Composite Mn-based catalyst as well as preparation method and application thereof

By combining LwMnxNy hydrotalcite with TiO2 precursor, a composite Mn-based catalyst was prepared, which solved the problem of thermal stability and anti-SO2 poisoning at low temperatures, and achieved efficient removal of NOx and improved N2 selectivity.

CN119076011APending Publication Date: 2024-12-06QINGDAO AGRI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411306744.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Mn-based catalysts have problems such as insufficient thermal stability, insufficient N2 selectivity and susceptibility to SO2 poisoning at low temperatures, resulting in low application efficiency in SCR technology.

Method used

By combining LwMnxNy hydrotalcite with TiO2 precursor, a composite Mn-based catalyst was prepared, and the layered structure was destroyed by high-temperature calcination treatment, forming highly dispersed metal oxides, avoiding agglomeration, and improving the activity and sulfur resistance of the catalyst.

Benefits of technology

It realizes efficient removal of NOx at medium and low temperatures, improves N2 selectivity and catalyst stability, and maintains high NOx removal rate and anti-SO2 poisoning performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076011A_ABST
    Figure CN119076011A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of catalysts, in particular to a composite Mn-based catalyst as well as a preparation method and application thereof. The preparation method of the composite Mn-based catalyst comprises the following steps: step 1, calcining LwMnxNy hydrotalcite to obtain a catalyst precursor; step 2, adding the catalyst precursor into a solvent to prepare a suspension; step 3, adding a TiO2 precursor mixed solution into the suspension to generate a precipitate; and 4, centrifuging, washing, drying the precipitate, and calcining to obtain the composite Mn-based catalyst. The composite Mn-based catalyst provided by the invention generates more surface adsorption oxygen and active sites, has excellent oxidation-reduction ability, effectively adsorbs more NH3 to participate in SCR reaction and improves N2 selectivity, TiO2 loaded in the catalyst has high adsorbability to SO2, and the sulfur poisoning phenomenon of the catalyst in the flue gas denitration process is better promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and in particular to a composite Mn-based catalyst and a preparation method and application thereof. Background Art

[0002] Nitrogen oxides (NO x ) is one of the main pollutants in the atmosphere. x Excessive emissions will intensify the frequent occurrence of severe weather such as acid rain, photochemical smog, and haze, seriously affecting human health and the ecological environment. x It mainly comes from industrial furnaces such as thermal power plants and cement plants, while NO generated by human activities x It mainly comes from the combustion of fossil fuels such as automobile exhaust and diesel exhaust.

[0003] Selective Catalytic Reduction (SCR) is a process that reduces NO by adding an external reducing agent. x A flue gas treatment method that converts it into N2. Among them, the selective catalytic reduction (NH3-SCR) technology using NH3 as a reducing agent has received widespread attention at home and abroad in recent years due to its high denitration efficiency and relatively mature technology. In the entire technical process, the catalyst is the core part. However, some substances carried in the flue gas (SO2, water vapor, etc.) will be deposited on the catalyst to form ammonium bisulfate to cover the active sites, causing the catalyst to deactivate and reduce the denitration rate. Therefore, while improving the denitration efficiency, improving the SO2 resistance of the NH3-SCR catalyst is of great significance in industrial applications.

[0004] In addition to commercial vanadium-based catalysts, recent studies have found that other metal oxides, such as MnO x , CuO x ,FeO x and CeO x All of them showed good SCR denitrification performance. In terms of low-temperature catalysis, Mn-based catalysts are considered to be one of the catalysts with excellent performance, but due to their insufficient thermal stability, insufficient N2 selectivity, and susceptibility to SO2 poisoning, improving the N2 selectivity and sulfur resistance of the catalyst is an urgent problem to be solved for Mn-based catalysts. Summary of the invention

[0005] In view of this, the present invention provides a composite Mn-based catalyst and a preparation method and application thereof, so as to improve the N2 selectivity, denitration rate and sulfur resistance of the Mn-based catalyst.

[0006] To achieve the above object, the present invention provides the following solutions:

[0007] One of the technical solutions of the present invention is a method for preparing a composite Mn-based catalyst, comprising the following steps:

[0008] Step 1: L w Mn x N y calcining the hydrotalcite-like substance to obtain a catalyst precursor;

[0009] Step 2, adding the catalyst precursor into a solvent to prepare a suspension;

[0010] Step 3, adding a TiO2 precursor mixed solution to the suspension to generate a precipitate;

[0011] Step 4, centrifuging, washing, drying and then calcining the precipitate to obtain the composite Mn-based catalyst;

[0012] The L w Mn x N y Wherein L is at least one of Cu, Ni and Co, N is Al and / or Fe, w, x, y are the molar fractions of L, Mn and N respectively, w:y is 1 / 8 to 2 / 1, x:y is 1 / 8 to 2 / 1. More preferably, w:y is 1 / 2 to 3 / 2, x:y is 1 / 2 to 3 / 2; more preferably, w:y is 1 / 2, x:y is 3 / 2.

