Method for separating natural sylvinite from sodium-containing carnallite, natural sylvinite and application thereof
The sodium-containing light halide was treated by reverse flotation and cold crystallization, and the natural potassium salt with a particle size of 600-800μm was sieved, which solved the problem of complex and high cost of preparation of natural potassium salt, and achieved high efficiency and low efficiency Cost of natural potassium salt separation and application.
Patent Information
- Application Number
- CN202411229954.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
Smart Images

Figure CN119080028A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of development and utilization of carnallites, and in particular to a method for separating natural sylvite from sodium-containing carnallites, the natural sylvite and applications thereof. Background Art
[0002] Qinghai is a resource-rich province with a wide variety of natural resources, among which the representative resources are salt lake resources, and the salt lake resources mainly include sedimentary resources and brine resources. Salt lake brine is a liquid chloride mineral resource, rich in various components. It can be processed to produce potassium chloride to produce potash fertilizer. Potash fertilizer is one of the three major chemical fertilizers along with nitrogen, phosphorus and potassium. Potassium plays a significant role in regulating the life processes in plants, and is beneficial to improving the water absorption, synthesis and transfer of sugars in plants. The use of potash fertilizer can effectively increase the yield and quality of crops.
[0003] There are many processes for producing potash fertilizer using salt lake brine, such as drying in salt pans to obtain potassium salt, and then using hot dissolution-cold crystallization to produce KCl. However, potassium salt is relatively scarce, while salt lake brine contains abundant carnallite resources. After salt lake brine is evaporated and concentrated in salt pans, sodium-containing carnallite is obtained. Carnallite is a pure compound salt (xKCl·yMgCl) that can exist stably in a wide temperature range (-21℃~167.65℃). 2 ·zH 2 O), while sodium-containing carnallite is NaCl and xKCl·yMgCl 2 ·zH 2 O is a mixture of eutectics, and natural sylvite is formed in the process of drying sodium-containing carnallite in salt fields. Natural sylvite has a eutectic structure.
[0004] At present, the main source of natural potassium salt is natural mining or brine evaporation crystallization. The difference between it and artificial potassium salt is that artificial potassium salt has similar components but different molecular crystal forms. Natural potassium salt is a eutectic of sodium chloride and potassium chloride, while artificial potassium salt is a mixture of sodium chloride and potassium chloride. Artificial potassium salt is generally used to prepare potassium chloride, while natural potassium salt is widely used to prepare low-sodium salt due to its relatively pure composition. It can also be used to prepare KCl. Compared with artificial potassium salt, potassium chloride prepared by natural potassium salt has higher purity.
[0005] The currently disclosed method for producing natural potash salt is the sun-drying method: the technical process is to dissolve the carnallite ore obtained by sun-drying the intercrystalline brine with fresh water and discharge it into the potash pool. Potassium chloride is first precipitated separately in the potash pool. When the brine in the potash pool is concentrated to saturation with sodium chloride, the brine at this time is potash salt point brine, and potash salt is produced by sun-drying. The production of potash salt by this method requires a long sun-drying time and a long production cycle. In addition, it is necessary to build special potash pools and potash salt pools, and the process is relatively complicated.
[0006] The following methods for preparing artificial sylvite have been published: (1) cold decomposition-washing method: this technical process is to completely decompose carnallites to obtain artificial sylvite; (2) cold decomposition-flotation method: this technical process is to completely decompose carnallites with fresh water or refined potassium mother liquor to obtain artificial sylvite; (3) cold decomposition-hot melt crystallization method: this technical process is to completely decompose carnallites with fresh water to obtain artificial sylvite. For example, the patent application with application number CN202111244185.7 provides a method for preparing low-sodium salt, and the sylvite mentioned therein only explains that the sylvite obtained by decomposing carnallites is artificial sylvite, which is used to prepare KCl; the patent application with application number CN202010371560.3 provides a method for preparing potassium chloride using carnallites, which is based on obtaining low-sodium carnallites after adding brine to brine, and then cold-decomposing the low-sodium carnallites to obtain artificial sylvite. The main purpose of this invention is to produce KCl; the patent application with application number CN202010371558.6 provides a method for preparing low-sodium carnallites and potassium chloride using high-sodium carnallites, and the sylvite mentioned therein is also artificial sylvite, which is based on the high-temperature evaporation of low-temperature potassium saturated liquid to precipitate sodium chloride, thereby reducing the sodium chloride content in low-sodium carnallites in the subsequent stage, and increasing the potassium chloride content in artificial sylvite, and then selectively dissolving the low temperature to prepare KCl.
