Hollow O-shaped rubber sealing ring forming method supported by liquid gasification

By injecting volatile liquid during the vulcanization process of hollow O-shaped rubber sealing rings to generate internal air pressure support, the problem of air pressure uneven caused by chemical reaction instability is solved, the product shape stability and safety is improved, and production is reduced Cost and process difficulty.

CN119078078APending Publication Date: 2024-12-06NORTHWEST RUBBER & PLASTIC RES & DESIGN INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411366817.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the existing hollow O-shaped rubber sealing ring molding process, chemical reactions are unstable, resulting in uneven internal air pressure, and there may be high-pressure gas residues, affecting product quality and safety.

Method used

The molding method of liquid gasification support is adopted. By injecting volatile liquids such as ethanol or methanol during the vulcanization process, it is heated and vaporized to generate internal air pressure support to ensure the stability of the product shape and condense into liquid after cooling to avoid high-pressure gas. Remaining.

Benefits of technology

It realizes controllability and stability of internal air pressure, reduces product defects and burst risks, improves production efficiency, product safety and sealing performance, and reduces production costs and process difficulty.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119078078A_ABST
    Figure CN119078078A_ABST
Patent Text Reader

Abstract

The invention provides a method for forming a hollow O-shaped rubber sealing ring supported by liquid gasification, which comprises the following steps of: preparing a rubber material into a rubber sheet with a preset thickness, and cutting the rubber sheet into a rubber strip; respectively putting rubber strips into a forming lower mold cavity and a forming upper mold cavity of the forming mold, closing the corresponding shaping mold, and performing pre-shaping to form a lower mold rubber part and an upper mold rubber part; opening the mold, and injecting volatile liquid into the cavity of the rubber part of the lower mold; roughening and gluing the joint surfaces of the rubber parts of the upper die and the lower die; and closing the upper die and the lower die, and pressurizing and vulcanizing in a press vulcanizer. In the vulcanization process, the volatilizable liquid is heated and gasified, and internal air pressure is generated to support the hollow inner wall. After vulcanization is finished, the sealing ring is taken out and placed in a cooling medium to be cooled, the gasified volatile liquid is condensed into liquid, and no high-pressure gas exists in the product. The method is easy and convenient to operate, the technological process is controllable, and the method is suitable for forming the hollow O-shaped rubber sealing rings with different sizes and section shapes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rubber molding, and in particular relates to a method for molding a hollow O-shaped rubber sealing ring supported by liquid gasification. Background Art

[0002] O-rings are widely used as sealing elements and are usually solid. However, hollow O-rings are limited in application due to their complex manufacturing process and difficulty in molding. Hollow-structured sealing rings are more easily deformed under external forces and have good elasticity. They can perform excellent performance in terms of buffering, shock absorption and sealing, meeting the functional requirements under specific working conditions.

[0003] At present, the preparation method of hollow O-shaped rubber sealing rings in China is mainly to add ammonium bicarbonate or sodium bicarbonate and other substances to the hollow part in advance during the vulcanization molding process. These substances are decomposed by heat during the vulcanization temperature rise process to produce high-pressure gases such as ammonia, carbon dioxide and water vapor, which support the inner wall of the hollow part, prevent the product from deforming during the vulcanization process, and make the finished product smooth and without collapse.

[0004] However, this approach has the following problems:

[0005] Reaction instability: The decomposition ratio of chemical substances is difficult to control accurately. Some substances may not react completely, resulting in unstable air pressure inside the product, affecting the stability of product quality.

[0006] The reaction process is difficult to control: During the vulcanization process, the outer wall of the product has undergone vulcanization cross-linking, while the internal chemical reaction may lag behind, resulting in insufficient internal air pressure and inability to effectively support the inner wall, ultimately leading to product appearance defects.

[0007] Residual high-pressure gas inside: Due to the irreversibility of chemical reactions, there is still gas pressure inside the product after vulcanization. This may cause the cross-sectional dimensions of the product to be unstable, and there is a risk of bursting during installation and pressure use, and the expected use effect cannot be achieved.

