Carbon carrier as well as preparation method and application thereof
By graphitizing and nitrogen-doping carbon carriers through low-temperature chemical vapor deposition, the method addresses corrosion and agglomeration issues, enhancing the stability and performance of PEMFC catalysts.
Patent Information
- Application Number
- CN202411043187.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-12-06
AI Technical Summary
Current carbon supports for proton exchange membrane fuel cells (PEMFCs) face issues such as corrosion, agglomeration of platinum nanoparticles, and poor durability due to high carbon corrosion, which affect the overall performance and stability of the catalysts.
A method involving graphitization, oxidation treatment, and chemical vapor deposition using low-boiling nitrogen precursors to dope carbon carriers, achieving a balance between graphitization and surface properties, enhancing the interaction and dispersion of platinum nanoparticles.
The method results in a nitrogen-doped carbon carrier with improved corrosion resistance and catalyst stability, leading to higher activity and durability of the fuel cell catalysts.
Smart Images

Figure CN119079987A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of fuel cell technology, and in particular to a carbon carrier and a preparation method and application thereof. Background Art
[0002] With the increase in fossil fuel consumption and the acceleration of greenhouse gas emissions, clean energy technologies have attracted increasing attention. Among them, proton exchange membrane fuel cells (PEMFCs) have become a promising technology due to their high energy density, high energy efficiency, fast refueling and zero emissions. Despite having witnessed rapid development, high cost, unsatisfactory performance and insufficient durability remain the main limiting factors for the wider commercialization of PEMFCs.
[0003] Among them, the catalyst used for electrochemical reactions in the membrane electrode assembly (MEA) determines the overall performance and durability of PEMFC. Currently, Pt or Pt-based materials are still the most commonly used catalysts, showing state-of-the-art performance in ORR. The catalyst support plays a crucial role in determining the overall MEA performance because it participates in the construction of the three-phase boundary for charging and mass transfer. Carbon black, as a widely used support material for fuel cell catalysts, including XC-72 and Ketjen black, is adopted due to its high conductivity, low cost and good performance. However, the corrosion of carbon black supports at high potentials can significantly reduce the catalyst performance through migration and agglomeration, as well as the separation of surface-loaded Pt nanoparticles. In addition, due to severe carbon corrosion, the collapse of the supporting pore structure and the loss of hydrophobic properties deteriorate the mass transfer of the cathode catalyst layer. Since carbon with a low degree of graphitization is easily corroded, the ideal carbon support should have a sufficient long-range ordered graphite structure. In addition, the ideal carbon support should have good surface properties to strengthen the interaction between the metal and the support and uniformly disperse the nanoparticles. Only by achieving an optimal balance between the graphitization degree and surface properties of the carbon support can the overall performance of MEAs be improved.
[0004] Heteroatom doping is the most popular strategy for developing new carbon carriers. Due to the difference in electronegativity between heteroatoms and carbon atoms, the charge redistribution between carbon atoms can be regulated, thereby giving carbon carrier materials new physical and electrochemical properties. Among them, nitrogen is the most widely used heteroatom for doping carbon materials, which may be due to the fact that nitrogen has a relatively large electronegativity value compared to carbon. The introduction of nitrogen components can effectively regulate the overall acid-base properties and wettability of the catalyst and improve its ability to activate reactant or product molecules. At the same time, given the huge challenges of depositing Pt nanoparticles on highly graphitized carbon carriers, heteroatom doping helps to optimize the electron donor properties of carbon carriers, enhance the carrier / catalyst bonding, and thus enhance the stability of the catalyst. At present, the methods for preparing nitrogen-doped carbon materials are mainly to introduce nitrogen source and carbon source precursors, and then perform high temperature treatment or hydrothermal carbonization in an inert atmosphere to achieve one-step synthesis of nitrogen-doped carbon materials; or to react the pre-mixed carbon materials with nitrogen component precursors [such as urea, dicyandiamide, dimethylformamide or melamine, etc.] to prepare nitrogen-doped carbon materials, which usually requires the use of additives and long-term treatment under high temperature conditions to ensure the successful introduction of nitrogen species. The samples obtained by these preparation methods generally have low yields, many impurities, high costs, harsh preparation conditions, and may cause structural damage to the carbon bulk material or carrier material. The preparation temperature is high, and the formed metal particles have a wide particle size distribution. Summary of the invention
[0005] The present application provides a carbon carrier and a preparation method and application thereof, which can prepare a nitrogen-doped carbon carrier with relatively low preparation difficulty.
