Graphitized cathode, preparation method, aluminum electrolysis cell and aluminum electrolysis method

By covering the TiB2 composite layer on the graphitized cathode, the problem of sodium-potassium permeation failure in the low-temperature aluminum electrolytic cell is solved, the cathode's anti-permeability and hardness are improved, and the service life of the electrolytic cell is extended.

CN119080533APending Publication Date: 2024-12-06ZHENGZHOU NON FERROUS METALS RES INST CO LTD OF CHALCO
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN202411239772.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the low-temperature aluminum electrolyte, the problem of sodium-potassium permeation and damage of the graphitized cathode by the low-temperature electrolyte, resulting in cathode expansion, cracking and layered powdering, affecting the normal operation and life of the electrolyte cell.

Method used

The TiB2 composite layer is used to cover the graphitized cathode matrix with a carbon content of less than 20 wt.%, and a thickness of 5mm-50mm. The dense composite layer is formed by integrated press molding and sintering to enhance the anti-permeability and hardness.

Benefits of technology

It effectively resists the sodium-potassium permeation and expansion of low-temperature electrolytes, improves the wettability and hardness of the cathode, extends the service life of the electrolytic cell, and avoids layered powdering and peeling of the cathode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080533A_ABST
    Figure CN119080533A_ABST
Patent Text Reader

Abstract

The invention provides a graphitized cathode, a preparation method, an aluminum electrolysis cell and an aluminum electrolysis method, and belongs to the field of aluminum smelting. Comprising a graphitized cathode substrate; the invention discloses a graphitized cathode which comprises a graphitized cathode substrate and a TiB2 composite layer, at least part of the surface of the graphitized cathode substrate is covered with the TiB2 composite layer, the carbon content of the TiB2 composite layer is smaller than 20 wt.%, and the thickness of the TiB2 composite layer ranges from 5 mm to 50 mm. Firstly, the TiB2 composite material can show excellent anti-permeation performance; and secondly, when the carbon content in the TiB2 composite material is less than 20wt.%, the prepared cathode has good wettability with aluminum water and high hardness, and can effectively resist sodium-potassium permeation expansion of low-temperature electrolyte. And thirdly, the thickness of the composite layer is limited to be 5mm-50mm, so that the permeation and expansion resistance of the cathode and molten aluminum can be met. Therefore, the sodium-potassium permeation damage of the low-temperature electrolyte to the graphitized cathode is resisted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of aluminum smelting, and in particular to a graphitized cathode and a preparation method thereof, an aluminum electrolysis cell, and an aluminum electrolysis method. Background Art

[0002] Graphitized cathode is a cathode carbon block made of petroleum coke, asphalt coke, etc. as the main raw materials, through molding, roasting, impregnation and high-temperature graphitization treatment above 2300℃. In this process, the carbon elements in the raw materials are rearranged at high temperature to form a crystal structure similar to graphite, thus giving the carbon block excellent electrical conductivity, thermal conductivity and corrosion resistance. Graphitized cathode is mainly used as the cathode material of aluminum electrolytic cells. In the aluminum electrolytic production process, it is an important part of the conductor and the lining of the electrolytic cell, and plays a key role in improving current efficiency, reducing energy consumption, and extending the life of the electrolytic cell.

[0003] However, when low-temperature aluminum electrolysis is carried out on the current industrial pre-baked carbon anode aluminum electrolytic cell, the low-temperature electrolyte system usually contains a high potassium content, which has a strong penetration and damage effect on the carbon cathode, especially when the aluminum electrolytic cell uses ordinary carbon blocks, semi-graphite, and graphite cathode materials. The cathode is prone to expansion and cracking after being corroded by potassium. The risk of potassium expansion and cracking of graphitized cathodes is slightly smaller, but graphite is soft and weak in potassium penetration. There are also problems of layered powdering and flaking due to potassium corrosion in long-term operation. Therefore, it is urgent to develop a method that can solve the problem of sodium-potassium penetration and damage to the cathode by low-temperature electrolytes. Summary of the invention

[0004] The present application provides a graphitized cathode and a preparation method thereof, an aluminum electrolysis cell, and an aluminum electrolysis method to solve the following technical problem: how to resist the sodium-potassium penetration damage of a low-temperature electrolyte to a graphitized cathode.

[0005] In a first aspect, the present application provides a graphitized cathode, the graphitized cathode comprising:

[0006] a graphitized cathode substrate; and

[0007] A TiB2 composite layer, wherein the TiB2 composite layer covers at least a portion of the surface of the graphitized cathode substrate, the carbon content of the TiB2 composite layer is less than 20wt.%, and the thickness of the TiB2 composite layer is 5mm-50mm.

[0008] In a second aspect, the present application provides a method for preparing the graphitized cathode according to the first aspect, the method comprising:

[0009] Obtaining TiB2 composite paste material and / or TiB2 composite powder material;

[0010] Laying the TiB2 composite paste on the surface of the graphitized cathode paste to obtain a mixed material; or

[0011] Laying TiB2 composite powder material on the surface of graphitized cathode paste to obtain a mixed material; or

[0012] Laying a TiB2 composite paste on the surface of a graphitized cathode paste, and laying a TiB2 composite powder on the upper surface of the TiB2 composite paste to obtain a mixed material;

[0013] The mixed material is integrally pressed and sintered to obtain a graphitized cathode.

[0014] Optionally, the components of the TiB2 composite paste are: 12wt.%-15wt.% of asphalt, 0.1wt.%-1wt.% of graphite fiber, and the balance is TiB2 powder.

[0015] Optionally, the components of the TiB2 composite powder material are: 2wt.%-10wt.% TiN powder, 1wt.%-5wt.% CoB powder, 1wt.%-3wt.% ZrB2 powder, 1wt.%-3wt.% metal powder, 1wt.%-2wt.% polyvinyl alcohol binder, and the balance is TiB2 powder.

