Amorphous copolyester and preparation method thereof
Ca-SIPM salts are prepared by reacting dimethyl isophthalate-5-sulfonate with CaCl2 in the production of amorphous polyester materials and transesterified with ethylene glycol, combining dibasic acid and diol The copolymerization reaction solves the problems of high cost and high addition in the prior art, realizes the complete amorphization and cost reduction of polyester materials, and improves the competitiveness and application breadth of materials.
Patent Information
- Application Number
- CN202411338817.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-25
AI Technical Summary
The production cost of existing amorphous polyester materials is relatively high, and the addition of the third monomer needs to exceed 9% or 20% to achieve amorphous polyester, which affects the economics and application breadth of the material.
Ca-SIPM salt containing divalent metal ions is prepared by reacting dimethyl isophthalate-5-sulfonate with CaCl2 in water, and undergoing transesterification reaction with ethylene glycol to obtain Ca-SIPE, followed by binary The acid and diol were copolymerized and the completely amorphous polyethylene terephthalate was successfully synthesized, and the amount of the third monomer added was only 0.25 to 3% of the molar amount of the first monomer.
The complete amorphization of polyester materials has been achieved, which significantly reduces production costs, makes high-performance polyester materials more competitive in commercial applications, and broadens the application fields, with excellent physical and processing properties.
Smart Images

Figure CN119081092A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyester fibers, and in particular to an amorphous copolyester and a preparation method thereof. Background Art
[0002] Amorphous polyester has unique properties, such as high transparency, good toughness and easy processing. These properties make amorphous polyester suitable for the manufacture of extruded films, packaging materials, and medical equipment components. It is also widely used in many high-tech products. Its industrial development and technological innovation continue to promote the development of the field of materials science.
[0003] In the prior art, researchers synthesize amorphous polyethylene terephthalate copolyester by introducing isophthalic acid (IPA) (Journal of Applied Polymer Science, 2019, 136, 47186). However, the amount of IPA added in this synthesis method often needs to exceed 20% to make the polyester material completely amorphous; another method is to introduce 5-sulfobis(hydroxyethyl)sodium isophthalate (SIPE) (Industrial & Engineering Chemistry Research, 2023, 62, 14648) into the PET chain segment to reduce the crystallinity of the polyester and make it amorphous. However, this method often requires an addition amount of more than 9% to achieve the amorphous polyester, which makes the production material cost higher.
[0004] In view of this, it is necessary to design a cost-effective and efficient amorphous copolyester and a preparation method thereof. Summary of the invention
[0005] The purpose of the present application is to provide a method for preparing an amorphous copolyester, which uses a specific monomer sodium isophthalate-5-sulfonate dimethyl ester (Na-SIPM) and CaCl 2 The reaction was carried out in water to obtain a Ca-SIPM salt containing a divalent metal ion coordination. Then, the Ca-SIPM salt was subjected to an ester exchange reaction with ethylene glycol (EG) to obtain a new polyester precursor, namely Ca-SIPE. Finally, a new completely amorphous polyethylene terephthalate was successfully synthesized by copolymerizing Ca-SIPE with a dibasic acid and a diol. This preparation method achieves complete amorphization of polyester with a minimum addition of a third monomer (the amount of the third monomer added is 0.25 to 3% of the molar amount of the first monomer), significantly reducing production costs, making this high-performance polyester material more competitive in commercial applications, and providing new possibilities for the sustainable development and environmentally friendly applications of polyester materials.
[0006] In a first aspect, the present invention provides a method for preparing an amorphous copolyester, comprising the following steps:
[0007] S1, sodium dimethyl 5-sulfonate, CaCl 2 Dissolve in deionized water in a molar ratio of 2:(1.1-1.4) and mix in a reactor; stir the obtained mixture magnetically at room temperature for 2-3 days, then collect the precipitate by filtration and dry until a constant weight is reached to obtain Ca-SIPM salt;
[0008] S2, in a nitrogen environment, Ca-SIPM salt and ethylene glycol were subjected to transesterification reaction at a molar ratio of 1: (10.4-15.4) to obtain a transparent liquid product named Ca-SIPE; the catalyst used in the transesterification reaction was Mn(OAc) 2 ; the Mn(OAc) 2 The mass fraction is 0.3% to 0.6%;
[0009] S3, using terephthalic acid as the first monomer and ethylene glycol as the second monomer, the first monomer and the second monomer are put into a reaction kettle for esterification reaction; when the water output reaches the theoretical water output, the esterification reaction is completed;
[0010] S4, after the esterification is completed, the third monomer Ca-SIPE obtained in step S2 is added, and the mixture is reacted at normal pressure for 0.5 to 1 hour, and then a polycondensation reaction is carried out. The obtained copolymer is pelletized to obtain an amorphous copolyester.