[0006] In a first aspect, the present application provides a method for preparing a carbon carrier, the method comprising:
[0007] Graphitizing the carbon carrier raw material to obtain a first intermediate product;
[0008] performing oxidation treatment on the first intermediate product to obtain a second intermediate product;
[0009] The second intermediate product and a nitrogen precursor are mixed and then annealed to deposit nitrogen on the second intermediate product by chemical vapor deposition to obtain a nitrogen-doped carbon carrier; the boiling point of the nitrogen precursor is not higher than 200°C.
[0010] As an optional embodiment, the nitrogen precursor includes at least one of ammonia, acetonitrile and aniline.
[0011] As an optional implementation manner, the annealing temperature is 450° C. to 850° C.; and / or
[0012] The annealing time is 0.5h to 10h; and / or
[0013] The annealing atmosphere is a nitrogen atmosphere.
[0014] As an optional embodiment, the carbon carrier raw material includes at least one of Ketjen black, acetylene black and mesoporous carbon; and / or
[0015] The temperature of the graphitization treatment is 1300°C to 2500°C; and / or
[0016] The heating rate of the graphitization treatment is 5°C / min to 20°C / min; and / or
[0017] The graphitization treatment time is 1 h to 5 h.
[0018] As an optional embodiment, the step of performing oxidation treatment on the first intermediate product to obtain the second intermediate product comprises:
[0019] The first intermediate product and the oxidizing acid solution are mixed, and then heated to react and dried to obtain a second intermediate product.
[0020] As an optional embodiment, the oxidizing acid solution comprises a nitric acid solution; and / or
[0021] The molar concentration of the oxidizing acid solution is 5 mol / L to 15 mol / L; and / or
[0022] The temperature of the heating reaction is 100°C to 150°C; and / or
[0023] The heating reaction time is 1h to 5h; and / or
[0024] The drying temperature is 60°C to 100°C; and / or
[0025] The drying time is 6 hours to 12 hours.
[0026] In a second aspect, the present application provides a carbon carrier, which is prepared by the method provided in the first aspect.
[0027] As an optional implementation manner, the nitrogen doping mass in the carbon carrier is 0.5% to 8%.
[0028] In a third aspect, the present application provides a catalyst, the catalyst comprising an active material and the carbon carrier provided in the second aspect, the active material being supported on the carbon carrier; and / or
[0029] The active material includes Pt and / or a Pt-based material.
[0030] In a fourth aspect, the present application provides a fuel cell, wherein the fuel cell comprises a catalyst layer, wherein the catalyst layer comprises a catalyst, and wherein the catalyst comprises the catalyst provided in the third aspect.