[0016] In a third aspect, the present application provides a low-temperature aluminum electrolysis cell, which includes the graphitized cathode described in the first aspect.

[0017] Optionally, a forced heat dissipation device is provided on the side wall tank shell of the aluminum electrolysis tank;

[0018] The distance between the side wall lining of the aluminum electrolytic cell and the carbon anode is ≥320 mm;

[0019] After the graphitized cathode is connected to the cathode collector rod, the vertical distance between the upper surface of the graphitized cathode and the upper surface of the cathode collector rod is ≥300 mm.

[0020] Optionally, the distance between the side wall lining of the aluminum electrolytic cell and the carbon anode is 320 mm-380 mm;

[0021] The vertical distance between the upper surface of the graphitized cathode and the upper surface of the cathode collector rod is 300 mm-340 mm.

[0022] Optionally, the forced heat dissipation device includes: one or more of a vertical heat sink, an air-cooled heat exchanger, and a thermal oil-cooled heat exchanger;

[0023] The connection between the graphitized cathode and the cathode collector rod is cast by phosphorus pig iron, and the cathode collector rod is made of one of a high-conductivity steel rod and a copper-inserted steel rod.

[0024] In a fourth aspect, the present application provides a low-temperature aluminum electrolysis method, which adopts the low-temperature aluminum electrolysis cell described in any one of the third aspects, and the method includes the following parameters: the initial crystallization temperature of the low-temperature electrolyte is 820℃-850℃, the electrolysis temperature is 845℃-900℃, and the superheat is 20℃-50℃.

[0025] Optionally, the components of the low-temperature electrolyte are: KF: 12wt.%-15wt.%, LiF: 1wt.%-2wt.%, CaF2: 0-5wt.%, MgF2: 0-2wt.%, Al2O3: 2wt.%-4wt.%, NaF: 26wt.%-33wt.%, and the balance is AlF3.

[0026] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0027] The present application provides a graphitized cathode, which includes: a graphitized cathode substrate; and a TiB2 composite layer, wherein the TiB2 composite layer covers at least part of the surface of the graphitized cathode substrate, the carbon content of the TiB2 composite layer is less than 20wt.%, and the thickness of the TiB2 composite layer is 5mm-50mm. First, the TiB2 composite material exhibits excellent anti-permeation performance for the sodium-potassium permeation problem in the harsh environment of the electrolytic cell. Secondly, when the carbon content in the TiB2 composite material is less than 20wt.%, the prepared cathode has good wettability with aluminum water, high hardness, and can effectively resist the sodium-potassium permeation expansion of the low-temperature electrolyte. Thirdly, the thickness of the composite layer is limited to 5mm-50mm, which can meet the anti-permeation expansion performance of the cathode and aluminum water. In addition, when the thickness of the composite layer exceeds 50mm, due to the difference between the sintering shrinkage rate of the TiB2 composite material and the graphitized cathode, microcracks may be generated on the composite layer, thereby reducing its anti-permeation effect. This resists the sodium-potassium penetration damage to the graphitized cathode caused by the low-temperature electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0029] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0030] Figure 1A schematic diagram of a graphitized cathode provided in an embodiment of the present application;

[0031] Figure 2 A flow chart of a method for preparing a graphitized cathode provided in an embodiment of the present application;

[0032] Figure 3 A schematic diagram of a low-temperature aluminum electrolysis cell provided in an embodiment of the present application;

[0033] Description of the accompanying drawings:

[0034] 1- anode guide rod; 2- gas collecting hood and slot cover; 3- anode steel claw; 4- anode; 5- furnace side crust; 6- forced heat dissipation device; 7- TiB2 composite layer; 8- graphitized cathode matrix; 9- thermal insulation material; 10- cathode collector rod (copper-inserted steel rod); 11- aluminum liquid; 13- side wall lining; 14- electrolyte melt; 15 heat exchange medium outlet. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0036] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0037] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.

[0038] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0039] The creative ideas of this application are:

[0040] Low-temperature aluminum electrolysis has the advantages of reducing heat dissipation in aluminum electrolysis cells, reducing energy consumption, and improving current efficiency, and is considered an important direction for energy conservation in the aluminum electrolysis industry. In addition, low-temperature aluminum electrolysis is also an important way to solve the corrosion resistance of inert anodes, so low-temperature aluminum electrolysis has been widely studied in the field of aluminum smelting.

[0041] However, there are still many difficulties in carrying out low-temperature aluminum electrolysis production in the current industrial pre-baked carbon anode aluminum electrolysis cell. The main difficulties are: (1) The solubility and dissolution rate of alumina under low-temperature electrolysis conditions are low. If the alumina added to the electrolysis cell cannot be dissolved and diffused in time, it will precipitate to the bottom of the electrolysis cell. In addition, Na +The directional migration and enrichment effect toward the cathode cause the molecular ratio and initial crystallization temperature of the melt in the cathode area to increase. Under low-temperature electrolysis conditions, the high molecular ratio melt and alumina precipitate in the cathode area are very likely to form a crust, thus affecting the normal operation of the electrolytic cell. (2) If the problem of precipitation crust is simply solved by the high superheat method, it will bring about the problem of difficulty in forming a furnace wall crust on the side of the electrolytic cell to protect the side materials, and it will also affect the current efficiency and aggravate the volatilization of the electrolyte. (3) The low-temperature electrolyte system usually contains a high potassium content, which has a strong penetration and destructive effect on the carbon cathode. In particular, when the aluminum electrolytic cell uses ordinary carbon blocks, semi-graphite, and graphite cathode materials, the cathode is prone to expansion and cracking after being corroded by potassium. The risk of potassium expansion cracking in graphitized cathodes is slightly lower, but graphite is soft and weak in potassium penetration. In long-term operation, there are also problems of layered powdering and peeling due to potassium erosion. (4) Compared with conventional electrolyte systems, the conductivity of low-temperature electrolyte systems is usually low, which will lead to an increase in the cell voltage. If the cell voltage is directly reduced, the inter-electrode distance will be compressed. Due to the fluctuation of aluminum liquid, the compression of the inter-electrode distance will increase the oxidation loss of aluminum liquid and reduce the current efficiency. Therefore, before there are better measures to stabilize the flow (reduce aluminum liquid fluctuation), it is difficult to achieve low-voltage operation in low-temperature aluminum electrolysis, and the energy-saving effect of low-temperature aluminum electrolysis is limited.