[0007] It can be seen that the current method for producing and preparing natural sylvite is relatively complicated and the process is difficult to control. In the prior art, sylvite prepared by decomposing carnallites is mostly artificial sylvite, which is used to prepare KCl. How to prepare natural sylvite from sodium-containing carnallites is important for further improving the development value of sodium-containing carnallites. Summary of the invention
[0008] The main purpose of the present invention is to provide a method for separating natural sylvite from sodium-containing carnallite, natural sylvite and application thereof, so as to solve the problems of complex preparation process and high cost of natural sylvite in the prior art.
[0009] In order to achieve the above object, according to one aspect of the present invention, a method for separating natural sylvite from sodium-containing carnallite is provided, the method comprising: screening the crystal underflow obtained by reverse flotation and cold decomposition of the sodium-containing carnallite, collecting components with a particle size range of 600 to 800 μm, and obtaining natural sylvite.
[0010] Furthermore, in the crystallization underflow, the content of KCl in the solid component is greater than or equal to 72%, preferably 72% to 80%.
[0011] Furthermore, the solid content of the crystallization underflow is 25% to 35%.
[0012] Furthermore, the screening includes primary screening and secondary screening. The primary screening divides the crystallization bottom flow into a first screening product with a particle size greater than 800 μm and a second screening product with a particle size less than or equal to 800 μm. The secondary screening divides the second screening product into natural potassium salt with a particle size of 600-800 μm and a third screening product with a particle size less than 600 μm.
[0013] Furthermore, the first screening product includes: 8-10 wt% KCl, 3-4.5 wt% MgCl 2 and 78-85wt% NaCl.
[0014] Furthermore, the third screening product includes: 70-80 wt% KCl, 2.5-5 wt% MgCl 2 and 3-6wt% NaCl.
[0015] Furthermore, the sodium carnallite contains 17-21 wt% KCl, 27-28 wt% MgCl 2 and 17-19wt% NaCl.
[0016] Furthermore, the natural potassium salt includes: 35-45wt% KCl, 3-4.5wt% MgCl 2 and 40-45wt% NaCl.
[0017] In order to achieve the above object, according to one aspect of the present invention, a natural sylvite is provided, which is obtained by any of the above methods for separating natural sylvite from sodium-containing carnallite.
[0018] According to another aspect of the present invention, there is provided a use of the natural sylvite as described above as a raw material in the process of preparing low-sodium salt.
[0019] By using the technical solution of the present invention, since the sodium-containing carnallite is NaCl and xKCl·yMgCl 2 ·zH 2 In the process of studying the reverse flotation-cold crystallization method for producing KCl, the researchers of this application unexpectedly found that the component with a particle size of 600-800 μm in the crystallization underflow obtained after the reverse flotation-cold crystallization method is a natural sylvite with a eutectic structure. In the process of preparing potassium chloride by this method, natural sylvite can be separated; natural sylvite can be used to further prepare potassium chloride, and because its composition is relatively pure, it can also be used to prepare low-sodium salt, which can significantly improve the application value of sodium-containing carnallite.
[0020] Common sodium-containing carnallite contains 17-21wt% KCl and 27-28wt% MgCl 2and 17-19wt% NaCl. When using reverse flotation-cold crystallization to produce KCl, Figure 1 As shown, the sodium-containing carnallite is subjected to a reverse flotation process to remove the NaCl portion of the sodium-containing carnallite to obtain low-sodium carnallite. The low-sodium carnallite generally contains 17-21 wt% KCl and 17-21 wt% MgCl. 2 The content of Mg is 30-31wt% and the content of NaCl is 3.5-7wt%; the low-sodium carnallite is then subjected to a cold crystallization process, fresh water is added, and MgCl 2 After that, a mixture of crystallized products, namely the crystallization underflow, is obtained. The crystallization underflow contains high-grade crude potassium and incompletely decomposed solid particles. During the analysis and research of these solid particles, the researchers of this application unexpectedly found that the component with a particle size range of 600 to 800 μm is a natural potassium salt eutectic. Analysis and speculation indicate that the natural potassium salt eutectic is formed through the following process: sodium-containing carnallite is NaCl and xKCl·yMgCl 2 ·zH 2 O eutectic mixture, and in the process of drying sodium-containing carnallite in salt fields, a natural potassium salt eutectic structure will be formed. In the process of reverse flotation treatment of sodium-containing carnallite, the NaCl of sodium-containing carnallite is partially removed to form low-sodium carnallite. During the cold crystallization process of low-sodium carnallite, the MgCl 2 Dissolved into the liquid phase, part of potassium chloride is dissolved in water, and forms crystals with smaller particle size under saturated state. During the decomposition process, other components of natural potassium salt are decomposed, and the natural potassium salt itself also undergoes certain degradation. Under the cold crystallization treatment process, natural potassium salt eutectic with a particle size range of 600-800μm is formed. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0022] Figure 1 A schematic diagram of a process flow for preparing natural potassium salt according to an embodiment of the present invention is shown;
[0023] Figure 2 The SEM image of the natural sylvite of Example 1 of the present invention is shown.