[0013] The second technical solution of the present invention is a composite Mn-based catalyst prepared according to the above preparation method, the chemical composition of which is TiO2 / L w Mn x N y O z , wherein L is at least one of Cu, Ni and Co, N is at least one of Al and Fe, w, x, y, z are respectively the molar fractions of L, Mn, N and O in the composite Mn-based catalyst, w / y is 1 / 2 to 2 / 1, x / y is 1 / 2 to 2 / 1, w = 0.5 to 2, x = 0.5 to 2, y = 1; TiO2 and L w Mn x N y O z The mass ratio is 0.2~1.

[0014] The third technical solution of the present invention is that the above-mentioned composite Mn-based catalyst is used to remove NO from industrial flue gas. x The composite Mn-based catalyst selectively catalytically reduces NO x The temperature range is 100-300°C. Further preferably, the selective catalytic reduction of NO x The temperature range is 150-300°C. More preferably, the selective catalytic reduction of NO xThe temperature range is 200°C.

[0015] The present invention discloses the following technical effects:

[0016] The present invention provides a method for preparing a highly efficient composite Mn-based catalyst that can be used in medium- and low-temperature sulfur-resistant SCR technology. w Mn x N y O z The composite Mn-based catalyst TiO2 / L was prepared by loading TiO2 as a catalyst precursor. w Mn x N y O z The metal species are highly dispersed in the catalyst. The synthesis of a catalyst containing both active components and auxiliary components can produce more effective metal oxides for removing NO from industrial flue gas. x The catalyst not only effectively removes pollutants, but also has high N2 selectivity and stability, and can maintain high NO even in the presence of SO2. x Removal rate and material regeneration performance.

[0017] The present invention synthesizes a layered hydrotalcite-like (LDHs) material from three precursor substances containing L, N and Mn (such as Mn(NO3)2, Co(NO3)2·6H2O and Fe(NO3)3·9H2O). The LDHs are formed by the accumulation of interlayer anions and positively charged superposition plates. The LDHs are calcined at high temperature. During the treatment, the original layered hydroxide structure is destroyed due to the removal of hydroxyl groups and carbonate groups, and is converted into highly dispersed metal oxides and spinel phases. The agglomeration of active components in materials prepared by traditional loading methods can be effectively avoided. The obtained composite material has small grains, high dispersibility, large specific surface area, can inhibit sintering during high-temperature calcination, and has good catalytic performance and anti-poisoning performance.

[0018] The composite Mn-based catalyst of the present invention produces more surface adsorbed oxygen and active sites, excellent redox ability, effectively adsorbs more NH3 to participate in the SCR reaction and improves N2 selectivity. The TiO2 loaded in the catalyst has a high adsorption capacity for SO2, which better promotes the sulfur poisoning phenomenon of the catalyst during the flue gas denitrification process. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0020] Figure 1 a is the X-ray diffraction spectra of the catalysts prepared in Example 1 and Comparative Examples 1 and 2, and b is the X-ray diffraction spectra of TiO2(0.5) / Co after calcination in Example 1. 0.5 Mn 1.5 Fe1O z TEM-EDS images of the catalyst. DETAILED DESCRIPTION

[0021] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0022] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0023] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0024] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0025] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0026] The "%" described in the present invention, unless otherwise specified, refers to mass percentage.

[0027] The "room temperature" described in the present invention, unless otherwise specified, refers to 20-30°C.

[0028] The deposition and decomposition of sulfate are closely related to the physical structure. Comprehensive control of the physical structure and chemical properties of the catalyst is an important means to improve the overall performance and sulfur resistance of the Mn-based catalyst. Based on this, the present invention provides a composite Mn-based catalyst and its preparation method and application.

[0029] The first aspect of the present invention provides a method for preparing a composite Mn-based catalyst, comprising the following steps:

[0030] Step 1: L w Mn x N y calcining the hydrotalcite-like substance to obtain a catalyst precursor;

[0031] Step 2, adding the catalyst precursor into a solvent to prepare a suspension;

[0032] Step 3, adding a TiO2 precursor mixed solution to the suspension to generate a precipitate;

[0033] Step 4, centrifuging, washing, drying and then calcining the precipitate to obtain the composite Mn-based catalyst;

[0034] The L w Mn x N y Wherein L is at least one of Cu, Ni and Co, N is Al and / or Fe, w, x, y are the molar fractions of L, Mn and N respectively, w:y is 1 / 8 to 2 / 1, x:y is 1 / 8 to 2 / 1. More preferably, w:y is 1 / 2 to 3 / 2, x:y is 1 / 2 to 3 / 2; more preferably, w:y is 1 / 2, x:y is 3 / 2.

[0035] In some embodiments of the present invention, in step 1, the calcination is specifically: calcination at 350-600°C for 5 hours under oxygen-limited conditions, more preferably at 350-450°C.