[0042] At present, there are some related studies on low-temperature aluminum electrolysis. Patents CN201610868647.5, CN201210417817.X, and CN200910312193.3 provide low-temperature aluminum electrolytes above 880°C or above 850°C, focusing on solving the problems of low conductivity, low solubility and dissolution rate of alumina. Patents CN201010207080.X and CN201010587618.4 provide a highly conductive titanium boride cathode material and a preparation method thereof that can be highly wetted with aluminum liquid, resistant to electrolyte erosion and aluminum liquid erosion, and the cost can be lower than that of hot-pressed cathodes. However, from the perspective of the preparation process, it is still necessary to further research and develop to achieve large-scale application in existing prebaked anode aluminum electrolytic cells. Patents CN200710119898.4 and CN200710119908.4 introduce a production method for preparing a graphitized wettable cathode carbon block containing a TiB2 composite layer by vibration molding. However, the carbon content is still relatively high, even reaching about 80wt.%.

[0043] The above patented technologies all solve a single technical problem of low-temperature aluminum electrolysis from a single aspect, and simple integration cannot achieve low-temperature aluminum electrolysis. To solve the technical difficulties existing in the industrialization of low-temperature aluminum electrolysis, in addition to considering the cathode and low-temperature electrolyte system, it is also necessary to make overall improvements to the electrolytic cell structure, furnace side formation, low-voltage operation and other aspects in order to truly achieve low-temperature aluminum electrolysis. While selecting a reasonable low-temperature electrolyte system, maintaining matching process control parameters, and improving the dissolution performance of alumina, it is also necessary to effectively solve the sodium-potassium erosion problem of the electrolyte melt on the carbon cathode in the industrial electrolytic cell, solve the problem of furnace side formation under high superheat conditions of the low-temperature electrolyte system, and solve the problem of aluminum liquid stability and high current efficiency under low voltage conditions.

[0044] In summary, the field still lacks a complete set of low-temperature aluminum electrolysis technology to realize the industrial production of low-temperature aluminum electrolysis.

[0045] Figure 1 A schematic diagram of a graphitized cathode provided in an embodiment of the present application.

[0046] To address the above technical issues to a certain extent, please see Figure 1 , the present application provides a graphitized cathode, the graphitized cathode comprising:

[0047] a graphitized cathode substrate; and

[0048] A TiB2 composite layer, wherein the TiB2 composite layer covers at least a portion of the surface of the graphitized cathode substrate, the carbon content of the TiB2 composite layer is less than 20wt.%, and the thickness of the TiB2 composite layer is 5mm-50mm.

[0049] First, TiB2 composite materials can perform well in the harsh environment of electrolytic cells due to their high hardness, high melting point, wear resistance and corrosion resistance. In particular, for the sodium-potassium penetration problem in low-temperature electrolytes, TiB2 composite materials show excellent anti-penetration performance. Secondly, the results of laboratory-scale electrolysis tests show that when the carbon content in the TiB2 composite material is less than 20wt.%, the prepared cathode has good wettability with aluminum water, high hardness, and can effectively resist the sodium-potassium penetration expansion of low-temperature electrolytes. This discovery provides an important reference for industrial production. Thirdly, laboratory studies have found that the penetration depth of sodium-potassium penetration expansion is less than 5mm. Therefore, the thickness of the composite layer is limited to 5mm-50mm, which can meet the requirements of the wettability of the cathode with aluminum water, anti-penetration expansion performance and wear resistance. A thinner composite layer may not provide sufficient protection, while an overly thick composite layer will increase cost and weight. In addition, when the thickness of the composite layer exceeds 50mm, due to the difference between the sintering shrinkage of the TiB2 composite material and the graphitized cathode, microcracks may be generated on the composite layer, thereby reducing its anti-penetration effect. Exemplarily, the carbon content of the TiB2 composite layer can be 0, 2wt.%, 4wt.%, 6wt.%, 10wt.%, 12wt.%, 15wt.%, 19wt.%, etc., and the thickness of the TiB2 composite layer can be 5mm, 10mm, 15mm, 20mm, 30mm, 40mm, 50mm, etc.

[0050] Figure 2 A schematic flow chart of a method for preparing a graphitized cathode provided in an embodiment of the present application.

[0051] See also Figure 2 The present application provides a method for preparing the graphitized cathode described above, the method comprising:

[0052] S1, obtaining TiB2 composite paste material and / or TiB2 composite powder material;

[0053] S2a, laying the TiB2 composite paste on the surface of the graphitized cathode paste to obtain a mixture; or

[0054] S2b, laying TiB2 composite powder material on the surface of graphitized cathode paste to obtain a mixed material; or

[0055] S2c, laying the TiB2 composite paste on the surface of the graphitized cathode paste, and laying the TiB2 composite powder material on the upper surface of the TiB2 composite paste to obtain a mixed material;

[0056] S3, performing integrated pressing and sintering on the mixed material to obtain a graphitized cathode.

