Polyhydroxy dispersion and preparation method thereof

By using solution polymerization in aqueous hydroxyacrylic acid dispersions to connect oleic acid to the branch chain of acrylic acid, the molecular weight and activity of the polyhydroxy dispersion are improved, the problem of insufficient thixotropy is solved, and the high thixotropy of the coating is achieved and Stability, meets high standards for industrial applications.

CN119081022APending Publication Date: 2024-12-06WUXI HONGHUI NEW MATERIALS TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411242229.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing aqueous hydroxyacrylic dispersions have poor thixotropy, resulting in poor performance of coatings during construction and storage, making it difficult to meet the high standards of industrial applications.

Method used

The solution polymerization method is used to connect oleic acid to the branch chain of acrylic acid. Through the synergistic action of each component, the molecular weight and hydroxyl activity of the polyhydroxy dispersion are enhanced, and its flexibility and steric hindrance effect are enhanced, thereby improving the contact of the resin. transsexual.

Benefits of technology

It significantly improves the thixotropy of the coating, ensures good fluidity during construction and quickly restores viscosity at a static state, prevents pigment settlement and coating layering, and optimizes the construction performance and scope of application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0005029629640000021
    Figure BDA0005029629640000021
  • Figure BDA0005029629640000051
    Figure BDA0005029629640000051
Patent Text Reader

Abstract

The invention provides polyhydroxy dispersion and a preparation method thereof, and relates to the technical field of water-based resin.The preparation method comprises the steps that firstly, epoxy resin and oleic acid are mixed and heated under nitrogen protection, and heating continues after a catalyst is added; raising the temperature, and starting to dropwise add an alkene unsaturated monomer and part of the initiator; continuously dropwise adding an alkene unsaturated monomer and an initiator; cooling, slowly adding a neutralizer, and dropwise adding deionized water for dispersion; oleic acid is effectively connected into a branch chain of acrylic acid through a solution polymerization method, and under the synergistic effect of all the components, the prepared polyhydroxy dispersoid not only has the molecular weight and hydroxyl activity remarkably improved, but also has excellent flexibility and steric hindrance effect, so that the prepared polyhydroxy dispersoid has excellent mechanical properties on the premise of not sacrificing the performance of a paint film. The thixotropy of the resin is obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterborne resins, and in particular to a polyhydroxy dispersion and a preparation method thereof. Background Art

[0002] In the application field of water-based coatings, there are clear performance requirements for the thixotropy of resins. An ideal thixotropic resin can significantly reduce its viscosity when shear force is applied, which is convenient for construction operations; and in a static state, it can quickly return to a high viscosity state, thereby ensuring the storage stability of the coating; in addition, a resin with high thixotropy helps to prepare a thicker paint film and provides advantages for the directional arrangement of aluminum powder coatings.

[0003] At present, the vast majority of hydroxyl-containing water-based resins on the market are mainly water-based hydroxyl acrylic dispersions. These products are usually prepared by the solvent method, which relies on organic solvents to dissolve raw materials and adjust reaction conditions during the synthesis process. The molecular weight of the resulting water-based resin is often difficult to exceed 10,000, which directly affects the molecular chain structure and molecular weight distribution of the resin, resulting in poor thixotropy. Summary of the invention

[0004] In order to solve the problem of poor thixotropy of water-based hydroxy acrylic dispersions in the prior art, the present invention discloses a polyhydroxy dispersion and a preparation method thereof, wherein oleic acid is effectively connected to the side chains of acrylic acid by a solution polymerization method, and through the synergistic effect of the components, not only the molecular weight of the obtained polyhydroxy dispersion is significantly improved, but also the activity of the hydroxyl group is enhanced. In addition, the prepared polyhydroxy dispersion also has excellent flexibility and steric hindrance effect, thereby significantly improving the thixotropy of the resin without sacrificing the performance of the paint film.

[0005] The technical solution adopted by the present invention to solve its technical problem is:

[0006] A method for preparing a polyhydroxy dispersion comprises the following steps:

[0007] S1: Under nitrogen protection, epoxy resin and oleic acid are added to a reaction container, and when the temperature is raised to 100-102°C for dissolution, a catalyst is added; then the temperature is raised to 150-160°C with stirring; when the acid value of the polymer in the reaction system is less than 3, the temperature of the reaction system is lowered to 90-120°C, and an organic solvent is added; then, the temperature of the reaction system is raised to 135-145°C, and ethylenically unsaturated monomers and part of the initiator are added dropwise for 3-5 hours, followed by heat preservation and stirring;

[0008] S2: Then, continue to dropwise add ethylenically unsaturated monomers and a small amount of initiator for 1-3 hours; then add the remaining initiator, and then keep warm and stir;

[0009] S3: Finally, the temperature of the reaction system is cooled to 80-100°C, and a neutralizer is slowly added for 15-20 minutes, and then a portion of deionized water is added for dispersion, and the temperature is further cooled to 50-80°C, and then the remaining deionized water is gradually added and stirred for dispersion to obtain a polyhydroxy dispersion;

[0010] Wherein, by weight,

[0011]

[0012] The weight percentage of the initiator is the total weight percentage of the partial initiator, the small amount of initiator and the remaining initiator.

