Friction stir welding method for carbon steel and stainless steel

Through the friction stir welding method, combined with heat treatment and optimization of welding parameters, the difficulty and quality control problems of welding stainless steel and carbon steel are solved, and high-quality and low-cost welding effects are achieved, avoiding defects in traditional welding methods.

CN119077109APending Publication Date: 2024-12-06ANSTEEL BEIJING RES INST CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411224453.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The welding of stainless steel and carbon steel is difficult to weld due to material differences, the process is complicated and the quality of welds is difficult to control. Traditional welding methods are prone to the formation of decarbonization and softening layers and carbonization hardening layers.

Method used

By using friction stir welding method, carbon steel and stainless steel are welded by heat treatment and optimization of the stirring head structure and welding parameters. The stirring head rotates and translates to generate heat and mix mechanically, avoiding the formation of martensite structure, and using tungsten carbide Stir head to reduce wear.

Benefits of technology

High-quality welded joints are achieved, with good mechanical properties, simplified welding process, reduced costs, and avoided defects in traditional welding methods, such as the formation of high brittleness and decarbonization softened layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119077109A_ABST
    Figure CN119077109A_ABST
Patent Text Reader

Abstract

The invention relates to a friction stir welding method for carbon steel and stainless steel. The method comprises the following steps: (1) carrying out heat treatment on a carbon steel plate and a stainless steel plate with the same thickness; (2) respectively milling the carbon steel plate and the stainless steel plate subjected to heat treatment to remove oxide scales on the surfaces, milling to the same thickness, and then cleaning the surfaces; (3) aligning and abutting the cleaned edges to be welded of the carbon steel plate and the stainless steel plate, and fixing the carbon steel plate and the stainless steel plate on a machine tool workbench by using a clamp; (4) welding parameters are set, and the fixed carbon steel plate and stainless steel plate are subjected to friction stir welding; the problems that the friction stir welding quality of dissimilar metal materials is poor and the welding process is complex are effectively solved, a prepared welding joint is good in quality, few in defect and good in mechanical property, and friction stir welding is easy to operate and implement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal welding, and in particular to a friction stir welding method for carbon steel and stainless steel. Background Art

[0002] In many chemical equipment, the main part needs to use stainless steel to meet the requirements of corrosion resistance or cleanliness, while some non-critical parts such as supports may use carbon steel, so the equipment manufacturing process includes the welding process of stainless steel and carbon steel. The combination of different materials not only meets the functional requirements of the equipment, but also takes cost-effectiveness into consideration, that is, using carbon steel in parts without high corrosion resistance requirements can reduce costs while ensuring the performance and durability of the equipment.

[0003] However, the welding of stainless steel and carbon steel belongs to dissimilar metal welding. Due to the significant differences in chemical composition and material properties between the two, the welding difficulty is greatly increased. In order to ensure the quality of the weld, it is often necessary to reduce welding stress and deformation through preheating and post-heating, and it is necessary to use suitable welding materials, which leads to complex processes and difficult to control weld quality.

[0004] Friction stir welding (FSW) is a friction welding method that can be used to connect aluminum alloys, copper, titanium, stainless steel and magnesium alloys. The heat generated by the rapid rotation of the stirring head and the friction with the metal is used to soften and mechanically mix the same or different metals in the welding area, and a strong connection is achieved after cooling. The friction stir welding method can improve the problems existing in the welding of carbon steel and stainless steel. On the one hand, it overcomes the problem of increased brittleness of the welded joint caused by the formation of martensitic structure. On the other hand, the temperature of the stirring zone is only 60% to 90% of the melting point of the substrate, which effectively avoids the formation of decarburization softening layer and carburization hardening layer caused by traditional tungsten inert gas arc welding and post-weld heat treatment.

