Polyester type polymeric dispersant and preparation method thereof
By preparing high molecular weight polyester high dispersant, the steric hindrance stabilization effect is used to prevent pigment flocculation, the problem of insufficient dispersion efficiency and compatibility in the prior art is solved, and the stability and performance of pigment is improved, and suitable for solvents The coatings meet the needs of high solids content and low viscosity coatings.
Patent Information
- Application Number
- CN202411412951.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-12-06
AI Technical Summary
The existing polyester polymer dispersants have shortcomings in dispersion efficiency, compatibility and stability, resulting in uneven dispersion of pigments, degradation of product performance, and a single function cannot meet the needs of special application.
A polyester polymer dispersant preparation method is adopted to prevent pigment reflocculation through steric hindrance stabilization, improve pigment wetting and gloss, reduce viscosity, and prepare high molecular weight through specific reaction steps and catalyst use. Wetting and dispersing aids to ensure that the pigment carries the same charge and prevent flocculation.
It improves the pigment's tinting power and hue stability, reduces grinding time, reduces viscosity, avoids thixotropy, enhances dispersion efficiency and compatibility, and ensures the long-term stability and durability of the product.
Smart Images

Figure BDA0005078522650000041 
Figure BDA0005078522650000091 
Figure BDA0005078522650000092
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of dispersants, and in particular to a polyester type polymer dispersant and a preparation method thereof. Background Art
[0002] Polyester polymer dispersants are additives widely used in coatings, inks, adhesives and other industries. Their main function is to improve the dispersibility of pigments or fillers in the medium and improve the stability and performance of the product. They are usually composed of polyester polymers, which have good hydrophilicity and lipophilicity and can effectively disperse pigments and fillers in water-based and solvent-based systems. They adsorb on the surface of the pigment to form a protective film, reduce the interaction between pigment particles, thereby preventing agglomeration and precipitation, and improving the stability and rheology of the system.
[0003] Defects and shortcomings of the existing technology:
[0004] Limited dispersion efficiency: Some polyester polymer dispersants may not be efficient enough in dispersion, resulting in uneven pigment dispersion, affecting the color and gloss of the final product.
[0005] Compatibility issues: In some systems, polyester polymer dispersants may not be compatible with base materials or other additives, resulting in reduced product performance, such as coating adhesion and water resistance.
[0006] Single function: Existing polyester polymer dispersants may have relatively single functions and cannot meet the needs of some special applications, such as high-solid content coatings, low-viscosity coatings, etc.
[0007] Stability issues: Under long-term storage or extreme conditions, some polyester polymer dispersants may experience performance degradation, such as weakened dispersion effect and stratification. Summary of the invention
[0008] In order to solve the problems mentioned in the above background technology, the present invention provides a method for preparing a polyester-type polymer dispersant. The prepared polyester polymer dispersant is a high molecular weight wetting and dispersing aid for solvent-based coatings. It prevents the pigment from reflocculating by steric stabilization, thereby stabilizing the tinting power and hue of the pigment in the coating and pigment slurry. It improves pigment wetting, reduces the time required for the grinding process, improves gloss and leveling, reduces viscosity and avoids thixotropy. This additive makes the pigments carry the same charge, thereby preventing possible flocculation of different pigments. Due to the high molecular weight and resin-like structure, this polymer dispersant will not affect the durability of the coating base material.
[0009] In order to achieve the above object, the present invention adopts the following technical solutions:
[0010] A preparation method of a polyester type polymer dispersant, the first step of the reaction: tetradecanol opens cyclohexyl lactone under the action of a catalyst zirconium n-butoxide to generate a polycaprolactone chain segment with a hydroxyl group at the end, and this process is repeated continuously to form a long-chain polycaprolactone.
[0011] The second step reaction: The NCO group contained in the HDI dimer reacts with the hydroxyl group on the polycaprolactone segment under the action of the catalyst dibutyltin dilaurate to produce the final product. It includes the following steps:
[0012] Add tetradecanol and caprolactone to the reactor in turn, stir for 10 minutes to mix evenly, then evacuate to remove air, then turn off the vacuum and introduce nitrogen to break the vacuum, keeping the nitrogen flow rate at 0.2-0.3m 3 / h, start stirring and heating;
[0013] When the temperature rises to 80±5℃, turn off the nitrogen to evacuate, and continue to raise the temperature to 100±5℃ (to remove moisture from the raw materials);
[0014] At 100±5℃, break the vacuum with nitrogen, add zirconium n-butoxide, and maintain the nitrogen flow rate at 0.2~0.3m 3 / h, raise the temperature to 130±5℃ and keep the reaction for 2 hours, then take samples for GPC testing. When the molecular weight is 2000±100 and no small peak appears, it is considered to have reached the reaction endpoint; if the requirement is not met, take samples every 2 hours until the requirement is met;
[0015] Cool down to 80±5℃, add catalyst dibutyltin dilaurate and inhibitor 2,6-di-tert-butyl-p-cresol, then add HDI dimer in batches, and control the addition within 40min to 60min. This process is an exothermic reaction, and the process temperature is controlled at 80±5℃;
[0016] After 2 hours of heat treatment at 80±5℃, take samples to test the NCO value. When the NCO value is ≤0.1%, the reaction is considered to be over. If it does not meet the requirement, take samples every 1 hour until it meets the requirement.
