Cinnamomum camphora leaf-based hard carbon negative electrode material and preparation method and application thereof

Through a simplified process, camphor leaf-based hard carbon anode material is prepared, which solves the problems of complex and high cost of preparation of sodium ion battery anode material, achieves high specific capacity and cycle stability of the material, and reduces environmental pollution. .

CN119079975APending Publication Date: 2024-12-06ZHONGHE TIANCHENG TECH DEV (BEIJING) CO LTD

Patent Information

Application Number
CN202411205389.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The preparation process of existing sodium ion battery negative electrode materials is complex and costly, and it fails to effectively utilize camphor leaf resources, which has environmental pollution problems.

Method used

Camphor leaves are prepared by drying, crushing, heating to 1400°C and insulated under nitrogen protection, and then immersing in hydrochloric acid to treat, which simplifies the process and reduces production costs.

Benefits of technology

The prepared camphor leaf-based hard carbon anode material has excellent specific capacity and cycle stability, which solves the environmental pollution problem and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079975A_ABST
    Figure CN119079975A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a hard carbon negative electrode material, which comprises the following steps: 1) drying and crushing camphor tree leaves extracted from camphor tree oil to obtain a powder material; 2) heating the powder material to 1400 DEG C under the protection of nitrogen or inert gas, and preserving heat for more than 2 hours to obtain a pyrolytic carbon material; and 3) soaking the pyrolytic carbon material in hydrochloric acid for more than 12 hours, then washing to be neutral, and drying to obtain the camphor tree leaf-based hard carbon negative electrode material. The camphor tree leaf-based hard carbon negative electrode material provided by the invention has relatively good specific capacity and excellent cycle stability, the preparation method is simple and low in cost, and the problem of environmental pollution existing in the raw materials is also solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hard carbon negative electrode material, in particular to a camphor leaf-based hard carbon negative electrode material for a sodium ion battery. Background Art

[0002] The basic structure of sodium-ion batteries is similar to that of lithium batteries, including positive electrodes, electrolytes, separators, negative electrodes, and shells. The working principle of sodium-ion batteries is also similar to that of lithium batteries. Its reversible charge and discharge is achieved through the migration of sodium ions between the positive and negative electrodes. It is also a "rocking chair" battery.

[0003] The negative electrode material of sodium ion battery does not provide a source of sodium ions, but plays the role of carrying / releasing sodium ions from the positive electrode. The reported negative electrode materials of sodium ion batteries are mainly carbon-based, titanium-based, organic, alloy and other materials.

[0004] Camphor leaves generate a large amount of waste after extracting camphor oil, which is currently mainly treated by incineration, which not only fails to fully utilize the waste, but also causes environmental pollution. There is no report on the use of camphor leaves to prepare hard carbon negative electrode materials for sodium ion batteries in this field. In addition, the preparation process of biomass-based hard carbon negative electrode materials in this field generally has the problem of being too complicated and having high production costs. Summary of the invention

[0005] In one aspect, the present invention provides a method for preparing a hard carbon negative electrode material, comprising:

[0006] 1) drying and crushing the camphor leaves extracted with camphor oil to obtain a powder material;

[0007] 2) heating the powder material to 1400° C. under nitrogen or inert gas protection and then keeping the temperature for more than 2 hours to obtain a pyrolytic carbon material; and

[0008] 3) Soaking the pyrolytic carbon material in hydrochloric acid for more than 12 hours, then washing with water until neutral, and drying to obtain a camphor leaf-based hard carbon negative electrode material.

[0009] In some embodiments, the camphor oil is extracted by steam distillation.

[0010] In some embodiments, the camphor oil is extracted by steam distillation over water.

[0011] In some embodiments, step 1) further comprises crushing the camphor tree leaves and passing them through a 300-mesh sieve.

[0012] In some embodiments, the concentration of the hydrochloric acid is 1 mol / L.

[0013] In some embodiments, the camphor tree leaf is a Cinnamomum camphora leaf.

[0014] In another aspect, the present invention provides a hard carbon negative electrode material prepared by the above method.

