Antioxidant special for PBSA and preparation method of high-performance PBSA
By preparing the high molecular weight antioxidant tetra[3-[3,5-(1,1-dimethylpropanol)-4-hydroxyphenyl]propionic acid]pentaerythritol combined with tetrabutyl titanate and trimethyl phosphate by preparing the high molecular weight antioxidant tetramethyl phosphate The method solves the oxidation resistance and mechanical properties of PBSA polyester under high temperature conditions, and achieves the high performance improvement of polyester, which is suitable for a variety of application fields.
Patent Information
- Application Number
- CN202411047808.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-12-06
AI Technical Summary
The existing PBSA polyester materials have poor oxidation resistance and mechanical properties under high temperature conditions, and traditional antioxidants are difficult to effectively improve, and sodium dihydrogen phosphate is easily decomposed by heat, β-(3,5-di-tert-butyl-4-hydroxybenzene Major)propenyl ester is not suitable for the preparation of PBSA.
Tetrakis[3-[3,5-(1,1-dimethylpropanol)-4-hydroxyphenyl]propionic acid]pentaerythritol is used as a high molecular weight antioxidant, and through alkylation, addition and transesterification reaction Preparation, combined with tetrabutyl titanate and trimethyl phosphate as catalysts and stabilizers, esterification and polycondensation reactions were carried out to prepare high-performance heat-resistant oxidized polysuccinic acid/butylene adipate.
It significantly improves the thermal oxidation resistance and mechanical properties of PBSA polyester, has higher molecular weight and excellent thermal stability, has increased the thermal decomposition temperature to 340℃, has a tensile strength of 40.4 MPa, and does not contain heavy metals. It is suitable for food packaging and medical care. Instruments and other fields.
Smart Images

Figure CN119080608A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and more specifically, relates to a special antioxidant for PBSA and a preparation method of high-performance PBSA. Background Art
[0002] With the continuous development of modern social economy, people's consumption of resources is increasing, and the demand for plastic products is expanding. However, traditional plastics are difficult to be degraded by microorganisms in nature, which can easily cause serious environmental pollution problems. Degradable polybutylene succinate-adipate (PBSA) prepared from adipic acid, succinic acid and butanediol has attracted extensive attention from industry and academia as a new type of biodegradable polyester material. Patent CN106366296A uses succinic anhydride, adipic acid and 1,4-butanediol as raw materials to prepare PBSA, which reduces the by-product water in the esterification reaction by 90%, reducing the production of by-products.
[0003] However, the above patents do not solve the problems of poor heat oxidation resistance and mechanical properties of PBSA. The current method to improve the oxidation resistance and mechanical properties of polyester materials is mainly to add stabilizers or inhibitors during the preparation and processing of polyester. Patent CN202120862886.0 discloses a polyester and polyester alloy composition resistant to heat oxidation aging and a preparation method thereof. The active molecular chain ends of the polyester are passivated by using octadecenoate stabilizers and sodium dihydrogen phosphate as ester exchange agents to reduce aging degradation caused by thermal oxidation. Patent CN113637310B discloses a long-term heat-stable polyester and polyester alloy composition and a preparation method thereof. β-(3,5-di-tert-butyl-4-hydroxyphenyl) propylene glycol ester and tris(2,4-di-tert-butylphenyl) phosphite are blended with polyester as antioxidants to improve the heat oxidation resistance of the polyester and polyester alloy composition. The above method has defects. Sodium dihydrogen phosphate is a low molecular weight compound and is easily decomposed by heat during processing and use, which reduces the thermal oxidation resistance of polyester materials. In addition, traditional hindered phenol-type antioxidants such as β-(3,5-di-tert-butyl-4-hydroxyphenyl) propylene glycol ester are not suitable for the preparation of PBSA polyester. This is because in the early stage of condensation polymerization of PBSA polyester, the molecular chain of PBSA polyester is short and the stability of the ester bond is poor. It is easy to break under high temperature conditions and form a large number of active free radicals. Traditional hindered phenol-type antioxidants such as β-(3,5-di-tert-butyl-4-hydroxyphenyl) propylene glycol ester are difficult to completely capture under appropriate conditions (without affecting the reaction polymerization rate and product polymerization degree), which reduces the mechanical properties of PBSA.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] In order to solve the defects of the above-mentioned technology, the present invention provides an antioxidant dedicated to biodegradable polyester PBSA and heat-resistant oxidation-resistant polybutylene succinate / adipate with excellent mechanical properties and a preparation method thereof. Compared with traditional antioxidants, the special antioxidant has the advantages of high molecular weight and excellent thermal stability, and significantly improves the oxidation resistance and mechanical properties of the product.
