Method for preparing mineral compound fertilizer from graphite tailings
By purifying and grinding graphite tailings, combining agricultural waste to process in a high-temperature reactor, and fermenting and drying, mineral compound fertilizers are prepared, which solves the problems of environmental pollution and high costs of graphite tailings and realizes resources Chemical treatment and green and environmentally friendly agricultural waste utilization have reduced the use of fertilizers and raw material costs.
Patent Information
- Application Number
- CN202411299855.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-12-06
AI Technical Summary
Jixi Liumao graphite tailings has huge output, serious environmental pollution, high stacking costs, and a single resource treatment method.
By purifying and grinding the graphite tailings, reacting in a high-temperature reactor with agricultural waste, nutrient supplements and activation catalysts, and then adding a ripening agent for fermentation and drying, mineral compound fertilizer with suitable particle size is prepared.
The resource-based treatment of graphite tailings has been realized, the storage cost has been reduced, and the green and environmentally friendly agricultural waste treatment method has been provided, which has shortened the treatment time, reduced the use of fertilizers, and reduced the price of raw materials.
Smart Images

Figure BDA0005047302770000051 
Figure BDA0005047302770000052 
Figure BDA0005047302770000061
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing mineral compound fertilizer by utilizing graphite tailings. Background Art
[0002] Graphite is one of the most promising non-metallic mineral materials in the 21st century. Graphite minerals have many excellent properties. The invention of graphene has brought revolutionary changes to graphite in the fields of microelectronics, information, and new energy. Natural graphite is increasingly becoming an important mineral resource supporting the development of high-tech in many fields, and its strategic position is prominent. Jixi City, Heilongjiang Province is one of the world's largest high-quality flake graphite reserves, with proven resource reserves of 1 billion tons, and large flake crystalline graphite accounts for more than 50%. Among them, Liumao Mining Area is one of the most important graphite mining areas in Jixi and the birthplace of Jixi graphite mining. Liumao graphite has excellent quality and is well-known at home and abroad. It has been exported to more than 30 countries and regions. However, to collect 1 ton of concentrated ore, 2.6 tons of waste soil and stone need to be stripped out, and 1 ton of graphite needs to be produced, and the amount of tailings generated exceeds 100 tons. The generation of a large amount of tailings has caused serious environmental problems, and requires large-scale factory buildings for stacking, which is too costly. Therefore, it is particularly important to seek a reasonable way to treat the tailings as a resource.
[0003] In order to strengthen the management and comprehensive utilization of tailings and achieve the reduction, harmlessness and resource utilization of graphite tailings, the present invention provides a method for preparing mineral compound fertilizer using graphite tailings, which can effectively treat graphite tailings. Summary of the invention
[0004] The invention aims to solve the problems of huge output of existing Jixi willow hair graphite tailings, serious environmental pollution, high stacking cost and single resource treatment method, and provide a method for preparing mineral compound fertilizer by using graphite tailings.
[0005] A method for preparing mineral compound fertilizer using graphite tailings is specifically completed by the following steps:
[0006] 1. Purify the graphite tailings, remove impurities and large-grained stones, and obtain purified graphite tailings;
[0007] 2. Grind and crush the purified graphite tailings with a ball mill, and then screen them with a grading screen to obtain graphite tailings with a particle size of 0.1 mm to 2 mm;
[0008] 3. Add a certain amount of agricultural waste, nutrient supplements, activated catalysts and graphite tailings with a particle size of 0.5mm to 2mm into a high-temperature reactor, adjust the heating program to allow them to fully react and fuse under high temperature conditions, and after standing to a suitable temperature, fully stir and soak the product, and perform solid-liquid separation after a certain period of time to obtain a solid product;
[0009] 4. Under certain temperature and humidity conditions, add a maturation agent to the solid product, ferment it under anaerobic conditions for a period of time, and then dry, compact and crush it to obtain a mineral compound fertilizer.