[0013] Optionally, the molar ratio of the ethylenically unsaturated monomer in step S1 to the ethylenically unsaturated monomer in step S2 is (2-3):1.

[0014] Optionally, the molar ratio of the part of the initiator in step S1, the small amount of initiator in step S2 and the remaining initiator is (5-6):(3-4):1.

[0015] Optionally, the molar ratio of the portion of deionized water to the remaining deionized water in step S3 is (1-1.5):1.

[0016] Optionally, the ethylenically unsaturated monomer is composed of the following raw materials in parts by weight:

[0017] 0.1 to 5 parts of carboxyl-containing vinyl monomer;

[0018] 3-25 parts of vinyl monomer;

[0019] 3-6 parts of hydroxyl monomer.

[0020] Optionally, in step S1, the molar ratio of the carboxyl-containing olefinic monomer in the olefinic unsaturated monomer to the oleic acid and the epoxy resin is (1-1.2):(1-1.2):1.

[0021] Optionally, the carboxyl-containing vinyl monomer is at least one of acrylic acid and methacrylic acid.

[0022] Optionally, the vinyl monomer is at least one of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-butyl acrylate, butyl methacrylate, isooctyl acrylate, isobornyl methacrylate, benzyl methacrylate, lauryl methacrylate, and styrene.

[0023] Optionally, the hydroxy monomer is at least one of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, hydroxyhexyl acrylate and hydroxyhexyl methacrylate.

[0024] Another object of the present invention is to provide a polyhydroxy dispersion prepared by the preparation method as described above.

[0025] The present invention has the following beneficial effects:

[0026] The present invention adopts a solution polymerization method to introduce monofunctional oleic acid into the side chain of acrylic acid. Through the synergistic effect of various components, not only the molecular weight of the obtained polyhydroxy dispersion is significantly improved, but also the activity of the hydroxyl group is enhanced, thereby making the coating product have excellent mechanical properties and chemical resistance. In addition, the introduction of oleic acid gives the prepared polyhydroxy dispersion higher flexibility and steric hindrance effect, thereby significantly improving the thixotropy of the resin without sacrificing the performance of the paint film, thereby making the prepared coating more fluid during construction, and quickly recovering the viscosity in a static state, preventing pigment sedimentation and coating stratification; and, thanks to the high thixotropy, the coating can still maintain excellent construction quality and stability during long-term storage, thereby optimizing the construction performance and scope of application. DETAILED DESCRIPTION

[0027] The present invention is now further described in detail. The embodiments described below are exemplary and intended to be used to explain the present invention, but cannot be understood as limiting the present invention. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention belong to the scope of protection of the present invention.

[0028] At present, the vast majority of hydroxyl-containing water-based resins on the market are mainly water-based hydroxyl acrylic dispersions. These products are usually prepared by the solvent method, which relies on organic solvents to dissolve raw materials and adjust reaction conditions during the synthesis process. The molecular weight of the resulting water-based resin is often difficult to exceed 10,000, which directly affects the molecular chain structure and molecular weight distribution of the resin, and thus leads to poor thixotropy. Although another emulsion polymerization method can prepare dispersions, the initial viscosity of the resulting product is low and the activity of the hydroxyl group is also weak, which makes the performance of the final prepared paint film unable to meet the high standards of industrial applications.

[0029] In order to solve the problem of poor thixotropy of aqueous hydroxy acrylic dispersion in the prior art, the present invention provides a method for preparing a polyhydroxy dispersion, comprising the following preparation steps:

[0030] S1: Under nitrogen protection, epoxy resin and oleic acid are added to a reaction container, and when the temperature is raised to 100-102°C for dissolution, a catalyst is added; then the temperature is raised to 150-160°C with stirring; when the acid value of the polymer in the reaction system is less than 3, the temperature of the reaction system is lowered to 90-120°C, and an organic solvent is added; then, the temperature of the reaction system is raised to 135-145°C, and ethylenically unsaturated monomers and part of the initiator are added dropwise for 3-5 hours, followed by heat preservation and stirring;

[0031] S2: Then, continue to dropwise add ethylenically unsaturated monomers and a small amount of initiator for 1-3 hours; then add the remaining initiator, and then keep warm and stir;

[0032] S3: Finally, the temperature of the reaction system is cooled to 80-100°C, and a neutralizer is slowly added for 15-20 minutes, and then a portion of deionized water is added for dispersion, and the temperature is further cooled to 50-80°C, and then the remaining deionized water is gradually added and stirred for dispersion to obtain a polyhydroxy dispersion;

[0033] Wherein, by weight,

[0034]

[0035] The weight percentage of the initiator is the total weight percentage of the partial initiator, the small amount of initiator and the remaining initiator; when the ethylenically unsaturated monomer and the initiator in the preparation step are both liquid, they can be added separately; when the initiator is solid, the initiator and the ethylenically unsaturated monomer must be mixed before adding.