[0005] The Chinese patent application with publication number CN 116275458 A discloses "a friction stir welding device, a friction stir welding method and a workpiece". The friction stir welding method is to fix two workpieces to be welded side by side on a fixture to form a weld, drive a stirring head with a pressure ring to rotate to penetrate the workpiece to a preset depth, drive the stirring head to rotate through the weld, and achieve the purpose of friction stir welding the workpiece; set a follower pressure ring to roll the welding surface and remove the flash, and the materials suitable for the workpiece are aluminum and aluminum alloys, magnesium alloys, copper and copper alloys, and titanium alloys. Compared with this method, the present invention further expands the friction stir welding method to the field of welding of dissimilar steels, and optimizes the structure and welding parameters of the stirring head.

[0006] The Chinese patent application with publication number CN 108817647 A discloses "a titanium-steel dissimilar metal structure and its preparation method", which obtains a serrated structure with high fit by stacking and overlapping, and then obtains a composite plate by meshing connection, and then achieves high-quality welding of titanium-steel dissimilar metals by stir friction welding. Compared with this method, the present invention welds stainless steel and carbon steel plates, and the welded edge does not need to be processed into a serrated structure. By using optimized stirring needles and welding parameters, the vertical edge cut by the band saw can be stir friction welded.

[0007] The Chinese patent application with publication number CN 103600167 A discloses "a method for welding carbon steel and stainless steel composite plates", in which two composite plates are machined into isosceles triangle grooves, which are then aligned and filled with welding wire, and the stirring needle applies pressure from one end of the weld and rotates to the other end. Compared with this method, the present invention does not require machining of grooves and filling of welding wire, and high-quality welds can be obtained by using appropriate welding parameters. Summary of the invention

[0008] The present invention provides a friction stir welding method for carbon steel and stainless steel, which effectively solves the problems of poor quality and complicated welding process of friction stir welding of dissimilar metal materials. The prepared welded joint has good quality, few defects and good mechanical properties. The friction stir welding operation is simple and easy to implement.

[0009] In order to achieve the above object, the present invention adopts the following technical solutions:

[0010] A friction stir welding method for carbon steel and stainless steel comprises the following steps:

[0011] (1) Heat treat carbon steel plates and stainless steel plates of the same thickness to eliminate hot-rolled structures and unify grain sizes;

[0012] (2) The heat-treated carbon steel plate and the stainless steel plate are respectively ground to remove the surface oxide scale, ground to the same thickness, and then the surface is cleaned;

[0013] (3) Align and close the cleaned carbon steel plate and the edge to be welded of the stainless steel plate, and fix them on the machine tool workbench with a clamp;

[0014] (4) Setting welding parameters to perform friction stir welding on the fixed carbon steel plate and the stainless steel plate; the welding parameters include: a stirring head rotation speed of 950 to 960 rpm, a stirring head holding time of 25 to 30 s, a stirring head translation speed of 24 to 25.5 mm / min, and a stirring head penetration depth of 0.34 to 0.355 mm.

[0015] Furthermore, the initial thickness of the carbon steel plate and the stainless steel plate is 9 to 11 mm.

[0016] Furthermore, in the step (1), the heat treatment process is as follows: the stainless steel plate is kept at 1070-1090°C for more than 90 minutes, the carbon steel plate is kept at 910-930°C for more than 15 minutes, and then cooled to room temperature in the furnace.

[0017] Furthermore, in the step (2), the thickness of the carbon steel plate and the stainless steel plate after removing the surface oxide scale is not less than 5 mm.

[0018] Furthermore, the stirring head is made of tungsten carbide.

[0019] Furthermore, the stirring head is composed of a stirring head body and a stirring needle; the stirring head body is a truncated cone structure, and the angle between the side and the bottom is less than 90°; the stirring needle is a truncated cone structure, and the large end is connected to the stirring head body.

[0020] Furthermore, the bottom diameter of the stirring head body is 16 mm, and the angle between the side and the bottom is 87°; the diameter of the large end of the stirring needle is 5 mm, and the diameter of the small end is 2 mm; the height of the stirring needle is 2 mm.