[0017] The temperature was lowered to 60±5°C and pressure filtered to obtain the final product.
[0018] Preferably, the mass ratio of the reactants tetradecanol: caprolactone: HDI dimer is: (10-20): (60-70): (10-20).
[0019] Preferably, the amount of zirconium n-butoxide as the catalyst for the first step reaction accounts for 0.40 wt% of the total mass of the feed.
[0020] Preferably, the amount of dibutyltin dilaurate as the catalyst for the second step reaction accounts for 0.06wt% of the total mass of the feed.
[0021] Preferably, the amount of the polymerization inhibitor 2,6-di-tert-butyl-p-cresol used in the second step reaction accounts for 0.06 wt % of the total mass of the feed.
[0022] The polyester type polymer dispersant is prepared by the preparation method.
[0023] Reaction formula of the present invention is as follows:
[0024]
[0025] Note: n=7.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The technical problem solved by the present invention is to provide a new method for preparing a polyester polymer dispersant, which is a high molecular weight wetting and dispersing aid for solvent-based coatings. It prevents the re-flocculation of pigments through steric stabilization, thereby stabilizing the tinting strength and hue of the pigments in the coatings and pigment slurries. It improves the wetting of pigments, reduces the time required for the grinding process, improves the gloss and leveling, reduces the viscosity and avoids thixotropy. This additive makes the pigments carry the same charge, thereby preventing possible flocculation of different pigments. Due to the high molecular weight and resin-like structure, this polymer dispersant will not affect the durability of the coating base material. The product has stable performance, high dispersion efficiency, strong compatibility, will not affect the weakening of the coating, improves the wettability of the pigment to a certain extent, and has a good market prospect. DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Unless otherwise specified, the raw materials used in the present invention are all conventional products purchased from the market.
[0030] Example 1
[0031] Add 60g tetradecanol and 230g caprolactone into a four-necked flask with a thermometer and a vacuum connection tube. Stir for 10 minutes to mix well and then vacuum to remove the air in the flask. Maintain a nitrogen flow rate of 0.2m 3 / h, start stirring and heating; when the temperature rises to 80℃, turn off the nitrogen to evacuate, continue to heat to 100℃, break the vacuum with nitrogen, add 1.40g zirconium n-butoxide, and maintain the nitrogen flow rate at 0.2m 3 / h, heat to 130℃ and keep warm for reaction for 2 hours, then take samples for GPC detection, when the molecular weight is 2000±100 and no small peak appears, cool to 80℃; add 0.20g dibutyltin dilaurate and 0.21g 2,6-di-tert-butyl-p-cresol, then add 56.50g HDI dimer in portions, and control the addition within 40min. This process is an exothermic reaction, and the process temperature is controlled at 80℃. After keeping warm at 80℃ for reaction for 2 hours, take samples for detection of NCO value, and when NCO value ≦0.1%, the reaction is deemed to be over, cool to 60℃, and filter under pressure to obtain a colorless and transparent polyester polymer dispersant product.
[0032] Example 2
[0033] Add 60.01g tetradecanol and 230.02g caprolactone into a four-necked flask with a thermometer and a vacuum connection tube. Stir for 10 minutes to mix well and then vacuum to remove the air in the flask. Maintain a nitrogen flow rate of 0.25m 3 / h, start stirring and heating; when the temperature rises to 81°C, turn off the nitrogen to evacuate, continue to heat to 102°C, break the vacuum with nitrogen, add 1.42g zirconium n-butoxide, and maintain the nitrogen flow rate at 0.25m 3 / h, heat to 132℃ and keep warm for reaction for 2 hours, then take samples for GPC detection, when the molecular weight is 2000±100 and no small peak appears, cool to 82℃; add 0.21g dibutyltin dilaurate and 0.20g 2,6-di-tert-butyl-p-cresol, then add 56.51g HDI dimer in portions, and control the addition within 45min. This process is an exothermic reaction, and the process temperature is controlled at 82℃. After keeping warm at 82℃ for reaction for 2 hours, take samples for detection of NCO value, and when NCO value ≦0.1%, the reaction is deemed to be over, cool to 60℃, and filter under pressure to obtain a colorless and transparent polyester polymer dispersant product.
