Repeatable wide-temperature-range self-lubricating composite ceramic and preparation method thereof

By using the core-shell structure and Ag interface of ZrO2 and SrSO4 in ceramic materials, combined with the optimization of sintering process and the addition of Al2O3, the problem of failure of ceramic self-lubricating materials after high temperature is solved, and continuous lubrication and multiple repetitions in a wide temperature range are achieved. Use meets the lubrication requirements of equipment in multiple startups and repeated service.

CN119080492APending Publication Date: 2024-12-06LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411274452.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing ceramic self-lubricating materials lose their lubrication effect after high temperatures in an oxidizing environment, and cannot be reused in a wide temperature range, and cannot meet the lubrication needs of multiple start-up and repeated service equipment.

Method used

ZrO2 is used as the matrix and SrSO4 is the lubricating phase to form a core-shell structure, and Ag is introduced at the interface. By optimizing the sintering process and adding Al2O3, it can improve the bonding strength and overall mechanical properties of the material, avoid oxidation and decomposition, and achieve room temperature to 1000℃. Continuous lubrication performance.

Benefits of technology

Continuous lubrication and multiple reuses in a wide temperature range (room temperature to 1000°C), avoiding residual stress and cracking problems caused by poor thermal matching, and maintaining excellent lubrication performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080492A_ABST
    Figure CN119080492A_ABST
Patent Text Reader

Abstract

The invention discloses a self-lubricating composite ceramic capable of continuously lubricating in a wide temperature range and being repeatedly used. Wherein the ZrO2 is used as a matrix, the SrSO4 is used as a lubricating phase, the SrSO4 is distributed in the ZrO2 matrix in a granular manner, and a core-shell structure of ZrO2 coated SrSO4 particles is formed after sintering; according to the structural design, the problem that materials are difficult to sinter or follow-up cracking is caused due to large residual stress caused by poor two-phase thermal matching can be solved; and meanwhile, effective lubricating performance is realized by combining the soft property of SrSO4 and the surface texture property formed by the distribution form of the SrSO4. According to the wide-temperature-range continuous-lubricating and reusable self-lubricating composite ceramic material disclosed by the invention, components with low melting points or low decomposition temperatures are not involved in each phase, so that the phase composition is not influenced by the temperature after high-temperature service, and the material still has excellent lubricating performance at the room temperature to 1000 DEG C when being repeatedly used.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composite ceramic material, in particular to a self-lubricating composite ceramic with a wide temperature range and which can be repeatedly used, and a preparation method thereof. Background Art

[0002] Lubricating materials are the key to ensuring that the moving parts of various mechanical equipment can serve normally. They achieve efficient, stable and long-life service of sliding parts by reducing the friction coefficient and wear rate of the friction pair. Solid lubricating materials are widely used in harsh environments with high temperature, high speed, corrosive media and other conditions. They are the core of lubrication guarantee for moving parts of equipment. They are usually used in the form of sliding bearings, sliding bushings, slide rails and other forms in moving parts of various equipment. With the rapid development and upgrading of equipment, the service conditions of solid lubricating materials have become more and more harsh. Not only has the service temperature increased significantly, but it is also required to be able to continuously lubricate in a wide temperature range and maintain long-life cyclical service.

[0003] Ceramic self-lubricating composite materials are the most promising of high-temperature and wide-temperature self-lubricating composite materials. Since ceramic-based materials have good designability, solid lubricating phases are usually added to the ceramic matrix to achieve lubrication functions for specific working conditions. China's invention patent (CN117683464A) discloses wide-temperature lubrication and protective coatings, which utilize the lubrication properties of molybdenum disulfide (MoS2), graphite, MXene, inorganic oxygen-containing acid salts, etc. at different temperatures to achieve effective lubrication in the range of 25°C to 800°C at room temperature. However, in an oxidizing environment, MoS2 and graphite will lose their lubricating effect due to oxidation after being exposed to a high temperature of 800°C, so they cannot repeatedly play a lubricating role in an oxidizing environment. China's invention patent (CN111549258A) reports a high-temperature lubricating material that has excellent lubrication properties at 800°C to 1000°C. Although its phase composition will not decompose or fail due to oxidation within this temperature range, it cannot meet the demand for excellent lubrication properties in the medium and low temperature service environment. In summary, the lubricating materials in the existing related technologies can only be used for one-way lubrication from low temperature to high temperature during use, because some lubricating phases oxidize or decompose under high temperature conditions, causing them to lose their lubricating properties under low temperature conditions; or they can meet the repeated lubrication requirements under high temperature service conditions, but cannot meet the lubrication requirements in the medium and low temperature ranges. Therefore, for equipment and mechanisms that are started up multiple times and repeatedly served, it is still necessary to develop a wide temperature range lubricating material to meet their application needs. Summary of the invention