[0057] The present application adopts an integrated molding sintering technology to directly form a layer of TiB2 composite material layer on the surface of the graphitized cathode. This technology not only ensures the close combination between the composite layer and the graphitized cathode substrate, but also avoids the possible shedding problem of traditional coatings. At the same time, the raw material for forming the TiB2 composite layer of the present application can be a TiB2 composite paste, a TiB2 composite powder, or a combination of a TiB2 composite paste and a TiB2 composite powder. When the raw material of the TiB2 composite layer is a combination of a TiB2 composite paste and a TiB2 composite powder, a transition from a low-carbon to a carbon-free TiB2 composite material can be achieved, and the thickness of the TiB2 composite layer can be increased.

[0058] In some embodiments, the TiB2 composite paste is prepared by hot mixing and kneading.

[0059] In some embodiments, the TiB2 composite paste comprises: 12wt.%-15wt.% of asphalt, 0.1wt.%-1wt.% of graphite fiber, and the remainder is TiB2 powder.

[0060] Before being formed with the graphitized cathode paste, the TiB2 composite material exists in the form of a paste. This paste has good fluidity and plasticity, which is convenient for coating and molding on the surface of the graphitized cathode. Through specific pressing means (such as molding, extrusion, etc.), the paste can be evenly coated on the cathode surface, and after high-temperature sintering, a dense composite layer is formed. Asphalt is used as a binder. Asphalt can melt at high temperatures and firmly bond other components together to form a dense and stable composite layer. At the same time, asphalt also has a certain corrosion resistance and can protect the matrix from electrolyte erosion to a certain extent. The addition of graphite fiber can enhance the strength and toughness of the composite material and improve its wear resistance and anti-penetration performance during the electrolysis process. In addition, graphite fiber also has good conductivity, which helps to maintain the normal operation of the electrolyzer. TiB2 powder is the main component of the composite material, and its content accounts for the balance. Due to the high hardness and high melting point of TiB2, the composite material performs well in the harsh environment of the electrolyzer. At the same time, by controlling the amount of TiB2 powder, the carbon content of the composite material can be ensured to be less than 20wt.% to meet specific performance requirements. For example, the content of asphalt can be 12wt.%, 12.5wt.%, 13wt.%, 13.5wt.%, 14wt.%, 15wt.%, etc., and the content of graphite fiber can be 0.1wt.%, 0.3wt.%, 0.5wt.%, 0.7wt.%, 0.9wt.%, 1wt.%, etc.

[0061] In some embodiments, the TiB2 composite powder material is prepared by wet ball milling and spray granulation.

[0062] In some embodiments, the components of the TiB2 composite powder material are: 2wt.%-10wt.% TiN powder, 1wt.%-5wt.% CoB powder, 1wt.%-3wt.% ZrB2 powder, 1wt.%-3wt.% metal powder, 1wt.%-2wt.% polyvinyl alcohol binder, and the balance is TiB2 powder.

[0063] Before being formed with the graphitized cathode paste, the TiB2 composite material exists in the form of a powder. This powder is convenient for mixing and evenly dispersing various components, and is also convenient for subsequent molding processing. Through specific process pressing means (such as molding, extrusion, etc.), the powder can be evenly coated on the cathode surface, and a dense composite layer is formed after high-temperature sintering. TiN (titanium nitride) is a material with high hardness, high wear resistance and good chemical stability. Its addition can enhance the hardness and wear resistance of the TiB2 composite material, thereby improving the service life of the electrolytic cell cathode. CoB powder can improve the strength and conductivity of the composite material. ZrB2 (zirconium diboride) is a material with high melting point, high hardness and good corrosion resistance. Its addition can further improve the high temperature resistance and corrosion resistance of the composite material. The addition of metal powder can improve the conductivity and mechanical properties of the composite material, and can also assist sintering. Common metal powders include one or more alloys of nickel, iron and copper. Polyvinyl alcohol, as a binder, can form a strong bond between powder particles, so that the composite material can maintain a stable shape and structure during the molding process. Exemplarily, the content of TiN powder can be 2wt.%, 3wt.%, 4wt.%, 5wt.%, 6wt.%, 7wt.%, 9wt.%, 10wt.%, etc., the content of CoB powder can be 1wt.%, 2wt.%, 3wt.%, 4wt.%, 5wt.%, etc., the content of ZrB2 powder can be 1wt.%, 1.5wt.%, 2wt.%, 2.5wt.%, 3wt.%, etc., the content of metal powder can be 1wt.%, 1.5wt.%, 2wt.%, 2.5wt.%, 3wt.%, etc., and the content of polyvinyl alcohol binder can be 1wt.%, 1.2wt.%, 1.4wt.%, 1.6wt.%, 1.8wt.%, 2wt.%, etc.

[0064] The product prepared by the method for preparing the graphitized cathode is the above-mentioned graphitized cathode. The chemical composition and organizational structure of the graphitized cathode prepared by the method for preparing the graphitized cathode can refer to the above-mentioned embodiment. Since the method for preparing the graphitized cathode adopts part or all of the technical solutions of the graphitized cathode embodiment, it at least has all the beneficial effects brought by the technical solutions of the graphitized cathode embodiment, which will not be repeated here one by one.

[0065] Figure 3A schematic diagram of a low-temperature aluminum electrolysis cell provided in an embodiment of the present application.

[0066] See also Figure 3 Based on a general inventive concept, the present application provides a low-temperature aluminum electrolysis cell, which includes the graphitized cathode described above.

[0067] In some embodiments, a forced heat dissipation device is provided on the side wall tank shell of the aluminum electrolysis cell;

[0068] The distance between the side wall lining of the aluminum electrolytic cell and the carbon anode is ≥320 mm;

[0069] After the graphitized cathode is connected to the cathode collector rod, the vertical distance between the upper surface of the graphitized cathode and the upper surface of the cathode collector rod is ≥300 mm.