[0031] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0032] The method provided in the embodiment of the present application selects a low-boiling nitrogen precursor and uses chemical vapor deposition to nitrogen-dope the carbon carrier, which can achieve a balance between graphitization and functionalization of the carbon carrier at a relatively low temperature. Compared with the existing method of high-temperature treatment of mixed nitrogen organic precursors and carbon carriers, it is easy to operate, controllable in process, scalable, and has low destructiveness to the carbon structure. The carbon carrier after graphitization has improved the corrosion resistance of the carrier in the fuel cell due to its stable graphite carbon structure. Further oxidation treatment and doping of nitrogen atoms to modify the surface of the carbon carrier improves the dispersibility of the carbon carrier during the catalyst synthesis process, which is beneficial to the loading of active materials and dispersion on the carrier when preparing the catalyst; in addition, the bonding between nitrogen and the active material is formed, the electronegativity of the active material is improved and the interaction between the active material and the carrier is enhanced, so that the prepared catalyst has higher activity and stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0034] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0035] Figure 1 A schematic diagram of a process for a method provided in an embodiment of the present application;
[0036] Figure 2 Transmission infrared spectra of the carbon carriers provided in Example 1 and Comparative Example 2 of the present application;
[0037] Figure 3 This is a transmission electron microscope image of the catalyst provided in Example 1 of the present application;
[0038] Figure 4 Transmission electron microscope image of the catalyst provided in Comparative Example 1 of the present application;
[0039] Figure 5 This is a graph showing the electrochemical performance test results of the catalysts provided in Example 1 and Comparative Example 1 of the present application;
[0040] Figure 6 This is a diagram showing the durability test results of the catalyst provided in Example 1 of the present application;
[0041] Figure 7 This is a diagram showing the durability test results of the catalyst provided in Comparative Example 2 of the present application. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0043] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0044] The present application intends to provide a method for preparing a carbon carrier, using a low-boiling nitrogen precursor in a carbon carrier by a CVD method, regulating reaction parameters at a relatively low calcination temperature, and preparing a nitrogen-doped carbon carrier with high consistency and controllable nitrogen doping, and the preparation method is simple and scalable, low cost, and less pollution. The prepared nitrogen-doped carbon carrier can achieve a balance between graphitization and carbon carrier surface properties, promote the dispersion and anchoring of loaded metal particles, and improve the performance and stability of the catalyst in the fuel cell.
[0045] Figure 1 A flow chart of the method provided in the embodiment of the present application is as follows: Figure 1 As shown, the present application embodiment provides a method for preparing a carbon carrier, the method comprising:
[0046] S1. Graphitizing the carbon carrier raw material to obtain a first intermediate product;
[0047] In some embodiments, the carbon carrier raw material may be selected from carbon black, specifically, may be at least one of Ketjen black, acetylene black and mesoporous carbon.
[0048] In some embodiments, the temperature of the graphitization treatment is 1300° C. to 2500° C.; the heating rate of the graphitization treatment is 5° C. / min to 20° C. / min; and the time of the graphitization treatment is 1 h to 5 h.
[0049] Exemplarily, the temperature of the graphitization treatment may be 1300° C., 1400° C., 1500° C., 1600° C., 1700° C., 1800° C., 1900° C., 2000° C., 2100° C., 2200° C., 2300° C., 2400° C., or 2500° C., etc., and it may also be any value in the range of 1300° C. to 2500° C. The heating rate of the graphitization treatment may be 5° C. / min, 6° C. / min, 7° C. / min, 8° C. / min, 9° C. / min, 10° C. / min, 11° C. / min, 12° C. / min, 13° C. / min, 14° C. / min, 15° C. / min, 16° C. / min, 17° C. / min, 18° C. / min, 19° C. / min, or 20° C. / min, etc., and it may also be any value in the range of 5° C. / min to 20° C. / min. The time of the graphitization treatment may be 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h or 5 h, etc., and may also be any value within the range of 1 h to 5 h.
[0050] Specifically, in this embodiment, a carbon carrier raw material is added to a crucible, heated to a specified temperature in an inert atmosphere for high-temperature graphitization treatment, and then cooled to room temperature to obtain a first intermediate product; wherein the carbon carrier raw material is Ketjen black, acetylene black, and mesoporous carbon; the inert atmosphere is argon; the heating temperature is 1300-2500 degrees Celsius, the heating rate is 5-20 degrees Celsius / minute, and the treatment time is 1-5 hours.
[0051] S2. oxidizing the first intermediate product to obtain a second intermediate product;
[0052] In some embodiments, the oxidation treatment of the first intermediate product to obtain the second intermediate product includes: mixing the first intermediate product with an oxidizing acid solution, and then heating and drying to obtain the second intermediate product.