[0004] The purpose of the present invention is to disclose a self-lubricating composite ceramic that can be repeatedly used in a wide temperature range and a preparation method thereof, so as to obtain a self-lubricating composite ceramic that can continuously lubricate and be reusable in a wide temperature range from room temperature to 1000°C, thereby meeting the new demand for lubricating materials in mechanical equipment.

[0005] The present invention provides a self-lubricating composite ceramic with continuous lubrication in a wide temperature range and reusable properties. Among them, ZrO2 is used as a matrix, SrSO4 is used as a lubricating phase, SrSO4 is distributed in the ZrO2 matrix in a granular form, and after sintering, a core-shell structure of ZrO2-coated SrSO4 particles is formed; wherein the mass fraction of SrSO4 powder (accounting for the total weight of the mixed powder) is 20% to 70%, and the size range is 0.05 to 0.3 mm, preferably 0.15 to 0.2 mm; the mass fraction of ZrO2 powder (accounting for the total weight of the mixed powder) is 80% to 30%, and the particle size range is 20 nm to 10 μm, preferably 20 to 100 nm.

[0006] This structural design can avoid large residual stress caused by poor thermal matching between the two phases, which makes it difficult to sinter the material or causes subsequent cracking problems; at the same time, it combines the soft properties of SrSO4 and the surface texture characteristics formed by its distribution form to achieve effective lubrication performance.

[0007] In addition, a layer of Ag interface can be introduced at the interface between ZrO2 matrix and SrSO4 particles, such as Figure 1 As shown, it can effectively enhance the bonding strength between the particles and the matrix, and at the same time separate the two phases to avoid the reaction between ZrO2 and SrSO4 during the sintering process to generate hard phases such as SrZrO3. Ag can also be further distributed in the ZrO2 matrix, which can promote low-temperature lubrication and, more importantly, stabilize the friction state at various temperatures.

[0008] The content of Ag accounts for 2% to 10% of the total mass of the material, and the particle size of the added silver powder ranges from 0.1 to 3 μm. Excessive Ag is easy to flow out during the sintering process and it is not easy to control the content. Moreover, when used at a high temperature of 1000°C, it is easy to precipitate to the surface to form spherical particles or flow away, so the content of Ag is extremely critical.

[0009] The SrSO4 is in rod-like form, with a diameter of 0.10-0.20 micrometers and a length of 0.25-1.00 micrometers. Figure 2 The SrSO4 can also be replaced by BaSrSO4.

[0010] In order to improve the overall mechanical properties of the material, a small amount of ZrO2 can be introduced into the sulfate particles in advance, with a mass content of no more than 10% (accounting for the relative weight of the lubricant), or Al2O3 with a mass fraction of no more than 15% (accounting for the relative weight of the matrix) can be introduced into the ZrO2 matrix in advance to strengthen the particles and the matrix, such as Figure 1 shown.

[0011] The present invention also provides a method for preparing the above ceramic material, the steps are as follows: 1) Preparation of SrSO4 particles: rod-shaped SrSO4 is used as the initial raw material, 2% PVA solution is used as the crosslinking agent, the mixture is loaded into a ball mill, and the particles are agglomerated into particles by high-speed vibration and shaking, and then gradient sieved according to the particle size range of 0.05 mm for standby use; wherein the mass ratio of SrSO4 to PVA solution is 20:0.5~2, the vibration frequency is 15~40 Hz, and the vibration shaking time is 3~5 min; 2) Coating the Ag interface: Weigh 0.15-0.2 mm SrSO4 particles and 0.1-3 μm Ag powder according to the mass ratio and put them into a ball mill. Coat the surface of the SrSO4 particles with Ag by slow vibration and shaking to form a double-layer structure; the frequency is 15-40 Hz and the vibration and shaking time is 3-5 min; When it is necessary to add Ag powder to the ZrO2 matrix, Ag can be evenly distributed in the ZrO2 powder by ball milling.