[0024] Figure 3 The SEM image of the natural sylvite of Example 2 of the present invention is shown. DETAILED DESCRIPTION
[0025] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0026] As analyzed in the background technology of this application, the prior art has the problem that the preparation process of natural sylvite is complicated and the cost is high. In order to solve this problem, this application provides a method for separating natural sylvite from sodium-containing carnallite, natural sylvite and its application.
[0027] According to a typical embodiment of the present application, a method for separating natural sylvite from sodium-containing carnallites, natural sylvite and applications thereof are provided, the method comprising: screening a crystalline underflow obtained by treating the sodium-containing carnallites by reverse flotation and cold crystallization, collecting components with a particle size range of 600 to 800 μm, and obtaining natural sylvite.
[0028] Since sodium-containing carnallite is NaCl and xKCl·yMgCl 2 ·zH 2 In the process of studying the reverse flotation-cold crystallization method for producing KCl, the researchers of this application unexpectedly found that the component with a particle size of 600-800 μm in the crystallization underflow obtained after the reverse flotation-cold crystallization method is a natural sylvite with a eutectic structure. In the process of preparing potassium chloride by this method, natural sylvite can be separated; natural sylvite can be used to further prepare potassium chloride, and because its composition is relatively pure, it can also be used to prepare low-sodium salt, which can significantly improve the application value of sodium-containing carnallite.
[0029] Common sodium-containing carnallite contains 17-21wt% KCl and 27-28wt% MgCl 2 and 17-19wt% NaCl. When using reverse flotation-cold crystallization to produce KCl, Figure 1 As shown, the sodium-containing carnallite is subjected to a reverse flotation process to remove the NaCl portion of the sodium-containing carnallite to obtain low-sodium carnallite. The low-sodium carnallite generally contains 17-21 wt% KCl and 17-21 wt% MgCl. 2 The content of Mg is 30-31wt% and the content of NaCl is 3.5-7wt%; the low-sodium carnallite is then subjected to a cold crystallization process, fresh water is added, and MgCl 2 After that, a mixture of crystallized products, namely the crystallization underflow, is obtained. The crystallization underflow contains high-grade crude potassium and incompletely decomposed solid particles. During the analysis and research of these solid particles, the researchers of this application unexpectedly found that the component with a particle size range of 600 to 800 μm is a natural potassium salt eutectic. Analysis and speculation indicate that the natural potassium salt eutectic is formed through the following process: sodium-containing carnallite is NaCl and xKCl·yMgCl2 ·zH 2 O eutectic mixture, and in the process of drying sodium-containing carnallite in salt fields, a natural potassium salt eutectic structure will be formed. In the process of reverse flotation treatment of sodium-containing carnallite, the NaCl of sodium-containing carnallite is partially removed to form low-sodium carnallite. During the cold crystallization process of low-sodium carnallite, the MgCl 2 Dissolved, enter the liquid phase, a part of potassium chloride is dissolved in water, and forms crystals with smaller particle size under saturation state, in which the natural potassium salt decomposes other components during the decomposition process, and also undergoes certain degradation, and forms natural potassium salt eutectic with a particle size range of 600-800 μm under the cold crystallization process. Of course, natural potassium salt can also be obtained by separating particles with any particle size range within the particle size range of 600-800 μm in the above-mentioned crystallization bottom flow.
[0030] In the process of preparing potassium chloride by other processes, for example, the cold decomposition-flotation method, the eutectic structure of sylvite in carnallite is decomposed and destroyed, and the sylvite obtained is mostly a mixture of sodium chloride and potassium chloride, that is, artificial sylvite.
[0031] In some typical embodiments of the present application, the natural potassium salt prepared by the above method includes: 35-45wt% KCl, 3-4.5wt% MgCl 2 and 40-45wt% NaCl.