[0053] Furthermore, the oxidizing acid solution may be selected from a nitric acid solution. The molar concentration of the oxidizing acid solution may be 5 mol / L to 15 mol / L.
[0054] Exemplarily, the molar concentration of the oxidizing acid solution can be 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L, 13 mol / L, 14 mol / L or 15 mol / L, etc., and it can also be any value within the range of 5 mol / L to 15 mol / L.
[0055] Furthermore, the drying temperature is 60° C. to 100° C.; and the drying time is 6 h to 12 h.
[0056] Exemplarily, the drying temperature may be 60° C., 70° C., 80° C., 90° C. or 100° C., etc., and it may also be any value within the range of 60° C. to 100° C. The drying time may be 6 h, 6.5 h, 7 h, 7.5 h, 8 h, 8.5 h, 9 h, 9.5 h, 10 h, 10.5 h, 11 h, 11.5 h or 12 h, etc., and it may also be any value within the range of 6 h to 12 h.
[0057] Specifically, in this embodiment, the first intermediate product after graphite treatment is mixed with an oxidizing acid solution, stirred and heated to a specific temperature and kept warm for a period of time, and then left to cool. The cooled dispersion is filtered and washed to neutrality. Then it is dried to obtain a second intermediate product; wherein the concentration of the oxidizing acid solution is a nitric acid solution of 5-15M; the heating temperature is 100-150 degrees Celsius, and the holding time is 1-5 hours. The drying time is 6 hours to 12 hours, and the drying temperature is 60-100 degrees Celsius.
[0058] S3. Mixing the second intermediate product and a nitrogen precursor, and then annealing, so that nitrogen is deposited on the second intermediate product by chemical vapor deposition to obtain a nitrogen-doped carbon carrier; the boiling point of the nitrogen precursor is not higher than 200°C.
[0059] In some embodiments, the nitrogen precursor includes at least one of ammonia, acetonitrile, and aniline.
[0060] In some embodiments, the annealing temperature is 450° C. to 850° C.; the annealing time is 0.5 h to 10 h; and the annealing atmosphere is a nitrogen atmosphere.
[0061] Exemplarily, the annealing temperature may be 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C or 850°C, etc., and it may also be any value within the range of 450°C to 850°C. The annealing time may be 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h or 10h, etc., and it may also be any value within the range of 0.5h to 10h. In other embodiments, the annealing atmosphere may also be an inert atmosphere, such as an argon atmosphere, etc.
[0062] Specifically, in this embodiment, the second intermediate product is placed in a quartz boat and placed in a high-temperature tube furnace, and a nitrogen precursor is introduced into the furnace for annealing under a nitrogen atmosphere. The annealing temperature is 450 to 850 degrees Celsius, the annealing time is 0.5 to 10 hours, and the nitrogen precursor is ammonia, acetonitrile, aniline, etc.
[0063] This method selects a low-boiling nitrogen precursor and uses chemical vapor deposition to dope the carbon carrier with nitrogen, which can achieve a balance between graphitization and functionalization of the carbon carrier at a lower temperature. Compared with the existing method of high-temperature treatment of mixed nitrogen organic precursors and carbon carriers, it is simple to operate, controllable in process, scalable, and less destructive to the carbon structure. The graphitized carbon carrier has improved corrosion resistance in fuel cells due to its stable graphite carbon structure. Further oxidation treatment and doping of nitrogen atoms to modify the surface of the carbon carrier improves the dispersibility of the carbon carrier during catalyst synthesis, which is beneficial to the loading of active materials and dispersion on the carrier when preparing the catalyst. In addition, the bonding between nitrogen and the active material is formed, which improves the electronegativity of the active material and enhances the interaction between the active material and the carrier, so that the prepared catalyst has higher activity and stability.
[0064] Based on a general inventive concept, an embodiment of the present application further provides a carbon carrier, which is prepared by the method provided above.