[0021] Furthermore, the friction stir welding process in step (4) is specifically as follows: the angle between the axis of the stirring head and the forward direction of the stirring head is greater than 90°; after the stirring head starts to rotate at a set rotation speed, the lower surface of the stirring head body reaches a set penetration depth below the surface to be welded, and after reaching a set holding time, the stirring head moves forward at a set translation speed, and after moving to the end point, the stirring head moves out from the surface of the steel plate.

[0022] Furthermore, the angle between the axis of the stirring head and the forward direction of the stirring head is 93°.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) It provides a simple and easy welding method. It does not require the preparation of welding interfaces of special sizes. The vertical incisions processed by the band saw can be welded. In addition, no special welding materials are required, which reduces the welding cost.

[0025] (2) The friction stir welding method was optimized, and high-quality welds were obtained by optimizing welding parameters (such as tool rotation speed, translation speed, and tool penetration depth);

[0026] (3) In conventional welding, carbon steel and austenitic steel are mixed in the weld zone, which reduces the content of austenite-forming elements such as Cr, Ni, and Ti, resulting in the formation of brittle martensite in the weld. High chromium-nickel welding rods are usually required to ensure the quality of the weld. The present invention uses a stir friction welding method to weld carbon steel and stainless steel, which can effectively refine the structure, inhibit the formation of martensite, form pearlite and fine-grained ferrite, and improve the mechanical properties of the weld.

[0027] (4) The stirring head is made of tungsten carbide with high hardness and high wear resistance, which effectively reduces the degree of wear during the welding process of dissimilar metals, reduces the cost and efficiency problems caused by frequent replacement of stirring heads, and effectively improves the weld penetration, thereby improving the quality and performance of the weld. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of friction stir welding of a 45# carbon steel plate and a 304L stainless steel plate in an embodiment of the present invention.

[0029] Figure 2 It is a schematic diagram of the setting direction of the stirring head in an embodiment of the present invention (the center line of the stirring head forms an angle of 3° with the normal line of the steel plate).

[0030] Figure 3 Schematic diagram of the structure and dimensions of a tungsten carbide stirring head in an embodiment of the present invention.

[0031] Figure 4 This is a photo of the weld structure prepared by the stir friction welding method in an embodiment of the present invention.

[0032] In the picture: 1.45# carbon steel plate 2.304L stainless steel plate DETAILED DESCRIPTION

[0033] The specific implementation of the present invention will be further described below in conjunction with the accompanying drawings:

[0034] The friction stir welding method for carbon steel and stainless steel of the present invention comprises the following steps:

[0035] (1) Heat treat carbon steel plates and stainless steel plates of the same thickness to eliminate hot-rolled structures and unify grain sizes;

[0036] (2) The heat-treated carbon steel plate and the stainless steel plate are respectively ground to remove the surface oxide scale, ground to the same thickness, and then the surface is cleaned;

[0037] (3) Align and close the cleaned carbon steel plate and the edge to be welded of the stainless steel plate, and fix them on the machine tool workbench with a clamp;

[0038] (4) Setting welding parameters, performing friction stir welding on the fixed carbon steel plate and stainless steel plate; the welding parameters include: stirring head rotation speed 950-960rpm, stirring head pressure holding time 25-30s, stirring head translation speed 24-25.5mm / min, stirring head penetration depth 0.34-0.355mm. When the rotation speed is lower than 950rpm and the stirring head translation speed is less than 24mm / min, defects such as wrinkles and gaps will appear, while if the rotation speed is too high, defects such as flash will appear.

[0039] Furthermore, the initial thickness of the carbon steel plate and the stainless steel plate is 9 to 11 mm.

[0040] Furthermore, in the step (1), the heat treatment process is as follows: the stainless steel plate is kept at 1070-1090°C for more than 90 minutes, the carbon steel plate is kept at 910-930°C for more than 15 minutes, and then cooled to room temperature in the furnace.

