Device and method for testing welding liquefaction crack sensitivity of aluminum alloy

By designing a test device for aluminum alloy, using temperature acquisition and load application devices, the sensitivity test of liquefied cracks in aluminum alloy welding is simplified, and the problems of large size and complex testing in the existing methods are solved, and accurate evaluation and Cost reduction.

CN119077094APending Publication Date: 2024-12-06HARBIN INST OF TECH AT WEIHAI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411468745.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing test methods for liquefied crack sensitivity testing of aluminum alloy welding have problems such as large size, complex testing procedures, high cost and difficulty in accurately evaluating the test plate, especially during the welding process of aluminum alloy materials.

Method used

A test device including a temperature acquisition device and a load application device is designed. The liquefied crack sensitivity test is performed using a smaller aluminum alloy test plate. The temperature change and the loading are applied in real time to measure the maximum crack length by thermocouple, and the brittleness is calculated. Temperature range, simplifying testing operations and reducing costs.

Benefits of technology

Accurate quantitative evaluation of the sensitivity of liquefied cracks in aluminum alloy welding is achieved, the testing procedures are simplified, the testing difficulty and cost are reduced, and the pre-processing of test plates and weld retention in traditional methods is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119077094A_ABST
    Figure CN119077094A_ABST
Patent Text Reader

Abstract

The invention discloses a device and a method for testing the welding liquefaction crack sensitivity of aluminum alloy, belongs to the technical field of aluminum alloy welding testing, and aims to solve the problems of large size of a test plate required by an existing test method and the like. The device comprises a load applying device and a base, an aluminum alloy testing plate is fixed to the top end of the base, the load applying device is arranged on the base, the output end of the load applying device faces the aluminum alloy testing plate upwards, and a welding gun of a TIG welding machine keeps a welding working distance away from the aluminum alloy testing plate downwards. A temperature acquisition device is arranged in the range of the heat affected zone on one side of the spot welding test position of the aluminum alloy test plate, the test procedure is simple, beveling does not need to be carried out on the aluminum alloy test plate, the situation that a long welding seam is left on the aluminum alloy test plate in a traditional detection method is avoided, the aluminum alloy test plate with the small size can be used for detection, and the detection efficiency is improved. The cost is reduced, the aluminum alloy welding liquefaction crack sensitivity can be accurately and quantitatively evaluated, and the evaluation result is not influenced by parameters of the device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum alloy welding testing, and in particular relates to a device and method for testing aluminum alloy welding liquefaction crack sensitivity. Background Art

[0002] Under the action of welding heat cycle, metal materials form low-melting eutectics in the heat-affected zone (or low-melting eutectics exist on the original grain boundaries) and melt. During the subsequent cooling and shrinkage process, cracks appearing at the molten grain boundaries are called liquefaction cracks. Due to the limitations of the profile extrusion process and the characteristics of the material itself, the surface of aluminum alloys inevitably forms a coarse-grained structure, which makes it very easy for welded joints to produce welding liquefaction crack defects in the heat-affected zone. Therefore, in the process of developing new aluminum alloys that can be used in various fields, it is necessary to carry out welding liquefaction crack sensitivity evaluation.

[0003] At present, the commonly used liquefaction crack sensitivity test methods include: inclined Y-type groove test method, T-joint test method, fishbone test method, longitudinal adjustable restraint test method, etc.; these test methods have the disadvantages of large test plate size, the need to groove the test plate in advance, and complicated test procedures, which bring many limitations and difficulties to the test of liquefaction crack sensitivity of aluminum alloy welding. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a device and method for testing the liquefaction crack sensitivity of aluminum alloy welding, which can use a smaller test plate to complete the test of the liquefaction crack sensitivity, simplify the test operation, reduce the test difficulty, and has the advantages of being simple, effective, and reducing costs. The technical solution adopted by the present invention is as follows:

[0005] A device for testing the liquefaction crack sensitivity of aluminum alloy welding, comprising a temperature collection device, a load applying device and a base, wherein the base comprises two side wall parts arranged on the left and right, the lower ends of the two side wall parts are connected through a bottom plate part, the left and right ends of an aluminum alloy test plate are respectively connected to the top ends of the two side wall parts, and the welding gun of a TIG spot welding machine is downwardly directed to maintain a welding working distance from the aluminum alloy test plate;

[0006] The load applying device comprises a pressure head, a lifting platform and a loading cylinder, wherein the loading cylinder is arranged on the bottom plate, the piston rod of the loading cylinder is arranged upward, the lifting platform is connected to the piston rod of the loading cylinder, the pressure head is arranged on the lifting platform, the loading cylinder is connected to the air pump through the electromagnetic valve group, the cylinder controller is electrically connected to the electromagnetic valve group, and the welding gun, the pressure head and the loading cylinder are vertically aligned from top to bottom;

[0007] The temperature acquisition device includes a plurality of thermocouples, which are arranged within a heat-affected zone on one side of a spot welding test position on the aluminum alloy test plate. The plurality of thermocouples are spaced from near to far relative to the spot welding test position of the aluminum alloy test plate.

[0008] Furthermore, the aluminum alloy test plate is connected to the side wall portion through a restraint device, which includes a clamping piece. A flange structure is provided on the top of the side wall portion. Two clamping pieces are connected to the flange structures of the two side wall portions one by one up and down through bolts respectively. The two clamping pieces respectively clamp the two ends of the aluminum alloy test plate on the upper end surfaces of the two side wall portions.

[0009] Furthermore, an oblong hole is provided on the flange structure, the oblong hole extends left and right, and a circular hole is provided on the clamping member, and the circular hole is connected to the corresponding oblong hole by bolts.

[0010] Furthermore, the number of the thermocouples is three, and the three thermocouples are arranged in sequence with an interval of 0.5 mm.

[0011] Furthermore, the base is a stainless steel stand.

[0012] Furthermore, there are several pressing heads, the upper end surfaces of the pressing heads are spherical surfaces protruding upward, the curvature radii of the upper end surfaces of the several pressing heads increase successively, and any one of the pressing heads can be detachably arranged on the lifting platform.

[0013] The present invention also provides a method for testing the liquefaction crack sensitivity of aluminum alloy welding, which is implemented based on the above-mentioned device for testing the liquefaction crack sensitivity of aluminum alloy welding, and includes the following steps:

[0014] Step 1: Select a sample with the same properties as the aluminum alloy test plate, use a TIG spot welder to spot weld the sample, and test the range of the heat affected zone formed during spot welding of the sample;

[0015] Step 2, fixing the aluminum alloy test plate on two side wall parts, the vertical foot of the welding gun and the aluminum alloy test plate is the spot welding test position, and setting a plurality of thermocouples within the heat affected zone range on one side of the spot welding test position. The heat affected zone range of the aluminum alloy test plate is divided according to the heat affected zone range formed by the sample plate;

[0016] Step 3: Perform TIG spot welding on the aluminum alloy test plate, maintain the current output and inert gas output of the TIG spot welder, so that the molten pool formed by spot welding remains stable. After the aluminum alloy test plate is completely welded through, the TIG spot welder extinguishes the arc, and the loading cylinder applies a load to the aluminum alloy test plate through the pressure head, so that the aluminum alloy test plate is forced to deform according to the shape of the arc-shaped pressure head;

[0017] Step 4: Measure the temperature change of the heat-affected zone of the aluminum alloy test plate in step 3 by using several thermocouples, and draw a temperature-time curve to obtain the temperature gradient G T ;

[0018] Step 5: Take a photo of the maximum crack in the heat-affected zone of the aluminum alloy test plate through an optical microscope, and measure the maximum crack length MCL;

[0019] Step 6. Calculate the brittle temperature range BTR of the aluminum alloy test plate according to the following formula to quantitatively evaluate the welding liquefaction crack sensitivity of the aluminum alloy material:

[0020] BTR=T L -MCL×G T

[0021] Where, T L is the liquidus temperature;

[0022] The larger the BTR value, the greater the liquefaction crack sensitivity of the aluminum alloy material.