[0065] The carbon carrier is realized based on the above method. The specific steps of the method can refer to the above embodiment. Since the carbon carrier adopts part or all of the technical solutions of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment, which will not be described one by one here.
[0066] In some embodiments, the doping mass of nitrogen in the carbon carrier is 0.5% to 8%. For example, the doping mass of nitrogen in the carbon carrier can be 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5% or 8%, etc., and it can also be any value in the range of 0.5% to 8%.
[0067] Based on a general inventive concept, an embodiment of the present application further provides a catalyst, which includes an active material and a carbon carrier as provided above, wherein the active material is loaded on the carbon carrier.
[0068] The catalyst is realized based on the above-mentioned carbon carrier. The specific content of the carbon carrier can refer to the above-mentioned embodiment. Since the catalyst adopts part or all of the technical solutions of the above-mentioned embodiments, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be described one by one here.
[0069] Therein, the active material may be selected from Pt and / or Pt-based materials.
[0070] Based on a general inventive concept, an embodiment of the present application further provides a fuel cell, wherein the fuel cell includes a catalyst layer, wherein the catalyst layer includes a catalyst, and wherein the catalyst includes the catalyst provided above.
[0071] The fuel cell is realized based on the above-mentioned catalyst. The specific content of the catalyst can be referred to the above-mentioned embodiments. Since the fuel cell adopts part or all of the technical solutions of the above-mentioned embodiments, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be described one by one here.
[0072] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0073] Example 1
[0074] A catalyst, the preparation process of which is as follows:
[0075] 1) Weigh 2 g of carbon material and place it in a high-temperature graphitization furnace under an argon atmosphere and heat it to 2200 degrees Celsius. Keep it warm for 2 hours and then cool it to room temperature to obtain a graphitized carbon carrier.
[0076] 2) Weigh 1 g of graphitized carbon support and 100 mL of concentrated nitric acid in a flask and mix them, heat them to 120 degrees Celsius and keep them warm for 2 hours, then cool them to room temperature, filter and wash them until they are neutral, and place the washed sample in an oven at 80 degrees to dry for 12 hours to obtain an oxidized graphitized carbon support.
[0077] 3) Weigh 500 mg of the oxidized graphitized carbon support and place it in the middle of a tube furnace and purge it with nitrogen. Heat the tube furnace to 650 degrees Celsius and then introduce saturated acetonitrile vapor and keep it for 6 hours. After cooling to room temperature, take it out to obtain a nitrogen-doped graphitized carbon support.
[0078] 4) The platinum precursor and the nitrogen-doped graphitized carbon carrier are mixed and stirred by an impregnation method, dried, and then heat-treated to obtain an electrocatalyst.
[0079] Example 2
[0080] A catalyst, the preparation process of which is as follows:
[0081] 1) Weigh 2 g of carbon material and place it in a high-temperature graphitization furnace under an argon atmosphere and heat it to 2200 degrees Celsius. Keep it warm for 2 hours and then cool it to room temperature to obtain a graphitized carbon carrier.
[0082] 2) Weigh 1 g of graphitized carbon support and 100 mL of concentrated nitric acid in a flask and mix them, heat them to 120 degrees Celsius and keep them warm for 2 hours, then cool them to room temperature, filter and wash them until they are neutral, and place the washed sample in an oven at 80 degrees to dry for 12 hours to obtain an oxidized graphitized carbon support.
[0083] 3) Weigh 500 mg of the oxidized graphitized carbon support and place it in the middle of a tube furnace and purge it with nitrogen. Heat the tube furnace to 850 degrees Celsius and then introduce saturated acetonitrile vapor and keep it for 6 hours. After cooling to room temperature, take it out to obtain a nitrogen-doped graphitized carbon support.
[0084] 4) The platinum precursor and the nitrogen-doped graphitized carbon carrier are mixed and stirred by an impregnation method, dried, and then heat-treated to obtain an electrocatalyst.