[0070] In some embodiments, the distance between the side wall lining of the aluminum electrolysis cell and the carbon anode is 320 mm-380 mm;

[0071] The vertical distance between the upper surface of the graphitized cathode and the upper surface of the cathode collector rod is 300 mm-340 mm.

[0072] In some embodiments, the forced heat dissipation device includes: one or more of a vertical heat sink, an air-cooled heat exchanger, and a thermal oil-cooled heat exchanger;

[0073] The connection between the graphitized cathode and the cathode collector rod is cast by phosphorus pig iron, and the cathode collector rod is made of one of a high-conductivity steel rod and a copper-inserted steel rod.

[0074] The present application solves the problem that low-temperature electrolyte is not easy to form a furnace wall crust to protect the side wall lining by adding a forced heat dissipation device to the side wall of the electrolytic cell, and designing a wide distance between the side lining and the carbon anode. Adding a forced heat dissipation device to the side wall of the electrolytic cell is conducive to the formation of a furnace wall crust on the side wall lining of the electrolyte melt inside the electrolytic cell. The wide distance design of 320mm-380mm between the side lining and the carbon anode leaves dynamic adjustment space for the thickening and thinning of the furnace wall crust. In addition, the forced heat dissipation device can also be used as a means of thermal balance adjustment to enable the electrolytic cell to have the ability of current intensification or variable load production. Exemplarily, the distance between the side wall lining of the aluminum electrolytic cell and the carbon anode can be 320mm, 330mm, 340mm, 350mm, 360mm, 370mm, 380mm, etc.

[0075] The present application reduces the horizontal current in the aluminum liquid of the aluminum electrolytic cell and improves the stability of the aluminum liquid by controlling the vertical distance between the upper surface of the collector rod and the upper surface of the graphitized cathode, thereby achieving low pole distance, low voltage and high efficiency operation. The stability of the aluminum liquid in the electrolytic cell is affected by the Lorentz force generated by the vertical magnetic field and the horizontal current. The vertical magnetic field is determined by the cathode busbar system of the electrolytic cell and is difficult to change. Therefore, reducing the horizontal current becomes the main means to improve the stability of the aluminum liquid. The research results show that when a graphitized cathode is used, the vertical distance between the upper surface of the high-conductivity cathode collector rod and the upper surface of the graphitized cathode is greater than 300mm, which can significantly reduce the horizontal current in the aluminum liquid. The larger the vertical distance, the better the effect, but considering the actual height range of the cathode and the cross-sectional area of ​​the collector rod, it is more reasonable to control the vertical distance to 300mm-340mm. For example, the vertical distance between the upper surface of the graphitized cathode and the upper surface of the cathode collector rod can be 300mm, 310mm, 320mm, 330mm, 340mm, etc.

[0076] The present application provides a low-temperature aluminum electrolysis method, which adopts any of the low-temperature aluminum electrolysis cells described above, and the method includes the following parameters: the initial crystallization temperature of the low-temperature electrolyte is 820°C-850°C, the electrolysis temperature is 845°C-900°C, and the superheat is 20°C-50°C.

[0077] In some embodiments, the components of the low-temperature electrolyte are: KF: 12wt.%-15wt.%, LiF: 1wt.%-2wt.%, CaF2: 0-5wt.%, MgF2: 0-2wt.%, Al2O3: 2wt.%-4wt.%, NaF: 26wt.%-33wt.%, and the balance is AlF3.

[0078] First, the present invention uses a low-temperature electrolyte with a primary crystallization temperature in the range of 820-850°C. The setting of this temperature range is based on the optimization of the electrolysis process and the consideration of cathodic protection. At the same time, the electrolyte system has a relatively high conductivity and alumina saturation concentration, which helps to improve the electrolysis efficiency and reduce the precipitation of alumina. In order to further improve the performance of the electrolyte, the present invention adds two additives, LiF and KF, to the electrolyte. However, the addition amount of these two additives needs to be strictly controlled to balance their different effects on the electrolyte performance. The addition of LiF can significantly improve the conductivity of the electrolyte, but it also significantly reduces the saturated solubility of alumina. Experimental studies have shown that when the content of LiF exceeds 3wt.%, its effect on the saturated solubility of alumina becomes significant. Therefore, in order to keep the saturated solubility of alumina at a certain level, the present invention controls the content of LiF within 2wt.%. The addition of KF can improve the saturated solubility of alumina, but at the same time, it will increase the penetration damage to the carbon cathode. Experimental studies have found that when the content of KF is within 15wt.%, the potassium expansion effect on the graphitized cathode is small. Therefore, the present invention controls the content of KF to a level close to but not exceeding 15wt.% to ensure the stability and safety of the cathode. After determining the addition amount of LiF and KF, the present invention further adjusts the composition of the electrolyte by keeping the ratio of KF / (KF+NaF) unchanged and reducing the molecular ratio (i.e., increasing the content of AlF3). In this way, the optimal electrolyte component with relatively high conductivity and saturated solubility of alumina can be obtained while keeping the initial crystallization temperature range unchanged. Finally, the present invention also verifies the effect of the low-temperature electrolyte system at an overheat of 20-50°C through laboratory-scale electrolysis tests. The test results show that within this overheat range, the cathode will not produce crusting. Therefore, the present invention controls the superheat between 20-50°C to ensure the smooth progress of the electrolysis process and the stable operation of the cathode. In summary, the present invention successfully solves the problem of alumina precipitation crusting by optimizing the electrolyte composition and superheat control, and provides new ideas and solutions for the development of the aluminum electrolysis industry. The initial crystallization temperature of the low-temperature electrolyte is 820°C, 825°C, 830°C, 835°C, 840°C, 845°C, 850°C, etc., the electrolysis temperature can be 845°C, 855°C, 865°C, 875°C, 885°C, 895°C, 900°C, etc., and the superheat can be 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, etc.