[0008] Therefore, the prior art has many deficiencies in the molding process of the hollow O-shaped rubber sealing ring, and a new process method is urgently needed to solve the above problems and improve the quality and performance of the product. Summary of the invention

[0009] The invention provides a method for forming a hollow O-shaped rubber sealing ring supported by liquid gasification, which solves the problems of unstable internal supporting air pressure, poor product quality and potential safety hazards caused by residual high-pressure gas in the hollow rubber products in the prior art.

[0010] In order to achieve the above object, the technical solution of the present invention is as follows:

[0011] The hollow O-shaped rubber sealing ring molding method using liquid gasification support comprises the following steps:

[0012] The rubber material is prepared into a film with a predetermined thickness, and cut into rubber strips;

[0013] The rubber strip is placed in the lower molding cavity of the molding mold, and the upper molding mold of the molding mold is closed to perform pre-molding to form the rubber part of the lower mold;

[0014] The rubber strip is placed in the upper molding cavity of the molding mold, and the lower molding mold of the molding mold is closed to perform pre-molding to form the upper mold rubber part;

[0015] The mold is opened, and a volatile liquid is injected into the cavity of the rubber part of the lower mold of the molding mold;

[0016] The upper mold with the upper mold rubber part and the lower mold with the lower mold rubber part are molded together and placed in a flat vulcanizer for pressurized vulcanization. The volatile liquid is heated and vaporized during the vulcanization process, generating internal air pressure to support the hollow inner wall of the O-shaped rubber sealing ring;

[0017] After the vulcanization is completed, the molding mold is opened to take out the O-shaped rubber sealing ring, and the product is placed in a cooling medium to cool down so that the vaporized volatile liquid condenses into a liquid state, and there is no high-pressure gas inside the O-shaped rubber sealing ring.

[0018] Furthermore, it is characterized in that the boiling point of the volatile liquid is lower than the vulcanization temperature.

[0019] Furthermore, the volatile liquid is ethanol, methanol or ether.

[0020] Furthermore, the volume of the injected volatile liquid is calculated and determined by the following formula:

[0021]

[0022] Where V 液 : The volume of volatile liquid to be injected, in milliliters (mL);

[0023] P: The internal pressure required at the vulcanization temperature, in Pascals (Pa);

[0024] V: the internal volume of the hollow part of the O-ring, in milliliters (mL);

[0025] M: molar mass of the volatile liquid in grams per mole (g / mol);

[0026] R: gas constant, R = 8.314 J / (mol·K);

[0027] T: vulcanization temperature, in degrees Celsius (℃);

[0028] ρ: Density of volatile liquid in grams per milliliter (g / mL).

[0029] Furthermore, the volatile liquid is a mixed solvent composed of at least two volatile liquids with different boiling points, so as to achieve gradient control of the internal gas pressure during the vulcanization process.

[0030] Furthermore, the vulcanization temperature is 140°C to 180°C.

[0031] Furthermore, the thickness of the film is 8 mm to 8.5 mm, the length of the rubber strip is 1.015 times to 1.025 times the inner circumference of the product, and the width is 96% to 97% of the outer diameter of the product cross section.

[0032] Furthermore, the joint surfaces of the upper mold rubber part and the lower mold rubber part are subjected to surface treatment, wherein the surface treatment includes roughening and gluing.

[0033] Furthermore, the molding die comprises an upper molding die and a lower molding die, and the upper molding die and the lower molding die are respectively provided with semicircular grooves, and after the molds are closed, an annular cavity for molding an O-shaped rubber sealing ring is formed;

[0034] The shaping mold comprises a corresponding shaping upper mold and a shaping lower mold, wherein the shaping upper mold and the shaping lower mold are respectively provided with semicircular bosses corresponding to the forming mold for pre-shaping the rubber strip to form an upper mold rubber part and a lower mold rubber part.