[0036] In some embodiments of the present invention, in step 2, the solvent is a mixed solution of tetrahydrofuran and dimethylformamide in a volume ratio of 4 to 5: 1. In step 2, the process of adding the catalyst precursor to the solvent to obtain a suspension is: first adding the catalyst precursor to the solvent to obtain a suspension, and then ultrasonically dispersing for not less than 1 hour to obtain a suspension.

[0037] In some embodiments of the present invention, the mass volume ratio of the catalyst precursor to the TiO2 precursor is 0.15 g: (0.25-1.5) mL, more preferably 0.15 g: (0.25-1) mL, and more preferably 0.15 g: 0.5 mL.

[0038] In some embodiments of the present invention, in step 3, the TiO2 precursor in the TiO2 precursor mixed solution is tetrabutyl titanate, and the solvent is tetrahydrofuran.

[0039] In the actual preparation process, after adding the TiO2 precursor mixed solution to the suspension and stirring for 1 hour, a mixed solution of H2O and tetrahydrofuran in a volume ratio of 1:20 can be added and ultrasonic dispersion is performed for not less than 30 minutes to ensure complete hydrolysis of the TiO2 precursor.

[0040] The concentration of the suspension and the concentration of the titanium source solution have no significant effect on the catalytic effect of the composite Mn-based catalyst. Therefore, the present invention does not impose any particular limitation on the concentrations of the suspension and the titanium source solution.

[0041] In step 4, the washing is specifically washing with tetrahydrofuran and anhydrous ethanol for 3 times respectively.

[0042] In step 4, after drying the precipitate, the step further includes grinding the precipitate into powder.

[0043] In some embodiments of the present invention, in step 4, the calcination is specifically calcination at 400° C. for 2 hours under oxygen-limited conditions in a muffle furnace.

[0044] The calcinations in step 1 and step 4 are both carried out in a muffle furnace. The initial calcination atmosphere is an air atmosphere, but the amount of air is insufficient in the later stage of combustion. Therefore, the calcination atmosphere in the muffle furnace is called oxygen-limited conditions.

[0045] In some embodiments of the present invention, the L w Mn x N y The preparation method of hydrotalcite-like material comprises the following steps:

[0046] (1) mixing three precursor materials containing L, N and Mn respectively to form a precursor solution;

[0047] (2) adding the precursor solution to a Na2CO3 aqueous solution to obtain a mixed solution, controlling the pH value of the mixed solution to be alkaline (8 to 12, more preferably 9.5 to 10.5), and aging the mixed solution;

[0048] (3) The aged mixed solution is filtered and washed, and then dried to obtain the L w Mn x Ny Hydrotalcite-like.

[0049] In step (2), the filtration and washing process is specifically as follows: under the condition of filtration, the mixed solution is repeatedly washed with deionized water until the pH value of the filtrate is 6-7, and when the filtrate is almost dried up, it is washed once with anhydrous ethanol, and dried to obtain a precipitate; the obtained precipitate is placed in a container filled with anhydrous ethanol, and vigorously stirred at room temperature, and then filtered, and the filter cake is repeatedly washed with anhydrous ethanol.

[0050] The step (2) is carried out at room temperature under the condition of being isolated from air and aerated with nitrogen, and the aging time is greater than 10 hours.

[0051] The present invention firstly obtains L by calcining a hydrotalcite containing L, Mn and N at a high temperature. w Mn x N y O z The material is used as a catalyst precursor, and then L w Mn x N y O z The composite material was loaded with different contents of tetrabutyl titanate and then calcined at high temperature to obtain TiO2 / L w Mn x N y O z The composite Mn-based catalyst can not only efficiently catalyze and reduce nitrogen oxides in flue gas at medium and low temperatures, but also has good sulfur resistance.

[0052] The second aspect of the present invention provides a composite Mn-based catalyst prepared according to the above preparation method, the chemical composition of which is TiO2 / L w Mn x N y O z , wherein L is at least one of Cu, Ni and Co, N is at least one of Al and Fe, w, x, y, z are respectively the molar fractions of L, Mn, N and O in the composite Mn-based catalyst, w / y is 1 / 2 to 2 / 1, x / y is 1 / 2 to 2 / 1, w = 0.5 to 2, x = 0.5 to 2, y = 1; TiO2 and L w Mn x N y O z The mass ratio is 0.2~1.

[0053] The present invention does not impose any particular limitation on the value range of z in the catalyst. In the present invention, the valence state of the metal in the composite Mn-based catalyst is a mixed form of multiple valence states, and Z represents the corresponding amount of O.

[0054] In some embodiments of the present invention, the TiO2 / Lw Mn x N y O z Mn in Mn 2+ , Mn 3+ and Mn 4+ It exists in 2 or 3 mixed valence forms.