[0034] Example 3
[0035] Add 60.03g tetradecanol and 229.99g caprolactone into a four-necked flask with a thermometer and a vacuum connection tube. Stir for 10 minutes to mix well and then vacuum to remove the air in the flask. Maintain a nitrogen flow rate of 0.25m 3 / h, start stirring and heating; when the temperature rises to 75℃, turn off the nitrogen to evacuate, continue to heat to 95℃, break the vacuum with nitrogen, add 1.41g zirconium n-butoxide, and maintain the nitrogen flow rate at 0.25m 3 / h, heat to 125℃ and keep warm for reaction for 2 hours, then take samples for GPC detection, when the molecular weight is 2000±100 and no small peak appears, cool to 75℃; add 0.22g of dibutyltin dilaurate and 0.22g of 2,6-di-tert-butyl-p-cresol, and then add 56.53g of HDI dimer in portions, and control the addition within 45min. This process is an exothermic reaction, and the process temperature is controlled at 75℃. After keeping warm for reaction at 75℃ for 2 hours, take samples for detection of NCO value, and when NCO value ≦0.1%, the reaction is deemed to be over, cool to 55℃, and filter under pressure to obtain a colorless and transparent polyester polymer dispersant product.
[0036] Example 4
[0037] Add 59.99g tetradecanol and 230.02g caprolactone into a four-necked flask with a thermometer and a vacuum connection tube. Stir for 10 minutes to mix well and then vacuum to remove the air in the flask. Maintain a nitrogen flow rate of 0.3m 3 / h, start stirring and heating; when the temperature rises to 85℃, turn off the nitrogen to evacuate, continue to heat to 105℃, break the vacuum with nitrogen, add 1.39g zirconium n-butoxide, and maintain the nitrogen flow rate at 0.3m 3 / h, heat to 130℃ and keep warm for reaction for 2 hours, then take samples for GPC detection, when the molecular weight is 2000±100 and no small peak appears, cool to 85℃; add 0.19g of dibutyltin dilaurate and 0.20g of 2,6-di-tert-butyl-p-cresol, and then add 56.49g of HDI dimer in portions, and control the addition within 40min~60min. This process is an exothermic reaction, and the process temperature is controlled at 85℃. After keeping warm for reaction at 85℃ for 2 hours, take samples for detection of NCO value, and when NCO value ≦0.1%, the reaction is deemed to be over, cool to 65℃, and filter under pressure to obtain a colorless and transparent polyester polymer dispersant product.
[0038] Example 5
[0039] Add 60.05g tetradecanol and 230.01g caprolactone into a four-necked flask with a thermometer and a vacuum connection tube. Stir for 10 minutes to mix well and then vacuum to remove the air in the flask. Maintain a nitrogen flow rate of 0.3m 3 / h, start stirring and heating; when the temperature rises to 80℃, turn off the nitrogen to evacuate, continue to heat to 100℃, break the vacuum with nitrogen, add 1.40g zirconium n-butoxide, and maintain the nitrogen flow rate at 0.3m 3 / h, heat to 130℃ and keep warm for reaction for 2 hours, then take samples for GPC detection, when the molecular weight is 2000±100 and no small peak appears, cool to 80℃; add 0.21g of dibutyltin dilaurate and 0.21g of 2,6-di-tert-butyl-p-cresol, and then add 56.55g of HDI dimer in portions, and control the addition within 60min. This process is an exothermic reaction, and the process temperature is controlled at 80℃. After keeping warm at 80℃ for reaction for 2 hours, take samples for detection of NCO value, and when NCO value ≦0.1%, the reaction is deemed to be over, cool to 60℃, and filter under pressure to obtain a colorless and transparent polyester polymer dispersant product.
[0040] Example 6
[0041] Add 60.01g tetradecanol and 230.05g caprolactone into a four-necked flask with a thermometer and a vacuum connection tube. Stir for 10 minutes to mix well and then vacuum to remove the air in the flask. Maintain a nitrogen flow rate of 0.3m 3 / h, start stirring and heating; when the temperature rises to 85℃, turn off the nitrogen to evacuate, continue to heat to 105℃, break the vacuum with nitrogen, add 1.42g zirconium n-butoxide, and maintain the nitrogen flow rate at 0.2m 3 / h, heat to 135℃ and keep warm for reaction for 2 hours, then take samples for GPC detection, when the molecular weight is 2000±100 and no small peak appears, cool to 85℃; add 0.21g dibutyltin dilaurate and 0.23g 2,6-di-tert-butyl-p-cresol, then add 56.50g HDI dimer in portions, and control the addition within 60min. This process is an exothermic reaction, and the process temperature is controlled at 85℃. After keeping warm for reaction at 85℃ for 2 hours, take samples for detection of NCO value, and when NCO value ≦0.1%, the reaction is deemed to be over, cool to 65℃, and filter under pressure to obtain a colorless and transparent polyester polymer dispersant product.