[0015] On the other hand, the present invention provides the use of the above-mentioned hard carbon negative electrode material in the preparation of sodium ion batteries.

[0016] The camphor leaf-based hard carbon negative electrode material provided by the invention has good specific capacity and excellent cycle stability, and the preparation method is simple and low in cost, and also solves the environmental pollution problem existing in the raw materials themselves. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a SEM image of the camphor leaf-based hard carbon negative electrode material HC-1400 prepared in the present invention.

[0018] Figure 2 This is the XRD spectrum of the camphor leaf-based hard carbon negative electrode material HC-1400 prepared in the present invention.

[0019] Figure 3 The first cycle charge and discharge curve of the camphor leaf-based hard carbon negative electrode material HC-1400 prepared in the present invention is shown.

[0020] Figure 4 The rate performance curve of the camphor leaf-based hard carbon negative electrode material HC-1400 prepared by the present invention is shown.

[0021] Figure 5 The cycle performance of the camphor leaf-based hard carbon negative electrode material HC-1400 prepared by the present invention is shown. DETAILED DESCRIPTION

[0022] Unless defined otherwise, all technical and scientific terms used herein have the same meanings as commonly understood by one of ordinary skill in the art.

[0023] Herein, the term "comprising" generally means including the elements explicitly specified but not excluding other elements, and also includes the case consisting of these elements.

[0024] In this document, the term "above" includes the number, for example, 12 hours or more refers to 13 hours, 14 hours, 15 hours or more, also including 12 hours.

[0025] The present invention provides a method for preparing a camphor leaf-based hard carbon negative electrode material by one-step pyrolysis. Compared with the existing method for preparing a biomass hard carbon negative electrode material, the preparation method of the present invention is simple and only requires one heating process. In addition, the method of the present invention is particularly suitable for camphor leaves from which camphor oil has been extracted by water steam distillation (i.e., the camphor leaves are not immersed in water during the distillation process). Not only is the production cost low, but it also solves the problem that camphor leaf waste is difficult to handle.

[0026] The present invention is further illustrated by the following specific examples.

[0027] Example 1 Preparation of camphor leaf-based hard carbon material

[0028] Camphor tree oil is extracted (using water steam distillation method) from camphor tree leaves (from Cinnamomum camphora) as raw material, and then dried, crushed and sieved through a 300-mesh sieve to obtain a powder material, which is then directly heated to 1400°C under nitrogen (or inert gas) protection and kept warm for 2 hours. The carbon material obtained after pyrolysis is immersed in 1 mol / L hydrochloric acid for 12 hours, then washed with water until neutral, and dried to obtain a camphor tree leaf-based hard carbon material (HC-1400).

[0029] Example 2 Preparation of camphor leaf-based hard carbon material (Comparative Example)

[0030] The camphor leaf-based hard carbon material was prepared according to the method of Example 1, except that the camphor leaves were used to extract camphor oil by steam distillation in water.

[0031] Example 3 Preparation of camphor leaf-based hard carbon material (Comparative Example)

[0032] The camphor leaf-based hard carbon material was prepared according to the method of Example 1, except that the camphor leaves used were used to extract camphor oil by a solvent (ethanol or petroleum ether) extraction method.

[0033] Example 4 Preparation of camphor leaf-based hard carbon material (Comparative Example)

[0034] The camphor leaf-based hard carbon material was prepared according to the method of Example 1, except that the camphor leaves used were not subjected to camphor oil extraction.

[0035] Example 5 Electrical Performance Comparison

[0036] The camphor leaf-based hard carbon material prepared in Example 1-4 was used to prepare the negative electrode sheet, and the metal sodium sheet was used as the counter electrode to prepare the half-cell, and the first reversible specific capacity was tested. The results are listed in Table 1.