[0032] In order to increase the proportion of natural sylvite in the crystallization underflow, and further improve the quality of natural sylvite, in some embodiments of the present application, in the crystallization underflow formed by the reverse flotation-cold crystallization method, the content of KCl in the solid component is greater than or equal to 72%, and when the content of KCl in the solid component is within the above range, it indicates that the low-sodium carnallite is completely decomposed in the cold crystallizer process. If the low-sodium carnallite is not completely decomposed, low-sodium carnallite is likely to appear in the underflow, resulting in a large amount of low-sodium carnallite in addition to sylvite in the component with a particle size range of 600 to 800 μm. Considering that there are limitations to achieving a high content of KCl in the solid component in the current actual production, the content of KCl in the solid component is preferably 72% to 80%, and illustratively, the content of KCl in the solid component is 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80% or any range between the two.
[0033] In some typical embodiments of the present application, the solid content of the crystallization underflow is 25% to 35%. As an example, the crystallization underflow is 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35% or any range therebetween.
[0034] In some typical embodiments of the present application, the above-mentioned screening includes primary screening and secondary screening, the primary screening divides the crystallization bottom flow into a first screening product with a particle size greater than 800 μm and a second screening product with a particle size less than or equal to 800 μm, and the secondary screening divides the second screening product into natural potassium salt with a particle size of 600 to 800 μm and a third screening product with a particle size less than 600 μm, such as Figure 1 Through this treatment process, different products obtained in the process of producing KCl by reverse flotation-cold crystallization can be separated and recovered to improve K + The recovery rate and economic value of sodium-containing carnallite.
[0035] The above-mentioned primary screening and secondary screening can be performed using screening devices with apertures of 800 μm and 600 μm, respectively, to separate the crystallization bottom flow into a first screening product with a particle size greater than 800 μm, natural potassium salt with a particle size of 600-800 μm, and a third screening product with a particle size less than 600 μm.
[0036] Among them, the first screening product with a particle size greater than 800 μm is tailings, which can be dissolved in water by adding water in the salt washing device to form mineralized brine for sun-drying sodium-containing carnallite, and the solid phase forms high-grade industrial salt, which is used as a raw material for soda ash production. In some embodiments of the present application, the first screening product includes: 8-10wt% KCl, 3-4.5wt% MgCl 2 and 78-85wt% NaCl.
[0037] The third screening product is a component with a particle size of less than 600 μm in the crystallization bottom flow. In some embodiments of the present application, the third screening product includes: 70-80 wt% KCl, 2.5-5 wt% MgCl 2 and 3-6 wt% NaCl. The third screening product can enter the next process refining process for purification to obtain high-grade KCl.
[0038] According to another typical embodiment of the present application, a natural sylvite is provided, which is obtained by any of the above-mentioned methods for separating natural sylvite from sodium-containing carnallite.
[0039] Since sodium-containing carnallite is NaCl and xKCl·yMgCl 2 ·zH 2In the process of studying the reverse flotation-cold crystallization method for producing KCl, the researchers of this application unexpectedly found that the component with a particle size of 600-800 μm in the crystallization bottom flow obtained after the reverse flotation-cold crystallization method is a natural potassium salt with a eutectic structure. Natural potassium salt has good quality and can be used to prepare low-sodium salt. Due to the above preparation method, it is separated in the process of preparing potassium chloride without additional treatment, so the preparation cost is significantly reduced, and the market prospect is broad.
[0040] According to another typical embodiment of the present application, the application of the above-mentioned natural potassium salt as a raw material in the process of preparing low sodium salt is provided. The natural potassium salt prepared by the method of the present application has a particle size in the range of 600 to 800 μm, uniform particles, good quality, and low cost, and has a good application effect as a raw material in the preparation of low sodium salt.
[0041] Since the composition of natural potassium rock salt is relatively pure, the process of using it to prepare edible low-sodium salt is relatively simple, and it is beneficial to improve the quality of low-sodium salt. The specific process of using the natural potassium rock salt of the present application as a raw material to prepare low-sodium salt can refer to the prior art, and the present application will not be described in detail here.
[0042] The beneficial effects that can be achieved by the present application will be further illustrated below in combination with embodiments and comparative examples.
[0043] Example 1
[0044] The main components of sodium carnallite are KCl: 18.26%, MgCl 2 : 28.16%, NaCl: 18.56%, the crystallization underflow generated in the process of preparing potassium chloride by the "reverse flotation-cold crystallization" process, wherein the solid content in the crystallization underflow is 25.56%, and the content of KCl is 73.01%.
