Preparation method of efficient denitration catalyst capable of adjusting acid site

The solvent-free doping method for MnCr and MnCr x Ni1-x catalysts addresses the limitations of V2O5-WO3/TiO2 by enhancing low-temperature denitrification and SO2 resistance, achieving high denitrification efficiency and economic benefits.

CN119076009APending Publication Date: 2024-12-06HENAN POLYTECHNIC UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411178107.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing commercial V2O5-WO3/TiO2 catalysts are ineffective at low temperatures and prone to deactivation by SO2, and are toxic, necessitating the development of low-temperature denitrification catalysts with improved SO2 resistance and adjustable acidity.

Method used

A solvent-free doping method is used to prepare MnCr and MnCr x Ni1-x catalysts with adjustable acidity by incorporating Ni sources, enhancing the catalyst's anti-deactivation ability and optimizing the denitrification temperature range.

Benefits of technology

The catalysts exhibit high denitrification activity at 150-200°C and 200-250°C, with excellent resistance to SO2/H2O inactivation and a simple preparation process, improving economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076009A_ABST
    Figure CN119076009A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of denitration catalysts, in particular to a preparation method of an efficient denitration catalyst capable of adjusting an acid site. According to the invention, Mn (CH3COO) 2.4 H2O and KMnO4 are used as Mn sources, Cr (NO3) 3.9 H2O is used as a Cr source, Ni (NO3) 2.6 H2O or Ni (CH3COO) 2.4 H2O is used as a Ni source, and a solvent-free doping method is used for preparation; different Ni sources are used for doping MnCr, so that regulation and control on acidity are realized. The catalyst MnCrxNi < 1-x-n > and the catalyst MnCrxNi < 1-x-c > which are finally prepared by the method disclosed by the invention show different catalytic behaviors, and the catalyst reaches the optimal denitration activity at the temperature of 150-200 DEG C and the temperature of 200-250 DEG C respectively. The catalyst prepared by the preparation method disclosed by the invention has excellent inactivation resistance on SO2 / H2O and SO2 + H2O.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of denitration catalysts, and in particular to a method for preparing a high-efficiency denitration catalyst with adjustable acidic sites. Background Art

[0002] Currently, V 2 O 5 -WO 3 / TiO 2 As the most commonly used commercial catalyst, it has a good denitrification effect in the temperature range of 300-400℃. However, most industrial exhaust gases cannot reach above 300℃, so the development of efficient denitrification catalysts at low temperatures is essential. And in the actual working process, V 2 O 5 -WO 3 / TiO 2 It is easy to adsorb SO 2 Gases cause the catalyst to deactivate, and the catalyst itself is toxic. The catalyst is placed downstream of the desulfurizer and particle controller for treatment, which requires the development of catalysts with better low-temperature denitrification performance. Summary of the invention

[0003] The present invention is to overcome the denitration catalyst V in the prior art 2 O 5 -WO 3 / TiO 2 The present invention provides a method for preparing a highly efficient denitration catalyst with adjustable acidity. The catalyst of the present invention is enhanced by Ni doping to improve the catalyst's SO 2 / H 2 O's anti-deactivation ability is improved, and Ni doping is used to achieve the regulation of the optimal denitrification temperature range.

[0004] The present invention specifically adopts the following technical solutions: The present invention uses a solvent-free doping method to prepare MnCr and MnCr x Ni 1-x Series of denitrification catalysts.

[0005] Preparation of MnCr catalyst, Mn(CH 3 COO 2 ·4H 2 O and KMnO 4 As Mn source, Cr(NO 3 ) 3 9H 2 O is a Cr source, comprising the following steps: Step 1: First, the raw material Mn(CH3 COO 2 ·4H 2 O, KMnO 4 Cr(NO 3 ) 3 9H 2 O Weigh and mix according to the molar ratio of 3:2:3. Then, grind the raw materials until the medicine is evenly mixed. Put the mixed medicine in an environment of 75-85℃ for drying.

[0006] Step 2: Then, take out the completely dried sample and add deionized water to dissolve it. Then, gradually add the dissolved sample into the funnel for filtration and washing until the filtrate is completely clear. Put the obtained precipitate into the environment of 75-85°C again until it is completely dried. Specifically, the drying time is 12 hours.