[0035] Furthermore, the parting surfaces of the forming mold and the shaping mold are provided with chamfered smooth transition and conical surface positioning structures. Compared with the prior art, the beneficial effects of the present invention are as follows:

[0036] The present invention injects a volatile liquid during the vulcanization process and utilizes the internal air pressure support generated by the heated gasification to avoid uneven air pressure caused by unstable chemical reactions, thereby ensuring the size and shape stability of the product during the vulcanization process. The physical gasification and condensation process of the volatile liquid is reversible and controllable. Compared with irreversible chemical reactions, it is easier to control the internal air pressure during the vulcanization process, reduce product defects, and improve production efficiency. After the vulcanization is completed, the gaseous volatile liquid inside the product condenses into a liquid during the cooling process, and there is no residual high-pressure gas inside, which avoids the unstable product size caused by the internal air pressure and the risk of bursting during use, thereby improving the safety of the product. Using common volatile liquids such as ethanol, methanol or ether, there is no need for complex chemical additives and reaction control, the operation is simple and convenient, and the production cost and process difficulty are reduced. The selected volatile liquid is non-toxic and harmless, friendly to human health and the environment, meets environmental protection requirements, and reduces the health risks to production personnel. The structural design of the molding mold and the shaping mold is reasonable, and the chamfered smooth transition and conical positioning structure are adopted to avoid damage to the mold and the product during operation, extend the service life of the mold, and improve the dimensional accuracy and quality consistency of the product. This method is suitable for the molding of hollow O-shaped rubber sealing rings of different sizes and cross-sectional shapes, meeting diverse application needs and broadening the application range of the product. Since the process is controllable, the product defect rate and rework rate are reduced, the production efficiency is improved, and it has significant economic benefits. The volatile liquid used is a common industrial solvent, which is easy to obtain and low in cost, further reducing the production cost. By optimizing the internal support during the vulcanization process, the density and mechanical properties of the rubber sealing ring are improved, the cushioning, shock absorption and sealing effects of the product are enhanced, and the service life of the product is extended.

[0037] Of course, the implementation of the various technical solutions of the present invention does not necessarily require achieving all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, drawings of other embodiments can be obtained based on these drawings without paying creative work.

[0039] Figure 1 This is a schematic structural diagram of a hollow O-shaped rubber sealing ring according to Embodiment 1 of the present invention;

[0040] Figure 2 for Figure 1 AA side section view;

[0041] Figure 3It is a schematic diagram of the cooperation between the shaping upper die and the forming lower die;

[0042] Figure 4 It is a schematic diagram of the cooperation between the forming upper die and the shaping lower die;

[0043] Figure 5 It is a schematic diagram of the cooperation between the upper forming die and the lower forming die;

[0044] Figure 6 The overall structure and cross-sectional structure photos of the O-shaped rubber sealing ring finally obtained in Example 1 of the present invention;

[0045] Figure 7 This is a flow chart of the preparation method of Example 1 of the present invention.

[0046] In the figure, 101 is a molding upper mold, 102 is a molding lower mold, 201 is a molding upper mold, and 202 is a molding lower mold. DETAILED DESCRIPTION

[0047] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0048] In the description of this patent, it should be understood that the terms "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing this patent and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on this patent.

[0049] In the description of this patent, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", and "set" should be understood in a broad sense, for example, it can be fixedly connected, set, or detachably connected, set, or integrally connected, set. For ordinary technicians in this field, the specific meanings of the above terms in this patent can be understood according to specific circumstances. The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.

[0050] Embodiment 1:

[0051] In order to better illustrate the molding method of the present invention, a manufacturing example of a hollow O-shaped rubber sealing ring is given below in combination with specific data and formulas.

[0052] See also Figure 1 and Figure 2 The hollow O-shaped rubber sealing ring in this embodiment is a perfect circular structure, and the hollow cross section is a perfect circle. The product specifications are as follows:

[0053] Product inner diameter: D 内 : 300mm;

[0054] Product section outer diameter: d 外 : 25mm;

[0055] Product section inner diameter: d 内 : 12mm;

[0056] A method for forming a hollow O-shaped rubber sealing ring using liquid gasification support, see Figure 7 , including the following steps:

[0057] Step 1: Preparation of adhesive strips:

[0058] Sheet thickness: The rubber material is rolled on an open mixing mill into a sheet with a thickness of 8.2 mm.