[0012] 3) Densification sintering: Mix the mixed particles obtained in step 2) with the corresponding amount of ZrO2 powder, and mix them evenly by mechanical shaking. Then put the mixed powder into a graphite mold and cold press it by bidirectional pressure at a pressure of 10-15MPa for 5-10min. Finally, sinter it at a high temperature of 1100-1300℃ for 10-30min and maintain the pressure at 20-40MPa. During the heat and pressure maintenance period, an oscillation pressure action can be performed every 3-5min, and the pressure oscillation amplitude is 10-20MPa.

[0013] The beneficial effects of the present invention are as follows: The self-lubricating composite ceramic material with wide temperature range continuous lubrication and reusable properties involved in the present invention does not involve components with low melting points or low decomposition temperatures. Therefore, the phase composition is not affected by temperature after high-temperature service, and it still has excellent lubrication properties at room temperature to 1000°C when reused. The melting point of Ag is close to 1000°C (about 960°C), but because its content is very small, it mainly plays the function of stabilizing the friction state. It will not cause corresponding loss under 1000°C conditions and can also meet the needs of repeated use. Therefore, this material not only meets the needs of continuous lubrication from room temperature to 1000°C, but also can achieve the function of repeated use. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a schematic diagram of the structure of the wide temperature range self-lubricating composite ceramic of the present invention.

[0015] Figure 2 This is a photo of the rod-shaped SrSO4 used in the wide temperature range self-lubricating composite ceramic of the present invention.

[0016] Figure 3This is a photo of the self-lubricating composite ceramic prepared in Example 2 of the present invention.

[0017] Figure 4 This is a typical friction coefficient curve of the self-lubricating composite ceramic prepared in Example 3 of the present invention at different temperatures.

[0018] Figure 5 The average friction coefficient of the self-lubricating composite ceramic prepared in Example 4 of the present invention in cyclic tests at different temperatures. DETAILED DESCRIPTION

[0019] The following is a detailed description of the self-lubricating composite ceramic capable of repeated use over a wide temperature range and its preparation method in conjunction with specific embodiments of the present invention.

[0020] Example 1 SrSO4 powder was mixed with PVA solution with a mass concentration of 2% at a mass ratio of 20:1, stirred evenly, and then put into a vibrating ball mill and shaken to form particles of different diameters. A stainless steel sieve was used to screen the particles according to a gradient in the particle size range of 0.05 mm, and 7.5 g of SrSO4 particles with a particle size of 0.10-0.15 mm were selected and mixed with 7.5 g of ZrO2 powder with a particle size of 20-100 nm. The mixture was shaken to make it evenly mixed and form a core-shell structure of ZrO2-coated SrSO4 particles. Finally, it was put into a graphite mold and cold pressed by bidirectional pressure at a pressure of 15 MPa for 5 min. The sample and the mold were put into a vacuum hot pressing sintering furnace for sintering to obtain a ZrO2-based composite ceramic material. The sintering temperature was 1100 ° C, the temperature and pressure were kept for 30 min, and the pressure was 20 MPa.

[0021] After testing, the prepared ZrO2-based composite ceramics were subjected to friction tests at room temperature, 200°C, 400°C, 600°C, 800°C and 1000°C by a reciprocating friction and wear tester. Although the friction coefficient fluctuates within the entire temperature range, the average friction coefficient at each temperature point does not exceed 0.40.

