Ce / HZSM-5 catalyst as well as preparation method and application thereof
By loading 1 to 2 wt% Ce on the HZSM-5 catalyst, combined with constant temperature heating and ultrasonic cavitation, the problems of acidity regulation and pore volume reduction are solved, and the conversion rate of oxygen-containing compounds in PET cracking oil is improved and The activity of the catalyst achieves efficient catalytic effect.
Patent Information
- Application Number
- CN202411206091.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The acidity of the existing HZSM-5 catalysts is difficult to regulate, resulting in a low conversion rate of oxygen-containing compounds in PET cracking oil, and the accumulation of Ce in the catalyst results in a decrease in pore volume and pore size, affecting catalytic activity and selectivity.
By loading 1 to 2 wt% Ce on HZSM-5, and using constant temperature heating and ultrasonic cavitation, the impregnation of Ce salt solution is strengthened to ensure that Ce effectively penetrates into the inner surface of the catalyst, adjusts acidity, avoids Ce accumulation, and improves the catalyst activity and selectivity.
The high conversion rate of oxygen-containing compounds in PET cracking oil is achieved, the hydrocarbon activity and selectivity of the catalyst is improved, the pore volume and pore size are reduced, and the performance of the catalyst is enhanced.
Smart Images

Figure CN119076049A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysts and relates to a Ce / HZSM-5 catalyst, in particular to a Ce / HZSM-5 catalyst and a preparation method and application thereof. Background Art
[0002] Photovoltaic modules are the core components of photovoltaic power stations, and their service life is generally 20 to 30 years. With the rapid development of the photovoltaic industry, the number of waste photovoltaic modules is also increasing. It is estimated that by 2050, the global scrap volume of photovoltaic modules will reach 78 million tons. These waste photovoltaic modules are mainly composed of glass, EVA, battery cells, TPT backboards and other materials. PET (polyethylene terephthalate) is a polymer widely used in synthetic fibers and plastic materials. It accounts for about 80% of TPT backboards. Therefore, the amount of PET waste in waste photovoltaic modules is very considerable. If it is not effectively recycled and utilized, it will cause serious waste of resources and environmental pollution. In order to effectively recycle and utilize PET waste, a feasible method is to thermally crack it to obtain pyrolysis oil containing components such as aromatic hydrocarbons, olefins and oxygen-containing compounds. However, the pyrolysis oil contains a high proportion of oxygen-containing compounds (alcohols, carboxylic acids, benzoic acid, terephthalic acid and its derivatives), which will reduce the quality of pyrolysis oil and is not suitable for direct use in engine combustion. Therefore, the fuel must be improved through a catalytic reforming process. Reforming processes include hydrogenation, deoxygenation, aromatization and cyclization of unsaturated functional groups, especially cleavage of CC, CO and CO bonds.
[0003] HZSM-5 molecular sieve is a commonly used catalyst with the advantages of large specific surface area, unique pore structure, adjustable surface acidity, high selectivity, strong adsorption capacity, etc. Most oxygen-containing compounds can move to the active acid sites along the pores of HZSM-5. Acid centers and Lewis acid centers, in the catalytic process Acid centers are more likely to participate in catalytic deoxygenation reactions. The presence of acid centers in the catalyst makes it easier to break and separate CC and CO bonds in the reactants through reactions such as dehydration, cracking, aromatization, isomerization, oligomerization, decarboxylation and dealkylation. Hydrocarbons and coke are also produced with the help of acid centers on the catalyst. Therefore, the acidity of the catalyst should be just right to produce the best hydrocarbon yield, while reducing more hydrocarbon polymerization to form coke materials, avoiding blocking the pores and covering the active acid sites of the HZSM-5 structure, which reduces the activity and selectivity of hydrocarbons. However, the acidity of the HZSM-5 molecular sieve catalyst disclosed in the prior art is difficult to control, and its activity and selectivity for hydrocarbons are low.
[0004] CN111085253A discloses a method for preparing a HZSM-5 catalyst loaded with Mn and Ce at the same time, the steps are as follows: dissolving Mn(NO3)4 and Ce(NO3)4 in deionized water, adding HZSM-5 molecular sieve, impregnating for 4-6 hours, drying in an oven at 75-85°C for 25-27 hours, calcining the obtained precursor in a muffle furnace at 485-495°C for 7-8 hours, and cooling. The method is simple, fast, and easy to operate. The prepared catalyst has more surface chemically adsorbed oxygen species, which contribute to the oxidation and combustion of soot, and thus exhibits a higher catalytic soot combustion activity.
