase hydrogenation as well as preparation method and application of catalyst

    CN116037193A

  • Catalyst for hydrogenation of dimethyl oxalate to ethylene glycol, and preparation method of catalyst

    WO2023236341A1