[0036] The preparation method of the polyhydroxy dispersion provided by the present invention has a simple preparation process, temperature control and simple operation; a solution polymerization method is adopted to connect monofunctional oleic acid to the side chain of acrylic acid, and through the synergistic effect of each component, not only the molecular weight of the obtained polyhydroxy dispersion is significantly improved, but also the activity of the hydroxyl group is enhanced, thereby making the coating product have excellent mechanical properties and chemical resistance; in addition, the introduction of oleic acid gives the prepared polyhydroxy dispersion higher flexibility and steric hindrance effect, thereby significantly improving the thixotropy of the resin without sacrificing the performance of the paint film, thereby making the prepared coating more fluid during construction, and quickly recovering the viscosity in a static state, preventing pigment sedimentation and coating stratification; and, thanks to the high thixotropy, the coating can still maintain excellent construction quality and stability during long-term storage, thereby optimizing the construction performance and application range.

[0037] Specifically, the preferred epoxy resin of the present invention is at least one of E51 bisphenol A epoxy resin, 1,6-hexanediol diglycidyl ether, or polyalkylene glycol diglycidyl ethers with a molecular weight of 200 to 500.

[0038] In the present invention, the molar ratio of the olefinic unsaturated monomer in step S1 to the olefinic unsaturated monomer in step S2 is preferably (2-3):1; in this way, in step S1, the dripping speed of the olefinic unsaturated monomer is relatively fast to ensure that the concentration of the monomer in the reaction system is high, thereby promoting the rapid progress of the polymerization reaction; while in step S2, the dripping speed of the olefinic unsaturated monomer is relatively slow to control the reaction rate and avoid overheating of the system and the occurrence of side reactions; and the carboxyl groups that do not participate in the reaction can be concentrated in step S2, which can make the viscosity of the dispersion lower; in addition, through this staged dripping method, the molecular weight distribution of the polymer can be effectively controlled, so that the final polyhydroxy dispersion has better performance.

[0039] In order to better control the rate of the polymerization reaction, the molar ratio of part of the initiator in step S1, a small amount of initiator in step S2 and the remaining initiator is preferably (5-6):(3-4):1.

[0040] Furthermore, the preferred initiator of the present invention is at least one of azobisisobutyronitrile, azobisisoheptylnitrile, di-tert-amyl peroxide, di-tert-butyl peroxide, benzoyl peroxide, tert-butyl perbenzoate, tert-amyl perbenzoate, tert-butyl peracetate, tert-amyl peracetate, tert-butyl peracetate, tert-butyl peracetate, tert-butyl peroxide 2-ethylhexyl acid tert-amyl peroxide, and isopropylbenzene peroxide.

[0041] In order to ensure the stability and viscosity of the dispersion, the molar ratio of the partial deionized water to the remaining deionized water in step S3 is preferably (1-1.5):1.

[0042] The preferred ethylenically unsaturated monomers of the present invention are composed of the following raw materials in parts by weight:

[0043] 0.1 to 5 parts of carboxyl-containing vinyl monomer;

[0044] 3-25 parts of vinyl monomer;

[0045] 3-6 parts of hydroxyl monomer.

[0046] Furthermore, in the preferred step S1 of the present invention, the molar ratio of the carboxyl-containing olefinic monomer in the olefinic unsaturated monomer to oleic acid and epoxy resin is (1-1.2):(1-1.2):1; so that oleic acid can be effectively connected to the side chain of acrylic resin, so that it has excellent thixotropy and stability; the main function of the carboxyl-containing olefinic monomer in the olefinic unsaturated monomer in step S1 of the present invention is to provide an active double bond, copolymerize with the carboxyl group of oleic acid, and connect oleic acid to the side chain formed by acrylic acid through esterification or amidation. This process not only enhances the molecular weight and hydroxyl activity of the polyhydroxy dispersion, but also gives it excellent flexibility and steric hindrance effect, thereby effectively improving the thixotropy of the resin without reducing the performance of the paint film; at the same time, at high temperature, the thorough reaction of the monomer with the epoxy resin and oleic acid removes the free carboxyl groups in the resin, which helps to improve the water resistance and chemical stability of the resin.

[0047] The main function of the carboxyl-containing olefinic monomer in the olefinic unsaturated monomer in step S2 of the present invention is to provide hydrophilicity, thereby improving the comprehensive performance of the water-based resin; the carboxyl-containing olefinic monomer can form hydrogen bonds with water molecules, enhance the hydrophilicity of the resin, and thus improve its stability and dispersibility in the aqueous system; in addition, the carboxyl-containing olefinic monomer can also improve the water resistance and adhesion of the coating by forming more hydrogen bonds, thereby enabling the water-based resin to maintain good coating performance while also having excellent water resistance and chemical resistance, meeting the needs of different application scenarios.

[0048] In the present invention, the carboxyl-containing vinyl monomer is preferably at least one of acrylic acid and methacrylic acid.