[0023] Furthermore, the T L Obtained by differential scanning calorimetry.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The temperature acquisition device can measure the temperature of the heat affected zone of the aluminum alloy test plate in real time. The cylinder controller can control the lifting and lowering of the piston rod of the loading cylinder, thereby driving the lifting platform and the pressure head thereon to move, and is used to apply a load to the aluminum alloy test plate, measure the maximum crack length caused by the deformation of the aluminum alloy test plate under the load, and calculate the brittle temperature range of the aluminum alloy material through the temperature change range of the heat affected zone of the aluminum alloy test plate and the maximum crack length, so as to evaluate the liquefaction crack sensitivity of the aluminum alloy welding. The test procedure of the present invention is simple, and the result can be obtained by only one test. There is no need to perform pre-processing such as beveling on the aluminum alloy test plate, which avoids the traditional detection method leaving a long weld on the aluminum alloy test plate. A smaller-sized aluminum alloy test plate can be used for detection, which reduces the cost, and can accurately quantify the liquefaction crack sensitivity of the aluminum alloy welding, and the evaluation result is not affected by the parameters of the device itself. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is a front view of the device of the present invention;

[0027] Figure 2 is an axonometric view of the device of the present invention;

[0028] Figure 3 This is an axonometric view of the base.

[0029] In the figure, 1. base, 2. loading cylinder, 3. lifting platform, 4. clamping piece, 5. aluminum alloy test plate, 6. welding gun, 7. pressure head, 8. thermocouple, 9. side wall, 10. bottom plate, 11. flange structure, 12. oblong hole. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is described below by the specific embodiments shown in the accompanying drawings. However, it should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0031] The connection mentioned in the present invention is divided into fixed connection and detachable connection. The fixed connection is a non-detachable connection including but not limited to conventional fixed connection methods such as folding connection, rivet connection, bonding connection and welding connection. The detachable connection includes but not limited to conventional detachable methods such as bolt connection, snap connection, pin connection and hinge connection. When the specific connection method is not clearly defined, it is assumed that at least one connection method can be found in the existing connection methods to achieve the function, and those skilled in the art can choose according to their needs. For example: welding connection is selected for fixed connection, and bolt connection is selected for detachable connection.

[0032] The present invention will be further described in detail below in conjunction with the accompanying drawings. The following embodiments are provided to explain the present invention, but the present invention is not limited to the following embodiments.

[0033] Embodiment 1: Figure 1 to Figure 3 As shown, a device for testing the liquefaction crack sensitivity of aluminum alloy welding includes a temperature acquisition device, a load application device and a base 1, the base 1 includes two side wall parts 9 arranged on the left and right, the lower ends of the two side wall parts 9 are connected through a bottom plate part 10, the left and right ends of the aluminum alloy test plate 5 are respectively connected to the top ends of the two side wall parts 9, the aluminum alloy test plate 5 is arranged horizontally, the welding gun 6 of the TIG spot welding machine maintains a welding working distance downward with the aluminum alloy test plate 5, and the welding gun 6 is arranged perpendicular to the aluminum alloy test plate 5;

[0034] The load applying device includes a pressure head 7, a lifting platform 3 and a loading cylinder 2, the loading cylinder 2 is arranged on the bottom plate 10, the piston rod of the loading cylinder 2 is arranged upward, the lifting platform 3 is connected to the piston rod of the loading cylinder 2, the pressure head 7 is arranged on the lifting platform 3, the loading cylinder 2 is connected to the air pump through the electromagnetic valve group, the cylinder controller is electrically connected to the electromagnetic valve group, and the welding gun 6, the pressure head 7 and the loading cylinder 2 are vertically aligned from top to bottom;

[0035] The temperature acquisition device includes a plurality of thermocouples 8, which are arranged within the heat-affected zone on one side of the spot welding test position on the aluminum alloy test plate 5, and the plurality of thermocouples 8 are arranged in sequence from near to far relative to the spot welding test position of the aluminum alloy test plate 5.