[0022] Example 2 SrSO4 powder was mixed with PVA solution with a mass concentration of 2% at a mass ratio of 20:1, stirred evenly, and then put into a vibrating ball mill and shaken to form particles of different diameters. A stainless steel sieve was used to sieve the particles according to a gradient in the particle size range of 0.05 mm for later use. First, 7.05g of SrSO4 particles with a particle size of 0.15-0.20mm and 0.45g of Ag powder with a particle size range of 0.1-3μm were weighed in proportion, shaken and mixed evenly to form a core-shell structure of Ag-coated SrSO4 particles, and then 7.5g of ZrO2 powder with a particle size of 20-100nm was weighed and mixed and added to it and shaken again to make it evenly mixed to prepare a three-layer core-shell structure of ZrO2-Ag-SrSO4 particles. The obtained powder with a three-layer core-shell structure was put into a graphite mold and cold pressed by bidirectional pressure at a pressure of 15MPa and maintained for 5min. Finally, the sintering was carried out in a vacuum hot pressing sintering furnace. The sintering process was as follows: temperature of 1225°C, pressure of 10-20 MPa oscillation pressure, oscillation frequency of 3 min, and heat preservation for 20 min.

[0023] The optical photograph of the prepared ZrO2-based wide temperature range friction and wear composite ceramic material after polishing is shown in Figure 2. Figure 3 The friction tests were carried out at room temperature, 200℃, 400℃, 600℃, 800℃ and 1000℃ by a reciprocating friction tester, and the average friction coefficients in the corresponding temperature sections were 0.25, 0.41, 0.28, 0.42, 0.28 and 0.40 respectively.

[0024] Example 3 BaSrSO4 powder was mixed with 2% PVA solution at a mass ratio of 20:1, stirred evenly, and then put into a vibrating ball mill to shake the BaSrSO4 powder to form particles of different diameters. A stainless steel sieve was used to sieve the particles in a gradient range of 0.05 mm for later use. ZrO2 powder and Ag powder were mixed at a mass ratio of 16:1 and placed in a ball mill, and Al2O3 grinding balls twice the mass of the powder and a certain amount of anhydrous ethanol were added. After ball milling for 96 hours, the powder was dried and passed through a 100-sieve to prepare Ag-ZrO2 mixed powder. First, weigh 8.5g of BaSrSO4 particles with a particle size of 0.15~0.20mm and 0.5g of Ag powder in proportion, shake and mix them evenly to form a core-shell structure of Ag-coated BaSrSO4 particles, then weigh 6g of Ag+ZrO2 powder and mix them in, shake them again to make them evenly mixed to prepare a three-layer core-shell structure of (Ag+ZrO2)-Ag-BaSrSO4 particles. The obtained powder with a three-layer core-shell structure is loaded into a graphite mold and cold pressed by bidirectional pressure at a pressure of 15MPa for 5min. Finally, it is sintered in a vacuum hot pressing sintering furnace. The sintering process is a temperature of 1210℃, a pressure of 10~20 MPa oscillation pressure, an oscillation time interval of 5min, and a heat preservation of 30min.

[0025] The prepared ZrO2-based wide temperature range friction and wear composite ceramic material was polished and then subjected to reciprocating friction and wear tests. The friction coefficient curves at room temperature, 200℃, 400℃, 600℃, 800℃ and 1000℃ are shown in Figure 2. Figure 4 As shown, the friction coefficient is no higher than 0.3 at each temperature.

[0026] Example 4 SrSO4 powder was mixed with 2% PVA solution at a mass ratio of 20:1, stirred evenly, and then placed in a vibrating ball mill to shake the SrSO4 powder to form particles of different diameters. A stainless steel sieve was used to sieve the particles in a gradient range of 0.05 mm for later use. ZrO2 powder and Ag powder were mixed at a mass ratio of 16:1 and placed in a ball mill, and Al2O3 grinding balls twice the mass of the powder and a certain amount of anhydrous ethanol were added. After ball milling for 96 hours, the powder was dried and passed through a 100-sieve to prepare Ag-ZrO2 mixed powder. First, weigh 5.6g of SrSO4 particles with a particle size of 0.15-0.20mm and 0.1g of Ag powder in proportion, shake and mix them evenly to form a core-shell structure of Ag-coated SrSO4 particles, then weigh 4.3g of Ag+ZrO2 powder and mix them in, shake them again to make them evenly mixed to prepare a three-layer core-shell structure of (Ag+ZrO2)-Ag-SrSO4 particles. The obtained powder with a three-layer core-shell structure is loaded into a graphite mold and cold pressed by bidirectional pressure at a pressure of 15MPa for 5min. The sample is sintered in a spark plasma sintering furnace, where the sintering temperature is 1210℃ and the pressure is 40 MPa. The target material is obtained after keeping the temperature and pressure for 10min.

