Forming method of 2A14 aluminum alloy large-size special-shaped thin-wall cabin section forge piece

By controlling the heating temperature and the deformation amount of multi-party forging, combined with multiple forging and heat treatment, the problem of unevenness in the interior of the 2A14 aluminum alloy special-shaped thin-wall cabin section forgings is solved, and the mechanical properties of the forgings are significantly improved.

CN119076844APending Publication Date: 2024-12-06SOUTHWEST ALUMINUM GRP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411183689.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is easy to cause unevenness in the product interior when preparing 2A14 aluminum alloy special-shaped thin-walled cabin forging molded parts, which affects the mechanical properties.

Method used

By controlling the heating temperature and the single deformation amount of multi-party forging, multiple forgings and heat treatments, including heating, backextrusion die forging, machining, quenching and aging, the deformation uniformity and mechanical properties of forging are improved.

Benefits of technology

The horizontal, longitudinal and high-direction mechanical properties of the forging are significantly improved, making the forging more uniform tissue, more uniform performance, and the comprehensive mechanical properties are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005014163600000061
    Figure BDA0005014163600000061
  • Figure BDA0005014163600000071
    Figure BDA0005014163600000071
  • Figure BDA0005014163600000081
    Figure BDA0005014163600000081
Patent Text Reader

Abstract

The invention provides a forming method of a 2A14 aluminum alloy large-size special-shaped thin-wall cabin section forge piece, which comprises the following steps: S1) heating a 2A14 aluminum alloy cast ingot, and carrying out one-time multi-direction forging to obtain an initial blank; (S2) the initial blank is heated, and the heated blank is subjected to secondary multi-direction forging; and (S3) the blank obtained in the step (S2) is heated to 450-470 DEG C again, backward extrusion die forging, machining, quenching and aging are sequentially conducted, and the large-size special-shaped thin-wall cabin section forged piece is obtained. In the forming process of the 2A14 aluminum alloy large-size special-shaped thin-wall cabin section forge piece, by controlling the heating temperature of forging, the deformation uniformity of the forge piece can be improved, the single deformation amount of multi-directional forging can be controlled, equivalent strain can be improved, the forging penetration of the forge piece can be improved, and finally the uniformity and mechanical property of crystal grains in all directions of the forge piece can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy processing and forming, and in particular to a forming method of a 2A14 aluminum alloy large-size special-shaped thin-wall cabin section forging. Background Art

[0002] 2A14 aluminum alloy is a kind of hard aluminum alloy. Its main chemical components include Zn, Fe, Mg, Al, etc. It has the advantages of good machinability, resistivity, spot welding and seam welding performance. Therefore, 2A14 aluminum alloy can be used as special-shaped thin-walled cabin section forging parts.

[0003] The existing technology for preparing 2A14 aluminum alloy special-shaped thin-walled cabin section forging parts generally adopts the following process: material preparation → ingot heating (heating temperature 440°C) → single deformation forging (single deformation 46%) → heating (heating temperature 440°C) → reverse extrusion die forging → machining → quenching → aging → flaw detection → sampling and testing. However, the size of the special-shaped thin-walled cabin section forging parts is large, and the above preparation process is likely to cause unevenness inside the product. Therefore, in the process of preparing forging parts, it is necessary to reasonably allocate the process means to make the internal structure and performance uniform. Summary of the invention

[0004] The technical problem solved by the present invention is to provide a forming method for a large-size, special-shaped, thin-walled cabin section forging of a 2A14 aluminum alloy, which can obtain a uniform fine-grained structure and significantly improve the mechanical properties of the forging in the transverse, longitudinal and axial directions.

[0005] In view of this, the present application provides a forming method for a 2A14 aluminum alloy large-size special-shaped thin-walled cabin section forging, comprising the following steps:

[0006] S1) heating the 2A14 aluminum alloy ingot and performing multi-directional forging to obtain an initial billet; the heating temperature is 450-470° C., and the single deformation amount of the multi-directional forging is 50-54%;

[0007] S2) heating the blank, and performing secondary multi-directional forging on the heated blank; the heating temperature is 450-470° C., and the single deformation amount of the multi-directional forging is 50-54%;

[0008] S3) The blank obtained in step S2) is heated again to 450-470° C., and then reverse extrusion die forging, machining, quenching and aging are performed in sequence to obtain a large-sized special-shaped thin-walled cabin section forging.

[0009] Preferably, the total number of upsetting and drawing of the first multi-directional forging and the second multi-directional forging is 6 to 8 times.

[0010] Preferably, in step S1), the heating temperature is 460-470°C.