[0005] CN101757943A discloses a catalyst for synthesizing methanol by hydrogenation of carbon dioxide and a preparation method thereof. The catalyst is prepared by using HZSM-5 molecular sieve as a carrier and cerium zirconium as an auxiliary agent by a co-current coprecipitation impregnation method. The mol ratio of Cu / Zn is 2-4:1, the mol ratio of Ce / Zr is 1-3:1, the mass content of Cu-Zn is 30%-70%, and the mass content of HZSM-5 is 5%-50%. The patent has the advantages of simple catalyst preparation process, no pollution, low energy consumption and production cost in the preparation process, high catalyst strength and long life, and can significantly increase the economic efficiency of CO2 chemical utilization, achieving the purpose of energy saving and emission reduction and turning harm into treasure.
[0006] The currently disclosed HZSM-5 molecular sieve catalysts have certain defects, such as the difficulty in controlling the acidity, low activity and selectivity for hydrocarbons, which leads to low conversion rate of oxygen-containing compounds in PET pyrolysis oil. Therefore, it is very important to develop and design a new Ce / HZSM-5 catalyst and its preparation method. Summary of the invention
[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide a Ce / HZSM-5 catalyst and a preparation method and application thereof. The mass fraction of Ce in the Ce / HZSM-5 catalyst provided by the present invention is 1-2wt%. The Ce loaded on HZSM-5 can not only adjust the acidity of the Ce / HZSM-5 catalyst, but also avoid the accumulation of Ce in the zeolite channel of HZSM-5, thereby preventing the pore volume and pore diameter of the Ce / HZSM-5 catalyst from decreasing. Therefore, the Ce / HZSM-5 catalyst has higher activity and selectivity for hydrocarbons, thereby improving the conversion rate of oxygen-containing compounds in PET cracking oil.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a Ce / HZSM-5 catalyst, wherein the mass fraction of Ce in the Ce / HZSM-5 catalyst is 1-2 wt %, based on the mass of the Ce / HZSM-5 catalyst being 100%.
[0010] The mass fraction of Ce in the Ce / HZSM-5 catalyst of the present invention is 1-2wt%, for example, it can be 1wt%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.7%, 1.8%, 1.9% or 2t%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0011] Since Ce exhibits good catalytic activity in catalytic deoxygenation reactions and has a small particle size, it can penetrate into the interior of the zeolite channels, reducing Therefore, Ce was used to load HZSM-5 in this application to obtain Ce / HZSM-5 catalyst.
[0012] However, if only a small amount of Ce is loaded on HZSM-5, it cannot effectively interact with the active sites of HZSM-5, resulting in the inability to adjust the acidity of Ce / HZSM-5; if too high a content of Ce is loaded on HZSM-5, it will cause Ce to accumulate in the zeolite channels of HZSM-5, significantly reducing the pore volume and pore size of Ce / HZSM-5, restricting the diffusion of reactants and products in the channels, and causing Ce / HZSM-5 to deactivate.
[0013] The mass fraction of Ce in the Ce / HZSM-5 catalyst provided by the present invention is 1-2wt%. The Ce loaded on HZSM-5 can not only adjust the acidity of the Ce / HZSM-5 catalyst, but also avoid the accumulation of Ce in the zeolite channel of HZSM-5, thereby preventing the pore volume and pore diameter of the Ce / HZSM-5 catalyst from decreasing. Therefore, the Ce / HZSM-5 catalyst has higher activity and selectivity for hydrocarbons, thereby improving the conversion rate of oxygen-containing compounds in PET cracking oil.
[0014] In a second aspect, the present invention provides a method for preparing the Ce / HZSM-5 catalyst according to the first aspect, the preparation method comprising:
[0015] The Ce salt solution and HZSM-5 are mixed, wherein the mixing includes constant temperature heating and ultrasonic cavitation to obtain a mixed solution, and then heat treatment is performed to obtain a Ce / HZSM-5 catalyst.
[0016] If Ce salt solution is simply used directly on HZSM-5, most of the Ce salt solution will be adsorbed on the surface of silicon oxide, and only a small amount will enter the position of tetracoordinate aluminum, which cannot effectively interact with the active sites of HZSM-5, resulting in low utilization efficiency of the active components in the Ce salt solution.