[0007] For efficient denitrification catalyst MnCr with adjustable acid position x Ni 1-x For example, its preparation is based on Mn(CH 3 COO 2 ·4H 2 O and KMnO 4 As Mn source, Cr(NO 3 ) 3 9H 2 O is the source of Cr, Ni(NO 3 ) 2 6H 2 O or Ni(CH 3 COO 2 ·4H 2 O is a Ni source, and the acidity is regulated by doping MnCr with different Ni sources, which specifically includes the following steps: Step 1: Prepare the raw material Mn(CH 3 COO 2 ·4H 2 O, KMnO 4 Cr(NO 3 ) 3 9H 2 O and Ni source are weighed and mixed in a molar ratio of 3:2:(0.9-2.1):(0.9-2.1). Then, the raw materials are ground to mix evenly. The mixed raw materials are placed in an environment of 75-85°C for drying. The Ni source is Ni(NO 3 ) 2 6H 2 O or Ni(CH 3 COO 2 ·4H 2 O. Preferably, the raw material Mn(CH3 COO 2 ·4H 2 O, KMnO 4 Cr(NO 3 ) 3 9H 2 The molar ratio of O and Ni sources is 3:2:2.1:0.9.

[0008] Step 2: Then take out the completely dried sample and add an appropriate amount of deionized water to dissolve it. Then, gradually add the dissolved sample into the funnel for filtration and washing until the filtrate is completely clear. Put the obtained precipitate into an environment of 75-85°C again until the precipitate is completely dried. Specifically, the drying time is 12 hours.

[0009] Take Ni(NO 3 ) 2 6H 2 O and Ni(CH 3 COO 2 ·4H 2 O is MnCr x Ni 1-x The Ni sources of the catalyst are denoted as MnCr x Ni 1-x -n and MnCr x Ni 1-x -c.

[0010] The beneficial effects of the present invention are: 1. Catalyst MnCr prepared by the present invention x Ni 1-x -n and MnCr x Ni 1-x -c uses different Ni sources to dope MnCr to achieve the regulation of acidity, and finally makes the catalyst MnCr x Ni 1-x -n and MnCr x Ni 1-x -c exhibits different catalytic behaviors, which is manifested in that the catalyst achieves the best denitrification activity at 150-200°C and 200-250°C, respectively.

[0011] 2. Catalyst MnCr prepared by the present invention x Ni 1-x -n and MnCr x Ni 1-x -c for SO 2 / H 2 O and SO 2 +H 2 O has excellent resistance to inactivation.

[0012] 3. Catalyst MnCr prepared by the present invention 0.3 Ni 0.7 The large number of acid sites and low activation energy in MnCr-n enable the catalyst to perform efficient denitration reactions at lower temperatures. 0.3 Ni 0.7 -c's strong redox ability improves the activity of the catalyst.

[0013] 4. Catalyst MnCr of the present invention x Ni 1-x -n and MnCr x Ni 1-x -c has a simple preparation process, which improves the economic benefits of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 NO conversion rate of MnCr catalysts prepared by different methods at 100-325℃.

[0015] Figure 2 MnCr x Ni 1-x -n and MnCr x Ni 1-x -c NO x Conversion rate.

[0016] Figure 3 For the catalyst MnCr, MnCr 0.7 Ni 0.3 -n and MnCr 0.7 Ni 0.3 -c Anti-H 2 O / SO 2 Poisoning ability.

[0017] Figure 4 MnCr 0.3 Ni 0.7 -n、MnCr 0.3 Ni 0.7 -c series catalysts NH 3 Programmed temperature desorption curve (a) and NH 3 Desorption amount (b). DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution in the embodiment of the present invention will be clearly described below in conjunction with the drawings in the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] Example 1 Comparison of MnCr catalysts prepared by different methods: MnCr catalysts were prepared by co-precipitation method, citric acid method and solvent-free doping method, respectively.