[0055] The third aspect of the present invention provides a composite Mn-based catalyst for removing NO from industrial flue gas. x The composite Mn-based catalyst selectively catalytically reduces NO x The temperature range is 100-300°C. Further preferably, the selective catalytic reduction of NO x The temperature range is 150-300°C. More preferably, the selective catalytic reduction of NO x The temperature range is 200°C.

[0056] The technical solutions described in the present invention, unless otherwise specified, are all conventional solutions in the art, and the reagents or raw materials used, unless otherwise specified, are purchased from commercial channels or have been disclosed.

[0057] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0058] Comparative Example 1: Co 0.5 Mn 1.5 Fe1O z Method for preparing catalyst

[0059] (1) Dissolve 8.715 mL of 50% Mn(NO3)2 solution, 3.6379 g of Co(NO3)2·6H2O and 10.1 g of Fe(NO3)3·9H2O in 100 mL of deionized water to obtain a stable, transparent homogeneous solution.

[0060] (2) At room temperature, nitrogen aeration and vigorous stirring, the above homogeneous solution was added dropwise into a 100 mL solution containing 5.2995 g of Na2CO3 (the solvent was deionized water), and the pH value of the system was maintained at 10 with a 4 mol / L NaOH solution. After the addition was completed, the system was aged for 12 h.

[0061] (3) The aged mixed solution is filtered and repeatedly washed with deionized water until the pH value of the filtrate is 6-7 (measured by pH test paper). When the filtrate is almost dry, it is washed once with anhydrous ethanol and dried to obtain a precipitate. The obtained precipitate is placed in a beaker containing 200-300 mL of anhydrous ethanol, vigorously stirred for 1 hour (1-2 hours) at room temperature, then filtered, and the filter cake is repeatedly washed with anhydrous ethanol. The obtained filter cake is placed in a 60°C blast oven, dried overnight, and then ground into a powder state to obtain Co 0.5 Mn 1.5 Fe1 type hydrotalcite.

[0062] (4) The above Co 0.5 Mn 1.5 Fe1 hydrotalcite was placed in a muffle furnace and calcined at 400℃ for 5 hours to obtain Co 0.5 Mn 1.5 Fe1O z catalyst, as a control catalyst.

[0063] Co prepared in Comparative Example 1 0.5 Mn 1.5 Fe1O z The catalyst was subjected to XPS analysis, and the results showed that the Mn in the catalyst was Mn 2+ , Mn 3+ and Mn 4+ A mixed form of three valence states, and Mn 2+ and Mn 3+ Accounting for 76.2%, Mn 4+ It accounts for 23.8%.

[0064] Example 1: TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z Catalyst preparation

[0065] (1) The Co prepared in Comparative Example 1 0.5 Mn 1.5 Fe1O z Catalyst as precursor, take 0.15gCo 0.5 Mn 1.5 Fe1O z The catalyst was dissolved in a mixed solution of 240 mL of tetrahydrofuran (THF) and 48 mL of dimethylformamide (DMF) to obtain a stable, transparent suspension.

[0066] (2) The suspension was ultrasonically dispersed for 1 hour to obtain a suspension. Then, 50 mL of a THF solution containing 0.5 mL of tetrabutyl titanate was added dropwise to the suspension under vigorous stirring to gradually generate a precipitate.

[0067] (3) After the above solution was stirred for 1 hour, a mixed solution of 0.5 mL H2O and 10 mL THF was added to ensure complete hydrolysis of the tetrabutyl titanate precursor, and the mixed solution was ultrasonically dispersed for 30 minutes. After centrifugation, THF and anhydrous ethanol were washed three times respectively. The obtained product was dried in a 60°C forced air drying oven and ground into powder.

[0068] (4) The dried powder was placed in a muffle furnace and calcined at 400°C for 2 hours to obtain TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z catalyst.

[0069] The TiO2(0.5) / Co prepared in Example 1 0.5 Mn 1.5 Fe1O z The catalyst was subjected to XPS analysis, and the results showed that the Mn in the catalyst was Mn 2+ , Mn 3+ and Mn 4+ A mixed form of three valence states, and Mn 2+ and Mn 3+ Accounting for 77.6%, Mn 4+ Proper amount of Mn 4+ The species contribute to the catalyst's excellent denitrification performance and N2 selectivity.

[0070] Comparative Example 2: Preparation method of 10wt% Co-Mn-Fe / TiO2 catalyst

[0071] A 10 wt% Co-Mn-Fe / TiO2 catalyst was prepared by a conventional loading method: 0.325 g Co(NO3)2·6H2O, 0.2012 g Fe(NO3)3·9H2O and 0.4427 mL Mn(NO3)2 were dissolved in 5 mL deionized water to obtain a transparent homogeneous solution. 2.5 mL of the homogeneous solution was loaded onto a 2 g TiO2 carrier by an impregnation method, placed in an 80°C forced air drying oven, dried for 12 hours, and the dried powder was placed in a muffle furnace and calcined at 500°C for 4 hours to obtain a 10 wt% Co-Mn-Fe / TiO2 catalyst as another control catalyst.