[0017] In the present invention, ultrasonic cavitation is performed while heating at a constant temperature to strengthen the impregnation of HZSM-5 with Ce salt solution, so that Ce precursor can effectively penetrate into the inner surface of the catalyst, thereby reducing The number of strong acid sites enables the adjustment of the acidity of the Ce / HZSM-5 catalyst, thereby improving the activity and selectivity of the Ce / HZSM-5 catalyst for hydrocarbons and improving the conversion rate of oxygen-containing compounds in PET pyrolysis oil.
[0018] Preferably, the mass ratio of Ce salt to HZSM-5 in the Ce salt solution is (0.024-0.048):1, for example, it can be 0.024:1, 0.026:1, 0.028:1, 0.03:1, 0.032:1, 0.034:1, 0.036:1, 0.038:1, 0.04:1, 0.042:1, 0.044:1, 0.046:1 or 0.048:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0019] Preferably, the mass ratio of the solvent to HZSM-5 in the Ce salt solution is (15-20):1, for example, 15:1, 16:1, 17:1, 18:1, 19:1 or 20:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] Preferably, the method for preparing the Ce salt solution is: placing the Ce salt in water and dissolving it by stirring.
[0021] Preferably, the preparation method further comprises drying and cooling the HZSM-5 in sequence before the mixing.
[0022] Preferably, the drying temperature is 105-120° C. and the drying time is 10-14 hours.
[0023] The drying temperature in the present invention is 105-120° C., for example, 105° C., 110° C., 115° C. or 120° C., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0024] The drying time in the present invention is 10 to 14 hours, for example, 10 hours, 11 hours, 12 hours, 13 hours or 14 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0025] Preferably, the silicon-to-aluminum ratio in the HZSM-5 is (20-30):1, for example, it can be 20:1, 21:1, 22:1, 23:1, 24:1, 25:1, 26:1, 27:1, 28:1, 29:1 or 30:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] Preferably, the mixing time is 30 to 90 min, for example, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, 65 min, 70 min, 75 min, 80 min, 85 min or 90 min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] Preferably, the constant temperature heating temperature is 60-100°C, for example, it can be 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or 100°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] Preferably, the constant temperature heating is carried out in a jacketed glass reactor.
[0029] Preferably, the constant temperature heating comprises constant temperature oil bath heating.
[0030] Preferably, the heating medium used in the constant temperature oil bath heating includes any one of dimethyl silicone oil, methyl silicone oil or benzyl silicone oil, or a combination of at least two of them. Typical but non-limiting combinations include a combination of dimethyl silicone oil and methyl silicone oil, a combination of methyl silicone oil and benzyl silicone oil, or a combination of dimethyl silicone oil, methyl silicone oil and benzyl silicone oil.
[0031] Preferably, the mixing further comprises stirring which is performed synchronously with the constant temperature heating and the ultrasonic cavitation.
[0032] Preferably, the stirring speed is 300-900 rpm, for example, it can be 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm, 550 rpm, 600 rpm, 650 rpm, 700 rpm, 750 rpm, 800 rpm, 850 rpm or 900 rpm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] Preferably, the power of the ultrasonic cavitation is 300-600 W, for example, 300 W, 350 W, 400 W, 450 W, 500 W, 550 W or 600 W, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] Preferably, the ultrasonic cavitation is performed using an external ultrasonic transmitter.
[0035] Preferably, drying is further included between the mixing and the heat treatment.
[0036] Preferably, the drying temperature is 105-120° C. and the drying time is 10-14 hours.
[0037] The drying temperature in the present invention is 105-120°C, for example, it can be 105°C, 106°C, 108°C, 110°C, 112°C, 114°C, 116°C, 118°C or 120°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0038] The drying time in the present invention is 10 to 14 hours, for example, it can be 10 hours, 10.5 hours, 11 hours, 11.5 hours, 12 hours, 12.5 hours, 13 hours, 13.5 hours or 14 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0039] Preferably, the heat treatment includes sequential heating and heat preservation.
[0040] Preferably, the heating rate is 1 to 10°C / min, for example, 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, preferably 4 to 6°C / min.
[0041] Preferably, the terminal temperature of the heating is 550-650°C, for example, it can be 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, 610°C, 620°C, 630°C, 640°C or 650°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, preferably 590-610°C.