[0049] The preferred vinyl monomer of the present invention is at least one of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-butyl acrylate, butyl methacrylate, isooctyl acrylate, isobornyl methacrylate, benzyl methacrylate, lauryl methacrylate and styrene.

[0050] The preferred hydroxy monomer of the present invention is at least one of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, hydroxyhexyl acrylate and hydroxyhexyl methacrylate.

[0051] In order to improve the stability of the dispersion in the aqueous system and prevent instability and flocculation caused by carboxyl groups, the present invention uses a neutralizer to neutralize the carboxyl groups in the system into salts; further, the present invention preferably uses at least one of the neutralizer of triethanolamine, N,N-dimethylethanolamine, triethylamine, N-dimethylethanolamine, diethylethanolamine, and N,N-dimethylisopropanolamine.

[0052] The preferred organic solvent of the present invention is at least one of propylene glycol methyl ether, propylene glycol butyl ether, ethylene glycol butyl ether, propylene glycol methyl ether acetate, diethylene glycol butyl ether, diethylene glycol phenyl ether, hydrocarbons such as toluene and xylene, ketones such as methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, esters such as ethyl acetate and butyl acetate, and acetate cellosolves such as methyl cellosolve acetate and acetate cellosolve; these solvents are all inactive solvents, because they do not contain active hydrogen, the chemical stability of the coating is guaranteed.

[0053] Furthermore, the preferred organic solvent of the present invention is at least one of propylene glycol methyl ether, propylene glycol butyl ether, ethylene glycol butyl ether, propylene glycol methyl ether acetate, diethylene glycol butyl ether, and diethylene glycol phenyl ether.

[0054] In particular, for the coating manufactured using the present invention, cellosolves and alcohol solvents can be used as diluent solvents. These solvents with active hydrogen can react with the resin to optimize the performance of the coating. This flexible solvent selection strategy provides a wide range of adjustment space for the coating formulation to meet the needs of different application scenarios.

[0055] In order to further shorten the reaction time and improve production efficiency, the preferred catalyst of the present invention is at least one of tetrabutylammonium bromide, ethyltriphenylphosphine bromide and boron trifluoride complex.

[0056] Another object of the present invention is to provide a polyhydroxy dispersion prepared by the preparation method as described above.

[0057] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below.

[0058] Unless otherwise specified, the epoxy resin in each embodiment of the present invention and the comparative example is E51 bisphenol A epoxy resin; the catalyst is tetrabutylammonium bromide; the organic solvent is propylene glycol methyl ether; the initiator is azobisisobutyronitrile; the neutralizer is triethanolamine; and the amount of materials used in each embodiment and the comparative example is measured in parts by weight.

[0059] Example 1

[0060] This embodiment provides a method for preparing a polyhydroxy dispersion, comprising the following preparation steps:

[0061] S1: Under nitrogen protection, epoxy resin and oleic acid are added to a reaction vessel, and when the temperature is raised to 100°C for dissolution, a catalyst is added; then the temperature is raised to 150°C with stirring; when the acid value of the polymer in the reaction system is less than 3, the temperature of the reaction system is lowered to 90°C, and an organic solvent is added; then, the temperature of the reaction system is raised to 135°C, and ethylenically unsaturated monomers and part of the initiator are added dropwise for 3 hours, followed by heat preservation and stirring;

[0062] S2: Then, continue to dropwise add ethylenically unsaturated monomers and a small amount of initiator for 1 hour; then dropwise add the remaining initiator, and then keep warm and stir;

[0063] S3: Finally, the temperature of the reaction system is cooled to 80°C, and a neutralizing agent is slowly added for 15 minutes, and then a portion of deionized water is added for dispersion, and the temperature is further cooled to 50°C, and then the remaining deionized water is gradually added for stirring and dispersion to obtain a polyhydroxy dispersion;

[0064] Wherein, by weight,

[0065]

[0066] Specifically, the molar ratio of the ethylenic unsaturated monomer in step S1 to the ethylenic unsaturated monomer in step S2 is 2:1; the molar ratio of part of the initiator in step S1, a small amount of initiator in step S2 and the remaining initiator is 5:4:1; the molar ratio of part of the deionized water in step S3 to the remaining deionized water is 1:1;

[0067] The ethylenically unsaturated monomer in step S1 is composed of the following raw materials in parts by weight:

[0068] 0.57 parts of acrylic acid;

[0069] Methyl acrylate 12 parts;

[0070] 3 parts of hydroxyethyl acrylate;

[0071] Wherein, in step S1, the molar ratio of the carboxyl-containing vinyl monomer in the ethylenically unsaturated monomer to oleic acid and epoxy resin is 1:1:1;

[0072] The ethylenically unsaturated monomer in step S2 is composed of the following raw materials in parts by weight:

[0073] 3 parts of acrylic acid;

[0074] 3 parts of methyl methacrylate;

[0075] 3 parts of hydroxyethyl methacrylate.