[0079] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.

[0080] Example 1

[0081] In a certain aluminum electrolytic enterprise, a 300kA prebaked carbon anode aluminum electrolytic cell was overhauled and transformed into a low-temperature aluminum electrolytic cell for low-temperature aluminum electrolysis production.

[0082] The average thickness of the low-carbon content TiB2 composite layer on the surface of the graphitized cathode substrate is about 50 mm, and the measured carbon content of the TiB2 composite layer is 7.96%. The low-carbon content TiB2 composite material is composed of 12 wt.% of asphalt, 1 wt.% of graphite fiber, and 87 wt.% of TiB2 powder. The low-carbon content TiB2 composite material is prepared into a paste by hot kneading, evenly spread on the surface of the graphitized cathode paste, and integrated with the graphitized cathode paste by pressing and sintering to obtain a graphitized cathode. A high-conductive steel rod (room temperature resistivity 11×10 -8 Ω·m), phosphorus pig iron casting, the vertical distance between the upper surface of the steel rod and the upper surface of the graphitized cathode is h=340mm; the forced heat dissipation device arranged on the side wall tank shell of the electrolytic cell is a vertical heat sink, and in order to better realize convection heat dissipation, heat dissipation holes 12 are opened on the horizontal groove edge plate of the electrolytic cell; the side wall lining adopts silicon carbide combined with silicon nitride material with a thickness of 60mm, and the distance between the lining and the carbon anode is b=320mm.

[0083] The design composition of the low-temperature electrolyte is: KF 14wt.%; LiF 2wt.%; CaF2 4wt.%; MgF20.5wt.%; Al2O33.2wt.%; NaF 32wt.%; AlF3 44.3wt.%; molecular ratio CR=1.44. During the electrolysis process, the electrolyte at different positions of the electrolytic cell was sampled and the initial crystallization temperature was tested. The average value was 846℃, the electrolysis temperature was 895-900℃, the superheat was about 50℃; the anode current density was 0.762A / cm 2 , the effect coefficient is less than 0.06 times / bath day, the furnace wall thickness is 183.6mm, the electrolytic cell operating voltage is 3.774V, the current efficiency is 93.95wt.%, and the DC power consumption is 11971kWh / t-Al. During the operation cycle of the electrolytic cell of this embodiment, the graphitized cathode with the low-carbon TiB2 composite material on the electrolytic cell is not damaged, and no alumina crust is found on the bottom of the cell.

[0084] Example 2

[0085] In a certain aluminum electrolytic enterprise, a 300kA prebaked carbon anode aluminum electrolytic cell was overhauled and transformed into a low-temperature aluminum electrolytic cell for low-temperature aluminum electrolysis production.

[0086] The average thickness of the low-carbon TiB2 composite layer on the surface of the graphitized cathode substrate is about 30 mm, and the measured carbon content of the TiB2 composite layer is 8.3%. The low-carbon TiB2 composite material is composed of 15 wt.% of asphalt, 0.1 wt.% of graphite fiber, and 84.9 wt.% of TiB2 powder. The low-carbon TiB2 composite material is prepared into a paste by hot kneading, evenly spread on the surface of the graphitized cathode paste, and integrated with the graphitized cathode paste by pressing and sintering to obtain a graphitized cathode. A copper-inserted cathode steel rod (with a room temperature resistivity of 7.8×10 -8 Ω·m), phosphorus pig iron casting, the vertical distance between the upper surface of the steel rod and the upper surface of the graphitized cathode is h=300mm; the forced heat dissipation device arranged on the side wall tank shell of the electrolytic cell is a vertical heat sink, and in order to better realize convection heat dissipation, heat dissipation holes 12 are opened on the horizontal groove edge plate of the electrolytic cell; the side wall lining adopts silicon carbide combined with silicon nitride material with a thickness of 60mm, and the distance between the lining and the carbon anode is b=320mm.

[0087] The design composition of the low-temperature electrolyte is: KF 15wt.%; LiF 2wt.%; CaF2 2.5wt.%; MgF22wt.%; Al2O33.2wt.%; NaF 31wt.%; AlF3 44.3wt.%; molecular ratio CR=1.40. During the electrolysis process, the electrolyte at different positions of the electrolytic cell was sampled and the initial crystallization temperature was tested. The average value was 838℃, the electrolysis temperature was 870-875℃, the superheat was about 35℃; the anode current density was 0.762A / cm 2 , the effect coefficient is less than 0.07 times / bath day, the furnace wall thickness is 196.4mm, the electrolytic cell operating voltage is 3.768V, the current efficiency is 93.88wt.%, and the DC power consumption is 11961kWh / t-Al. During the operation cycle of the electrolytic cell of this embodiment, the graphitized cathode with the low-carbon TiB2 composite material on the electrolytic cell is not damaged, and no alumina crust is found on the bottom of the cell.

[0088] Example 3

[0089] In a certain aluminum electrolytic enterprise, a 300kA prebaked carbon anode aluminum electrolytic cell was overhauled and transformed into a low-temperature aluminum electrolytic cell for low-temperature aluminum electrolysis production.