[0020] Among them, the Mn source and Cr source used in the preparation of MnCr catalysts by coprecipitation method and citric acid method were Mn(CH 3 COO 2 ·4H 2 O and Cr(NO 3 ) 3 9H 2 O, preparation method reference (Fengyu Gao, Xiaolong Tang, Honghong Yi, Shunzheng Zhao, Jiangen Wang, Tian Gu, Improvement of activity, selectivity and H 2 O&SO 2 -tolerance of micro-mesoporous CrMn 2 O 4 spinel catalyst for low-temperature NH 3 -SCR of NOx,Applied Surface Science,Volume 466,2019,Pages 411-424,ISSN 0169-4332,https: / / doi.org / 10.1016 / j.apsusc.2018.09.227.) The solvent-free doping method is used to prepare the MnCr catalyst. The specific steps are as follows: Step 1: Mn(CH 3 COO 2 ·4H 2 O, KMnO 4 Cr(NO 3 ) 3 9H 2 O was weighed and mixed in a molar ratio of 3:2:3. Then, the raw materials were ground in an agate mortar until the mixture was uniform. The mixed raw materials were placed in a blast drying oven at 80° C. for drying.

[0021] Step 2: Then take out the completely dried sample and add an appropriate amount of deionized water to dissolve it. Then, gradually add the dissolved sample into the funnel for filtration and washing until the filtrate is completely clear. Put the obtained precipitate into the drying oven at 80°C and dry it for 12 hours.

[0022] Then the NO conversion rates of the catalysts were compared. Figure 1 As shown. It can be seen that the MnCr catalyst prepared by the co-precipitation method has poor activity in the entire temperature range, and the best denitrification efficiency (74%) is achieved at 150-200°C. The catalyst prepared by the citric acid method has improved effect, reaching 87% NO conversion rate at 200-225°C. Although the catalytic effect has improved, the temperature range has decreased. The MnCr catalyst prepared by the solvent-free doping method achieved a conversion rate of 91% at 175-225°C, and the denitrification effect reached more than 80% within 150-300°C. It shows that the MnCr catalyst prepared by the solvent-free doping method has a better denitrification effect.

[0023] Example 2 Preparation of low-temperature denitrification catalyst MnCr by solvent-free doping method x Ni 1-x -n, include: Step 1: Prepare the raw material Mn(CH 3 COO 2 ·4H 2 O, KMnO 4 Cr(NO 3 ) 3 9H 2 O and Ni (NO 3 ) 2 6H 2 O were weighed and mixed in a molar ratio of 3:2:2.1:0.9, 3:2:1.5:1.5, and 3:2:0.9:2.1. Then, the raw materials were ground in an agate mortar until the medicines were evenly mixed. The mixed raw materials were placed in a blast drying oven at 80°C for drying.

[0024] Step 2: Then take out the completely dried sample and add an appropriate amount of deionized water to dissolve it. Then, gradually add the dissolved sample into the funnel for filtration and washing until the filtrate is completely clear. Put the obtained precipitate into the drying oven at 80°C and dry it for 12 hours.

[0025] Example 3 Preparation of low-temperature denitrification catalyst MnCr by solvent-free doping method x Ni 1-x -c, include: Step 1: Prepare the raw material Mn(CH 3 COO 2 ·4H 2 O, KMnO 4 Cr(NO 3 ) 3 9H2 O and Ni(CH 3 COO 2 ·4H 2 O Weigh and mix according to the molar ratio of 3:2:2.1:0.9, 3:2:1.5:1.5, and 3:2:0.9:2.1. Then, grind the raw materials in an agate mortar until the medicine is evenly mixed. Put the mixed raw materials into a blast drying oven at 80°C for drying.

[0026] Step 2: Then take out the completely dried sample and add an appropriate amount of deionized water to dissolve it. Then, gradually add the dissolved sample into the funnel for filtration and washing until the filtrate is completely clear. Put the obtained precipitate into the drying oven at 80°C and dry it for 12 hours.

[0027] Catalyst activity evaluation: A fixed reactor with an inner diameter of 6 mm and an outer diameter of 8 mm was used to 3 -SCR performance was evaluated. 40 to 60 g of the catalysts (0.3 g) of Example 1 (solvent-free doping method), Example 2, and Example 3 were screened and loaded on the reaction bed. 2 , O 2 (5 vol%), NO (500 ppm), NH 3 (500ppm), SO 2 (100ppm) and H 2 O (10 vol%) mixed atmosphere for 60000h -1 The SCR reaction is carried out at a space velocity of 1.5 %. The NO x (NO+NO 2 ) concentration data were processed according to the corresponding formula to obtain the NO x and NH 3 conversion rate.