[0006] A method for preparing a special antioxidant for PBSA comprises the following steps: S1. Mix the reaction raw materials with aluminum triphenolate, p-cresol and toluene, and then carry out an alkylation reaction to obtain a reaction product 1.
[0007] S2. Mix the reaction product 1 with methyl acrylate and sodium methoxide and perform an addition reaction to obtain a reaction product 2.
[0008] S3, mixing the reaction product 2 with pentaerythritol, dimethyl sulfoxide and sodium methoxide, and then performing an ester exchange reaction to obtain a final product.
[0009] Preferably, in the preparation process of the antioxidant, in step S1, the reaction raw materials are selected from two of phenol, isobutylene, isopentenol, p-phenylenediamine, β-naphthol, methanol, ethanol, and vinyl acetate, preferably phenol and isopentenol.
[0010] Preferably, in the preparation process of the antioxidant, in step S1, the reaction temperature is 120-130° C., the reaction pressure is 1-1.4 MPa, and the reaction time is 6-10 h.
[0011] Preferably, in the preparation process of the antioxidant, in step S2, the reaction temperature is 120-125° C., and the reaction time is 2-4 h.
[0012] Preferably, in the preparation process of the antioxidant, in step S3, the reaction temperature is 135-145° C., and the reaction time is 3-5 h.
[0013] Preferably, the antioxidant has a molecular structure of chemical formula (1).
[0014] (1) The antioxidant is named pentaerythritol tetrakis[3-[3,5-(1,1-dimethylpropanol)-4-hydroxyphenyl]propanoate].
[0016] A method for preparing high-performance PBSA comprises the following steps: S4-1. Succinic acid, 1,4-butanediol, an esterification catalyst and a heat stabilizer are mixed and then subjected to an esterification reaction to obtain an ester reaction product a.
[0017] S4-2, mixing adipic acid, 1,4-butanediol, an esterification catalyst and a heat stabilizer, and performing an esterification reaction to obtain an ester reaction product b.
[0018] S5-1. Mix the ester reaction product a and the ester reaction product b with a polycondensation catalyst, a heat stabilizer and an antioxidant, and then conduct a pre-polycondensation reaction to obtain a pre-polycondensation product.
[0019] S5-2, subjecting the pre-polycondensation product to polycondensation reaction to obtain heat-resistant oxidation-resistant polybutylene succinate / adipate having excellent mechanical properties.
[0020] Preferably, in the above technical solution, the molar ratio of the diacid monomer to butanediol is 1:1-3, and the molar ratio of succinic acid to adipic acid is 3:7.
[0021] Preferably, in the above technical solution, in step S1-1, during the esterification reaction, the reaction temperature is 130-200°C, and the reaction time is 3-5 h.
[0022] Preferably, in the above technical solution, in step S1-2, during the esterification reaction, the reaction temperature is 130-200° C., and the reaction time is 3-5 h.
[0023] Preferably, in the above technical solution, in step S1-1, the esterification reaction is carried out under the action of an esterification catalyst and a heat stabilizer, and the added mass of the esterification catalyst is 0.001-1% of the sum of the mass of the dibasic acid and the diol. The added mass of the heat stabilizer is 0.001-1% of the sum of the mass of the dibasic acid and the diol.
[0024] Preferably, in the above technical solution, in step S1-2, the esterification reaction is carried out under the action of an esterification catalyst and a heat stabilizer, and the added mass of the esterification catalyst is 0.001-1% of the sum of the mass of the dibasic acid and the diol. The added mass of the heat stabilizer is 0.001-1% of the sum of the mass of the dibasic acid and the diol.