[0090] The average thickness of the low-carbon TiB2 composite layer on the surface of the graphitized cathode substrate is about 5 mm, and the measured carbon content of the TiB2 composite layer is less than 0.01%. The components of the low-carbon TiB2 composite material are 10wt.% TiN powder, 1wt.% CoB powder, 1wt.% ZrB2 powder, 3wt.% nickel-iron alloy powder (nickel: 40wt.%, iron: 60wt.%), 2wt.% polyvinyl alcohol binder (CAS No.: 9002-89-5), and 83wt.% TiB2 powder, which are prepared into powder by wet ball milling and spray granulation. The powder is evenly spread on the surface of the graphitized cathode paste, and is pressed and sintered together with the graphitized cathode paste to obtain a graphitized cathode. A copper-inserted cathode steel rod (normal temperature resistivity 7.8×10 -8 Ω·m), phosphorus pig iron casting, the vertical distance between the upper surface of the steel rod and the upper surface of the graphitized cathode is h=300mm; the forced heat dissipation device arranged on the side wall tank shell of the electrolytic cell is a vertical heat sink, and in order to better realize convection heat dissipation, heat dissipation holes 12 are opened on the horizontal groove edge plate of the electrolytic cell; the side wall lining adopts silicon carbide combined with silicon nitride material with a thickness of 60mm, and the distance between the lining and the carbon anode is b=320mm.

[0091] The design composition of the low-temperature electrolyte is: KF 12; LiF 1wt.%; Al2O3 3.2wt.%; CaF2 0wt.%; MgF2 2wt.%; NaF 33wt.%; AlF3 48.8wt.%; molecular ratio CR = 1.35. During the electrolysis process, the electrolyte at different positions of the electrolytic cell was sampled and the initial crystallization temperature was tested. The average value was 832°C, the electrolysis temperature was 870-875°C, the superheat was about 40°C, and the anode current density was 0.762A / cm 2 , the effect coefficient is less than 0.07 times / bath day, the furnace wall thickness is 190.6mm, the electrolytic cell operating voltage is 3.776V, the current efficiency is 94.05wt.%, and the DC power consumption is 11964kWh / t-Al. During the operation cycle of the electrolytic cell of this embodiment, the graphitized cathode with the low-carbon TiB2 composite material on the electrolytic cell is not damaged, and no alumina crust is found on the bottom of the cell.

[0092] Example 4

[0093] In a certain aluminum electrolytic enterprise, a 300kA prebaked carbon anode aluminum electrolytic cell was overhauled and transformed into a low-temperature aluminum electrolytic cell for low-temperature aluminum electrolysis production.

[0094] The average thickness of the low-carbon TiB2 composite layer on the graphitized cathode substrate is about 50 mm, the carbon content of the TiB2 composite layer is less than 0.01% on the surface layer, and 8.12% on the inner layer; the low-carbon TiB2 composite material uses two types of paste and powder. The paste is composed of 12 wt.% of asphalt, 2 wt.% of graphite fiber, and 86 wt.% of TiB2 powder, which is prepared into a paste by hot kneading, evenly spread on the surface of the graphitized cathode paste, and then evenly spread on the powder. The powder material is composed of 2wt.% TiN powder, 5wt.% CoB powder, 3wt.% ZrB2 powder, 1wt.% nickel-iron alloy powder (nickel: 40wt.%, iron: 60wt.%), 1wt.% polyvinyl alcohol binder, and 88wt.% TiB2 powder. The powder material is prepared by wet ball milling and spray granulation, and then integrated with graphitized cathode paste by pressing and sintering to obtain a graphitized cathode. A copper-inserted cathode steel rod (room temperature resistivity 7.8×10 -8 Ω·m), phosphorus pig iron casting, the vertical distance between the upper surface of the steel rod and the upper surface of the graphitized cathode is h=300mm; the forced heat dissipation device arranged on the side wall tank shell of the electrolytic cell is an air-cooled heat exchanger, and the heat exchange medium 15 is air; the side wall lining adopts silicon carbide combined with silicon nitride material with a thickness of 60mm, and the distance between the lining and the carbon anode is b=320mm.

[0095] The design composition of the low-temperature electrolyte is: KF 14; LiF 2wt.%; CaF2 5wt.%; MgF2 0wt.%; Al2O33.2wt.%; NaF 30wt.%; AlF3 45.8wt.%; molecular ratio CR = 1.31. During the electrolysis process, the electrolyte at different positions of the electrolytic cell was sampled and the initial crystallization temperature was tested. The average value was 823°C, the electrolysis temperature was 850-855°C, the superheat was about 30°C, and the anode current density was 0.762A / cm 2 , the effect coefficient is less than 0.07 times / bath day, the furnace wall thickness is 195.7mm, the electrolytic cell operating voltage is 3.759V, the current efficiency is 93.81wt.%, and the DC power consumption is 11941kWh / t-Al. During the operation cycle of the electrolytic cell of this embodiment, the graphitized cathode with the low-carbon TiB2 composite material on the electrolytic cell is not damaged, and no alumina crust is found on the bottom of the cell.

[0096] Example 5

[0097] In a certain aluminum electrolytic enterprise, a 400kA prebaked carbon anode aluminum electrolytic cell was overhauled and transformed into a low-temperature aluminum electrolytic cell for low-temperature aluminum electrolysis production.

[0098] The average thickness of the low-carbon TiB2 composite layer on the surface of the graphitized cathode substrate is about 50mm, and the carbon content of the TiB2 composite layer is less than 0.01% in the surface layer and 8.23% in the inner layer. The low-carbon TiB2 composite material uses two types of paste and powder. The paste is composed of 12wt.% asphalt, 2wt.% graphite fiber, and 86wt.% TiB2 powder. The paste is prepared by hot kneading and evenly spread on the surface of the graphitized cathode paste, and then evenly spread on the powder. The powder is composed of 5wt.% TiN powder, 5wt.% CoB powder, 1wt.% ZrB2 powder, 1wt.% nickel-iron alloy powder (nickel: 40wt.%, iron: 60wt.%), 1wt.% polyvinyl alcohol binder, and 87wt.% TiB2 powder. The powder is prepared by wet ball milling and spray granulation. Finally, the graphitized cathode paste was integrated into a pressed and sintered state to obtain a graphitized cathode. A copper-inserted cathode steel rod (with a room temperature resistivity of 8.05×10 -8 Ω·m), phosphorus pig iron casting, the vertical distance between the upper surface of the steel rod and the upper surface of the graphitized cathode is h=320mm; the forced heat dissipation device arranged on the side wall tank shell of the electrolytic cell is a heat transfer oil heat exchanger, and the heat exchange medium 15 is heat transfer oil; the side wall lining adopts silicon carbide combined with silicon nitride material with a thickness of 60mm, and the distance between the lining and the carbon anode is b=380mm.