[0011] Preferably, in step S4, the amount of the third monomer added is 0.25-3% of the molar amount of the first monomer.
[0012] Preferably, in step S3, the molar ratio of the first monomer to the second monomer is 1:(1.2-1.6).
[0013] Preferably, in step S2, the reaction temperature of the transesterification reaction is 160-200° C., and the reaction time is 3.5-4.5 h.
[0014] Preferably, in step S2, the end point of the transesterification reaction is when no methanol is distilled out.
[0015] Preferably, in step S4, the specific process of the polycondensation reaction is: first, slowly evacuate to 80-100 Pa within 1-3 hours for pre-polycondensation treatment, then heat the system to 260-280° C., and continue the reaction for 1-2 hours.
[0016] Preferably, in step S3, during the esterification reaction, the reaction temperature is 240-260° C., the reaction time is 2-4 h, and the pressure in the reactor is 100 kPa-360 kPa.
[0017] Preferably, in step S3, the catalyst added to the esterification reaction is Sb 2 O 3 , the added amount of the catalyst is 400 to 600 ppm.
[0018] In a second aspect, an embodiment of the present application provides an amorphous copolyester, which is prepared by the preparation method described in the aforementioned technical solution.
[0019] The beneficial effects of the present invention are:
[0020] 1. The preparation method of the amorphous copolyester provided by the present invention first explores a new type of ion exchange technology by using a specific monomer sodium isophthalate-5-sulfonate dimethyl isophthalate (Na-SIPM) and CaCl 2 The reaction was carried out in water, and the Ca-SIPM salt containing divalent metal ions was successfully prepared. This key step laid the foundation for the subsequent transesterification reaction, ensuring the high efficiency of the reaction and the purity of the product. Subsequently, the Ca-SIPM salt was transesterified with ethylene glycol (EG) to obtain a new polyester precursor, namely Ca-SIPE. The synthesis of this intermediate is crucial to achieving a completely amorphous structure of polyester because it introduces special structural features (Ca ions can coordinate two sulfonate groups, making its ionic structure present up-down symmetry). Specifically, because the Ca-SIPE molecular structure is large, the introduction of Ca-SIPE into the molecular chain completely destroys the regularity of the entire polyester molecular chain, increases the amorphous region in the polyester molecular chain, and helps to inhibit the orderly arrangement of the polyester molecular chain. Finally, by copolymerizing Ca-SIPE with dibasic acids and diols, a new completely amorphous polyethylene terephthalate was successfully synthesized.
[0021] 2. The innovative synthesis route provided by the present invention not only realizes the amorphization of polyester materials, but also realizes the complete amorphization of polyester with a minimum addition amount of the third monomer (the addition amount of the third monomer is 0.25-3% of the molar amount of the first monomer). Compared with the prior art where the addition amount of the third monomer must be more than 9% or 20% to achieve the amorphization of polyester, the production cost is significantly reduced, making this high-performance polyester material more competitive in commercial applications and broadening the application field of polyester.
[0022] 3. The amorphous copolyester prepared by the present invention not only exhibits excellent physical properties, such as high transparency and good mechanical strength, but also has remarkable processing properties, such as rapid prototyping and excellent thermal stability. This achievement not only reflects our technological progress in the field of materials science, but also provides new possibilities for the sustainable development and environmentally friendly application of polyester materials.
[0023] 4. The copolyester prepared by the present invention can be completely amorphous, and the production process matches the traditional polyester production process, and there is no need to modify the existing equipment. The materials are cheap, the preparation process is simple, and it has the potential for industrial production.
[0024] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings used in the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0026] Figure 1 The synthetic route of Ca-SIPM and Ca-SIPE salts in the present invention is shown in FIG.
[0027] Figure 2 The synthetic route of PET-CaSIPE copolyester in the present invention.