[0076] Example 2

[0077] This embodiment provides a method for preparing a polyhydroxy dispersion, comprising the following preparation steps:

[0078] S1: Under nitrogen protection, epoxy resin and oleic acid are added to a reaction container, and when the temperature is raised to 102°C and dissolved, a catalyst is added; then the temperature is raised to 160°C with stirring; when the acid value of the polymer in the reaction system is less than 3, the temperature of the reaction system is lowered to 120°C, and an organic solvent is added; then, the temperature of the reaction system is raised to 145°C, and ethylenically unsaturated monomers and part of the initiator are added dropwise for 5 hours, followed by heat preservation and stirring;

[0079] S2: Then, continue to dropwise add ethylenically unsaturated monomers and a small amount of initiator for 3 hours; then dropwise add the remaining initiator, and then keep warm and stir;

[0080] S3: Finally, the temperature of the reaction system is cooled to 100°C, and a neutralizer is slowly added for 20 minutes, and then a portion of deionized water is added for dispersion, and the temperature is further cooled to 80°C, and then the remaining deionized water is gradually added and stirred for dispersion to obtain a polyhydroxy dispersion;

[0081] Wherein, by weight,

[0082]

[0083] Specifically, the molar ratio of the ethylenic unsaturated monomer in step S1 to the ethylenic unsaturated monomer in step S2 is 2.75:1; the molar ratio of part of the initiator in step S1, a small amount of initiator in step S2 and the remaining initiator is 6:3:1; the molar ratio of part of the deionized water in step S3 to the remaining deionized water is 1.5:1;

[0084] The ethylenically unsaturated monomer in step S1 is composed of the following raw materials in parts by weight:

[0085] 1.2 parts of methacrylic acid;

[0086] Ethyl acrylate 21 parts;

[0087] Hydroxypropyl acrylate 6 parts;

[0088] Wherein, in step S1, the molar ratio of the carboxyl-containing vinyl monomer in the ethylenically unsaturated monomer to oleic acid and epoxy resin is 1:1:1;

[0089] The ethylenically unsaturated monomer in step S2 is composed of the following raw materials in parts by weight:

[0090] 2.2 parts of acrylic acid;

[0091] 3 parts of ethyl acrylate;

[0092] Hydroxypropyl methacrylate 6 parts.

[0093] Example 3

[0094] This embodiment provides a method for preparing a polyhydroxy dispersion, comprising the following preparation steps:

[0095] S1: Under nitrogen protection, epoxy resin and oleic acid are added to a reaction vessel, and when the temperature is raised to 101°C and dissolved, a catalyst is added; then the temperature is raised to 155°C with stirring; when the acid value of the polymer in the reaction system is less than 3, the temperature of the reaction system is lowered to 100°C, and an organic solvent is added; then, the temperature of the reaction system is raised to 140°C, and ethylenically unsaturated monomers and part of the initiator are added dropwise for 4 hours, followed by heat preservation and stirring;

[0096] S2: Then, continue to dropwise add ethylenically unsaturated monomers and a small amount of initiator for 2 hours; then dropwise add the remaining initiator, and then keep warm and stir;

[0097] S3: Finally, the temperature of the reaction system is cooled to 90°C, and a neutralizer is slowly added for 18 minutes, and then a portion of deionized water is added for dispersion, and the temperature is further cooled to 66°C, and then the remaining deionized water is gradually added for stirring and dispersion to obtain a polyhydroxy dispersion;

[0098] Wherein, by weight,

[0099]

[0100] Specifically, the molar ratio of the ethylenic unsaturated monomer in step S1 to the ethylenic unsaturated monomer in step S2 is 3:1; the molar ratio of part of the initiator in step S1, a small amount of initiator in step S2 and the remaining initiator is 5.5:3.5:1; the molar ratio of part of the deionized water in step S3 to the remaining deionized water is 1.2:1;

[0101] The ethylenically unsaturated monomer in step S1 is composed of the following raw materials in parts by weight:

[0102] Acrylic acid 1.0 part;

[0103] Isobornyl methacrylate 20 parts;

[0104] Hydroxyhexyl acrylate 5 parts;

[0105] Wherein, in step S1, the molar ratio of the carboxyl-containing vinyl monomer in the ethylenically unsaturated monomer to oleic acid and epoxy resin is 1:1:1;

[0106] The ethylenically unsaturated monomer in step S2 is composed of the following raw materials in parts by weight:

[0107] 3 parts of methacrylic acid;

[0108] 4 parts of butyl methacrylate;

[0109] Hydroxypropyl acrylate 3 parts.