[0045] Screening is performed through a two-stage screening device. First, a first-stage screening device is used for screening. The aperture of the first-stage screening device is 800μm, and the tailings with a particle size greater than 800μm and the filter material with a particle size less than 800μm in the underflow are separated; the filter material with a particle size less than 800μm is screened by a second-stage screening device with an aperture of 600μm, and the natural potassium salt with a particle size range of 600-800μm and the component with a particle size less than 600μm, that is, crude potassium, are separated. The tailings with a particle size greater than 800μm account for 5% of the underflow weight, the natural potassium salt with a particle size range of 600-800μm accounts for 5% of the underflow weight, and the component with a particle size less than 600μm accounts for 90% of the underflow weight.
[0046] The separated natural potassium salt was analyzed by scanning electron microscope, and its SEM image is as follows Figure 2As shown in the SEM image, it can be seen that the material has the crystal structure of natural potassium salt. Among them, the KCl content is 40.47%, the Mg 2 The Cl content is 4.15% and the NaCl content is 44.67%.
[0047] In crude potassium, the content of KCl is 73.01wt%, MgCl 2 The content of O is 3.86wt%, and the content of NaCl is 6.67wt%, which are used for further preparation of potassium chloride.
[0048] Example 2
[0049] The main components of sodium carnallite are KCl: 17.96%, MgCl 2 : 28.55%, NaCl: 18.92%, the crystallization underflow generated in the process of preparing potassium chloride by the "reverse flotation-cold crystallization" process, wherein the solid content in the crystallization underflow is 26.56%, and the content of KCl is 75.26%.
[0050] Screening is carried out through a two-stage screening device. First, a first-stage screening device is used for screening. The aperture of the first-stage screening device is 800μm. The tailings with a particle size greater than 800μm and the filter material with a particle size less than 800μm in the underflow are separated, and the weight ratio of the two is 5:95; the filter material with a particle size less than 800μm is screened by a second-stage screening device with an aperture of 600μm to separate natural potassium salt with a particle size range of 600-800μm and a component with a particle size less than 600μm, that is, crude potassium, and the weight ratio of the two is 5:90.
[0051] The separated natural potassium salt was subjected to SEM analysis, and the characterization results were as follows Figure 3 As shown, the content of KCl is 38.45wt%, MgCl 2 The content of Ag was 3.75wt% and the content of NaCl was 43.24wt%.
[0052] The crude potassium content is 75.26 wt% KCl, 75.26 wt% MgCl 2 The content of N is 2.74%wt% and the content of NaCl is 4.55%wt%, which are used to further prepare potassium chloride.
[0053] Example 3
[0054] The main components of sodium carnallite are KCl: 18.26%, MgCl 2 : 28.16%, NaCl: 18.56%, the crystallization underflow generated in the process of preparing potassium chloride by the "reverse flotation-cold crystallization" process, wherein the solid content in the crystallization underflow is 34.36%, and the content of KCl is 65wt%.
[0055] Screening is carried out through a two-stage screening device. First, a first-stage screening device with an aperture of 800μm is used for screening. The tailings with a particle size greater than 800μm and the filter material with a particle size less than 800μm in the underflow are separated, and the weight ratio of the two is 5:95; the filter material with a particle size less than 800μm is screened by a second-stage screening device with an aperture of 600μm. The weight ratio of the two is 5:90, and natural potassium salt with a particle size range of 600-800μm and components with a particle size less than 600μm, that is, crude potassium, are separated.
[0056] The separated natural potassium salt was subjected to component determination, wherein the content of KCl was 36.43wt%, MgCl 2 The content of Ag was 4.36 wt% and the content of NaCl was 44.73 wt%.
[0057] The crude potassium content is 65.26 wt% KCl, 65.26 wt% MgCl 2 The content of O is 5.88wt% and the content of NaCl is 8.56wt%, which are used to further prepare potassium chloride.
[0058] Comparative Example 1
[0059] The composition of the crystallization underflow is the same as in Example 1.
[0060] Screening is performed through a two-stage screening device. First, a first-stage screening device is used for screening. The aperture of the first-stage screening device is 1000μm. The tailings with a particle size greater than 1000μm and the filter material with a particle size less than 1000μm in the underflow are separated, and the weight ratio of the two is 1:99; the filter material with a particle size less than 1000μm is screened by a second-stage screening device with an aperture of 800μm to separate the components with a particle size range of 800-1000μm and the components with a particle size less than 800μm, and the weight ratio of the two is 3:96.