[0010] Beneficial effects of the present invention:
[0011] 1. The present invention transforms the Jixi Liumao graphite tailings into a mineral compound fertilizer with nutrient-rich elements, thus turning waste into treasure and greatly reducing the storage cost of the tailings;
[0012] 2. The present invention utilizes the Jixi willow hair graphite tailings for resource processing and also processes agricultural waste represented by straw in a green way, which is more environmentally friendly than the traditional incineration method;
[0013] 3. The method provided by the present invention realizes the resource processing of Jixi Liumao graphite tailings in a short time, with fast processing speed and good effect;
[0014] 4. The mineral fertilizer prepared by the present invention can be used in combination with traditional fertilizers, which greatly reduces the use of chemical fertilizers and is more green and clean;
[0015] 5. The raw materials required for the present invention are cheap and easy to operate, and are suitable for large-scale promotion and application. DETAILED DESCRIPTION
[0016] Specific implementation method 1: This implementation method is a method for preparing mineral compound fertilizer using graphite tailings, which is specifically completed by the following steps:
[0017] 1. Purify the graphite tailings, remove impurities and large-grained stones, and obtain purified graphite tailings;
[0018] 2. Grind and crush the purified graphite tailings with a ball mill, and then screen them with a grading screen to obtain graphite tailings with a particle size of 0.1 mm to 2 mm;
[0019] 3. Add a certain mass of agricultural waste, nutrient supplements, activated catalysts and graphite tailings with a particle size of 0.5mm to 2mm into a high-temperature reactor, adjust the heating program to allow them to fully react under high temperature conditions, and after standing to a suitable temperature, fully stir and soak the product, and perform solid-liquid separation after a certain period of time to obtain a solid product;
[0020] 4. Under certain temperature and humidity conditions, a maturation agent is added to the solid product II, and the solid product II is fermented under anaerobic conditions for a period of time, and then dried, compacted and crushed to obtain a mineral compound fertilizer.
[0021] Specific implementation method 2: This implementation method is different from the specific implementation method 1 in that the graphite tailings described in step 1 are Jixi Liumao graphite tailings. The other steps are the same as those in the specific implementation method 1.
[0022] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the agricultural waste in step 3 is eucalyptus leaves, corn stalks or rice stalks. The other steps are the same as those in specific implementation method 1 or 2.
[0023] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the nutrient supplement described in step 3 is a mixture of potassium hydroxide and calcium hydroxide, wherein the mass ratio of potassium hydroxide to calcium hydroxide is 1:(3-6). The other steps are the same as those of specific embodiments 1 to 3.
[0024] Specific implementation method 5: This implementation method is different from specific implementation methods 1 to 4 in that: the activation catalyst in step 3 is a mixture of one or more of ammonia water and sodium hydroxide; the mass fraction of the ammonia water is 25% to 30%. The other steps are the same as specific implementation methods 1 to 4.
[0025] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that the mass ratio of agricultural waste, nutrient supplement, activation catalyst and graphite tailings with a particle size of 0.5 mm to 2 mm described in step 3 is (5 to 30): (1 to 5): (1 to 5): (1 to 10). The other steps are the same as those of specific embodiments 1 to 5.
[0026] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that the temperature rise procedure described in step 3 is a three-stage process, the first stage is to heat the temperature to 180°C to 220°C at a heating rate of 5°C / min to 15°C / min, the second stage is to maintain the temperature at 180°C to 220°C for 20h to 24h, and the third stage is a cooling stage, which ends after the temperature drops from 180°C to 220°C to room temperature. The other steps are the same as those of specific embodiments 1 to 6.
[0027] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that the soaking time in step 3 is 24 hours to 48 hours. The other steps are the same as those in specific embodiments 1 to 7.
[0028] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that: the certain temperature and humidity conditions described in step 4 are: temperature 35°C to 45°C, humidity 50% to 60%; the ripening agent described in step 4 is a mixture of biologically active enzymes and citric acid, wherein the mass ratio of biologically active enzymes to citric acid is (1 to 2): (3 to 8); the citric acid is purchased from Chengdu Huahong Biotechnology Co., Ltd.; the biologically active enzymes are purchased from Shandong Hongqi Agricultural Technology Co., Ltd. The other steps are the same as specific embodiments 1 to 8.
[0029] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that: the mass ratio of the solid product II to the aging agent in step 4 is (10-20): (1-3); the fermentation in step 4 is: fermentation under anaerobic conditions at 50°C to 70°C for 40h to 48h; the particle size of the mineral compound fertilizer in step 4 is 0.2mm to 1mm. The other steps are the same as those in specific embodiments 1 to 9.