[0036] The temperature acquisition device can measure the temperature of the heat-affected zone of the aluminum alloy test plate 5 in real time. The cylinder controller can control the lifting and lowering of the piston rod of the loading cylinder 2, thereby driving the lifting platform 3 and the pressure head 7 thereon to move, and is used to apply a load to the aluminum alloy test plate 5, measure the maximum crack length caused by the deformation of the aluminum alloy test plate 5 under the load, and calculate the brittle temperature range of the aluminum alloy material through the temperature change range of the heat-affected zone of the aluminum alloy test plate 5 and the maximum crack length, so as to evaluate the liquefaction crack sensitivity of the aluminum alloy welding. The test procedure of the present invention is simple, and the result can be obtained by only one test. There is no need to perform pre-processing such as beveling on the aluminum alloy test plate 5, which avoids the traditional detection method leaving a long weld on the aluminum alloy test plate 5. A smaller-sized aluminum alloy test plate 5 can be used for detection, which reduces the cost, and can accurately quantify the liquefaction crack sensitivity of the aluminum alloy welding, and the evaluation result is not affected by the parameters of the device itself.

[0037] The aluminum alloy test plate 5 is connected to the side wall portion 9 through a restraining device, which includes a clamping piece 4. A flange structure 11 is provided on the top of the side wall portion 9. The two clamping pieces 4 are connected to the flange structures 11 of the two side wall portions 9 one by one up and down through bolts respectively. The two clamping pieces 4 respectively clamp the two ends of the aluminum alloy test plate 5 on the upper end surfaces of the two side wall portions 9.

[0038] The flange structure 11 is provided with an oblong hole 12, which passes through the corresponding flange structure 11 vertically and extends to the left and right. The clamping member 4 is provided with a circular hole, which is connected to the corresponding oblong hole 12 by bolts. The clamping member 4 can slide left and right relative to the base 1, so as to match aluminum alloy test plates 5 of different lengths.

[0039] There are three thermocouples 8 , which are arranged in sequence with an interval of 0.5 mm, and can collect the temperature of the heat-affected zone of the aluminum alloy test plate 5 in real time.

[0040] The base 1 is a stainless steel stand.

[0041] There are several pressure heads 7, the upper end surface of the pressure head 7 is a spherical surface convex upward, the curvature radius of the upper end surfaces of the several pressure heads 7 increases successively, and any pressure head 7 can be detachably arranged on the lifting platform 3. Pressure heads 7 with different curvature radii can be replaced at any time to correspond to different applied strains.

[0042] Embodiment 2: Figure 1 to Figure 3 As shown, a method for testing the liquefaction crack sensitivity of aluminum alloy welding is implemented based on the device for testing the liquefaction crack sensitivity of aluminum alloy welding described in Example 1, and includes the following steps:

[0043] Step 1: Select a sample with the same properties as the aluminum alloy test plate 5, use a TIG spot welder to spot weld the sample, and test the range of the heat affected zone formed during spot welding of the sample;

[0044] Step 2, fix the aluminum alloy test plate 5 on the two side wall parts 9, the vertical foot of the welding gun 6 and the aluminum alloy test plate 5 is the spot welding test position, and set a plurality of thermocouples 8 in the heat affected zone range on one side of the spot welding test position. The heat affected zone range of the aluminum alloy test plate 5 is divided according to the heat affected zone range formed by the sample;

[0045] Step 3: Perform TIG spot welding on the aluminum alloy test plate 5, maintain the current output and inert gas output of the TIG spot welder, so that the molten pool formed by the spot welding remains stable. After the aluminum alloy test plate 5 is completely welded through, the TIG spot welder extinguishes the arc, and the loading cylinder 2 applies a load to the aluminum alloy test plate 5 through the pressure head 7, so that the aluminum alloy test plate 5 is forced to deform according to the shape of the arc-shaped pressure head 7;