[0037] Table 1 Electrical performance test results

[0038]

[0039] From the results in Table 1, it can be seen that the hard carbon negative electrode material prepared from camphor leaves without extracting camphor oil (Example 4) has the worst effect, and the hard carbon negative electrode material prepared from camphor leaves with camphor oil extracted by water steam distillation (Example 1) has the best effect. It is speculated that the camphor oil extraction process can just form sodium storage sites, which can effectively improve the sodium storage capacity of the prepared hard carbon negative electrode material, among which the sodium storage sites formed by water steam distillation are the largest in number and density. At present, water steam distillation is widely used for the extraction of camphor oil, and a large amount of camphor leaf waste is generated, which is unexpectedly suitable for the method of the present invention to prepare hard carbon negative electrode materials, which can greatly reduce the production cost of hard carbon negative electrode materials.

[0040] Example 6 HC-1400 Material Characteristics and Performance Testing

[0041] 6.1 Micromorphology Analysis

[0042] Figure 1 The SEM image of HC-1400 is shown. The microscopic morphology of HC-1400 is irregular blocks, and the microscopic size is mainly 5-10 μm. The camphor leaf-based hard carbon material prepared in Example 2-4 is similar to HC-1400 in microscopic morphology.

[0043] 6.2 XRD patterns

[0044] Figure 2 The XRD pattern of HC-1400 is shown. From the XRD pattern of HC-1400, it can be seen that the presence of SiC impurities in the obtained hard carbon promotes the growth of graphite crystallites of the hard carbon material during the pyrolysis process, resulting in a sharp graphite peak at 26°.

[0045] 6.3 Half-cell electrochemical performance

[0046] Figure 3 The first cycle charge and discharge curve of HC-1400 is shown. As can be seen from the figure, the charge and discharge curve of HC-1400 presents a typical hard carbon charge and discharge curve, among which the first coulomb efficiency can reach 89.11%, which is at a relatively high level among biomass hard carbons. By analyzing its charging curve, it can be concluded that the specific capacity in the platform area reaches 136.57 mAh g -1 , accounting for 67.50% of the overall specific capacity, which is beneficial to improving the energy density of the full battery device.

[0047] Figure 4 The rate performance curve of HC-1400 is shown. When the current density is 1C, the capacity retention rate of the half-cell is as high as 79.01%, and when the current density reaches 5C, it still shows a capacity retention rate of 40.17%.

[0048] Figure 5The half-cell is charged and discharged at a current density of 3C. It can be seen that after 300 cycles, it still shows 112.95 mAh g -1 The high specific capacity and the capacity retention rate compared with the first cycle are as high as 94.85%, showing excellent cycle stability.

[0049] Table 2 lists the electrochemical performance parameters of HC-1400.

[0050] Table 2 Summary of electrochemical properties of HC-1400

[0051]

[0052] Combination Figures 3 to 5 As shown in Table 2, HC-1400 has good specific capacity and platform capacity ratio, and the capacity retention rate is as high as 94.85% after 300 cycles, and the cycle stability is excellent. Therefore, it has high application value in electrochemical energy storage.

Claims

1. A method for preparing a hard carbon negative electrode material, comprising: 1) drying and crushing the camphor leaves extracted with camphor oil to obtain a powder material; 2) heating the powder material to 1400° C. under nitrogen or inert gas protection and then keeping the temperature for more than 2 hours to obtain a pyrolytic carbon material; as well as 3) Soaking the pyrolytic carbon material in hydrochloric acid for more than 12 hours, then washing with water until neutral, and drying to obtain a camphor leaf-based hard carbon negative electrode material.

2. The method of claim 1, wherein the camphor oil is extracted by steam distillation.

3. The method of claim 2, wherein the camphor oil is extracted by steam distillation over water.

4. The method according to claim 1, wherein step 1) further comprises crushing the camphor tree leaves and passing them through a 300 mesh sieve.

5. The method of claim 1, wherein the concentration of the hydrochloric acid is 1 mol / L. The method according to claim 1 , wherein the camphor tree leaves are camphor tree leaves.

7. A hard carbon negative electrode material prepared by the method according to any one of claims 1 to 6.

8. Use of the hard carbon negative electrode material according to claim 7 in the preparation of sodium ion batteries.

Citation Information

Patent Citations

  • Efficient microwave synthesis method for micro-nano structure of sodium ion battery hard carbon negative electrode material

    CN117446782A

Cited By

  • Preparation method and application of oak leaf-based hard carbon negative electrode material

    CN120987295A