[0059] Strip cutting:

[0060] Length: L = πD 内 ×1.02=π×300mm×1.02≈961mm.

[0061] Width: 96% of the outer diameter of the product section, i.e. W = d 外 ×0.96=25mm×0.96=24mm.

[0062] Step 2: Pre-order:

[0063] Lower mold rubber part:

[0064] Place the cut rubber strips into the lower molding cavity of the molding mold.

[0065] Close the upper mold of the molding mold and apply slight pressure to spread the rubber strip evenly in the mold cavity for pre-molding to form the rubber part of the lower mold.

[0066] Upper mold rubber part:

[0067] Repeat the above steps and place another rubber strip into the upper molding cavity of the molding mold.

[0068] The lower molding die of the molding die is closed to perform pre-molding to form the rubber part of the upper mold.

[0069] Step 3: Calculate the amount of volatile liquid injected:

[0070] Set the internal air pressure P: To meet the support requirements during the vulcanization process, the internal air pressure is set to 0.6MPa (600000Pa).

[0071] Calculate the volume V of the hollow part:

[0072] Hollow area of ​​cross section A:

[0073]

[0074] Inner circumference of sealing ring L 内 :

[0075] L 内 =πD 内 =π×300=mm≈942=mm

[0076] Hollow part volume V:

[0077] V=A×L 内 =113.1=mm 2 ×942=mm≈106611=mm 3

[0078] Convert to milliliters (1mL = 1000mm 3 ):

[0079] V=106611mm 3 / 1000=106.6mL

[0080] Volatile liquid selection: Ethanol is used, and its physical properties are as follows:

[0081] Molar mass M: 46.07 g / mol

[0082] Density ρ: 0.789 g / mL

[0083] Gas constant R: 8.314 J / (mol·K)

[0084] Vulcanization temperature T: 160℃

[0085] Calculate the volume of ethanol V to be injected 液 :

[0086]

[0087] Substitute the data into:

[0088]

[0089] Unit conversion and calculations:

[0090] Keep the volume V in milliliters (mL), but convert the pressure units from Pascals (Pa) to standard atmospheres (atm) or adjust the units in the formula for consistency. For simplicity, it is necessary to unify the units to the International System of Units (SI).

[0091] Convert volume V to cubic meters (1m 3 =1000000mL):

[0092] V = 106.6 mL = 106.6 × 10 -6 m 3

[0093] Convert molar mass M to kilograms per mole (kg / mol):

[0094] M=46.07g / mol=0.04607kg / mol

[0095] Convert density ρ to kilograms per cubic meter (kg / m):

[0096] ρ=0.789g / mL=789kg / m 3

[0097] Calculate the numerator: numerator = P × V × M

[0098] =600000Pa×106.6×10 -6 m 3 ×0.04607kg / mol≈2.946kg\cdotpm 2 / (mol\cdotps 2 )

[0099] Calculate the denominator: Numerator = R × T K ×ρ

[0100] =8.314J / (mol\cdotpK)×433.15K×789kg / m 3 ≈2846009kg\cdotpm 2 / (mol\cdotps 2 )

[0101] Calculate V fluid:

[0102] V 液 = denominator / numerator = 2946 / 2846009≈1.035×10 -6 m 3

[0103] Convert to milliliters (1m 3 =1000000mL):

[0104] V液 =1.035×10 -6 m 3 ×1000000=1.035mL

[0105] Actual injection volume: Taking into account the losses and safety margins during operation, the actual injected ethanol volume is set at 1.1 mL.

[0106] Step 4: Inject volatile liquid:

[0107] Using a precision syringe, inject 1.1 mL of ethanol into the cavity of the rubber portion of the lower mold of the molding die.

[0108] After the injection is completed, proceed to the next step quickly to prevent ethanol from evaporating.