[0099] The design composition of the low-temperature electrolyte is: KF 14; LiF 2wt.%; CaF2 4wt.%; MgF2 0.5wt.%; Al2O32.8wt.%; NaF 30.5wt.%; AlF3 46.2wt.%; molecular ratio CR = 1.32. During the electrolysis process, the electrolyte at different positions of the electrolytic cell was sampled and the initial crystallization temperature was tested. The average value was 826°C, the electrolysis temperature was 845-850°C, the superheat was about 20°C; the anode current density was 0.802A / cm 2 , the effect coefficient is less than 0.08 times / bath day, the furnace wall thickness is 205.7mm, the electrolytic cell operating voltage is 3.772V, the current efficiency is 93.88wt.%, and the DC power consumption is 11973kWh / t-Al. During the operation cycle of the electrolytic cell of this embodiment, the graphitized cathode with the low-carbon TiB2 composite material on the electrolytic cell is not damaged, and no alumina crust is found on the bottom of the cell.

[0100] In addition, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:

[0101] In the embodiments of the present invention, a synergistic solution and optimal parameters are determined through systematic research on the key issues faced by the industrial production of low-temperature aluminum electrolysis, forming a complete set of low-temperature aluminum electrolysis technology, which can realize industrialized low-temperature aluminum electrolysis production, has great practical significance, and has broad application prospects.

[0102] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A graphitized cathode, characterized in that: The graphitized cathode comprises: a graphitized cathode substrate; and A TiB2 composite layer, wherein the TiB2 composite layer covers at least a portion of the surface of the graphitized cathode substrate, the carbon content of the TiB2 composite layer is less than 20wt.%, and the thickness of the TiB2 composite layer is 5mm-50mm.

2. A method for preparing a graphitized cathode according to claim 1, characterized in that: The method comprises: Obtaining TiB2 composite paste material and / or TiB2 composite powder material; Laying the TiB2 composite paste on the surface of the graphitized cathode paste to obtain a mixed material; or Laying TiB2 composite powder material on the surface of graphitized cathode paste to obtain a mixed material; or Laying a TiB2 composite paste on the surface of a graphitized cathode paste, and laying a TiB2 composite powder on the upper surface of the TiB2 composite paste to obtain a mixed material; The mixed material is integrally pressed and sintered to obtain a graphitized cathode.

3. The method according to claim 2, characterized in that The components of the TiB2 composite paste are: 12wt.%-15wt.% of asphalt, 0.1wt.%-1wt.% of graphite fiber, and the balance is TiB2 powder.

4. The method according to claim 2, characterized in that: The components of the TiB2 composite powder material are: 2wt.%-10wt.% TiN powder, 1wt.%-5wt.% CoB powder, 1wt.%-3wt.% ZrB2 powder, 1wt.%-3wt.% metal powder, 1wt.%-2wt.% polyvinyl alcohol binder, and the balance is TiB2 powder.

5. A low-temperature aluminum electrolysis cell, characterized in that: The aluminum electrolysis cell comprises the graphitized cathode of claim 1.

6. The low-temperature aluminum electrolysis cell according to claim 5, characterized in that: A forced heat dissipation device is provided on the side wall tank shell of the aluminum electrolytic cell; The distance between the side wall lining of the aluminum electrolytic cell and the carbon anode is ≥320 mm; After the graphitized cathode is connected to the cathode collector rod, the vertical distance between the upper surface of the graphitized cathode and the upper surface of the cathode collector rod is ≥300 mm.

7. The low-temperature aluminum electrolysis cell according to claim 6, characterized in that: The distance between the side wall lining of the aluminum electrolytic cell and the carbon anode is 320mm-380mm; The vertical distance between the upper surface of the graphitized cathode and the upper surface of the cathode collector rod is 300 mm-340 mm.

8. The low-temperature aluminum electrolysis cell according to claim 6, characterized in that: The forced heat dissipation device includes: one or more of a vertical heat sink, an air-cooled heat exchanger, and a thermal oil-cooled heat exchanger; The connection between the graphitized cathode and the cathode collector rod is cast by phosphorus pig iron, and the cathode collector rod is made of one of a high-conductivity steel rod and a copper-inserted steel rod.

9. A low-temperature aluminum electrolysis method, characterized in that: The method adopts the low-temperature aluminum electrolysis cell according to any one of claims 5 to 8, and the method includes the following parameters: the initial crystallization temperature of the low-temperature electrolyte is 820°C-850°C, the electrolysis temperature is 845°C-900°C, and the superheat is 20°C-50°C.

10. The method according to claim 9, characterized in that The components of the low-temperature electrolyte are: KF: 12wt.%-15wt.%, LiF: 1wt.%-2wt.%, CaF2: 0-5wt.%, MgF2: 0-2wt.%, Al2O3: 2wt.%-4wt.%, NaF: 26wt.%-33wt.%, and the balance is AlF3.

Citation Information

Patent Citations

  • High performance room temperature cured titanium boride cathode coating for aluminium reduction cell

    CN102021606A

  • Alloy steel textile clippers with composite ceramic coating and manufacturing method thereof

    CN103409719A

  • Novel electrolytic bath for aluminum electrolysis and electrolysis technology thereof

    CN103484893A

  • TiB2-C composite cathode for aluminum electrolysis and preparation method thereof

    CN103643260A

  • Electrolyte for producing aluminum by molten electrolysis

    CN105473766A