[0046] Step 4: Measure the temperature change of the heat-affected zone of the aluminum alloy test plate 5 in step 3 by using a plurality of thermocouples 8, and draw a temperature-time curve to obtain the temperature gradient G T ;

[0047] Step 5: Take a photo of the maximum crack in the heat-affected zone of the aluminum alloy test plate 5 through an optical microscope, and measure the maximum crack length MCL;

[0048] Step 6: Calculate the brittle temperature range BTR of the aluminum alloy test plate 5 according to the following formula to quantitatively evaluate the welding liquefaction crack sensitivity of the aluminum alloy material:

[0049] BTR=T L -MCL×G T

[0050] Where, T L is the liquidus temperature;

[0051] The larger the BTR value, the greater the liquefaction crack sensitivity of the aluminum alloy material.

[0052] The T L Obtained by differential scanning calorimetry.

[0053] The test method of the present invention is further illustrated by taking 6082 aluminum alloy as an example:

[0054] 1. According to the length of the 6082 aluminum alloy test plate 5, adjust the clamping member 4 and fix the 6082 aluminum alloy test plate 5 on the base 1.

[0055] 2. Select the corresponding pressure head 7 according to the required strain amount.

[0056] 3. Perform TIG spot welding on the 6082 aluminum alloy test plate 5, keep the molten pool stable, and after 30 seconds, the 6082 aluminum alloy test plate 5 is completely welded and then the arc is extinguished.

[0057] 4. Start the loading cylinder 2 to apply a load to the 6082 aluminum alloy test plate 5 through the pressure head 7, so that the 6082 aluminum alloy test plate 5 is forced to deform according to the shape of the arc-shaped pressure head 7;

[0058] 5. Use three thermocouples 8 to measure the temperature changes at the fusion line formed by spot welding, 0.5mm away from the fusion line, and 1mm away from the fusion line, with an accuracy of 1°C and a collection frequency of 2Hz, and draw a temperature-time curve to obtain the temperature gradient G T ;

[0059] 6. Observe the specimen through an optical microscope and record the maximum crack length MCL of the heat affected zone;

[0060] 7. Calculate the brittle temperature range BTR according to the following formula:

[0061] BTR=T L -MCL×G T

[0062] Where, T L is the liquidus temperature.

[0063] 8. The BTR is used to quantitatively evaluate the liquefaction crack sensitivity of aluminum alloy welding. The larger the BTR, the greater the liquefaction crack sensitivity of the material.

[0064] The above embodiments are merely exemplary descriptions of the present invention and do not limit its protection scope. Those skilled in the art may also make partial changes thereto, which are within the protection scope of the present invention as long as they do not exceed the spirit of the present invention.

Claims

1. A device for testing the liquefaction crack sensitivity of aluminum alloy welding, characterized in that: The device comprises a temperature collecting device, a load applying device and a base (1), wherein the base (1) comprises two side wall portions (9) arranged on the left and right, wherein the lower ends of the two side wall portions (9) are connected via a bottom plate portion (10), and the left and right ends of an aluminum alloy test plate (5) are respectively connected to the top ends of the two side wall portions (9), and a welding gun (6) of a TIG spot welding machine is downwardly directed to maintain a welding working distance from the aluminum alloy test plate (5); The load applying device comprises a pressure head (7), a lifting platform (3) and a loading cylinder (2); the loading cylinder (2) is arranged on a bottom plate (10); a piston rod of the loading cylinder (2) is arranged upward; the lifting platform (3) is connected to the piston rod of the loading cylinder (2); the pressure head (7) is arranged on the lifting platform (3); the loading cylinder (2) is connected to an air pump via an electromagnetic valve group; a cylinder controller is electrically connected to the electromagnetic valve group; the welding gun (6), the pressure head (7) and the loading cylinder (2) are vertically aligned from top to bottom; The temperature collection device comprises a plurality of thermocouples (8), wherein the plurality of thermocouples (8) are arranged within a heat-affected zone on one side of a spot welding test position on the aluminum alloy test plate (5), and the plurality of thermocouples (8) are sequentially spaced from near to far relative to the spot welding test position of the aluminum alloy test plate (5).