[0011] Preferably, in step S1), the single deformation amount of the multi-directional forging is 52-53%, and the number of upsetting times of the multi-directional forging is 3-4 times.

[0012] Preferably, in step S2), the heating temperature is 460-470°C.

[0013] Preferably, in step S2), the single deformation amount of the secondary polygonal forging is 52-53%, and the number of upsetting times of the secondary polygonal forging is 3-4 times.

[0014] Preferably, in step S3), the reheating temperature is 460-470°C.

[0015] Preferably, the quenching temperature is 500-600°C.

[0016] Preferably, the aging parameter is 150-200°C.

[0017] Preferably, the maximum outer contour dimensions of the large-sized special-shaped thin-walled compartment forging are outer diameter Φ1100mm×inner diameter Φ820mm×height 1500mm, with the special-shaped part in the middle.

[0018] The present application provides a forming method for a large-sized special-shaped thin-walled cabin section forging of a 2A14 aluminum alloy, which first heats a 2A14 aluminum alloy ingot and then performs a multi-directional forging to obtain an initial blank; then the initial blank is heated, and the heated blank is subjected to a second multi-directional forging, and finally the obtained blank is heated again, and reverse extrusion die forging, machining, quenching and aging are performed in sequence, thereby obtaining a large-sized special-shaped thin-walled cabin section forging. In the forming process of the large-sized special-shaped thin-walled cabin section forging of a 2A14 aluminum alloy, by controlling the heating temperature of the forging, it is beneficial to improve the uniformity of the deformation of the forging, and controlling the single deformation amount of the multi-directional forging is beneficial to improve the equivalent strain, so as to improve the forging permeability of the forging; further, the total number of upsetting and drawing times of the first multi-directional forging and the second multi-directional forging is controlled, so that the anisotropic shape of the forging is reduced, the uniformity of the performance is improved, and finally it is beneficial to improve the comprehensive mechanical properties of the forging. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The figures are equivalent strain cloud diagrams of forgings of Example 1 and Comparative Example 1 at different forging temperatures; Figure (a) is the equivalent strain cloud diagram of the forging of Comparative Example 1 at a forging temperature of 440°C, and Figure (b) is the equivalent strain cloud diagram of the forging of Example 1 at a forging temperature of 460°C;

[0020] Figure 2The figures are photos of residual crystalline phase distribution morphology of forgings after air cooling at different single upsetting amounts in Example 1 and Comparative Example 2; Figure (a) is a photo of residual crystalline phase distribution morphology of Example 1 at a single upsetting deformation amount of 52%, and Figure (b) is a photo of residual crystalline phase distribution morphology of Comparative Example 2 at a single upsetting deformation amount of 46%;

[0021] Figure 3 The residual crystalline phase distribution morphology photos of the solid solution forgings of Example 1 and Comparative Example 2 at different single upsetting amounts; Figure (a) is a residual crystalline phase distribution morphology photo of Example 1 at a single upsetting deformation amount of 52%, and Figure (b) is a residual crystalline phase distribution morphology photo of Comparative Example 2 at a single upsetting deformation amount of 46%;

[0022] Figure 4 The residual crystalline phase distribution morphology photos of the solid solution forgings of Example 1 and Comparative Example 3 in different upsetting modes; Figure (a) is a residual crystalline phase distribution morphology photo of the solid solution forging of Example 1 after 7 multi-directional forgings, and Figure (b) is a residual crystalline phase distribution morphology photo of the solid solution forging of Comparative Example 3 after 4 multi-directional forgings;

[0023] Figure 5 The metallographic microstructures of the solid solution forgings of Example 1 and Comparative Example 3 in different upsetting and drawing modes are shown in Figure (a). The metallographic microstructures of the solid solution forgings of Example 1 after 7 multi-directional forgings are shown in Figure (b). The metallographic microstructures of the solid solution forgings of Comparative Example 3 after 4 multi-directional forgings are shown in Figure (a).