[0109] Step 5: Mold vulcanization:

[0110] The upper mold with the upper mold rubber part and the lower mold with the lower mold rubber part are molded together to ensure that the molds are tightly fitted without gaps.

[0111] The mold was placed in a flat vulcanizer, and the vulcanization temperature was set to 160°C, the pressure to 15 MPa, and the vulcanization time to 20 minutes.

[0112] During the vulcanization process, ethanol vaporizes due to heat, and the internal air pressure rises to about 0.6MPa, which effectively supports the hollow inner wall and prevents the product from collapsing or deforming.

[0113] Before closing the mold, the joint surface of the upper mold rubber part and the lower mold rubber part is treated to enhance the fusion of the two parts during the vulcanization process and ensure the overall strength of the product. The specific steps are as follows:

[0114] Roughening: Use fine sandpaper or grinding tools to roughen the joint surface of the upper mold rubber part and the lower mold rubber part to make the surface slightly rough, increase the contact area, and facilitate bonding.

[0115] Glue coating: Apply a layer of adhesive (such as vulcanized rubber or rubber adhesive) that is compatible with the rubber material evenly on the roughened joint surface. The glue coating should be thin and even to avoid excessive thickness that may cause the rubber to overflow during vulcanization.

[0116] After the surface treatment is completed, the upper mold with the upper mold rubber part and the lower mold with the lower mold rubber part are immediately aligned and closed to ensure that the molds are tightly fitted without gaps. When closing the molds, the conical surface positioning structure and chamfer design ensure the accurate alignment and sealing of the molds.

[0117] At the same time, under high temperature and high pressure, the coated adhesive undergoes a cross-linking reaction with the rubber matrix to form a strong bond, ensuring the overall strength and sealing performance of the product.

[0118] Step 6: Cooling and demoulding:

[0119] After vulcanization is completed, take out the mold and place it at room temperature to cool slightly.

[0120] Open the molding mold and take out the vulcanized O-shaped rubber sealing ring.

[0121] The product was immediately cooled in water at 20°C, ensuring that the internal temperature quickly dropped below the boiling point of ethanol (78.3°C).

[0122] As the temperature drops, the gaseous ethanol condenses into liquid, the internal air pressure returns to normal pressure, and the product size stabilizes. Finally, the internal liquid is not discharged, but remains in the hollow O-ring rubber seal in liquid form.

[0123] The following are the causes and effects of not designing to drain internal liquids:

[0124] The liquid volume is very small: Since the amount of volatile liquid initially injected is very small, the volume of the condensed liquid accounts for less than 2% of the total volume of the hollow part, and the effect on the size and shape of the product can be ignored.

[0125] Sealed environment: The structure of the hollow O-ring forms a closed space inside, in which the liquid volatile liquid is sealed without the need for additional discharge steps.

[0126] Non-toxic and harmless: The volatile liquids (such as ethanol, methanol or ether) selected will not have adverse effects on the product and the user in small doses. They are all commonly used industrial solvents and will not come into contact with the outside world in a sealed environment.

[0127] No impact on performance: The residual liquid volatile liquid inside will not have a negative impact on the elasticity, strength and sealing performance of the product. Due to its extremely small proportion, the performance of the product remains stable when it is compressed and deformed.

[0128] No additional treatment is required: If you try to drain the internal liquid, you may need to make holes in the product or perform other treatments, which will damage the integrity and sealing performance of the product. Therefore, keeping the liquid inside is the best option.

[0129] Step 7: Product Inspection:

[0130] Appearance inspection: The product surface is smooth, without defects such as bubbles, collapse, pitting, etc.

[0131] Dimension measurement: Use precision measuring tools to measure the inner diameter, outer diameter and cross-sectional dimensions of the product, all of which meet the design requirements.

[0132] Performance test: Test the sealing performance, elasticity, hardness, etc. The product performance meets the use requirements, see Figure 6The overall structure and cross-sectional structure of the finally obtained O-shaped rubber sealing ring are shown in the figure.