[0030] The following examples are used to verify the beneficial effects of the present invention:
[0031] Embodiment 1: A method for preparing mineral compound fertilizer using graphite tailings is specifically completed according to the following steps:
[0032] 1. Purify the graphite tailings, remove impurities and large-grained stones, and obtain purified graphite tailings;
[0033] The graphite tailings described in step 1 are Jixi Liumao graphite tailings;
[0034] 2. Grind and crush the purified graphite tailings with a ball mill, and then screen them with a grading screen to obtain graphite tailings with a particle size of 0.5 mm to 2 mm;
[0035] 3. Add a certain amount of agricultural waste, nutrient supplements, activated catalysts and graphite tailings with a particle size of 0.5 mm to 2 mm into a high-temperature reactor, adjust the heating program to allow them to fully react under high temperature conditions, let them stand at room temperature, fully stir and soak the product, and perform solid-liquid separation after a certain period of time to obtain a solid product;
[0036] The agricultural waste in step 3 is rice straw, and the particle size is 50-100 mesh;
[0037] The nutrient supplement described in step 3 is a mixture of potassium hydroxide and calcium hydroxide, wherein the mass ratio of potassium hydroxide to calcium hydroxide is 1:3;
[0038] The activation catalyst described in step 3 is a mixture of ammonia water and sodium hydroxide, wherein the mass ratio of ammonia water to sodium hydroxide is 2:1; the mass fraction of the ammonia water is 27%;
[0039] The mass ratio of the agricultural waste, nutrient supplement, activation catalyst and graphite tailings with a particle size of 0.5 mm to 2 mm described in step 3 is 10:2:3:5;
[0040] The heating program described in step 3 is a three-stage program. The first stage is to heat up to 200°C at a heating rate of 10°C / min, the second stage is to maintain the temperature at 200°C for 24 hours, and the third stage is a cooling stage, which ends after cooling from 200°C to room temperature.
[0041] The soaking time described in step 3 is 30h;
[0042] Fourth, under certain temperature and humidity conditions, adding a maturation agent to the solid product, fermenting it under anaerobic conditions for a period of time, and then drying, compacting and crushing it to obtain a mineral compound fertilizer;
[0043] The ripening agent in step 4 is a mixture of biologically active enzymes and citric acid, wherein the mass ratio of the biologically active enzymes to the citric acid is 1:3; the citric acid is purchased from Chengdu Huahong Biotechnology Co., Ltd.; the biologically active enzymes are purchased from Shandong Hongqi Agricultural Technology Co., Ltd.;
[0044] The mass ratio of the solid product to the maturation agent in step 4 is 10:3; the fermentation in step 4 is: fermentation under anaerobic conditions at 60° C. for 48 hours; the particle size of the mineral compound fertilizer in step 4 is 0.45 mm.
[0045] Embodiment 2: The difference between this embodiment and embodiment 1 is that the stirring and soaking time in step 3 is 24 hours. The other steps and parameters are the same as those in embodiment 1.
[0046] Embodiment 3: This embodiment differs from Embodiment 1 in that the stirring and soaking time is 48 hours. Other steps and parameters are the same as those of Embodiment 1.
[0047] Example 4: The difference between this example and Example 1 is that the fermentation in step 4 is carried out under anaerobic conditions at 60° C. for 24 hours. The other steps and parameters are the same as those in Example 1.
[0048] Example 5: The difference between this example and Example 1 is that the fermentation in step 4 is carried out under anaerobic conditions at 60° C. for 72 hours. The other steps and parameters are the same as those in Example 1.
[0049] Example 6: The difference between this example and Example 1 is that the fermentation described in step 4 is: in step 2, the graphite tailings after purification are ground and crushed by a ball mill, and then screened by a grading screen to obtain graphite tailings with a particle size of 0.1 mm to 0.5 mm. The other steps and parameters are also the same as in Example 1.
[0050] Example 7: The difference between this example and Example 1 is that the fermentation described in step 4 is: in step 2, the graphite tailings after purification are ground and crushed by a ball mill, and then screened by a grading screen to obtain graphite tailings with a particle size of 0.5 mm to 1 mm. The other steps and parameters are also the same as those in Example 1.
[0051] Example 8: The difference between this example and Example 1 is that the mass ratio of the solid product to the aging agent in step 4 is 10:1. The other steps and parameters are the same as those in Example 1.
[0052] Example 9: The difference between this example and Example 1 is that the mass ratio of the solid product to the aging agent in step 4 is 20:3. The other steps and parameters are the same as those in Example 1.
[0053] Experimental group: conventional seedling raising soil in Northeast China was selected, and the prepared mineral compound fertilizer was added to it. The specific operation was to fully mix the mineral compound fertilizer with the seedling raising soil according to the proportion for one week, and then water the seedlings. Then a 35-day seedling raising experiment was started, and the seedling raising soil and seedling indicators were measured after 35 days.