[0024] Figure 6 The recrystallized structure percentages of the solid solution forgings of Example 1 and Comparative Example 3 in different upsetting and drawing modes; Figure (a) shows the recrystallized structure percentage of the solid solution forgings of Example 1 after 7 multi-directional forgings, and Figure (b) shows the recrystallized structure percentage of the solid solution forgings of Comparative Example 3 after 4 multi-directional forgings;

[0025] Figure 7 It is a schematic structural diagram of the 2A14 aluminum alloy large-size special-shaped thin-walled cabin section forging of the present invention. DETAILED DESCRIPTION

[0026] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0027] In view of the special size characteristics and performance requirements of 2A14 aluminum alloy large-sized special-shaped thin-walled cabin section forgings in the prior art, the present application provides a forming method of 2A14 aluminum alloy large-sized special-shaped thin-walled cabin section forgings, which controls the deformation temperature and deformation amount to make the forgings more uniform, which is beneficial to improving the comprehensive mechanical properties of the forgings. Specifically, the embodiment of the present invention discloses a forming method of 2A14 aluminum alloy large-sized special-shaped thin-walled cabin section forgings, comprising the following steps:

[0028] S1) heating the 2A14 aluminum alloy ingot and performing multi-directional forging to obtain an initial billet; the heating temperature is 450-470° C., and the single deformation amount of the multi-directional forging is 50-54%;

[0029] S2) heating the initial blank, and performing secondary multi-directional forging on the heated blank; the heating temperature is 450-470° C., and the single deformation amount of the multi-directional forging is 50-54%;

[0030] S3) The blank obtained in step S2) is heated again to 450-470° C., and then reverse extrusion die forging, machining, quenching and aging are performed in sequence to obtain a large-sized special-shaped thin-walled cabin section forging.

[0031] In the forming method of 2A14 aluminum alloy large-size special-shaped thin-walled cabin section forgings of the present application, the present application prepares 2A14 aluminum alloy ingots, and the preparation method thereof is prepared according to a method well known to those skilled in the art, and the present application has no special restrictions on this.

[0032] In the present application, a 2A14 aluminum alloy ingot is heated and then subjected to a multi-way forging to obtain an initial blank; in this process, the heating temperature is 450-470°C, and the single deformation of the multi-way forging is 50-54%. Specifically, the heating temperature is 450°C, 460°C or 470°C, and the single deformation of the multi-way forging is 50%, 51%, 52%, 53%, 54%. In a specific embodiment, the heating temperature is 460°C, and the single deformation of the multi-way forging is 52%. In the present application, the multi-way forging is upsetting and drawing in multiple directions, and the multi-way forging can be two-pass upsetting and drawing, three-pass upsetting and drawing, or four-pass upsetting and drawing. In a specific embodiment, the multi-way forging is four-pass upsetting and drawing.

[0033] The present application then heats the above-mentioned blank again, and performs secondary multi-directional forging on the heated blank; during this process, the heating temperature is 450-470°C, and the single deformation of the multi-directional forging is 50-54%. Specifically, the heating temperature is 450°C, 460°C or 470°C, and the single deformation of the multi-directional forging is 50%, 51%, 52%, 53%, 54%. In a specific embodiment, the heating temperature is 460°C, and the single deformation of the multi-directional forging is 52%. In the present application, the multi-directional forging is upsetting and drawing in multiple directions, and the secondary multi-directional forging can be two-pass upsetting and drawing, three-pass upsetting and drawing, or four-pass upsetting and drawing. In a specific embodiment, the secondary multi-directional forging is three-pass upsetting and drawing. The total number of upsetting and drawing of the first multi-directional forging and the second multi-directional forging is 6 to 8 times, specifically 6 times, 7 times or 8 times. In a specific embodiment, the total number of upsetting and drawing of the first multi-directional forging and the second multi-directional forging is 7 times.

[0034] According to the present invention, the secondary multi-forged billet is then heated again to 450-470°C, and then reverse extrusion die forging, machining, quenching and aging are performed in sequence, thereby obtaining a large-sized, special-shaped, thin-walled cabin section forging. In the above process, the reheating temperature is 450-470°C, specifically, the heating temperature is 450°C, 460°C or 470°C, and in a specific embodiment, the heating temperature is 460°C. The reverse extrusion die forging and the machining are performed in a manner well known to those skilled in the art, and there is no particular limitation on this application. The quenching temperature is 500-600°C, specifically, the quenching temperature is 550-580°C, and the aging temperature is 150-200°C, specifically, the minimum temperature is 160-180°C.

[0035] The maximum outer contour size of the large-sized special-shaped thin-walled cabin section forging described in this application is Φ1100mm×Φ820mm×1500mm, and the middle is a special-shaped part, as shown in the following figure. Figure 7 shown.

[0036] In order to further understand the present invention, the forming method of the 2A14 aluminum alloy large-size special-shaped thin-walled cabin section forging provided by the present invention is described in detail below in combination with the embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0037] Example 1

[0038] 1) heating the 2A14 aluminum alloy ingot to 460° C. and then performing three multi-directional forging passes with a single-pass deformation of 52% to obtain an initial billet;

[0039] 2) heating the initial blank to 460° C. and subjecting the heated blank to four multi-directional forging passes, with a single-pass deformation of 52%;

[0040] 3) The blank obtained in step 2) is heated again to 460° C., and then reverse extrusion die forging, machining, quenching and aging are performed in sequence to obtain a large-sized special-shaped thin-walled cabin section forging; wherein the quenching temperature is 550° C., and the aging temperature is 160° C.