[0072] XPS analysis of the 10wt% Co-Mn-Fe / TiO2 catalyst prepared in Comparative Example 2 showed that the Mn in the catalyst was Mn 2+ , Mn 3+ and Mn 4+ A mixed form of three valence states, and Mn 2+ and Mn3+ Accounting for 85.8%, Mn 4+ It accounts for 14.2%.

[0073] Effect verification example 1: Catalyst performance test method

[0074] The catalytic performance test was carried out in a fixed bed microreactor (diameter d = 6 mm) at atmospheric pressure, with a test temperature range of 100-300°C. The sample size was 150 mg, and the gas composition of the simulated flue gas was: 500 ppm NO x , 500ppmNH3, 5%O2, Ar as balance gas. NO in the gas composition before and after the reaction x The samples were analyzed online using a 2.4 M Gas Cell and a Bruker INVENIO S analyzer (Bruker Optics).

[0075] Effect verification example 2: CoMnFeO with different molar ratios x Testing of the impact of catalyst performance

[0076] The method in Comparative Example 1 was used to prepare hydrotalcite-like materials with different ratios, different metals L, and different metals N, wherein the molar ratio of (Co+Mn) / Fe was 1 / 1 to 4 / 1, the molar ratio of Co / Mn was 0.5 / 1, 1 / 1, and 1.5 / 0.5; different metals L (Co, Ni, Cu); and different metals N (Fe, Al). The hydrotalcite-like materials were calcined at high temperature (calcination temperature was 400°C) to obtain the corresponding catalyst (i.e., the molar ratio of (Co+Mn) / Fe was adjusted to 1 / 1 to 4 / 1 on the basis of Comparative Example 1, or the molar ratio of Co / Mn was 0.5 / 1, 1 / 1, and 1.5 / 0.5, or the metal L was replaced by Co with Ni or Cu, or the metal N was replaced by Fe with Al, and the remaining steps and parameters were the same as those in Example 1) and used to treat laboratory simulated flue gas, and then the performance of the catalyst was determined by the performance test method in Effect Verification Example 1. The test results were shown in Tables 1-4. It shows that the catalysts prepared by different molar ratios of (Co+Mn) / Fe and Co / Mn in hydrotalcite are effective in treating NO in flue gas. x Different catalytic properties were shown in the process. Among them, the catalysts prepared with the molar ratios of (Co+Mn) / Fe and Co / Mn of 2:1 and 1:3 respectively and metals of Co and Fe had the best denitrification performance. When the test temperature was 200°C, Co1Mn1Fe1O x and Co 0.5 Mn 1.5 Fe1O x NO x The conversion rates reached 95.4% and 99.92% respectively.

[0077] Table 1 Effect of different molar ratios of (Co+Mn) / Fe on catalyst performance (calcination temperature is 400℃, test temperature is 200℃)

[0078]

[0079] Table 2 Effect of different molar ratios of Co / Mn on catalyst performance (calcination temperature is 400°C, test temperature is 200°C)

[0080]

[0081] Table 3 Effect of different metal L on catalyst performance (calcination temperature is 400℃, test temperature is 200℃)

[0082] Different metals L (Co, Ni, Cu) <![CDATA[Co 0.5 Mn 1.5 Fe1O z ]]> <![CDATA[Ni 0.5 Mn 1.5 Fe1O z ]]> <![CDATA[Cu 0.5 Mn 1.5 Fe1O z ]]> <![CDATA[NO x Conversion rate (%)]]> 99.92 92.46 90.18

[0083] Table 4 Effect of different metal N on catalyst performance (calcination temperature is 400℃, test temperature is 200℃)

[0084] Different metal N (Fe, Al) <![CDATA[Co 0.5 Mn 1.5 Fe1O z ]]> <![CDATA[Co 0.5 Mn 1.5 Al1O z ]]> <![CDATA[NO x Conversion rate (%)]]> 99.92 98.79

[0085] Effect verification example 3: Test on the effect of calcination temperature and space velocity on catalyst performance

[0086] The effects of calcination temperature and gas space velocity (GHSV) on catalyst performance are crucial. Different calcination temperatures and GHSV have different effects on the occurrence of redox reactions in the catalyst and the adsorption capacity of gas components. Therefore, in order to determine an optimal calcination temperature and GHSV, the catalyst Co 0.5 Mn 1.5 Fe1O z At different calcination temperatures (calcination temperature is 350-600℃, test temperature is 200℃; that is, the calcination temperature is adjusted to 350℃, 400℃, 500℃, 600℃ respectively on the basis of Comparative Example 1, and the other steps and parameters are the same as Comparative Example 1) and GHSV (80,000 and 120,000h -1 ) was used to treat laboratory simulated flue gas, and then the performance test method in effect verification example 1 was used to determine the catalyst performance. The test results are shown in Table 5-6, indicating that Co 0.5 Mn 1.5 Fe1O z The optimum calcination temperature of the catalyst is 400°C and the GHSV is 80,000h -1 .