[0028] Example 2 Preparation of MnCr x Ni 1-x -n, MnCr prepared in Example 3 x Ni 1-x The conversion rate comparison of MnCr prepared by solvent-free doping method in Example 1 is shown in FIG. Figure 2 MnCr 0.3 Ni 0.7 -n and MnCr 0.3 Ni 0.7 H-resistance of MnCr prepared by -c and solvent-free doping method 2 O / SO 2 and SO 2 +H2 O performance as Figure 3 shown.

[0029] Depend on Figure 2 It can be concluded that MnCr 0.3 Ni 0.7 -n and MnCr 0.3 Ni 0.7 -c has the best denitration efficiency among the entire series of catalysts, reaching a conversion rate of 96% at 150-200°C and 200-250°C respectively. 0.5 Ni 0.5 -n only reaches 91% at 150-200℃, MnCr 0.5 Ni 0.5 -c and MnCr 0.7 Ni 0.3 -n catalytic efficiency at 175-225℃ reaches 70% and 91% respectively, MnCr 0.7 Ni 0.3 -c The denitrification efficiency is 87% at 225-275℃.

[0030] Combination Figure 3 Get, MnCr 0.3 Ni 0.7 -n and MnCr 0.3 Ni 0.7 -c's anti-SO 2 / H 2 O is very good, and in the face of SO 2 +H 2 O when MnCr 0.3 Ni 0.7 -c showed the best resistance to inactivation.

[0031] Depend on Figure 4 (a) Get, MnCr 0.3 Ni 0.7 -n catalyst ratio MnCr 0.3 Ni 0.7 -c catalyst has 2 more NH 3 The analytical peak indicates that MnCr 0.3 Ni 0.7 -n has more types of acidic active centers. It also shows that different Ni forms different interactions with Mn and Cr. The peak at 125.5-284.5℃ belongs to weak acid, and the peak at 369.9-488.2℃ is considered to be medium-strong acid. The peak at 601.9-777.1℃ is related to strong acid. 0.3 Ni 0.7 -n weak acid, medium strong acid quantity is greater than MnCr 0.3 Ni 0.7-c Catalyst. Combination Figure 4 (b) It can be seen that Ni(NO 3 ) 2 6H 2 The introduction of O can strengthen the acidic environment of the catalyst, increase the number of acidic active sites, and promote the NH 3 The adsorption on the catalyst surface enables the catalyst to perform a stronger denitrification reaction at a lower temperature. 0.3 Ni 0.7 -c strong acid peak number and NH 3 The adsorption capacity is greater than that of MnCr 0.3 Ni 0.7 -n. This makes the catalyst more reactive to NH at higher temperatures. 3 Effective adsorption is carried out, which causes the optimal denitration temperature of the catalyst to shift to a higher temperature.

[0032] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a high-efficiency denitration catalyst with adjustable acidic sites, characterized in that: It is prepared by a solvent-free doping method using Mn(CH3COO)2·4H2O and KMnO4 as Mn sources, Cr(NO3)3·9H2O as Cr source, and Ni(NO3)2·6H2O or Ni (CH3COO)2·4H2O as Ni source; the acidity is controlled by doping MnCr with different Ni sources.

2. The method for preparing a high-efficiency denitration catalyst with adjustable acidic sites according to claim 1, characterized in that: The following steps are involved: Step 1: Weigh and mix the raw materials Mn(CH3COO)2·4H2O, KMnO4, Cr(NO3)3·9H2O and Ni source in a molar ratio of 3:2:(0.9-2.1):(0.9-2.1); then place the mixed raw materials in an environment of 75-85°C for drying; Step 2: Then, take out the completely dried sample and add deionized water to dissolve it; then, filter and wash the dissolved sample until the filtrate is completely clear; and place the obtained precipitate in an environment of 75-85°C again until the precipitate is completely dried.

3. The method for preparing a high-efficiency denitration catalyst with adjustable acidic sites according to claim 2, characterized in that: In step 1, the molar ratio of the raw materials Mn(CH3COO)2·4H2O, KMnO4, Cr(NO3)3·9H2O and Ni source is 3:2: 2.1:0.

9.

4. The method for preparing a high-efficiency denitration catalyst with adjustable acidic sites according to claim 2, characterized in that: In step 1, the drying temperature is 80°C.

5. The method for preparing a high-efficiency denitration catalyst with adjustable acidic sites according to claim 1, characterized in that: In step 2, the drying temperature is 80° C. and the drying time is 12 h.