[0025] Preferably, in the above technical solution, in step S1, the esterification catalyst is selected from one or more of zinc acetate, tetrabutyl titanate, tetrabutyl zirconate, and manganese acetate, preferably zinc acetate and tetrabutyl titanate. The heat stabilizer is selected from one or more of triphenyl phosphate, trimethyl phosphate, sodium hydrogen phosphate, sodium dihydrogen phosphate, potassium hydrogen phosphate, potassium dihydrogen phosphate, potassium phosphate, magnesium hydrogen phosphate, magnesium dihydrogen phosphate, magnesium phosphate, triphenyl phosphite, and trimethyl phosphite.
[0026] Preferably, in the above technical solution, in step S2-1, the reaction temperature is 130-200°C, the reaction pressure is 100-300 Pa, and the reaction time is 0.5-1 h.
[0027] Preferably, in the above technical solution, in step S2-2, the reaction temperature is 200-240° C., the reaction pressure is 5-50 Pa, and the reaction time is 2-8 h.
[0028] Preferably, in the above technical scheme, in step S2-1, the polycondensation catalyst is selected from one or more of tetrabutyl titanate, tetrabutyl zirconate, zinc acetate, and manganese acetate, preferably tetrabutyl titanate; the heat stabilizer is one or more of triphenyl phosphate, trimethyl phosphate, sodium hydrogen phosphate, sodium dihydrogen phosphate, potassium hydrogen phosphate, potassium dihydrogen phosphate, potassium phosphate, magnesium hydrogen phosphate, magnesium dihydrogen phosphate, magnesium phosphate, triphenyl phosphite, and trimethyl phosphite; and the antioxidant is pentaerythritol tetrakis[3-[3,5-(1,1-dimethylpropanol)-4-hydroxyphenyl]propanoate].
[0029] Preferably, in the above technical solution, in step S2-1, the added mass of the polycondensation catalyst is 0.001-1% of the sum of the mass of the esterification products, the added mass of the heat stabilizer is 0.001-1% of the sum of the mass of the esterification products, and the added mass of the antioxidant is 0.001-1% of the sum of the mass of the esterification products.
[0030] The present invention provides a heat-resistant oxidation-resistant polybutylene succinate / adipate, with a weight average molecular weight ( M w ) is 26×10 4 g / mol-29×10 4 g / mol, intrinsic viscosity ≥2.0 dL / g, thermal oxidation resistance T d5%(空气中) ≥340℃, tensile strength ≥40.4 MPa, while obtaining high molecular weight polyester, the thermal oxidation resistance of the product is improved.
[0031] Compared with the prior art, the present invention has the following advantages: (1) The present invention obtains a new type of antioxidant, which has a higher molecular weight than traditional antioxidants and significantly improves the thermal stability of the antioxidant in polyester.
[0032] (2) Compared with traditional antioxidants, the thermal decomposition temperature of PBSA polyester prepared by new antioxidants is T d5%(空气中) )≥340℃, molecular weight≥26×10 4 g / mol, intrinsic viscosity ≥2.0 dL / g, and tensile strength ≥40.4 MPa, which significantly improves the thermal oxidation resistance and mechanical properties of PBSA polyester.
[0033] (3) The novel antioxidant designed by the present invention does not contain heavy metal elements, has the advantages of being green, environmentally friendly, non-toxic and harmless, and has broad application prospects in the fields of food packaging, medical devices, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The reaction equation for preparing the antioxidant tetrakis[3-[3,5-(1,1-dimethylpropanol)-4-hydroxyphenyl]propionic acid] pentaerythritol. DETAILED DESCRIPTION
[0035] The embodiments described below are part of the embodiments of the present invention, but not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] The present invention is further explained below in conjunction with specific implementation modes.
[0037] In the following examples of the present invention, the raw materials used are all commercially available products and are used directly without special treatment.