[0028] Figure 3 This is a comparison chart of the DSC temperature rise curves of the PET-CaSIPE polyester prepared in Example 1 and pure polyester (PET).
[0029] Figure 4 This is a comparison chart of the TG curves of the PET-CaSIPE polyester prepared in Example 1 and pure polyester (PET).
[0030] Figure 5 This is a comparison chart of the DTG curves of the PET-CaSIPE polyester prepared in Example 1 and pure polyester (PET).
[0031] Figure 6 These are actual pictures of the PET-CaSIPE polyester tablets and pure polyester (PET) tablets prepared in Examples 1-4.
[0032] Figure 7 This is a comparison chart of the tensile stress-strain curves of the PET-CaSIPE polyester prepared in Example 1 and pure polyester (PET).
[0033] Figure 8 XRD patterns of PET-CaSIPE polyester flakes and pure polyester (PET) prepared in Examples 1-4. DETAILED DESCRIPTION
[0034] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0036] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0037] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0038] See also Figure 1 to Figure 2 As shown, the present invention provides a method for preparing an amorphous copolyester, comprising the following steps:
[0039] S1, sodium 5-sulfoisophthalate (Na-SIPM), CaCl 2 Dissolve in deionized water in a molar ratio of 2:(1.1-1.4) and mix in a glass reactor; stir the resulting mixture magnetically at room temperature for 2-3 days, then collect the precipitate by filtration and dry until a constant weight is reached to obtain Ca-SIPM salt;
[0040] By using a specific monomer sodium dimethyl 5-sulfoisophthalate (Na-SIPM) and CaCl 2 The reaction was carried out in water and Ca-SIPM salt with divalent metal ions was successfully prepared. This key step laid the foundation for the subsequent transesterification reaction and ensured the high efficiency of the reaction and the purity of the product.
[0041] S2, in a nitrogen environment, Ca-SIPM salt and ethylene glycol were subjected to transesterification reaction at a molar ratio of 1: (10.4-15.4) to obtain a transparent liquid product named Ca-SIPE; the catalyst used in the transesterification reaction was Mn(OAc) 2 ; Mn(OAc) 2 The mass fraction is 0.3% to 0.6%;
[0042] The Ca-SIPM salt was transesterified with ethylene glycol (EG) to obtain a new polyester precursor, namely Ca-SIPE. The synthesis of this intermediate is crucial to achieving a completely amorphous structure of polyester because it introduces special structural features (Ca ions can coordinate two sulfonate groups, making its ionic structure symmetrical up and down). Specifically, because the Ca-SIPE molecule has a large structure, the introduction of Ca-SIPE into the molecular chain completely destroys the regularity of the entire polyester molecular chain, increases the amorphous region in the polyester molecular chain, and helps to inhibit the orderly arrangement of the polyester molecular chain.
[0043] Specifically, in a nitrogen environment, Ca-SIPM salt, EG in a molar ratio of 1: (10.4-15.4) and Mn(OAc) with a mass fraction of 0.3%-0.6% are mixed. 2 The mixture was mixed in a 500 ml three-necked round-bottom flask and heated to 160-200° C. When reflux was observed in the reaction flask, the reaction time was started for 3.5-4.5 hours. When no methanol was distilled out, the reaction was stopped to obtain a transparent liquid product named Ca-SIPE.
[0044] S3, using terephthalic acid as the first monomer and ethylene glycol as the second monomer, the first monomer and the second monomer are put into a reaction kettle for esterification reaction; when the water output reaches the theoretical water output, the esterification reaction is completed;
[0045] During the esterification reaction, the reaction temperature is 240-260°C, the reaction time is 2-4 hours, and the pressure in the reactor is 100 kPa-360 kPa.
[0046] Specifically, after checking the sealing of the reactor, terephthalic acid is used as the first monomer and ethylene glycol is used as the second monomer. The molar ratio of the first monomer to the second monomer is 1: (1.2-1.6) and they are added into the reactor. Nitrogen is introduced into the reactor. After the pressure reaches 120 kPa, the valve is opened to release the pressure. After reaching normal pressure, the valve is closed and nitrogen is introduced into the reactor again. This operation is repeated three times to ensure that the air in the reactor is emptied. Then, nitrogen is introduced and the pressure reaches 100 kPa for esterification reaction. The reactor temperature is set to 260°C, the process tower temperature is set to 150°C, and the agitator is stirred; the frequency is set to 30 Hz. During this process, the temperature of the material in the reactor slowly rises to 260°C, and the pressure is controlled at 360 kPa. When water starts to drip out, the pressure is released. After the water output reaches the theoretical water output, it can be judged that the esterification reaction is over.