2. The device for testing the liquefaction crack sensitivity of aluminum alloy welding according to claim 1, characterized in that: The aluminum alloy test plate (5) is connected to the side wall portion (9) via a restraining device, wherein the restraining device comprises a clamping member (4), a flange structure (11) is provided at the top of the side wall portion (9), two clamping members (4) and the flange structures (11) of the two side wall portions (9) are respectively connected up and down in a one-to-one correspondence via bolts, and the two clamping members (4) respectively clamp the two ends of the aluminum alloy test plate (5) against the upper end surfaces of the two side wall portions (9).

3. The device for testing the liquefaction crack sensitivity of aluminum alloy welding according to claim 2, characterized in that: An oblong hole (12) is provided on the flange structure (11), and the oblong hole (12) extends leftward and rightward. A circular hole is provided on the pressing member (4), and the circular hole is connected to the corresponding oblong hole (12) by bolts.

4. The device for testing the liquefaction crack sensitivity of aluminum alloy welding according to claim 1, characterized in that: The number of the thermocouples (8) is three, and the three thermocouples (8) are arranged in sequence with an interval of 0.5 mm.

5. The device for testing the liquefaction crack sensitivity of aluminum alloy welding according to claim 1, characterized in that: The base (1) is a stainless steel stand.

6. A device for testing the liquefaction crack sensitivity of aluminum alloy welding according to any one of claims 1 to 5, characterized in that: There are a plurality of pressure heads (7), the upper end surface of each pressure head (7) is a spherical surface protruding upward, the curvature radii of the upper end surfaces of the plurality of pressure heads (7) increase in sequence, and any one of the pressure heads (7) can be detachably arranged on the lifting platform (3).

7. A method for testing the liquefaction crack sensitivity of aluminum alloy welding, which is realized by relying on the device for testing the liquefaction crack sensitivity of aluminum alloy welding according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1: Select a sample with the same properties as the aluminum alloy test plate (5), use a TIG spot welding machine to spot weld the sample, and test the range of the heat affected zone formed during spot welding of the sample; Step 2: fix the aluminum alloy test plate (5) on two side wall portions (9), with the vertical foot of the welding gun (6) and the aluminum alloy test plate (5) being the spot welding test position, and set a plurality of thermocouples (8) within the heat affected zone range on one side of the spot welding test position, wherein the heat affected zone range of the aluminum alloy test plate (5) is divided according to the heat affected zone range formed by the sample plate; Step 3: Perform TIG spot welding on the aluminum alloy test plate (5), maintain the current output and inert gas output of the TIG spot welder, so that the molten pool formed by the spot welding remains stable. After the aluminum alloy test plate (5) is completely welded through, the TIG spot welder extinguishes the arc, and the loading cylinder (2) applies a load to the aluminum alloy test plate (5) by pressing the pressure head (7) upward, so that the aluminum alloy test plate (5) is forced to deform according to the shape of the arc-shaped pressure head (7); Step 4: Measure the temperature change of the heat-affected zone of the aluminum alloy test plate (5) in step 3 by using a plurality of thermocouples (8), and draw a temperature-time curve to obtain the temperature gradient G T ; Step 5: photograph the maximum crack in the heat-affected zone of the aluminum alloy test plate (5) through an optical microscope, and measure the maximum crack length MCL; Step 6: Calculate the brittle temperature range BTR of the aluminum alloy test plate (5) according to the following formula to quantitatively evaluate the welding liquefaction crack sensitivity of the aluminum alloy material: BTR=T L -MCL×G T Where, T L is the liquidus temperature; The larger the BTR value, the greater the liquefaction crack sensitivity of the aluminum alloy material.

8. The method for testing aluminum alloy welding liquefaction crack sensitivity according to claim 7, characterized in that: The T L Obtained by differential scanning calorimetry.