[0038] In the following embodiments of the present invention, the analytical test methods used are described as follows: 1. Intrinsic viscosity: According to the GB / T14190-2017 test standard, the intrinsic viscosity of the sample was determined using an Ubbelohde viscometer. The test temperature was 25°C, and the solvent used was a mixture of 1,1,2,2-tetrachloroethane and phenol in a mass ratio of 1:1.
[0039] 2. Weight average molecular weight ( M w ): The weight average molecular weight of the sample was determined by gel permeation chromatography at a temperature of 45°C, a solvent of chromatographic grade chloroform, a flow rate of 1.0 ml / min, and polystyrene was used as a reference standard.
[0040] 3. Thermal decomposition temperature ( T d5% ) The thermal decomposition temperature of the samples was measured by thermogravimetric analysis. T d5% ), the sample was heated from room temperature to 600 °C at a heating rate of 20 °C / min in an air environment.
[0041] 4. Tensile strength: According to GB / T 1040.2-2006 standard, the tensile test was carried out at 25°C and a tensile rate of 50 mm / min using an Instron 1122 tensile testing machine. The test was performed 5 times and the average value was taken as the test result.
[0042] Example 1 A method for preparing a novel antioxidant for PBSA, specifically comprising: A certain amount of phenol and isopentenol were mixed and put into reactor a, and a certain amount of aluminum triphenolate, toluene and p-methylphenol were added. The mixture was heated to 120-130°C under stirring conditions and reacted for 6 h. The pressure was then gradually reduced to 1-1.4 MPa and reacted for 4 h. The intermediate product 1 was obtained after washing with water, standing for stratification and high vacuum distillation.
[0043] The intermediate product 1 was mixed with an appropriate amount of sodium methoxide and methyl acrylate and put into a new reactor b at a reaction temperature of 120-125°C for 2.5 h. After acidification, heating under reflux, cooling and standing, the intermediate product 2 was obtained.
[0044] The intermediate product 2 was mixed with a certain amount of pentaerythritol and added to reactor c. A certain amount of dimethyl sulfoxide and sodium methoxide were added. The temperature was gradually raised to 135-145°C and reacted for 3 h. The final product was obtained after neutralization with acetic acid, dissolution with petroleum ether, stratification and cooling and crystallization.
[0045] The synthesis method of copolyester PBSA specifically comprises: Succinic acid (7 mol) and 1,4-butanediol (14 mol) were placed in a 40 L reactor, and 0.05 wt% of tetrabutyl titanate based on the total mass of the input raw materials and 0.03 wt% of trimethyl phosphate based on the total mass of the input raw materials were added. Under nitrogen protection, an esterification reaction was carried out at 190°C under normal pressure for 3 h to obtain an esterification product 1.
[0046] Adipic acid (3 mol) and 1,4-butanediol (6 mol) were added into a 20 L reactor, and 0.05 wt% of tetrabutyl titanate and 0.03 wt% of trimethyl phosphate based on the total mass of the input raw materials were added. Under nitrogen protection, the esterification reaction was carried out at 200 °C under normal pressure for 3.5 h to obtain the esterified product 2.
[0047] The two esterification products were put into a 50 L reactor, and 0.15 wt% of tetrabutyl titanate, 0.3 wt% of trimethyl phosphate and 0.2 wt% of pentaerythritol tetrakis[3-[3,5-(1,1-dimethylpropanol)-4-hydroxyphenyl]propanoate] based on the total mass of the reaction raw materials were added. The pre-condensation temperature was 200°C, the pressure was reduced to 150 Pa and the reaction was carried out for 30 min, then the temperature was increased to 230°C within 30 min, the pressure was reduced to 30 Pa and the reaction was carried out for 4 h, and the polymer PBSA1 was obtained by discharging, pelletizing and drying.
[0048] Example 2 In Example 2, a total of 8 tests were conducted, namely, Test 2.1, Test 2.2, Test 2.3, Test 2.4, Test 2.5, Test 2.6, Test 2.7, and Test 2.8.