[0041] Furthermore, in the step (2), the thickness of the carbon steel plate and the stainless steel plate after removing the surface oxide scale is not less than 5 mm.

[0042] Furthermore, the stirring head is made of tungsten carbide.

[0043] Furthermore, the stirring head is composed of a stirring head body and a stirring needle; the stirring head body is a truncated cone structure, and the angle between the side and the bottom is less than 90°; the stirring needle is a truncated cone structure, and the large end is connected to the stirring head body.

[0044] Furthermore, the bottom diameter of the stirring head body is 16 mm, and the angle between the side and the bottom is 87°; the diameter of the large end of the stirring needle is 5 mm, and the diameter of the small end is 2 mm; the height of the stirring needle is 2 mm.

[0045] Furthermore, the friction stir welding process in step (4) is specifically as follows: the angle between the axis of the stirring head and the forward direction of the stirring head is greater than 90°; after the stirring head starts to rotate at a set rotation speed, the lower surface of the stirring head body reaches a set penetration depth below the surface to be welded, and after reaching a set holding time, the stirring head moves forward at a set translation speed, and after moving to the end point, the stirring head moves out from the surface of the steel plate, leaving only a pinhole.

[0046] Furthermore, the angle between the axis of the stirring head and the forward direction of the stirring head is 93°.

[0047] The following embodiments are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.

[0048] [Example]

[0049] In this embodiment, a 45# carbon steel plate and a 304L stainless steel plate are subjected to friction stir welding, and the specific process is as follows:

[0050] (1) Two 10 mm thick, 200 mm long, hot-rolled 45# carbon steel plates and 304L stainless steel plates were heat treated respectively; the 304L stainless steel plate was placed in a 1080°C heating furnace for 90 minutes, and the 45# carbon steel plate was placed in a 920°C heating furnace for 15 minutes, and then cooled to room temperature with the furnace.

[0051] The purpose of heat treatment is to eliminate the hot-rolled structure and obtain a recrystallized structure with similar grain size, so that the initial mechanical properties of 45# carbon steel plate and 304L stainless steel plate are similar.

[0052] (2) The heat-treated 45# carbon steel plate and 304L stainless steel plate were ground to remove the surface oxide scale and processed to the same thickness of 5 mm. Finally, acetone was used to clean the oil and impurities on the surface of the two steel plates.

[0053] (3) Align and tighten the edges of the 45# carbon steel plate and the 304L stainless steel plate to be welded, and use a clamp to fix them to the workbench of the machine tool to ensure that they do not move under the action of external forces (such as Figure 1 shown).

[0054] In this embodiment, the welding parameters of the friction stir welding are set, including: a stirring head rotation speed of 950 rpm, a stirring head pressure holding time of 25 s, a stirring head translation speed of 25 mm / min, and a stirring head penetration depth of 0.35 mm.

[0055] like Figure 3 As shown, in this embodiment, the bottom diameter of the stirring head body is 16 mm, and the angle between the side and the bottom is 87°; the diameter of the large end of the stirring needle is 5 mm, and the diameter of the small end is 2 mm; the height of the stirring needle is 2 mm.

[0056] In this embodiment, the setting angle of the stirring head is as follows: Figure 2 As shown, the angle between the central axis of the stirring head and the advancing direction is 93° (the angle between the central axis and the vertical plane is 3°).

[0057] (4) Figure 1 As shown, the stirring head is controlled to be pressed down to the surface of the steel plate in the docking area, and the stirring head is started to rotate at a speed of 950r / min. As the frictional heat is generated, the docking area of ​​the 45# carbon steel plate 1 and the 304L stainless steel plate 2 gradually turns red and melts. The stirring head is further pressed down until it penetrates 0.35mm below the surface of the steel plate. The stirring head is kept rotating for 25s, and then the stirring head moves forward at a speed of 25mm / min. After reaching the end point, the stirring head moves out from the surface of the steel plate, leaving only a pinhole.