[0042] The data comparison of the colorless and transparent polyester polymer dispersant prepared above is shown in Table 1:
[0043] Table 1
[0044] serial number Viscosity (25℃) Weight average molecular weight (GPC) Example 1 5688 31220 Example 2 5620 31447 Example 3 5597 30988 Example 4 5711 31125 Example 5 5723 31786 Example 6 5698 31824
[0045] From the above finished product test results, it can be observed that the performance indicators of the test finished products are stable.
[0046] The stability of the coating prepared with the above polymer dispersant at room temperature is shown in Table 2:
[0047] Table 2
[0048]
[0049] The stability of the coating prepared with the above polymer dispersant at 60°C is shown in Table 3:
[0050] Table 3
[0051]
[0052] It can be seen from Tables 2 and 3 above that the coating prepared with the dispersant described in this article has good storage stability.
[0053] Compatibility test of the above polymer dispersants
[0054] The polymer dispersants prepared in Examples 1 to 6 were uniformly mixed with solvents and a variety of film-forming resins in a mass ratio of 1:1:10. At the same time, the same type of polymer dispersants on the market were used as a control group for testing. After standing for 72 hours, the dispersion system was observed to see whether it was clear and transparent. Compatibility test, solvent: xylene, test results are shown in Table 4.
[0055] Table 4
[0056]
[0057] It can be seen from Table 4 that the polymer dispersant prepared by the present invention has better compatibility than similar products on the market.
[0058] Detection method:
[0059] 1. GPC: Waters e2695
[0060] 2. Viscosity: Brookfield digital viscometer DV3TRVTJO
[0061] 3. NCO value determination: according to the method specified in GB / T 12009.4
[0062] 4. Laser particle size analyzer: LA300.
[0063] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a polyester type polymer dispersant, characterized in that: The following steps are involved: S1. Add tetradecanol and caprolactone to the reactor in turn, stir and mix them evenly, then evacuate to remove the air, then turn off the vacuum and introduce nitrogen to break the vacuum, keeping the nitrogen flow rate at 0.2-0.3m 3 / h, start stirring and heating; S2. When the temperature rises to 80℃±5℃, turn off the nitrogen to evacuate. When the temperature continues to rise to 100±5℃, break the vacuum with nitrogen. Add zirconium n-butoxide and maintain the nitrogen flow rate at 0.2~0.3m 3 / h, raise the temperature to 130±5℃ and keep the reaction for 2 hours before sampling and GPC testing; S3, cool down to 80±5℃, add catalyst dibutyltin dilaurate and inhibitor 2,6-di-tert-butyl-p-cresol, then add HDI dimer in batches, control the addition within 40min~60min, and control the process temperature at 80±5℃; S4. After keeping the reaction at 80±5℃ for 2 hours, take a sample to detect the NCO value. When the NCO value is ≤0.1%, the reaction is considered to be over. Cool down to 60±5℃ and filter under pressure to obtain the final product.
2. The method for preparing a polyester polymer dispersant according to claim 1, characterized in that: The mass ratio of tetradecanol: caprolactone: HDI dimer is: (10-20): (60-70): (10-20).
3. The method for preparing a polyester type polymer dispersant according to claim 1, characterized in that: The amount of the catalyst zirconium n-butoxide used in S2 accounts for 0.40wt% of the total mass of the feed.
4. The method for preparing a polyester type polymer dispersant according to claim 1, characterized in that: In S2, when the molecular weight is 2000±100 and no small peak appears, the reaction endpoint is considered to be reached; if the requirement is not met, sampling and testing are performed every 2 hours until the requirement is met.
5. The method for preparing a polyester type polymer dispersant according to claim 1, characterized in that: When the NCO value in S4 does not meet the requirement, sampling and testing are carried out every hour until the NCO value reaches ≦0.1%.
6. The method for preparing a polyester polymer dispersant according to claim 1, characterized in that: The amount of the catalyst dibutyltin dilaurate used in S3 accounts for 0.06wt% of the total mass of the feed.
7. The method for preparing a polyester polymer dispersant according to claim 1, characterized in that: The amount of the polymerization inhibitor 2,6-di-tert-butyl-p-cresol used in S4 accounts for 0.06wt% of the total mass of the feed.
8. A polyester polymer dispersant prepared by the preparation method according to any one of claims 1 to 7.