[0054] Control group: conventional rice seedling raising soil in Northeast China was selected, and rice seedling strengthening agent purchased from Heilongjiang Wanfengda Fertilizer Co., Ltd. was added to it. The mass ratio of rice seedling strengthening agent to rice seedling raising soil was 800:1. The specific operation was to directly sprinkle the rice seedling strengthening agent into the rice seedling raising soil according to the proportion, mix it for a week, and then water the rice seedlings. Then a 35-day rice seedling raising experiment was started. After 35 days, the rice seedling raising soil and rice seedling indicators were measured respectively, as shown in the control group in Table 1 and Table 2;
[0055] At the same time, the original seedling raising soil was used as the blank control data, see the original seedling raising soil in Table 1 and Table 2.
[0056] Table 1 shows the effects of the original seedling raising soil, the existing seedling strengthening agent as a control group, and the mineral compound fertilizer prepared from graphite tailings in Example 1 on soil properties;
[0057] Table 1
[0058]
[0059] Table 2 shows the effects of the original rice seedling soil, the existing rice seedling strengthening agent as a control group, and the mineral compound fertilizer prepared from graphite tailings in Example 1 on rice seedlings (before transplanting);
[0060] Table 2
[0061]
[0062]
Claims
1. A method for preparing mineral compound fertilizer using graphite tailings, characterized in that The method is specifically completed according to the following steps:
1. Purify the graphite tailings, remove impurities and large-grained stones, and obtain purified graphite tailings; 2. Grind and crush the purified graphite tailings with a ball mill, and then screen them with a grading screen to obtain graphite tailings with a particle size of 0.1 mm to 2 mm; 3. Add a certain amount of agricultural waste, nutrient supplements, activated catalysts and graphite tailings with a particle size of 0.5mm to 2mm into a high-temperature reactor, adjust the heating program to allow them to fully react and fuse under high temperature conditions, and after standing to a suitable temperature, fully stir and soak the product, and perform solid-liquid separation after a certain period of time to obtain a solid product; 4. Under certain temperature and humidity conditions, add a maturation agent to the solid product, ferment it under anaerobic conditions for a period of time, and then dry, compact and crush it to obtain a mineral compound fertilizer.
2. A method for preparing mineral compound fertilizer using graphite tailings according to claim 1, characterized in that The graphite tailings described in step one are Jixi Liumao graphite tailings.
3. A method for preparing mineral compound fertilizer using graphite tailings according to claim 1, characterized in that The agricultural waste described in step 3 is eucalyptus leaves, corn stalks or rice stalks.
4. A method for preparing mineral compound fertilizer using graphite tailings according to claim 1, characterized in that The nutrient supplement described in step three is a mixture of potassium hydroxide and calcium hydroxide, wherein the mass ratio of potassium hydroxide to calcium hydroxide is 1:(3-6).
5. A method for preparing mineral compound fertilizer using graphite tailings according to claim 1, characterized in that The activation catalyst described in step 3 is one or a mixture of ammonia water, potassium hydroxide, and sodium hydroxide; the mass fraction of the ammonia water is 25% to 30%.
6. A method for preparing mineral compound fertilizer using graphite tailings according to claim 1, characterized in that The mass ratio of the agricultural waste, nutrient supplement, activation catalyst and graphite tailings with a particle size of 0.5 mm to 2 mm described in step three is (5 to 30): (1 to 5): (1 to 5): (1 to 10).
7. A method for preparing mineral compound fertilizer using graphite tailings according to claim 1, characterized in that The heating program described in step three is a three-stage program. The first stage is to heat the temperature to 180°C to 220°C at a heating rate of 5°C / min to 15°C / min. The second stage is to maintain the temperature at 180°C to 220°C for 20h to 24h. The third stage is a cooling stage, which ends after the temperature drops from 180°C to 220°C to room temperature.
8. A method for preparing mineral compound fertilizer using graphite tailings according to claim 1, characterized in that The soaking time described in step 3 is 24h to 48h.
9. A method for preparing mineral compound fertilizer using graphite tailings according to claim 1, characterized in that The certain temperature and humidity conditions described in step 4 are: temperature 35°C to 45°C, humidity 50% to 60%; the aging agent described in step 4 is a mixture of biologically active enzymes and citric acid, wherein the mass ratio of the biologically active enzymes to the citric acid is (1 to 2): (3 to 8).
10. A method for preparing mineral compound fertilizer using graphite tailings according to claim 1, characterized in that The mass ratio of the solid product to the maturation agent described in step 4 is (10-20):(1-3); the fermentation described in step 4 is: fermentation under anaerobic conditions at 50°C-70°C for 40h-48h; the particle size of the mineral compound fertilizer described in step 4 is 0.2mm-1mm.