[0087] Table 5 Effect of calcination temperature on catalyst performance

[0088]

[0089] Table 6 Effect of space velocity on catalyst performance

[0090]

[0091] Effect verification example 4: Co 0.5 Mn 1.5 Fe1O z Performance test of different TiO2 contents at different test temperatures

[0092] A new composite material (composite Mn-based catalyst) with hydrotalcite-like material loaded with TiO2 was prepared by the method in Example 1, and the TiO2 precursor content was 0.25-1 mL (that is, on the basis of Example 1, the content of tetrabutyl titanate in step (2) was adjusted to 0.25 mL, 0.75 mL, and 1 mL, respectively). The composite material was calcined at high temperature (calcination temperature was 400°C) to obtain the corresponding catalyst and used to treat laboratory simulated flue gas, and then the performance test method in effect verification example 1 was used to determine the catalyst performance. The effect of temperature is crucial in the catalyst performance test. Different test temperatures have different effects on the occurrence of redox reactions in the catalyst and the adsorption capacity of gas components. Therefore, Co 0.5 Mn 1.5 Fe1O z 、TiO2(0.25) / Co 0.5 Mn 1.5 Fe1O z 、TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z 、TiO2(0.75) / Co 0.5 Mn 1.5 Fe1O z and TiO2(1) / Co 0.5 Mn 1.5 Fe1O z The catalyst was used to treat laboratory simulated flue gas at different test temperatures (calcination temperature was 400°C, test temperature was 100-300°C). The test results (as shown in Table 7) show that the catalyst prepared with different concentrations of TiO2 in the composite material has a good effect on treating NO in flue gas. x Different catalytic properties were shown in the process. When the test temperature was 200℃, Co 0.5 Mn 1.5 Fe1O z 、TiO2(0.25) / Co 0.5 Mn 1.5 Fe1O z 、TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z、TiO2(0.75) / Co 0.5 Mn 1.5 Fe1O z and TiO2(1) / Co 0.5 Mn 1.5 Fe1O z NO x The conversion rates were 99.92%, 95.86%, 99.53%, 94.78% and 90.97%, respectively. The TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z The catalyst has the best catalytic performance, compared with Co 0.5 Mn 1.5 Fe1O z The catalyst is similar to the existing 10wt% Co-Mn-Fe / TiO2 NO prepared by the loading method. x At the same test temperature, the best conversion rate is 57.66%. By comparison, it can be concluded that the catalyst of the present invention has higher performance.

[0093] High N2 selectivity can effectively avoid the production of secondary pollutants (N2O). The test results (Table 8) show that TiO2 (0.5) / Co 0.5 Mn 1.5 Fe1O z It exhibits excellent N2 selectivity in the process of treating flue gas. At 200°C, the N2 selectivity can reach 86.5%. The N2 selectivity of 10wt% Co-Mn-Fe / TiO2 prepared by the loading method is only 70.98% at the same test temperature. By comparison, it is shown that the catalyst of the present invention has higher selectivity.

[0094] Table 7Co 0.5 Mn 1.5 Fe1O z , Co-Mn-Fe / TiO2 and TiO2(v) / Co 0.5 Mn 1.5 Fe1O z Catalyst activity (test temperature 100 ~ 300 ℃)

[0095]

[0096] Table 8Co 0.5 Mn 1.5 Fe1O z , 10wt%Co-Mn-Fe / TiO2 and TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O zN2 selectivity of catalyst (test temperature 100~300℃)

[0097]

[0098] Effect verification example 5: Catalyst sulfur resistance test

[0099] Low-temperature composite Mn-based SCR catalysts often have good reaction performance in flue gas without SO2. However, in actual working conditions, the SCR device is usually installed after the desulfurization and dust removal device. The flue gas still contains a small amount of SO2. Under such conditions, it is easy to be poisoned and deactivated, and the effect of SO2 on the catalyst is often irreversible. Therefore, the requirement for the sulfur resistance of the catalyst is essential. 0.5 Mn 1.5 Fe1O z 、TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z 、TiO2(0.75) / Co 0.5 Mn 1.5 Fe1O z and TiO2(1) / Co 0.5 Mn 1.5 Fe1O z catalyst as an example, and compare its sulfur resistance test results with those of Co 0.5 Mn 1.5 Fe1O z It was compared with 10wt% Co-Mn-Fe / TiO2 prepared by the loading method, as described below:

[0100] The sulfur resistance test of the catalyst was carried out in a fixed bed microreactor (diameter d = 6mm) at normal pressure. The sample amount was 150mg, the gas flow rate was 200mL / min, the test temperature was 100-300℃, the test time was 1h, and the gas composition of the simulated flue gas was: 500ppmNOx, 500ppmNH3, 100ppmSO2, 5%O2, and Ar was used as the balance gas. x The samples were analyzed online using a 2.4 M Gas Cell and a Bruker INVENIO S analyzer (Bruker Optics).