[0085] Example 3
[0086] A catalyst, the preparation process of which is as follows:
[0087] 1) Weigh 2 g of carbon material and place it in a high-temperature graphitization furnace under an argon atmosphere and heat it to 2200 degrees Celsius. Keep it warm for 2 hours and then cool it to room temperature to obtain a graphitized carbon carrier.
[0088] 2) Weigh 1 g of graphitized carbon support and 100 mL of concentrated nitric acid in a flask and mix them, heat them to 120 degrees Celsius and keep them warm for 2 hours, then cool them to room temperature, filter and wash them until they are neutral, and place the washed sample in an oven at 80 degrees to dry for 12 hours to obtain an oxidized graphitized carbon support.
[0089] 3) Weigh 500 mg of the oxidized graphitized carbon support and place it in the middle of a tube furnace and purge it with nitrogen. Heat the tube furnace to 650 degrees Celsius and then introduce saturated ammonia vapor and keep it for 6 hours. After cooling to room temperature, take it out to obtain a nitrogen-doped graphitized carbon support.
[0090] 4) The platinum precursor and the nitrogen-doped graphitized carbon carrier are mixed and stirred by an impregnation method, dried, and then heat-treated to obtain an electrocatalyst.
[0091] Comparative Example 1
[0092] A catalyst, the preparation process of which is as follows:
[0093] 1) Weigh 2 g of carbon material and place it in a high-temperature graphitization furnace under an argon atmosphere and heat it to 2200 degrees Celsius. Keep it warm for 2 hours and then cool it to room temperature to obtain a graphitized carbon carrier.
[0094] 2) Weigh 1 g of graphitized carbon support and 100 mL of concentrated nitric acid in a flask and mix them, heat them to 120 degrees Celsius and keep them warm for 2 hours, then cool them to room temperature, filter and wash them until they are neutral, and place the washed sample in an oven at 80 degrees to dry for 12 hours to obtain an oxidized graphitized carbon support.
[0095] 3) The platinum precursor and the oxidized graphitized carbon carrier are mixed and stirred by an impregnation method, and then heat-treated after drying to obtain an electrocatalyst.
[0096] Comparative Example 2
[0097] A catalyst, the preparation process of which is as follows:
[0098] 1) The platinum precursor is mixed and stirred with the untreated carbon material by an impregnation method, and then heat-treated after drying to obtain an electrocatalyst.
[0099] The carbon supports prepared in Example 1 and Comparative Example 2 were analyzed by transmission infrared spectroscopy. Figure 2 As shown in the figure, compared with Comparative Example 2, the infrared spectrum of the nitrogen-doped graphitized carbon carrier obtained in Example 1 has a characteristic absorption peak of nitrogen functional groups, indicating that the surface of the carbon carrier is modified with nitrogen. According to X-ray photoelectron spectroscopy analysis, the N content in the carbon carrier obtained in Example 1 is 3.8wt%.
[0100] The platinum catalysts prepared in Example 1 and Comparative Example 1 were characterized by electron microscopy. Figure 3 and Figure 4 As shown in the figure, it can be seen that the catalyst prepared in Example 1 has a smaller particle size and is well dispersed, indicating that the nitrogen-doped modified carbon support surface can promote the dispersion of the loaded platinum particles.
[0101] The electrochemical performance of the platinum catalysts prepared in Example 1 and Comparative Example 1 was tested: the electrochemical performance was measured by a standard three-electrode method, and the working electrodes were prepared using the electrocatalysts in Example 1 and Comparative Example 1, respectively. The test conditions were: 0.1 mol / L HClO saturated with oxygen at 25°C. 4 In aqueous solution, the potential scanning test was carried out at a voltage of 0.1-1.1V (vs. RHE), and the polarization curve in redox was shown in Figure 5 .Depend on Figure 5 It can be seen that the half-wave potential and the mass specific activity at 0.9V in the LSV curve of the electrocatalyst of Example 1 are both higher than those of the electrocatalyst of Comparative Example 1. Therefore, the performance of the proton exchange membrane fuel cell electrocatalyst prepared by the nitrogen-doped graphitized carbon carrier prepared in this application is better than that of the electrocatalyst prepared by the undoped graphitized carbon carrier. Nitrogen doping can promote the dispersibility of platinum on the carbon carrier and regulate the electronic state of the platinum particles, thereby promoting the ORR performance of the catalyst.