[0041] Comparative Example 1

[0042] The preparation method is basically the same as that of Example 1, except that the temperature in step 1) and step 2) is 440°C; on this basis, the influence of deformation temperature on deformation uniformity and microstructure properties is studied:

[0043] 1) Effect of deformation temperature on deformation uniformity

[0044] Figure 1 The equivalent strain cloud diagram of forgings at different forging temperatures shows that the average value of the equivalent strain of forgings increases slightly (from 10.0 to 10.5) with increasing temperature, and the mean square deviation of the equivalent strain is also small, indicating that increasing the temperature is beneficial to the deformation uniformity of forgings.

[0045] 2) Effect of deformation temperature on microstructure and properties of 2A14 aluminum alloy

[0046] The mechanical properties of forgings after heat treatment after 7 times of multi-directional forging + forming at different temperatures are shown in Table 1.

[0047] Table 1 Data table of the effect of blanking temperature on performance

[0048]

[0049] It can be seen from the table that increasing the deformation temperature of multi-directional forging is beneficial to improving the comprehensive mechanical properties of forgings. When the forging deformation temperature is increased to 460℃, the elongation of the forgings is above 6%, and the performance uniformity is better than that of forging at 440℃.

[0050] Therefore, increasing the deformation temperature of multi-directional forging is beneficial to obtaining fine and uniform grains after solution treatment. When the forging deformation temperature is 460°C, the grain size of the forging is about 20-30μm. When the deformation temperature is 440°C, the grain uniformity of the forging is reduced. This shows that increasing the deformation temperature is beneficial to improving the uniformity of the forging structure; increasing the forging temperature is beneficial to the refinement and equiaxed grains of 2A14 aluminum alloy, and the coarse residual crystalline phase is better broken and dissolved, and the elongation of the forging can reach 6.3-15%.

[0051] Comparative Example 2

[0052] The preparation method is basically the same as that of Example 1, except that the single deformation amount of the multi-sided forging in step 1) and step 2) is 42%; on this basis, the influence of the deformation amount on the deformation uniformity and the microstructure performance is studied:

[0053] 1) Influence of upsetting deformation on deformation uniformity

[0054] Increasing the single upsetting deformation can significantly improve the equivalent effect of forgings. After 7 multi-directional forgings, the total equivalent strain value of the forging with a single upsetting deformation of 52% is 10.6, while it is only 8.73 when the single upsetting deformation is 42%. This shows that increasing the single upsetting deformation can increase the equivalent strain and improve the forging permeability of the forging.

[0055] 2) Effect of deformation degree on microstructure and properties of 2A14 aluminum alloy

[0056] The effect of single upsetting deformation (46%, 52%) of multi-directional forging on the residual crystalline phase of 2A14 aluminum alloy was studied. When the single upsetting deformation was increased to 52% at the billet opening temperature of 460℃, the coarse residual crystalline phase in the ingot structure was more fully broken ( Figure 2 ), the residual crystalline phase is more dispersed, and the coarse residual crystalline phase cannot be fully dissolved in the subsequent solid solution process ( Figure 3 ), during the blanking process, increasing the amount of upsetting deformation makes the network coarse phase in the original ingot structure fully dispersed and crushed, which will be beneficial for the second phase to be fully dissolved into the aluminum matrix in the subsequent solid solution, thereby improving the comprehensive performance of the forging.

[0057] Comparative Example 3

[0058] The preparation method is basically the same as that of Example 1, except that the total number of upsetting and drawing in the multi-sided forging in step 1) and step 2) is 4 times;

[0059] According to the equivalent strain of forgings under different upsetting deformation, the average equivalent strain after 7 multi-directional forging is about 40% higher than that after 4 multi-directional forging. The effects of different upsetting times (7 multi-directional forging, 4 multi-directional forging) on ​​the microstructure and properties of 2A14 aluminum alloy at 460℃ were studied: Increasing the upsetting times is beneficial to fully crush the coarse residual crystalline phase ( Figure 4 ), the grain structure of the forging is also more uniform and fine ( Figure 5 ); The comprehensive mechanical properties of forgings are improved, the anisotropy of forgings is reduced, the uniformity of performance is improved, especially the radial elongation is increased from 3.3% to 6.8% as shown in Table 2;