[0042] Preferably, the insulation time is 3 to 5 hours, for example, it can be 3h, 3.2h, 3.4h, 3.6h, 3.8h, 4h, 4.2h, 4.4h, 4.6h, 4.8h or 5h, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable, preferably 3.5 to 4.5h.
[0043] As a preferred technical solution of the preparation method of the present invention, the preparation method comprises:
[0044] (1) mixing a Ce salt solution and HZSM-5, wherein the mixing includes constant temperature heating at 60-100° C., ultrasonic cavitation at a power of 300-600 W, and stirring at a speed of 300-900 rpm, and the mixing time is 30-90 min to obtain a mixed solution; the mass ratio of Ce salt to HZSM-5 in the Ce salt solution is (0.024-0.048):1, the mass ratio of solvent to HZSM-5 is (15-20):1, and the silicon-aluminum ratio in the HZSM-5 is (20-30):1;
[0045] (2) Drying the mixed solution obtained in step (1), heating it to 550-650° C. at a rate of 1-10° C. / min and then keeping it at that temperature for 3-5 hours to obtain a Ce / HZSM-5 catalyst.
[0046] In a third aspect, the present invention provides an application of the Ce / HZSM-5 catalyst described in the first aspect, wherein the Ce / HZSM-5 catalyst is used to convert oxygen-containing compounds in PET pyrolysis oil from waste photovoltaic modules into gasoline-grade hydrocarbons.
[0047] Compared with the prior art, the present invention has the following beneficial effects:
[0048] The mass fraction of Ce in the Ce / HZSM-5 catalyst provided by the present invention is 1-2wt%. The Ce loaded on HZSM-5 can not only adjust the acidity of the Ce / HZSM-5 catalyst, but also avoid the accumulation of Ce in the zeolite channel of HZSM-5, thereby preventing the pore volume and pore diameter of the Ce / HZSM-5 catalyst from decreasing. Therefore, the Ce / HZSM-5 catalyst has higher activity and selectivity for hydrocarbons, thereby improving the conversion rate of oxygen-containing compounds in PET cracking oil. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 It is the preparation device used in the preparation method of Ce / HZSM-5 catalyst in Example 1 of the present invention.
[0050] Figure 2NH3-TPD spectra of the Ce / HZSM-5 catalysts in Examples 1 and 2 of the present invention and the HZSM-5 catalyst provided in Comparative Example 4.
[0051] Among them, 1-ultrasonic transmitter; 2-transducer; 3-iron frame; 4-amplifier; 5-jacketed glass reactor; 6-oil circulation; 7-constant temperature circulation device; 8-glass stirring rod. DETAILED DESCRIPTION
[0052] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0053] Example 1
[0054] This embodiment provides a Ce / HZSM-5 catalyst. Taking the mass of the Ce / HZSM-5 catalyst as 100%, the mass fraction of Ce in the Ce / HZSM-5 catalyst is 1 wt%.
[0055] The preparation method of the Ce / HZSM-5 catalyst comprises:
[0056] (1) mixing an aqueous solution of cerium nitrate and HZSM-5, wherein the mixing comprises constant temperature heating at 80° C., ultrasonic cavitation at a power of 300 W, and stirring at a speed of 600 rpm, and the mixing time is 30 minutes to obtain a mixed solution; the mass ratio of cerium nitrate to HZSM-5 in the aqueous solution of cerium nitrate is 0.024:1, the mass ratio of water to HZSM-5 is 18:1, and the silicon-aluminum ratio in the HZSM-5 is 25;
[0057] (2) The mixed solution obtained in step (1) is dried, and then heated to 600° C. at a rate of 5° C. / min and kept at this temperature for 4 h to obtain a Ce / HZSM-5 catalyst.
[0058] The preparation method described in this embodiment adopts the preparation device as Figure 1 As shown, Figure 1 The ultrasonic transmitter 1 is used to provide ultrasonic waves to achieve ultrasonic cavitation, the transducer 2 is used to convert electrical energy into mechanical vibration energy, the iron frame 3 is used to fix the transducer 2, the horn 4 is used to adjust the amplitude of the ultrasonic wave, the jacketed glass reactor 5 is used as a reaction container, constant temperature heating is achieved through oil circulation 6 and constant temperature circulation device 7, and stirring is achieved by using a glass plate.