[0101] Co prepared by the methods of Comparative Examples 1, 2 and Example 1 0.5 Mn 1.5 Fe1O z 、TiO2(0.25) / Co 0.5 Mn 1.5 Fe1O z、TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z 、TiO2(0.75) / Co 0.5 Mn 1.5 Fe1O z and TiO2(1) / Co 0.5 Mn 1.5 Fe1O z The catalyst (calcined at 400°C) was treated with laboratory simulated flue gas, and then the sulfur resistance of the catalyst was measured using the above sulfur resistance test method. The test results are shown in Table 9, indicating that the catalyst has a strong sulfur resistance to Co 0.5 Mn 1.5 Fe1O z Compared with 10wt% Co-Mn-Fe / TiO2 prepared by the loading method, TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z The catalysts showed good SO2 resistance at 200℃. In the presence of 100ppm SO2, 10wt% Co-Mn-Fe / TiO2 and Co 0.5 Mn 1.5 Fe1O z NO x The conversion rates were 46.92% and 87.42% respectively. Compared with the case without SO2, NO x The conversion rates decreased by 10.74% and 12.5%, respectively. 0.5 Mn 1.5 Fe1O z 、TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z 、TiO2(0.75) / Co 0.5 Mn 1.5 Fe1O z and TiO2(1) / Co 0.5 Mn 1.5 Fe1O z Catalyst, in the presence of 100ppm SO2, at 200℃ NO x The conversion rates were 89.42%, 95.23%, 91.08% and 61.8%, respectively, which were 6.44%, 4.3%, 3.7% and 9.17% lower than those without SO2. It can be seen that SO2 has a great influence on the performance of catalysts prepared by the loading method and hydrotalcite-like catalysts. 0.5 Mn 1.5 Fe1O z、TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z 、TiO2(0.75) / Co 0.5 Mn 1.5 Fe1O z and TiO2(1) / Co 0.5 Mn 1.5 Fe1O z The effect of SO2 on the catalyst is relatively weak. It can be seen that the catalyst prepared by the present invention has improved sulfur resistance while ensuring high catalytic performance.

[0102] Table 9Co 0.5 Mn 1.5 Fe1O z Sulfur resistance test of TiO2 with different concentrations (calcination temperature is 400℃, test temperature is 100~300℃)

[0103]

[0104] Effect verification example 6: Co 0.5 Mn 1.5 Fe1O z 、TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z Regeneration test of 10wt% Co-Mn-Fe / TiO2 catalyst

[0105] The catalyst after the sulfur resistance test was regenerated by heat treatment at a temperature of 400°C for 30 minutes. The regenerated catalyst was treated with laboratory simulated flue gas. The performance of the catalyst was then measured using the performance test method in effect verification example 2. The test results (as shown in Table 10, the test temperature was 200°C) showed that Co 0.5 Mn 1.5 Fe1O z 、TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z After heat treatment and regeneration, the performance of the catalysts TiO2(0.5) / Co-Mn-Fe / TiO2 was restored to a certain extent, but not completely, which may be attributed to the loss of performance components during the regeneration process. 0.5 Mn 1.5 Fe1O z Compared to Co 0.5 Mn 1.5 Fe1O zand 10wt% Co-Mn-Fe / TiO2 still have higher performance, TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z The performance of Co 0.5 Mn 1.5 Fe1O z and 10wt% Co-Mn-Fe / TiO2 are 85.82% and 35.88% respectively. Combining the above test on the effect of calcination temperature on catalyst performance, it can be concluded that TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z It has good thermal stability, so relative to Co 0.5 Mn 1.5 Fe1O z The catalysts with 10wt% Co-Mn-Fe / TiO2 had higher performance after regeneration by heat treatment.

[0106] Table 10Co 0.5 Mn 1.5 Fe1O z 、TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z Regeneration test results of 10wt% Co-Mn-Fe / TiO2 catalyst

[0107]

[0108] Figure 1 a is an X-ray diffraction spectrum, which is respectively Co prepared before calcination in Comparative Example 1 0.5 Mn 1.5 Fe1-LDH (i.e. Co 0.5 Mn 1.5 Fe1 type hydrotalcite), TiO2(0.5) / Co prepared in Example 1 0.5 Mn 1.5 Fe1O z Catalyst, Co prepared after calcination in Comparative Example 1 0.5 Mn 1.5 Fe1O z Catalyst and Comparative Example 2 Co-Mn-Fe / TiO2 material prepared by the loading method (i.e., 10 wt% Co-Mn-Fe / TiO2); Figure 1 b is the TiO2(0.5) / Co after calcination in Example 1 0.5 Mn 1.5 Fe1O z TEM-EDS images of the catalyst.