[0049] The only difference between Experiment 2.1 and Example 1 is that the masses of tetrabutyl titanate and trimethyl phosphate put into the reactor before the polycondensation reaction in step S2-1 are 0.05 wt% and 0.1 wt% respectively based on the mass of the esterification product to obtain polymer PBSA2.
[0050] The only difference between Experiment 2.2 and Example 1 is that the masses of tetrabutyl titanate and trimethyl phosphate put into the reactor before the polycondensation reaction in step S2-1 are 0.2 wt% and 0.4 wt% respectively based on the mass of the esterification product, and polymer PBSA3 is obtained.
[0051] The only difference between Experiment 2.3 and Example 1 is that the masses of tetrabutyl titanate and trimethyl phosphate put into the reactor before the polycondensation reaction in step S2-1 are 0.25 wt% and 0.5 wt% respectively based on the mass of the esterification product, and polymer PBSA4 is obtained.
[0052] The only difference between Experiment 2.4 and Example 1 is that the masses of tetrabutyl titanate and trimethyl phosphate put into the reactor before the polycondensation reaction in step S2-1 are 0.3 wt% and 0.6 wt% respectively based on the mass of the esterification product, and polymer PBSA5 is obtained.
[0053] The only difference between Experiment 2.5 and Example 1 is that the masses of tetrabutyl titanate and trimethyl phosphate put into the reactor before the polycondensation reaction in step S2-1 are 0.35 wt% and 0.7 wt% respectively based on the mass of the esterification product, and polymer PBSA6 is obtained.
[0054] The only difference between Experiment 2.6 and Example 1 is that the masses of tetrabutyl titanate and trimethyl phosphate put into the reactor before the polycondensation reaction in step S2-1 are 0.4 wt% and 0.8 wt% respectively based on the mass of the esterification product, and polymer PBSA7 is obtained.
[0055] The only difference between Experiment 2.7 and Example 1 is that the masses of tetra-n-butyl titanate and trimethyl phosphate put into the reactor before the polycondensation reaction in step S2-1 are 0.45 wt% and 0.9 wt% respectively based on the mass of the esterification product, and polymer PBSA8 is obtained.
[0056] The only difference between Experiment 2.8 and Example 1 is that the masses of tetra-n-butyl titanate and trimethyl phosphate put into the reactor before the polycondensation reaction in step S2-1 are 0.5 wt% and 1 wt% respectively based on the mass of the esterification product, and polymer PBSA9 is obtained.
[0057] Example 3 In Example 3, a total of 4 tests were conducted, namely Test 3.1, Test 3.2, Test 3.3, and Test 3.4.
[0058] The only difference between Experiment 3.1 and Example 1 is that the antioxidant pentaerythritol tetrakis[3-[3,5-(1,1-dimethylpropanol)-4-hydroxyphenyl]propanoate] is added before the pre-condensation stage in step S2-1, with a mass of 0.03 wt% based on the total mass of the esterification product to obtain polymer PBSA10.
[0059] The only difference between Experiment 3.1 and Example 1 is that the weight of the antioxidant pentaerythritol tetrakis[3-[3,5-(1,1-dimethylpropanol)-4-hydroxyphenyl]propionic acid] added before the pre-polycondensation stage in step S2-1 is 0.05 wt% based on the total weight of the esterification product to obtain the polymer PBSA11.
[0060] The only difference between Experiment 3.1 and Example 1 is that the weight of the antioxidant pentaerythritol tetrakis[3-[3,5-(1,1-dimethylpropanol)-4-hydroxyphenyl]propionic acid] added before the pre-polycondensation stage in step S2-1 is 0.1 wt% based on the total weight of the esterification product to obtain polymer PBSA12.
[0061] The only difference between Experiment 3.1 and Example 1 is that the weight of the antioxidant pentaerythritol tetrakis[3-[3,5-(1,1-dimethylpropanol)-4-hydroxyphenyl]propionic acid] added before the pre-polycondensation stage in step S2-1 is 0.3 wt% based on the total weight of the esterification product to obtain PBSA13.