[0059] Example 2
[0060] This embodiment provides a Ce / HZSM-5 catalyst. Based on the mass of the Ce / HZSM-5 catalyst being 100%, the mass fraction of Ce in the Ce / HZSM-5 catalyst is 2 wt %.
[0061] The preparation method of the Ce / HZSM-5 catalyst comprises:
[0062] (1) mixing an aqueous solution of cerium nitrate and HZSM-5, wherein the mixing includes constant temperature heating at 80° C., ultrasonic cavitation at a power of 300 W, and stirring at a speed of 700 rpm, and the mixing time is 30 minutes to obtain a mixed solution; the mass ratio of cerium nitrate to HZSM-5 in the aqueous solution of cerium nitrate is 0.048:1, the mass ratio of water to HZSM-5 is 15:1, and the silicon-aluminum ratio in the HZSM-5 is 25:1;
[0063] (2) The mixed solution obtained in step (1) is dried, and then heated to 600° C. at a rate of 5° C. / min and kept at this temperature for 4 h to obtain a Ce / HZSM-5 catalyst.
[0064] Example 3
[0065] This embodiment provides a Ce / HZSM-5 catalyst. Based on the mass of the Ce / HZSM-5 catalyst being 100%, the mass fraction of Ce in the Ce / HZSM-5 catalyst is 1.5 wt %.
[0066] The preparation method of the Ce / HZSM-5 catalyst comprises:
[0067] (1) mixing an aqueous solution of cerium nitrate and HZSM-5, wherein the mixing comprises heating at a constant temperature of 60° C., performing ultrasonic cavitation at a power of 500 W, and stirring at a speed of 300 rpm, and the mixing time is 90 minutes to obtain a mixed solution; the mass ratio of cerium nitrate to HZSM-5 in the aqueous solution of cerium nitrate is 0.035:1, the mass ratio of water to HZSM-5 is 20:1, and the silicon-aluminum ratio in the HZSM-5 is 30:1;
[0068] (2) The mixed solution obtained in step (1) was dried, and then heated to 550° C. at a rate of 1° C. / min and kept at that temperature for 5 h to obtain a Ce / HZSM-5 catalyst.
[0069] Example 4
[0070] This embodiment provides a Ce / HZSM-5 catalyst. Based on the mass of the Ce / HZSM-5 catalyst being 100%, the mass fraction of Ce in the Ce / HZSM-5 catalyst is 1.8 wt %.
[0071] The preparation method of the Ce / HZSM-5 catalyst comprises:
[0072] (1) mixing an aqueous solution of cerium nitrate and HZSM-5, wherein the mixing comprises heating at a constant temperature of 100° C., performing ultrasonic cavitation at a power of 600 W, and stirring at a rotation speed of 900 rpm, and the mixing time is 60 minutes to obtain a mixed solution; the mass ratio of cerium nitrate to HZSM-5 in the aqueous solution of cerium nitrate is 0.043:1, the mass ratio of water to HZSM-5 is 20:1, and the silicon-aluminum ratio in the HZSM-5 is 25:1, to obtain a mixed solution;
[0073] (2) The mixed solution obtained in step (1) was dried, and then heated to 650° C. at a rate of 10° C. / min and kept at this temperature for 3 h to obtain a Ce / HZSM-5 catalyst.
[0074] Example 5
[0075] This embodiment provides a Ce / HZSM-5 catalyst, which is the same as Embodiment 1 except that the constant temperature heating is performed at 40°C.
[0076] Example 6
[0077] This embodiment provides a Ce / HZSM-5 catalyst, which is the same as that of Embodiment 1 except that the catalyst is heated at a constant temperature of 140°C.
[0078] Example 7
[0079] This embodiment provides a Ce / HZSM-5 catalyst, which is the same as that of Embodiment 1 except that ultrasonic cavitation is performed at a power of 200 W in the preparation method of the Ce / HZSM-5 catalyst.
[0080] Example 8
[0081] This embodiment provides a Ce / HZSM-5 catalyst, which is the same as that of Embodiment 1 except that ultrasonic cavitation is performed at a power of 800 W in the preparation method of the Ce / HZSM-5 catalyst.
[0082] Example 9
[0083] This embodiment provides a Ce / HZSM-5 catalyst, which is the same as that of Embodiment 1 except that the mixing time in the preparation method of the Ce / HZSM-5 catalyst is 15 minutes.