[0060] Table 2 Data table of the influence of upsetting times on performance

[0061]

[0062]

[0063] The 7-time multi-directional forging process has more upsetting and drawing times during the deformation process, and the accumulated dislocation storage energy is more, which is easy to induce the formation of more recrystallization nuclei in the subsequent solid solution process. The final recrystallization ratio of the forging is higher. The final recrystallization percentage of the 7-time multi-directional forging case reaches 46%, while the recrystallization percentage of the 4-time multi-directional forging case does not reach 10%. Figure 6 As shown, Figure 6 The first column represents the degree of recrystallization, the second column represents the degree of residual crystalline phase, and the third column represents the grain size. It can be seen that increasing the number of multi-directional forgings reduces the residual crystalline phase, the grain structure of the forgings becomes more uniform and fine, and the degree of recrystallization is improved.

[0064] The above research leads to the conclusion that increasing the number of multi-directional forgings is beneficial to fully crushing the coarse residual crystalline phase, making the grain structure of the forgings more uniform and fine, reducing the anisotropy of the forgings, and improving the uniformity of performance, especially the radial elongation increased from 3.3% to 6.8%.

[0065] Therefore, by controlling the deformation temperature before forging and the deformation amount of forging, the microstructure after quasi-isothermal die forging can be made as uniform and fine-grained as possible, thereby significantly improving the comprehensive mechanical properties.

[0066] Comparative Example 4

[0067] 1) heating the 2A14 aluminum alloy ingot to 440° C. and then performing four multi-directional forging passes with a single-pass deformation of 46% to obtain an initial billet;

[0068] 2) The initial blank is heated to 440°C, and then reverse extrusion die forging, machining, quenching and aging are performed in sequence to obtain a large-sized special-shaped thin-walled cabin section forging;.

[0069] The properties of the forgings prepared in Example 1 and Comparative Example 4 are compared, and the results are shown in Table 3;

[0070] Table 3 Performance data of forgings prepared in Example 1 and Comparative Example 4

[0071]

[0072]

[0073] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0074] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A forming method for a 2A14 aluminum alloy large-size, special-shaped, thin-walled cabin section forging, comprising the following steps: S1) heating the 2A14 aluminum alloy ingot and performing multi-directional forging to obtain an initial billet; the heating temperature is 450-470° C., and the single deformation amount of the multi-directional forging is 50-54%; S2) heating the blank, and performing secondary multi-directional forging on the heated blank; the heating temperature is 450-470° C., and the single deformation amount of the multi-directional forging is 50-54%; S3) The blank obtained in step S2) is heated again to 450-470° C., and then reverse extrusion die forging, machining, quenching and aging are performed in sequence to obtain a large-sized special-shaped thin-walled cabin section forging.

2. The molding method according to claim 1, characterized in that: The total number of upsetting and drawing of the first multi-directional forging and the second multi-directional forging is 6 to 8 times.

3. The molding method according to claim 1, characterized in that: In step S1), the heating temperature is 460-470°C.

4. The molding method according to claim 1, characterized in that: In step S1), the single deformation amount of the multi-directional forging is 52-53%, and the number of upsetting times of the multi-directional forging is 3-4 times.

5. The molding method according to claim 1, characterized in that: In step S2), the heating temperature is 460-470°C.

6. The molding method according to claim 1, characterized in that: In step S2), the single deformation amount of the secondary multi-directional forging is 52-53%, and the number of upsetting times of the secondary multi-directional forging is 3-4 times.

7. The molding method according to claim 1, characterized in that: In step S3), the reheating temperature is 460-470°C.

8. The molding method according to claim 1, characterized in that: The quenching temperature is 500-600°C.

9. The molding method according to claim 1, characterized in that: The aging parameter is 150-200°C.

10. The molding method according to any one of claims 1 to 9, characterized in that: The maximum outer contour dimensions of the large-sized special-shaped thin-walled cabin section forging are outer diameter Φ1100mm×inner diameter Φ820mm×height 1500mm, with the special-shaped part in the middle.

Citation Information

Patent Citations

  • Preparation process of 2A14 aluminum alloy high-cylinder part

    CN110170606A

  • Machining method of thin-wall aluminum alloy forge piece

    CN110773691A

  • Extrusion forming process and die for horseshoe-like special-shaped section die forging

    CN116493531A

  • Precise die forging forming die and method for aluminum alloy special-shaped barrel section

    CN116809833A

  • Preparation method for improving performance of aluminum alloy

    CN117165877A