[0058] In this embodiment, the mechanical properties of the 45# carbon steel plate, the 304L stainless steel plate and the friction stir weld are shown in Table 1.

[0059] Table 1 Mechanical properties of 45# carbon steel plate, 304L stainless steel plate and friction stir weld

[0060] project Yield strength / MPa Tensile strength / MPa Elongation / % 45# Carbon Steel Plate 275 540 23 304L stainless steel plate 287 534 55 Weld 231 639 7.2

[0061] In this embodiment, the friction stir welding effect of 45# carbon steel plate and 304L stainless steel plate is better. The prepared weld microstructure photo is as follows: Figure 4 As shown, the weld has no defects such as pores, cracks, flash, etc. The yield strength of the weld joint is close to that of the two base steels, and the tensile strength exceeds that of the two base steels.

[0062] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A friction stir welding method for carbon steel and stainless steel, It is characterized in that The following steps are involved: (1) Heat treat carbon steel plates and stainless steel plates of the same thickness to eliminate hot-rolled structures and unify grain sizes; (2) The heat-treated carbon steel plate and the stainless steel plate are respectively ground to remove the surface oxide scale, ground to the same thickness, and then the surface is cleaned; (3) Align and close the cleaned carbon steel plate and the edge to be welded of the stainless steel plate, and fix them on the machine tool workbench with a clamp; (4) Setting welding parameters to perform friction stir welding on the fixed carbon steel plate and the stainless steel plate; the welding parameters include: a stirring head rotation speed of 950 to 960 rpm, a stirring head holding time of 25 to 30 s, a stirring head translation speed of 24 to 25.5 mm / min, and a stirring head penetration depth of 0.34 to 0.355 mm.

2. A friction stir welding method for carbon steel and stainless steel according to claim 1, It is characterized in that The initial thickness of the carbon steel plate and the stainless steel plate is 9 to 11 mm.

3. The friction stir welding method for carbon steel and stainless steel according to claim 1, It is characterized in that In the step (1), the heat treatment process is as follows: the stainless steel plate is kept at 1070-1090°C for more than 90 minutes, the carbon steel plate is kept at 910-930°C for more than 15 minutes, and then cooled to room temperature in the furnace.

4. The friction stir welding method for carbon steel and stainless steel according to claim 1, It is characterized in that In the step (2), the thickness of the carbon steel plate and the stainless steel plate after removing the surface oxide scale is not less than 5 mm.

5. The friction stir welding method for carbon steel and stainless steel according to claim 1, It is characterized in that The stirring head is made of tungsten carbide.

6. The friction stir welding method for carbon steel and stainless steel according to claim 1, It is characterized in that The stirring head is composed of a stirring head body and a stirring needle; the stirring head body is a truncated cone structure, and the angle between the side and the bottom is less than 90°; the stirring needle is a truncated cone structure, and the large end is connected to the stirring head body.

7. A friction stir welding method for carbon steel and stainless steel according to claim 6, It is characterized in that The bottom diameter of the stirring head body is 16 mm, and the angle between the side and the bottom is 87°; the diameter of the large end of the stirring needle is 5 mm, and the diameter of the small end is 2 mm; the height of the stirring needle is 2 mm.

8. The friction stir welding method for carbon steel and stainless steel according to claim 1, It is characterized in that The friction stir welding process in step (4) is specifically as follows: the angle between the axis of the stirring head and the forward direction of the stirring head is greater than 90°; after the stirring head starts to rotate at a set rotation speed, the lower surface of the stirring head body reaches a set penetration depth below the surface to be welded, and after reaching a set holding time, the stirring head moves forward at a set translation speed, and after moving to the end point, the stirring head moves out from the surface of the steel plate.

9. A friction stir welding method for carbon steel and stainless steel according to claim 8, It is characterized in that The angle between the axis of the stirring head and the advancing direction of the stirring head is 93°.

Citation Information

Cited By

  • Laser stirring friction composite welding method for stainless steel special-shaped part

    CN120170236A