[0133] See also Figure 3-Figure 5 , Figure 3 It is a schematic diagram of the cooperation between the shaping upper die and the forming lower die, which is used to initially form the rubber part of the lower die; Figure 4 It is a schematic diagram of the cooperation between the forming upper die and the shaping lower die, which are used to initially form the rubber part of the upper die; Figure 5 This is a schematic diagram of the coordination between the upper molding die and the lower molding die, which are used for the final vulcanization molding of the product.

[0134] Specifically, in this embodiment, the forming mold and the shaping mold are used in conjunction with each other, and the forming mold is composed of a forming upper mold 101 and a forming lower mold 102. Semicircular grooves are respectively provided on the inner sides of the forming upper mold 101 and the forming lower mold 102, and the size and shape of the grooves match the cross-section of the hollow O-shaped rubber sealing ring to be formed. After the molds are closed, the semicircular grooves of the forming upper mold 101 and the forming lower mold 102 jointly form an annular cavity for the final vulcanization molding. The parting surface of the mold is designed with a chamfered smooth transition and a conical positioning structure to ensure that the upper and lower molds are accurately aligned when the molds are closed, prevent the rubber from overflowing, and improve the dimensional accuracy and appearance quality of the product.

[0135] The shaping mold is composed of a shaping upper mold 201 and a shaping lower mold 202. Different from the forming mold, the shaping upper mold 201 and the shaping lower mold 202 of the shaping mold 201 are respectively provided with semicircular bosses, and the size of the bosses corresponds to the semicircular groove of the forming mold. The function of the shaping mold is to pre-shape the rubber strip before vulcanization, so that it initially forms the upper mold rubber part and the lower mold rubber part, which is convenient for subsequent mold closing and vulcanization.

[0136] Embodiment 2:

[0137] In this embodiment, in order to achieve gradient control of the internal gas pressure during the vulcanization process, a mixed solvent consisting of two volatile liquids with different boiling points is used.

[0138] Volatile liquid options:

[0139] Methanol:

[0140] Boiling point: 64.7°C

[0141] Molar mass: 32.04 g / mol

[0142] Density: 0.7918 g / mL

[0143] Ethanol:

[0144] Boiling point: 78.3°C

[0145] Molar mass: 46.07 g / mol

[0146] Density: 0.789 g / mL

[0147] Mixed solvent ratio:

[0148] Methanol and ethanol were mixed in a volume ratio of 1:1 to form a mixed solvent with a total volume of 1.6 mL, including 0.8 mL of methanol and 0.8 mL of ethanol.

[0149] Gas pressure gradient control during vulcanization:

[0150] Stage 1 (64.7℃-78.3℃):

[0151] Methanol is first vaporized by heat, and when the temperature reaches 64.7°C, it begins to generate internal air pressure, providing initial support for the hollow inner wall and preventing the rubber product from collapsing and deforming in the early stages of vulcanization.

[0152] Stage 2 (78.3℃-160℃):

[0153] The ethanol is then vaporized by heat, and when the temperature reaches 78.3°C, the internal gas pressure further increases to about 0.6MPa, fully supporting the inner wall and ensuring the stability of the product shape.

[0154] This embodiment achieves gradient control of the internal air pressure during the vulcanization process by using a mixed solvent composed of methanol and ethanol, matching the physical property changes of the rubber material during the vulcanization process. In the early stage, methanol vaporizes at a lower temperature, producing a lower internal air pressure, avoiding excessive pressure on the rubber that is not fully cross-linked, and reducing product defects and internal stress; in the later stage, ethanol vaporizes at a higher temperature, and the internal air pressure is further increased, ensuring sufficient support for the inner wall and improving the dimensional accuracy and mechanical properties of the product. Combined with quality control measures such as precise proportioning of mixed solvents, temperature and pressure monitoring, and mold sealing inspection, the stability and consistency of product quality are ensured, providing a reliable technical solution for the production of high-quality hollow O-shaped rubber sealing rings.