[0110] Example 4

[0111] This embodiment provides a method for preparing a polyhydroxy dispersion, comprising the following preparation steps:

[0112] S1: Under nitrogen protection, epoxy resin and oleic acid are added to a reaction vessel, and when the temperature is raised to 100°C for dissolution, a catalyst is added; then the temperature is raised to 160°C with stirring; when the acid value of the polymer in the reaction system is less than 3, the temperature of the reaction system is lowered to 90°C, and an organic solvent is added; then, the temperature of the reaction system is raised to 145°C, and ethylenically unsaturated monomers and part of the initiator are added dropwise for 5 hours, followed by heat preservation and stirring;

[0113] S2: Then, continue to dropwise add ethylenically unsaturated monomers and a small amount of initiator for 1 hour; then dropwise add the remaining initiator, and then keep warm and stir;

[0114] S3: Finally, the temperature of the reaction system is cooled to 100°C, and a neutralizer is slowly added for 15 minutes, and then a portion of deionized water is added for dispersion, and the temperature is further cooled to 80°C, and then the remaining deionized water is gradually added and stirred for dispersion to obtain a polyhydroxy dispersion;

[0115] Wherein, by weight,

[0116]

[0117] Specifically, the molar ratio of the ethylenic unsaturated monomer in step S1 to the ethylenic unsaturated monomer in step S2 is 2:1; the molar ratio of part of the initiator in step S1, a small amount of initiator in step S2 and the remaining initiator is 5:4:1; the molar ratio of part of the deionized water in step S3 to the remaining deionized water is 1.5:1;

[0118] The ethylenically unsaturated monomer in step S1 is composed of the following raw materials in parts by weight:

[0119] 0.8 parts of acrylic acid;

[0120] Ethyl acrylate 23 parts;

[0121] Hydroxypropyl acrylate 6 parts;

[0122] Wherein, in step S1, the molar ratio of the carboxyl-containing vinyl monomer in the ethylenically unsaturated monomer to oleic acid and epoxy resin is 1:1:1;

[0123] The ethylenically unsaturated monomer in step S2 is composed of the following raw materials in parts by weight:

[0124] 4 parts of methacrylic acid;

[0125] 3 parts of isooctyl acrylate;

[0126] Hydroxypropyl acrylate 4 parts.

[0127] Example 5

[0128] This embodiment provides a method for preparing a polyhydroxy dispersion, comprising the following preparation steps:

[0129] S1: Under nitrogen protection, epoxy resin and oleic acid are added to a reaction vessel, and when the temperature is raised to 102°C and dissolved, a catalyst is added; then the temperature is raised to 160°C with stirring; when the acid value of the polymer in the reaction system is less than 3, the temperature of the reaction system is lowered to 120°C, and an organic solvent is added; then, the temperature of the reaction system is raised to 145°C, and ethylenically unsaturated monomers and part of the initiator are added dropwise for 4 hours, followed by heat preservation and stirring;

[0130] S2: Then, continue to dropwise add ethylenically unsaturated monomers and a small amount of initiator for 2 hours; then dropwise add the remaining initiator, and then keep warm and stir;

[0131] S3: Finally, the temperature of the reaction system is cooled to 80°C, a neutralizing agent is slowly added for 20 minutes, and then a portion of deionized water is added for dispersion, the temperature is further cooled to 50°C, and the remaining deionized water is gradually added for stirring and dispersion to obtain a polyhydroxy dispersion;

[0132] Wherein, by weight,

[0133]

[0134] Specifically, the molar ratio of the ethylenic unsaturated monomer in step S1 to the ethylenic unsaturated monomer in step S2 is 3:1; the molar ratio of part of the initiator in step S1, a small amount of initiator in step S2 and the remaining initiator is 6:3:1; the molar ratio of part of the deionized water in step S3 to the remaining deionized water is 1:1;

[0135] The ethylenically unsaturated monomer in step S1 is composed of the following raw materials in parts by weight:

[0136] 1 part of acrylic acid;

[0137] Styrene 13 parts;

[0138] Hydroxyhexyl acrylate 5 parts;

[0139] In step S1, the molar ratio of the carboxyl-containing vinyl monomer in the ethylenically unsaturated monomer to oleic acid and epoxy resin is 1:1:1;

[0140] The ethylenically unsaturated monomer in step S2 is composed of the following raw materials in parts by weight:

[0141] 4 parts of methacrylic acid;

[0142] 4 parts of ethyl acrylate;

[0143] 4 parts of hydroxybutyl methacrylate.

[0144] The difference between Comparative Example 1 and Example 1 is that oleic acid is not added.

[0145] The difference between Comparative Example 2 and Example 1 is that an equal amount of dimer acid is used to replace oleic acid.

[0146] The difference between Comparative Example 3 and Example 1 is that an equal amount of linoleic acid is used instead of oleic acid.

[0147] The difference between Comparative Example 4 and Example 1 is that an equal amount of 3,4-dihydroxyphthalic anhydride is used to replace the ethylenic unsaturated monomer in step S1.

[0148] The difference between Comparative Example 5 and Example 1 is that no acrylic acid is added to the ethylenically unsaturated monomer in step S1.

[0149] The difference between Comparative Example 6 and Example 1 is that the molar ratio of the carboxyl-containing olefinic monomer in the olefinic unsaturated monomer to oleic acid and epoxy resin in step S1 is 1.5:1.5:1.

[0150] The difference between Comparative Example 7 and Example 1 is that the molar ratio of the carboxyl-containing olefinic monomer in the olefinic unsaturated monomer to oleic acid and epoxy resin in step S1 is 0.8:0.8:1.