[0084] Example 10
[0085] This embodiment provides a Ce / HZSM-5 catalyst, which is the same as that of Embodiment 1 except that the mixing time in the preparation method of the Ce / HZSM-5 catalyst is 120 min.
[0086] Embodiment 11
[0087] This embodiment provides a Ce / HZSM-5 catalyst, which is the same as that of Embodiment 1 except that the silicon-to-aluminum ratio in the HZSM-5 is 15:1.
[0088] Example 12
[0089] This embodiment provides a Ce / HZSM-5 catalyst, which is the same as that of Embodiment 1 except that the silicon-aluminum ratio in the HZSM-5 is 40:1.
[0090] Comparative Example 1
[0091] This comparative example provides a Ce / HZSM-5 catalyst, which is the same as Example 1 except that the mass fraction of Ce in the Ce / HZSM-5 catalyst is 0.5wt%, that is, the mass ratio of Ce salt to HZSM-5 in the Ce salt solution in step (1) of the preparation method of the Ce / HZSM-5 catalyst is 0.0156:1.
[0092] Comparative Example 2
[0093] This comparative example provides a Ce / HZSM-5 catalyst, which is the same as Example 1 except that the mass fraction of Ce in the Ce / HZSM-5 catalyst is 3wt%, that is, the mass ratio of Ce salt to HZSM-5 in the Ce salt solution in step (1) of the preparation method of the Ce / HZSM-5 catalyst is 0.0958:1.
[0094] Comparative Example 3
[0095] This comparative example provides a Ce / HZSM-5 catalyst, which is the same as Example 1 except that the ultrasonic cavitation performed simultaneously with the constant temperature heating in step (1) of the preparation method of the Ce / HZSM-5 catalyst is omitted.
[0096] Comparative Example 4
[0097] This comparative example provides a HZSM-5 catalyst, and the HZSM-5 catalyst is the HZSM-5 in Example 1.
[0098] The Ce / HZSM-5 catalysts provided in Examples 1 and 2 and the HZSM-5 catalyst provided in Comparative Example 4 were subjected to NH3-TPD test, and the obtained curve of the desorption gas concentration changing with temperature is as follows: Figure 2 As shown;
[0099] The specific surface area, pore volume, pore diameter and total acid content of the Ce / HZSM-5 catalysts provided in Examples 1 to 12, Comparative Examples 1 to 3 and the HZSM-5 catalyst provided in Comparative Example 4 were tested. The test results are shown in Table 1.
[0100] The test method for specific surface area is: nitrogen adsorption and desorption experimental determination (BET method) (GB / T19587-2017 "Determination of specific surface area of solid substances by gas adsorption BET method");
[0101] The pore volume was determined by: nitrogen adsorption-desorption experimental determination (t-plot method);
[0102] The pore size test method is: the pore size information value calculated by the BET method;
[0103] The test method for total acid content is: NH3-TPD experimental determination, standard pulse peak calibration method: compare the sample signal peak area with the standard pulse peak area, calculate the NH3 volume of the sample peak area, and then calculate the "total acid content";
[0104] The oxygen-containing compounds in the PET pyrolysis oil were converted using the Ce / HZSM-5 catalysts provided in Examples 1 to 12, Comparative Examples 1 to 3, and the HZSM-5 catalyst provided in Comparative Example 4. The conversion method was: hydrodeoxygenation. The conversion rate of the oxygen-containing compounds in the PET pyrolysis oil obtained by testing is shown in Table 1.