[0155] The above specific examples are used to illustrate the present invention, which is only used to help understand the present invention and is not intended to limit the present invention. For those skilled in the art, according to the concept of the present invention, some simple deductions, modifications or substitutions can be made.

Claims

1. A method for forming a hollow O-shaped rubber sealing ring supported by liquid gasification, characterized in that: The following steps are involved: The rubber material is prepared into a film with a predetermined thickness, and cut into rubber strips; The rubber strip is placed in the lower molding cavity of the molding mold, and the upper molding mold of the molding mold is closed to perform pre-molding to form the rubber part of the lower mold; The rubber strip is placed in the upper molding cavity of the molding mold, and the lower molding mold of the molding mold is closed to perform pre-molding to form the upper mold rubber part; The mold is opened, and a volatile liquid is injected into the cavity of the rubber part of the lower mold of the molding mold; The upper mold with the upper mold rubber part and the lower mold with the lower mold rubber part are molded together and placed in a flat vulcanizer for pressurized vulcanization. The volatile liquid is heated and vaporized during the vulcanization process, generating internal air pressure to support the hollow inner wall of the O-shaped rubber sealing ring; After the vulcanization is completed, the molding mold is opened to take out the O-shaped rubber sealing ring, and the product is placed in a cooling medium to cool down so that the vaporized volatile liquid condenses into a liquid state, and there is no high-pressure gas inside the O-shaped rubber sealing ring.

2. The method for forming a hollow O-shaped rubber sealing ring using liquid gasification support according to claim 1, characterized in that: The volatile liquid has a boiling point below the vulcanization temperature.

3. The method for forming a hollow O-shaped rubber sealing ring using liquid gasification support according to claim 2, characterized in that: The volatile liquid is ethanol, methanol or ether.

4. The method for forming a hollow O-shaped rubber sealing ring using liquid gasification support according to claim 1, characterized in that: The volume of the injected volatile liquid is determined by the following formula: Where V 液 : The volume of volatile liquid to be injected, in milliliters (mL); P: The internal pressure required at the vulcanization temperature, in Pascals (Pa); V: the internal volume of the hollow part of the O-ring, in milliliters (mL); M: molar mass of the volatile liquid in grams per mole (g / mol); R: gas constant, R = 8.314 J / (mol·K); T: vulcanization temperature, in degrees Celsius (℃); ρ: Density of volatile liquid in grams per milliliter (g / mL).

5. The method for forming a hollow O-shaped rubber sealing ring using liquid gasification support according to claim 1, characterized in that: The volatile liquid is a mixed solvent, which is composed of at least two volatile liquids with different boiling points, so as to realize the gradient control of the internal gas pressure during the vulcanization process.

6. The method for forming a hollow O-shaped rubber sealing ring using liquid gasification support according to claim 1, characterized in that: The vulcanization temperature is 140°C to 180°C.

7. The method for forming a hollow O-shaped rubber sealing ring using liquid gasification support according to claim 1, characterized in that: The thickness of the film is 8mm to 8.5mm, the length of the rubber strip is 1.015 times to 1.025 times the inner circumference of the product, and the width is 96% to 97% of the outer diameter of the product cross section.

8. According to the method for forming a hollow O-shaped rubber sealing ring using liquid gasification support as described in claim 1, before pressurized vulcanization, the joint surface of the upper mold rubber part and the lower mold rubber part is surface treated, and the surface treatment includes roughening and gluing.

9. The method for forming a hollow O-shaped rubber sealing ring using liquid gasification support according to claim 1, characterized in that: The molding die comprises an upper molding die and a lower molding die, wherein the upper molding die and the lower molding die are respectively provided with semicircular grooves, and an annular cavity for molding an O-shaped rubber sealing ring is formed after the molds are closed; The shaping mold comprises a corresponding shaping upper mold and a shaping lower mold, wherein the shaping upper mold and the shaping lower mold are respectively provided with semicircular bosses corresponding to the forming mold for pre-shaping the rubber strip to form an upper mold rubber part and a lower mold rubber part.