[0151] The difference between Comparative Example 8 and Example 1 is that the molar ratio of the ethylenically unsaturated monomer in step S1 to the ethylenically unsaturated monomer in step S2 is 1:1.

[0152] The difference between Comparative Example 9 and Example 1 is that the molar ratio of the ethylenically unsaturated monomer in step S1 to the ethylenically unsaturated monomer in step S2 is 5:1.

[0153] Performance Evaluation

[0154] The properties of the polyhydroxy dispersions prepared in the embodiments of the present invention and the comparative examples were tested, and the specific testing methods are as follows:

[0155] Emulsion appearance: visual inspection;

[0156] Solid content: tested according to GB / T1725 standard;

[0157] Viscosity test: Use rotational viscometer CAP2000+ for testing, test conditions: temperature 25℃, 10# rotor, speed 250S-1.

[0158] Storage stability: Place the polyhydroxy water dispersion in an oven at 50°C for 30 days and observe whether the physical state of the dispersion changes (stratification, turbidity, etc.).

[0159] The test results are shown in Table 1:

[0160] Table 1

[0161] Test items Emulsion appearance Solid content (%) Viscosity Storage stability Example 1 Milky white liquid 47.5% 3500mPa.s No change Example 2 Milky white liquid 50% 3250mPa.s No change Example 3 Milky white liquid 52% 3300mPa.s No change Example 4 Milky white liquid 48.5% 4500mPa.s No change Example 5 Milky white liquid 49.5% 3150mPa.s No change Comparative Example 1 Milky white liquid 47.5% 3400mPa.s No change Comparative Example 2 Milky white liquid 47.5% 3650mPa.s No change Comparative Example 3 Milky white liquid 47.5% 12500mPa.s No change Comparative Example 4 Milky white liquid 47.5% 3600mPa.s No change Comparative Example 5 Milky white liquid 47.5% 3500mPa.s No change Comparative Example 6 Milky white liquid 47.5% 1500mPa.s Layering Comparative Example 7 Milky white liquid 47.5% 3700mPa.s No change Comparative Example 8 Milky white liquid 46.5% 15000mPa.s No change Comparative Example 9 Milky white liquid 47.5% 1600mPa.s Layering

[0162] application

[0163] The polyhydroxy water dispersions obtained in Examples 1-5 and Comparative Examples 1-9 were prepared into topcoats according to the following formula in parts by weight:

[0164]

[0165]

[0166] The topcoats obtained in Examples 1-5 and Comparative Examples 1-9 were applied to the surface of the sandblasted steel plate, and after curing to form a paint film, the relevant properties of the paint film were tested. The specific test method is as follows:

[0167] Adhesion is tested according to GB / T 1720-1979 (1989) paint film adhesion test method;

[0168] Hardness: Pencil hardness test is carried out according to GB / T 6739-1996;

[0169] Thixotropy test method for water-based paint: Using Brookfeald viscometer, the pseudoplasticity of silver powder paint is characterized by the thixotropy index. The thixotropy index is the ratio of the viscosity value of the water-based paint measured at 6r to the viscosity value measured at 60r. The larger the ratio, the stronger the thixotropy.

[0170] The specific test results are shown in Table 2:

[0171] Table 2

[0172] Test items Adhesion(grade) hardness Thixotropic index Example 1 Level 1 2H 7.5 Example 2 Level 1 2H 7.0 Example 3 Level 1 2H 6.8 Example 4 Level 1 2H 7.7 Example 5 Level 1 2H 6.5 Comparative Example 1 Level 1 3H 3.0 Comparative Example 2 Level 1 2H 3.5 Comparative Example 3 Level 1 3H 6.1 Comparative Example 4 Level 4 4H 7.0 Comparative Example 5 Level 1 2H 3.6 Comparative Example 6 Level 1 2H 6.8 Comparative Example 7 Level 1 3H 4.7 Comparative Example 8 Level 1 2H 6.3 Comparative Example 9 Level 1 2H 7.0

[0173] It can be seen from the data in the above table that the polyhydroxy dispersion and the preparation method thereof provided in each embodiment of the present invention adopt a solution polymerization method to effectively connect oleic acid to the side chain of acrylic acid. Through the synergistic effect of each component, not only the molecular weight of the obtained polyhydroxy dispersion is significantly improved, but also the activity of the hydroxyl group is enhanced. In addition, the prepared polyhydroxy dispersion also has excellent flexibility and steric hindrance effect, thereby significantly improving the thixotropy of the resin without sacrificing the performance of the paint film.

[0174] The difference between Comparative Example 1 and Example 1 is that oleic acid is not added, and the thixotropic index of the prepared polyhydroxy dispersion is greatly reduced.

[0175] The difference between Comparative Example 2 and Example 1 is that the thixotropic index of the polyhydroxy dispersion prepared by using an equal amount of dimer acid to replace oleic acid is greatly reduced.