[0105] Table 1
[0106]
[0107]
[0108] From Table 1 and Figure 2 We can get:
[0109] (1) The Ce / HZSM-5 catalysts provided in Examples 1 to 4 have a lower total acid content, and when the oxygen-containing compounds in the PET pyrolysis oil are converted, the oxygen-containing compounds show a higher conversion rate;
[0110] (2) By comparing Example 1 with Examples 5 and 6, it can be seen that the temperature of constant temperature heating in step (1) of the preparation method of Ce / HZSM-5 catalyst described in the present invention will affect the performance of Ce / HZSM-5 catalyst; when the temperature of constant temperature heating is low, the specific surface area, pore volume, pore size, total acid content and conversion rate of oxygen-containing compounds of Ce / HZSM-5 catalyst will be reduced. This is because the dissolution and dispersion of Ce salts are insufficient at low heating temperatures, and Ce species are deposited at the pores and channels of the molecular sieve, resulting in blockage of the molecular sieve channels and reduction of the pore size, thereby reducing the exposure of effective pores and active sites; when the temperature of constant temperature heating is high, the conversion rate of oxygen-containing compounds will be reduced. This is because the high temperature causes Ce sintering or destruction of the molecular sieve structure, thereby reducing the performance of the catalyst;
[0111] (3) By comparing Example 1 with Examples 7 and 8, it can be seen that the power of ultrasonic cavitation in step (1) of the preparation method of Ce / HZSM-5 catalyst in the present invention will affect the performance of Ce / HZSM-5 catalyst; when the power of ultrasonic cavitation is low, the conversion rate of oxygen-containing compounds will decrease, because the low ultrasonic cavitation power cannot generate sufficient local high temperature and high pressure to promote the uniform dispersion and loading of Ce species, and may block some pores; when the power of ultrasonic cavitation is high, the conversion rate of oxygen-containing compounds will decrease, because excessive ultrasonic cavitation will cause the HZSM-5 molecular sieve structure to be destroyed, thereby reducing the performance of the catalyst;
[0112] (4) By comparing Example 1 with Examples 9 and 10, it can be seen that the mixing time in step (1) of the preparation method of the Ce / HZSM-5 catalyst described in the present invention will affect the performance of the Ce / HZSM-5 catalyst; when the mixing time is short, the specific surface area, pore volume, pore size, total acid content and conversion rate of oxygen-containing compounds of the Ce / HZSM-5 catalyst will decrease. This is because the mixing time is insufficient, the interaction and dispersion between the Ce salt and HZSM-5 are insufficient, resulting in uneven loading and partial blockage of the pores by the undispersed Ce salt; if the mixing time is too long, it may cause the destruction of the molecular sieve structure or excessive dispersion of the Ce salt, thereby reducing the performance of the catalyst;
[0113] (5) By comparing Example 1 with Examples 13 and 14, it can be seen that the silicon-aluminum ratio in the HZSM-5 described in step (1) of the preparation method of the Ce / HZSM-5 catalyst described in the present invention will affect the performance of the Ce / HZSM-5 catalyst; when the silicon-aluminum ratio is low, the specific surface area, pore volume, pore size, total acid content and conversion rate of oxygen-containing compounds of the Ce / HZSM-5 catalyst will become smaller. This is because the HZSM-5 with a low silicon-aluminum ratio has a higher aluminum content, which leads to an increase in the acid sites of the catalyst. However, this will also reduce the stability of the catalyst structure and the pore structure is prone to collapse, thereby reducing the specific surface area and pore volume; high acidity will promote non-selective reactions and reduce the conversion rate of oxygen-containing compounds; when the silicon-aluminum ratio is high, the pore channels of the molecular sieve may be narrower and the pore walls thicker, which is not conducive to the diffusion of reactants and the contact efficiency of the catalyst. At the same time, aluminum is the main source of acid sites in the molecular sieve. The reduction in aluminum content will reduce the total acid content of the catalyst and affect its catalytic activity;
[0114] (6) By comparing Example 1 with Comparative Examples 1 and 2, it can be seen that if only a small amount of Ce is loaded on HZSM-5, it cannot effectively interact with the active sites of HZSM-5, resulting in the inability to adjust the acidity of Ce / HZSM-5; if too high a content of Ce is loaded on HZSM-5, Ce will accumulate in the zeolite channels of HZSM-5, significantly reducing the pore volume and pore size of Ce / HZSM-5, limiting the diffusion of reactants and products in the channels, and causing Ce / HZSM-5 to be deactivated;
[0115] (7) By comparing Example 1 with Comparative Example 3, it can be seen that the ultrasonic cavitation performed simultaneously with the constant temperature heating in step (1) of the preparation method of the Ce / HZSM-5 catalyst described in the present invention will affect the performance of the Ce / HZSM-5 catalyst; when the ultrasonic cavitation is omitted, the specific surface area, pore volume, pore size, total acid content and conversion rate of oxygen-containing compounds of the Ce / HZSM-5 catalyst will decrease. This is because the lack of ultrasonic cavitation process causes uneven dispersion of Ce species on HZSM-5, resulting in accumulation of some Ce species in the pores, causing pore blockage and covering of active sites;
[0116] (8) By comparing Examples 1 and 2 with Comparative Example 4, it can be seen that since the low-temperature desorption peak of 200°C is related to the release of NH3 from Lewis centers (weak acid centers) such as extra-framework aluminum, and the high-temperature desorption peak of 412°C is related to the release of NH3 from Bronsted acid centers (strong acid centers) of extra-framework aluminum, the peak area represents the number of acid sites, and the peak temperature represents the acid strength; therefore, compared with the original HZSM-5, the Ce / HZSM-5 catalyst provided in the present invention, when loaded with a lower amount of 1wt% and 2wt% Ce, the number and strength of its weak acid and strong acid centers are reduced to varying degrees, thereby reducing the total acidity, especially the Bronsted acid sites are significantly reduced.