[0062] Comparative Example 1 Succinic acid (7 mol), adipic acid (3 mol) and 1,4-butanediol (20 mol) were added to a 40 L reactor, and a composition of zinc acetate and tetrabutyl titanate at 0.05 wt% of the total mass of the reaction raw materials and trimethyl phosphate at 0.03 wt% of the total mass of the reaction raw materials were added. The esterification reaction was carried out at 190°C under nitrogen protection for 3 h to obtain esterification products 1 and 2. Then, 0.3 wt% of tetrabutyl titanate at 0.15 wt% of the total mass of the reaction raw materials and trimethyl phosphate at 0.15 wt% of the total mass of the reaction raw materials were added, the temperature was raised to 230°C for 30 min, the pressure was reduced to 15 Pa, the reaction was carried out at a constant temperature for 4 h, and then the polymer PBSA14 was obtained by discharging, pelletizing and drying.
[0063] Comparative Example 2 Succinic acid (7 mol), adipic acid (3 mol) and 1,4-butanediol (20 mol) were added to a 40 L reactor, and a composition of zinc acetate and tetrabutyl titanate at 0.05 wt% of the total mass of the reaction raw materials and trimethyl phosphate at 0.03 wt% of the total mass of the reaction raw materials were added. The esterification reaction was carried out at 190°C under nitrogen protection for 3 h to obtain esterification products 1 and 2. Then, tetrabutyl titanate at 0.3 wt% of the total mass of the reaction raw materials, trimethyl phosphate at 0.15 wt% of the total mass of the reaction raw materials and β-(3,5-di-tert-butyl-4-hydroxyphenyl)propenol ester at 0.2 wt% of the total mass of the reaction raw materials were added, the temperature was raised to 230°C for 30 min, the pressure was reduced to 15 Pa, the reaction was carried out at a constant temperature for 4 h, and then the polymer PBSA15 was obtained by discharging, pelletizing and drying.
[0064] Table 1 PBSA performance test sample <![CDATA[M w (10 4 g / mol)]]> <![CDATA[Thermal decomposition temperature T d5% (空气中) (°C)]]> Viscosity (dL / g) Tensile strength (MPa) PBSA1 26.6 353.8 2.4 40.2 PBSA2 26.2 352.4 2.2 40.0 PBSA3 27.3 354.7 2.5 41.5 PBSA4 26.5 353.5 2.4 40.6 PBSA5 26.9 355.1 2.4 40.8 PBSA6 26.4 353.2 2.4 40.3 PBSA7 26.1 352.9 2.3 40.1 PBSA8 25.9 353.7 2.3 40.0 PBSA9 25.5 353.9 2.3 40.0 PBSA10 26.9 355.2 2.5 40.7 PBSA11 27.2 355.5 2.5 41.4 PBSA12 27.9 354.7 2.6 42.6 PBSA13 27.1 354.3 2.5 41.3 PBSA14 26.7 324.1 2.4 40.7 PBSA15 25.3 335.3 2.3 40.1 All examples used a new reaction system to prepare PBSA, Comparative Example 1 used an acid method and did not introduce an antioxidant system to prepare PBSA, and Comparative Example 2 introduced a traditional antioxidant β-(3,5-di-tert-butyl-4-hydroxyphenyl)propenol ester to prepare PBSA. Experiment 3.3 was selected to compare the performance with the comparative example experiment, as shown in Table 1.
[0065] Table 1 shows the properties of all the PBSA prepared in the experiment. The PBSA prepared by using the new antioxidant has high molecular weight, excellent mechanical properties and thermal oxidation resistance. Compared with the PBSA prepared by the traditional method without introducing the antioxidant system and introducing the traditional oxidation system, the thermal oxidation resistance is significantly improved. T d5% (空气中) The temperature of the polyester was increased by 20℃ and 30℃ respectively. In addition, the new antioxidant does not contain heavy metals, which is crucial for the application of polyester in food, medical devices, films and other fields and the green and sustainable development of the economy.