[0102] The durability of the platinum catalysts prepared in Example 1 and Comparative Example 2 was tested: the standard three-electrode method was used to prepare the proton exchange membrane fuel cell electrocatalyst prepared by the nitrogen-doped graphitized carbon support of Example 1 and the catalyst prepared in Comparative Example 2 as working electrodes, respectively. 4 In aqueous solution, cyclic potential scans were performed at a voltage of 1-1.5 V (vs. RHE). Figure 6 and Figure 7As shown, after 5000 scans, the electrochemical active area (ECSA) of the electrocatalyst prepared using the nitrogen-doped graphitized carbon support of Example 1 was only reduced by 8.7%, while the Pt / C electrocatalyst using the untreated carbon support in Comparative Example 2 was attenuated by 18.8%, which significantly improved the durability of the carbon support.
[0103] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0104] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b and c can be single or multiple.
[0105] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for preparing a carbon carrier, It is characterized in that The method comprises: Graphitizing the carbon carrier raw material to obtain a first intermediate product; performing oxidation treatment on the first intermediate product to obtain a second intermediate product; The second intermediate product and a nitrogen precursor are mixed and then annealed to deposit nitrogen on the second intermediate product by chemical vapor deposition to obtain a nitrogen-doped carbon carrier; the boiling point of the nitrogen precursor is not higher than 200°C.
2. The method for preparing a carbon carrier according to claim 1, It is characterized in that The nitrogen precursor includes at least one of ammonia, acetonitrile and aniline.
3. The method for preparing a carbon carrier according to claim 1, It is characterized in that The annealing temperature is 450°C to 850°C; and / or The annealing time is 0.5h to 10h; and / or The annealing atmosphere is a nitrogen atmosphere.
4. The method for preparing a carbon carrier according to claim 1, It is characterized in that The carbon carrier raw material comprises at least one of Ketjen black, acetylene black and mesoporous carbon; and / or The temperature of the graphitization treatment is 1300°C to 2500°C; and / or The heating rate of the graphitization treatment is 5°C / min to 20°C / min; and / or The graphitization treatment time is 1 h to 5 h.
5. The method for preparing a carbon carrier according to claim 1, It is characterized in that The step of performing oxidation treatment on the first intermediate product to obtain the second intermediate product comprises: The first intermediate product and the oxidizing acid solution are mixed, and then heated to react and dried to obtain a second intermediate product.
6. The method for preparing a carbon carrier according to claim 5, It is characterized in that The oxidizing acid solution comprises a nitric acid solution; and / or The molar concentration of the oxidizing acid solution is 5 mol / L to 15 mol / L; and / or The temperature of the heating reaction is 100°C to 150°C; and / or The heating reaction time is 1h to 5h; and / or The drying temperature is 60°C to 100°C; and / or The drying time is 6 hours to 12 hours.
7. A carbon carrier, It is characterized in that The carbon carrier is prepared by the method according to any one of claims 1 to 6.
8. The carbon carrier according to claim 8, It is characterized in that The nitrogen doping mass in the carbon carrier is 0.5% to 8%.
9. A catalyst, It is characterized in that The catalyst comprises an active material and a carbon carrier according to any one of claims 7 to 8, wherein the active material is supported on the carbon carrier; and / or The active material includes Pt and / or a Pt-based material.
10. A fuel cell, It is characterized in that The fuel cell includes a catalyst layer, the catalyst layer includes a catalyst, and the catalyst includes the catalyst according to claim 9.
Citation Information
Patent Citations
Proton exchange membrane fuel cell catalyst and preparation method thereof
CN113782753A
Carbon support for fuel cell catalyst and preparation method thereof
US20170005342A1