[0117] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A Ce / HZSM-5 catalyst, characterized in that: Based on the mass of the Ce / HZSM-5 catalyst as 100%, the mass fraction of Ce in the Ce / HZSM-5 catalyst is 1-2wt%.
2. A method for preparing the Ce / HZSM-5 catalyst according to claim 1, characterized in that: The preparation method comprises: The Ce salt solution and HZSM-5 are mixed, wherein the mixing includes constant temperature heating and ultrasonic cavitation to obtain a mixed solution, and then heat treatment is performed to obtain a Ce / HZSM-5 catalyst.
3. The preparation method according to claim 2, characterized in that: The mass ratio of Ce salt to HZSM-5 in the Ce salt solution is (0.024-0.048):1; Preferably, the mass ratio of the solvent to HZSM-5 in the Ce salt solution is (15-20):
1.
4. The preparation method according to claim 2 or 3, characterized in that: The silicon-to-aluminum ratio in the HZSM-5 is (20-30):
1.
5. The preparation method according to any one of claims 2 to 4, characterized in that: The mixing time is 30 to 90 minutes Preferably, the constant temperature heating temperature is 60-100°C; Preferably, the mixing further comprises stirring performed simultaneously with the constant temperature heating and the ultrasonic cavitation; Preferably, the stirring speed is 300-900 rpm.
6. The preparation method according to any one of claims 2 to 5, characterized in that: The power of the ultrasonic cavitation is 300-600W.
7. The preparation method according to any one of claims 2 to 6, characterized in that: Drying is also included between the mixing and the heat treatment; Preferably, the drying temperature is 105-120° C. and the drying time is 10-14 hours.
8. The preparation method according to any one of claims 2 to 7, characterized in that: The heat treatment includes heating and heat preservation in sequence; Preferably, the heating rate is 1 to 10°C / min; Preferably, the terminal temperature of the heating is 550-650°C; Preferably, the insulation time is 3 to 5 hours.
9. The preparation method according to any one of claims 2 to 8, characterized in that: The preparation method comprises: (1) mixing a Ce salt solution and HZSM-5, wherein the mixing includes constant temperature heating at 60-100° C., ultrasonic cavitation at a power of 300-600 W, and stirring at a speed of 300-900 rpm, and the mixing time is 30-90 min to obtain a mixed solution; the mass ratio of Ce salt to HZSM-5 in the Ce salt solution is (0.024-0.048):1, the mass ratio of solvent to HZSM-5 is (15-20):1, and the silicon-aluminum ratio in the HZSM-5 is (20-30):1; (2) Drying the mixed solution obtained in step (1), heating it to 550-650° C. at a rate of 1-10° C. / min, and then keeping it at that temperature for 3-5 hours to obtain a Ce / HZSM-5 catalyst.
10. An application of the Ce / HZSM-5 catalyst according to claim 1, characterized in that: The Ce / HZSM-5 catalyst is used to convert oxygen-containing compounds in waste photovoltaic module PET pyrolysis oil into gasoline-grade hydrocarbons.
Citation Information
Patent Citations
Vinyl acetate catalyst and method for synthesizing vinyl acetate by use of ethylidene acetate
CN104549442A
Preparation method and application for hydrofluoroolefins hydrogenation catalyst
CN105107491A
Method for regenerating (RE / HZSM-5) catalysts for resolving methanethiol gas
CN105233866A
Catalyst for producing propylene by converting through coupling of methanol and C4-hydrocarbons and application of catalyst
CN105289712A
Metal modification ZSM-5 molecular sieve based catalyst and preparation method and application
CN106140266A