[0176] The difference between Comparative Example 3 and Example 1 is that an equal amount of linoleic acid is used to replace oleic acid, and the viscosity of the prepared polyhydroxy dispersion resin is relatively large.

[0177] The difference between Comparative Example 4 and Example 1 is that an equal amount of 3,4-dihydroxyphthalic anhydride is used to replace the ethylenic unsaturated monomer in step S1, and the prepared polyhydroxy dispersion has poor substrate adhesion.

[0178] The difference between Comparative Example 5 and Example 1 is that acrylic acid is not added to the ethylenically unsaturated monomer in step S1, oleic acid is connected to the straight chain of acrylic acid, and the thixotropic index of the prepared polyhydroxy dispersion is greatly reduced.

[0179] The difference between Comparative Example 6 and Example 1 is that the molar ratio of the carboxyl-containing vinyl monomer in the ethylenically unsaturated monomer to oleic acid and epoxy resin in step S1 is 1.5:1.5:1, and the prepared polyhydroxy dispersion resin has poor stability.

[0180] The difference between Comparative Example 7 and Example 1 is that the molar ratio of the carboxyl-containing vinyl monomer in the ethylenically unsaturated monomer to oleic acid and epoxy resin in step S1 is 0.8:0.8:1, and the thixotropic index of the prepared polyhydroxy dispersion decreases in a small range.

[0181] The difference between Comparative Example 8 and Example 1 is that the molar ratio of the ethylenically unsaturated monomer in step S1 to the ethylenically unsaturated monomer in step S2 is 1:1, and the prepared polyhydroxy dispersion resin has a relatively high viscosity.

[0182] The difference between Comparative Example 9 and Example 1 is that the molar ratio of the ethylenically unsaturated monomer in step S1 to the ethylenically unsaturated monomer in step S2 is 5:1, and the prepared polyhydroxy dispersion resin has poor stability.

[0183] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a polyhydroxy dispersion, characterized in that: The method comprises the following preparation steps: S1: Under nitrogen protection, epoxy resin and oleic acid are added to a reaction container, and when the temperature is raised to 100-102°C for dissolution, a catalyst is added; then the temperature is raised to 150-160°C with stirring; when the acid value of the polymer in the reaction system is less than 3, the temperature of the reaction system is lowered to 90-120°C, and an organic solvent is added; then, the temperature of the reaction system is raised to 135-145°C, and ethylenically unsaturated monomers and part of the initiator are added dropwise for 3-5 hours, followed by heat preservation and stirring; S2: Then, continue to dropwise add ethylenically unsaturated monomers and a small amount of initiator for 1-3 hours; then add the remaining initiator, and then keep warm and stir; S3: Finally, the temperature of the reaction system is cooled to 80-100°C, and a neutralizer is slowly added for 15-20 minutes, and then a portion of deionized water is added for dispersion, and the temperature is further cooled to 50-80°C, and then the remaining deionized water is gradually added and stirred for dispersion to obtain a polyhydroxy dispersion; Wherein, by weight, The weight percentage of the initiator is the total weight percentage of the partial initiator, the small amount of initiator and the remaining initiator.

2. The method for preparing a polyhydroxy dispersion according to claim 1, characterized in that: The molar ratio of the ethylenically unsaturated monomer in step S1 to the ethylenically unsaturated monomer in step S2 is (2-3):

1.

3. The method for preparing a polyhydroxy dispersion according to claim 1, characterized in that: The molar ratio of the part of the initiator in step S1, the small amount of initiator in step S2 and the remaining initiator is (5-6):(3-4):

1.

4. The method for preparing a polyhydroxy dispersion according to claim 1, wherein: The molar ratio of the partial deionized water to the remaining deionized water in step S3 is (1-1.5):

1.

5. The method for preparing a polyhydroxy dispersion according to claim 1, characterized in that: The ethylenically unsaturated monomer is composed of the following raw materials in parts by weight: 0.1 to 5 parts of carboxyl-containing vinyl monomer; 3-25 parts of vinyl monomer; 3-6 parts of hydroxyl monomer.

6. The method for preparing a polyhydroxy dispersion according to claim 5, characterized in that: The molar ratio of the carboxyl-containing vinyl monomer in the ethylenically unsaturated monomer in step S1 to the oleic acid and the epoxy resin is (1-1.2):(1-1.2):

1.

7. The method for preparing a polyhydroxy dispersion according to claim 5, characterized in that: The carboxyl-containing vinyl monomer is at least one of acrylic acid and methacrylic acid.

8. The method for preparing a polyhydroxy dispersion according to claim 5, characterized in that: The vinyl monomer is at least one of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-butyl acrylate, butyl methacrylate, isooctyl acrylate, isobornyl methacrylate, benzyl methacrylate, lauryl methacrylate and styrene.

9. The method for preparing a polyhydroxy dispersion according to claim 5, characterized in that: The hydroxy monomer is at least one of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, hydroxyhexyl acrylate and hydroxyhexyl methacrylate.

10. A polyhydroxy dispersion, characterized in that The polyhydroxy dispersion is prepared by the preparation method of any one of claims 1 to 9.