[0061] The fractions separated from the sample with a particle size range of 800 to 1000 μm contained 7.53 wt% KCl and 2.34 wt% MgCl. 2 The content of O is 5.43wt% and the content of NaCl is 72.56wt%, and the main components are carnallite and sodium chloride.
[0062] In the component with a particle size less than 800 μm, the content of KCl is 70.26 wt%, MgCl 2 The content of Ag was 4.83 wt% and the content of NaCl was 5.21 wt%.
[0063] Comparative Example 2
[0064] The composition of the crystallization underflow is the same as in Example 1.
[0065] Screening is performed through a two-stage screening device. First, a first-stage screening device is used for screening. The aperture of the first-stage screening device is 600μm. The tailings with a particle size greater than 600μm and the filter material with a particle size less than 600μm in the underflow are separated, and the weight ratio of the two is 10:90; the filter material with a particle size less than 600μm is screened by a second-stage screening device with an aperture of 500μm to separate the components with a particle size range of 500-600μm and the components with a particle size less than 500μm, and the weight ratio of the two is 10:90.
[0066] The fractions separated from the sample with a particle size range of 500 to 600 μm contained 78.77 wt% KCl and 28.77 wt% MgCl. 2 The content of O is 3.46wt% and the content of NaCl is 3.76wt%, and it contains almost no natural potassium salt.
[0067] In the component with particle size less than 500 μm, the content of KCl is 78.24 wt%, MgCl 2 The content of Ag was 2.54 wt% and the content of NaCl was 3.55 wt%.
[0068] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects: Since sodium-containing carnallite is NaCl and xKCl·yMgCl 2 ·zH 2 In the process of studying the reverse flotation-cold crystallization method for producing KCl, the researchers of this application unexpectedly found that the component with a particle size of 600-800 μm in the crystallization underflow obtained after the reverse flotation-cold crystallization method is a natural potassium salt with a eutectic structure. By using this method, natural potassium salt can be separated in the process of preparing potassium chloride, further improving the application value of sodium-containing carnallite, and the natural potassium salt has good quality and can be used to prepare low-sodium salt.
[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for separating natural sylvite from sodium-containing carnallite, characterized in that: include: The crystal underflow obtained by reverse flotation and cold decomposition of sodium-containing carnallite is screened, and components with a particle size range of 600 to 800 μm are collected to obtain natural potassium salt.
2. The method for separating natural sylvite from sodium-containing carnallite according to claim 1, characterized in that: In the crystallization bottom flow, the content of KCl in the solid component is greater than or equal to 72%, preferably 72% to 80%.
3. The method for separating natural sylvite from sodium-containing carnallite according to claim 1, characterized in that: The solid content of the crystallization underflow is 25% to 35%.
4. The method for separating natural sylvite from sodium-containing carnallite according to claim 1, characterized in that: The screening includes primary screening and secondary screening. The primary screening separates the crystallization bottom flow into a first screening product with a particle size greater than 800 μm and a second screening product with a particle size less than or equal to 800 μm. The secondary screening separates the second screening product into natural potassium salt with a particle size of 600 to 800 μm and a third screening product with a particle size less than 600 μm.
5. The method for separating natural sylvite from sodium-containing carnallite according to claim 4, characterized in that: The first screening product includes: 8-10wt% KCl, 3-4.5wt% MgCl2 and 78-85wt% NaCl.
6. The method for separating natural sylvite from sodium-containing carnallite according to claim 4, characterized in that: The third screening product includes: 70-80wt% KCl, 2.5-5wt% MgCl2 and 3-6wt% NaCl.
7. The method for separating natural sylvite from sodium-containing carnallite according to claim 1, characterized in that: The sodium-containing carnallite contains 17-21wt% of KCl, 27-28wt% of MgCl2 and 17-19wt% of NaCl.
8. The method for separating natural sylvite from sodium-containing carnallite according to claim 1, characterized in that: The natural potassium rock salt comprises: 35-45wt% KCl, 3-4.5wt% MgCl2 and 40-45wt% NaCl.
9. A natural potassium salt, characterized in that: The method for separating natural sylvite from sodium-containing carnallite according to any one of claims 1 to 8 is used to obtain the natural sylvite.
10. Use of the natural potassium rock salt as claimed in claim 9 as a raw material in the process of preparing low sodium salt.
Citation Information
Patent Citations
Method for preparing low-sodium-content carnallite and potassium chloride from high-sodium-content carnallite
CN111362730A
A method for producing potassium chloride using carnallite
CN111533138B
Preparation method of low-sodium salt
CN113753920A