[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a special antioxidant for PBSA, characterized in that: The steps include: S1, mixing the reaction raw materials with aluminum triphenolate, p-cresol and toluene, and then performing an alkylation reaction to obtain a reaction product 1; S2, mixing the reaction product 1 with methyl acrylate and sodium methoxide and performing an addition reaction to obtain a reaction product 2; S3, mixing the reaction product 2 with pentaerythritol, dimethyl sulfoxide and sodium methoxide, and performing an ester exchange reaction to obtain a final product; The reaction raw materials in step S1 are phenol and isopentenol.
2. The preparation method according to claim 1, characterized in that: The structural formula of the final product is: 。 3. The preparation method according to claim 1, characterized in that: The antioxidant is tetrakis[3-[3,5-(1,1-dimethylpropanol)-4-hydroxyphenyl]propionic acid] pentaerythritol.
4. A method for preparing high-performance PBSA, characterized in that: The following steps are involved: S4-1, mixing succinic acid, 1,4-butanediol, an esterification catalyst and a heat stabilizer, and performing an esterification reaction to obtain an ester reaction product a; S4-2, mixing adipic acid, 1,4-butanediol, an esterification catalyst and a heat stabilizer, and performing an esterification reaction to obtain an ester reaction product b; S5-1, mixing the ester reaction product a and the ester reaction product b with a polycondensation catalyst, a heat stabilizer, and an antioxidant, and then performing a pre-polycondensation reaction to obtain a pre-polycondensation product; S5-2, subjecting the pre-polycondensation product to polycondensation reaction to obtain heat-resistant oxidation-resistant polybutylene succinate / adipate having excellent mechanical properties.
5. The preparation method according to claim 4, characterized in that: In steps S4-1 and S4-2, the ratio of adipic acid to succinic acid is 3:
7.
6. The preparation method according to claim 4, characterized in that: In steps S4-1 and S4-2, the esterification reaction temperature is 130-200° C., and the reaction time is 3-5 h.
7. The preparation method according to claim 4, characterized in that: In steps S4-1 and S4-2, the esterification reaction is carried out under the action of an esterification catalyst and a heat stabilizer, wherein the added mass of the esterification catalyst is 0.001-1% of the sum of the mass of the dibasic acid and the diol; the added mass of the heat stabilizer is 0.001-1% of the sum of the mass of the dibasic acid and the diol.
8. The preparation method according to claim 7, characterized in that: The esterification catalyst is selected from one or more of zinc acetate, tetrabutyl titanate, tetrabutyl zirconate, and manganese acetate; The heat stabilizer is selected from one or more of triphenyl phosphate, trimethyl phosphate, sodium hydrogen phosphate, sodium dihydrogen phosphate, potassium hydrogen phosphate, potassium dihydrogen phosphate, potassium phosphate, magnesium hydrogen phosphate, magnesium dihydrogen phosphate, magnesium phosphate, triphenyl phosphite, and trimethyl phosphite.
9. The preparation method according to claim 4, characterized in that: In step S5-1, the pre-polycondensation reaction temperature is 130-200°C, the reaction pressure is 100-300 Pa, and the reaction time is 0.5-1 h.
10. The preparation method according to claim 4, characterized in that: In step S5-2, the polycondensation reaction temperature is 200-240°C, the reaction pressure is 5-50 Pa, and the reaction time is 2-8 h; And / or, in step S5-2, the polycondensation reaction is carried out under the action of a polycondensation catalyst, a heat stabilizer and an antioxidant, the mass of the polycondensation catalyst added is 0.001-1% of the sum of the mass of the esterification products, the mass of the heat stabilizer added is 0.001-1% of the sum of the mass of the esterification products, and the mass of the antioxidant added is 0.001-1% of the sum of the mass of the esterification products; the polycondensation catalyst is selected from one or more of tetrabutyl titanate, tetrabutyl zirconate, zinc acetate, and manganese acetate; the heat stabilizer is one or more of triphenyl phosphate, trimethyl phosphate, sodium hydrogen phosphate, sodium dihydrogen phosphate, potassium hydrogen phosphate, potassium dihydrogen phosphate, potassium phosphate, magnesium hydrogen phosphate, magnesium dihydrogen phosphate, magnesium phosphate, triphenyl phosphite, and trimethyl phosphite.