[0027] The prepared ZrO2-based composite ceramics were subjected to cyclic friction tests at room temperature, 200℃, 400℃, 600℃, 800℃ and 1000℃ using a reciprocating friction tester. The results are as follows: Figure 5 The average friction coefficient of the two tests in each temperature range was maintained at about 0.25, indicating excellent repeatable lubrication performance over a wide temperature range.

Claims

1. A self-lubricating composite ceramic that can be used repeatedly over a wide temperature range. It is characterized in that SrSO 4 The lubricating phase is evenly distributed in ZrO 2 Densification sintering in the matrix to form ZrO 2 Coated SrSO 4 The core-shell structure of the particles; SrSO 4 The mass fraction of the powder is 20%~70%, and the size range is 0.15~0.2mm; ZrO 2 The mass fraction of the powder is 80%~30%, and the particle size ranges from 20nm~10 μm.

2. A self-lubricating composite ceramic that can be repeatedly used over a wide temperature range as claimed in claim 1, It is characterized in that The SrSO 4 It can also be made of BaSrSO 4 Instead, BaSrSO 4 The mass fraction of the powder is 20%~70%, and the size range is 0.15~0.2mm.

3. A self-lubricating composite ceramic that can be repeatedly used over a wide temperature range as claimed in claim 1, It is characterized in that In the ZrO 2 Matrix and SrSO 4 A layer of Ag interface can also be introduced at the lubricating phase interface to form ZrO 2 -Ag-SrSO 4 The three-layer core-shell structure is formed; the particle size of the Ag powder ranges from 0.1 to 3 μm, and the mass fraction of the Ag powder is from 2% to 10%.

4. A method for preparing a self-lubricating composite ceramic that can be repeatedly used in a wide temperature range as claimed in claim 3, It is characterized in that The following steps are involved: 1) Preparation of SrSO 4 Particles: rod-shaped SrSO 4 As the initial raw material, 2% PVA solution is used as a crosslinking agent, and after mixing, it is loaded into a ball mill, and agglomerated into particles by high-speed vibration and shaking, and then gradient sieved according to the particle size range of 0.05 mm for use; Among them, SrSO 4 The mass ratio of the PVA solution is 20:0.5~2, the vibration frequency is 15~40 Hz, and the vibration shaking time is 3~5 min; 2) Wrapping Ag interface: Weigh 0.15~0.2 mm SrSO according to the mass ratio 4 The particles and 0.1~3 μm Ag powder were put into the ball mill and slowly vibrated to make Ag wrapped in SrSO 4 A double-layer structure is formed on the particle surface; the frequency is 15-40 Hz and the vibration time is 3-5 min; 3) Densification sintering: The mixed particles obtained in step 2) are mixed with a corresponding amount of ZrO 2 The powders are mixed and evenly mixed by mechanical shaking. The mixed powders are then loaded into a graphite mold and cold pressed by bidirectional pressurization at a pressure of 10-15 MPa for 5-10 min. Finally, they are pressurized and sintered at a high temperature of 1100-1300°C for 10-30 min and a pressure of 20-40 MPa.

5. A method for preparing a self-lubricating composite ceramic that can be repeatedly used in a wide temperature range as claimed in claim 4, It is characterized in that In step 3), during the heat and pressure holding period, an oscillating pressure action can be performed every 3 to 5 minutes, and the pressure oscillation amplitude is 10 to 20 MPa.

Citation Information

Patent Citations

  • High-strength low-burn resin-based self-lubricating grinding wheel and preparation method thereof

    CN115741506A

  • Preparation method of wide-temperature-range high-entropy alloy-based self-lubricating coating

    CN118064822A

  • self-lubricating ceramics

    JP2942830B1