[0109] Figure 1 The characteristic diffraction peaks ascribed to LDH appeared in a, indicating that Co 0.5 Mn 1.5 The successful preparation of Fe1-LDH hydrotalcite. Co prepared by calcination under oxygen-limited conditions in a muffle furnace 0.5 Mn 1.5 Fe1O z The catalyst showed a characteristic peak belonging to MnO2 species. The Co-Mn-Fe / TiO2 material prepared by the loading method only showed the characteristic peak of TiO2, while the TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z The catalyst showed characteristic peaks belonging to MnO2, TiO2 and Fe2Ti3O9 species. The electron transfer between various metal components contributed to the TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z The overall catalytic performance is improved. In addition, TEM-EDS elemental analysis found that TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z The metal elements are evenly distributed and highly dispersed.

[0110] The present invention is to prepare Co by calcining TiO2 0.5 Mn 1.5 Fe1O z Composite TiO2(0.5) / Co 0.5 Mn 1.5 Fe1O z Catalyst. By introducing a variety of metal elements into the LDH layer, the layered structure and the bonding between metals are used to effectively avoid the problems of limited loading of active components and easy agglomeration of metal particles in the preparation by the loading method. A variety of metals can be introduced in a large range, and highly dispersed MnO can be obtained after calcination. x Active components and auxiliary components can improve the activity and N2 selectivity of the catalyst. In addition, Co 0.5 Mn 1.5 Fe1O z The high specific surface area of ​​the catalytic material enables it to be used as a carrier and can efficiently load TiO2 species. By utilizing the ability of TiO2 to easily combine with sulfur species, TiO2 is used as a sacrificial site to protect MnO x Active components, thereby improving the sulfur resistance of the catalyst.

[0111] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a composite Mn-based catalyst, characterized in that: The following steps are involved: Step 1: L w Mn x N y Calcining the hydrotalcite-like substance to obtain a catalyst precursor; Step 2, adding the catalyst precursor into a solvent to prepare a suspension; Step 3, adding a TiO2 precursor mixed solution to the suspension to generate a precipitate; Step 4, centrifuging, washing, drying and then calcining the precipitate to obtain the composite Mn-based catalyst; The L w Mn x N y Wherein L is at least one of Cu, Ni and Co, N is Al and / or Fe, w, x, y are the molar fractions of L, Mn and N respectively, w:y is 1 / 8 to 2 / 1, and x:y is 1 / 8 to 2 / 1.

2. The method for preparing a composite Mn-based catalyst according to claim 1, characterized in that: In step 1, the calcination is specifically: calcination at 350-600° C. for 3-5 hours.

3. The method for preparing a composite Mn-based catalyst according to claim 1, characterized in that: In step 2, the solvent is a mixed solution of tetrahydrofuran and dimethylformamide in a volume ratio of 4 to 5:

1.

4. The method for preparing a composite Mn-based catalyst according to claim 1, characterized in that: The mass volume ratio of the catalyst precursor to the TiO2 precursor is 0.15g:(0.25-1.5)mL.

5. The method for preparing a composite Mn-based catalyst according to claim 1, characterized in that: In step 3, the TiO2 precursor in the TiO2 precursor mixed solution is tetrabutyl titanate, and the solvent is tetrahydrofuran.

6. The method for preparing a composite Mn-based catalyst according to claim 1, characterized in that: In step 4, the calcination is specifically: calcination at 400° C. for 1 to 3 hours.

7. The method for preparing a composite Mn-based catalyst according to claim 1, characterized in that: The L w Mn x N y The preparation method of hydrotalcite-like material comprises the following steps: (1) mixing three precursor materials containing L, N and Mn respectively to form a precursor solution; (2) adding the precursor solution to a Na2CO3 aqueous solution to obtain a mixed solution, controlling the pH value of the mixed solution to be alkaline, and aging the mixed solution; (3) The aged mixed solution is filtered and washed, and then dried to obtain the L w Mn x N y Hydrotalcite-like.

8. The composite Mn-based catalyst prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The chemical composition is TiO2 / L w Mn x N y O z , wherein L is at least one of Cu, Ni and Co, N is Al and / or Fe, w, x, y, z are respectively the molar fractions of L, Mn, N and O in the composite Mn-based catalyst, w / y is 1 / 2 to 2 / 1, x / y is 1 / 2 to 2 / 1, w = 0.5 to 2, x = 0.5 to 2, y = 1; TiO2 and L w Mn x N y O z The mass ratio is 0.2~1.

9. The composite Mn-based catalyst according to claim 8, characterized in that: TiO2 / L w Mn x N y O z Mn in Mn 2+ , Mn 3+ and Mn 4+ It exists in 2 or 3 mixed valence forms.

10. The composite Mn-based catalyst as claimed in claim 8 or 9 is used to remove NO from industrial flue gas. x The application is characterized in that The composite Mn-based catalyst selectively catalytically reduces NO x The temperature range is 100~300℃.