[0047] The catalyst added in the esterification reaction is Sb 2 O 3 , the amount of catalyst added is 400-600ppm.
[0048] S4, after the esterification is completed, the third monomer Ca-SIPE is added, and the reaction is carried out under normal pressure for 0.5 to 1 hour, and then a polycondensation reaction is carried out, and the obtained copolymer is pelletized to obtain an amorphous copolyester.
[0049] A new and completely amorphous polyethylene terephthalate was successfully synthesized by copolymerizing Ca-SIPE with dibasic acid and diol.
[0050] The added amount of the third monomer is 0.25-3% of the molar amount of the first monomer.
[0051] The specific process of the polycondensation reaction is as follows: first, slowly evacuate to 80-100 Pa within 1-3 hours for pre-polycondensation treatment, then heat the system to 260-280° C. and continue the reaction for 1-2 hours.
[0052] Specifically, after the esterification is completed, the third monomer Ca-SIPE is added from the feed port. After reacting for 1 to 3 hours at normal pressure, the valve between the reactor and the process tower is closed, and the heating switch of the process tower is turned off. The temperature of the reactor is adjusted to 260 to 280°C, and the valve between the reactor and the polycondensation condenser is opened to enter the polycondensation stage. During the polycondensation process, the vacuum pump is turned on, and the vacuum degree in the reactor is controlled by the vacuum fine-tuning valve to maintain a rate of 10min / 20kPa and slowly decrease until it reaches a vacuum state. Polycondensation is then carried out for 1 to 2 hours. As the reaction proceeds, the viscosity of the material will gradually increase, which will cause the power of the agitator to gradually increase. Therefore, the power of the agitator should be paid attention to during the polycondensation process. If the power is too large, the stirring frequency of the agitator needs to be set to 25Hz to continue the reaction. When the stirring power reaches a certain value, the reaction ends, and the material is released from the bottom of the reactor and pelletized.
[0053] The present invention also provides an amorphous copolyester prepared by the above-mentioned preparation method. The amorphous copolyester not only exhibits excellent physical properties, such as high transparency and good mechanical strength, but also has significant processing properties, such as rapid molding and excellent thermal stability.
[0054] Some specific embodiments are listed below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be obtained commercially.
[0055] Example 1
[0056] This embodiment provides a method for preparing an amorphous copolyester, comprising the following steps:
[0057] S1, Na-SIPM, CaCl 2 Dissolve in deionized water at a molar ratio of 2:1.1 and mix in a glass reactor; stir the resulting mixture magnetically at room temperature for 3 days, and then collect the precipitate by filtration. After a comprehensive drying process until a constant weight is reached, the Ca-SIPM salt is obtained;
[0058] S2, in a nitrogen environment, Ca-SIPM, EG in a molar ratio of 1:10.6 and Mn(OAc) with a mass fraction of 0.4% were added. 2 Mix in a 500 ml three-necked round-bottom flask and heat to 180°C. When reflux is seen in the reaction flask, start timing the reaction for 4 hours. When no methanol is distilled out, stop the reaction and obtain a transparent liquid product named Ca-SIPE.
[0059] S3, using terephthalic acid as the first monomer and ethylene glycol as the second monomer, the first monomer and the second monomer are added into a reactor in a molar ratio of 1:1.3 to carry out an esterification reaction; when the water output reaches the theoretical water output, the esterification reaction is completed;
[0060] S4, after the esterification is completed, the third monomer Ca-SIPE is added, and the amount of the third monomer added is 3% of the molar amount of the first monomer. After reacting for 0.5h under normal pressure, a polycondensation reaction is carried out for 1h, and the obtained copolymer is pelletized to obtain an amorphous copolyester.
[0061] Figure 3This is a comparison chart of the DSC heating curves of the amorphous polyester prepared in Example 1 and pure polyester (PET). It can be seen that the DSC heating curve of pure PET shows Tg (glass transition temperature), Tcc (cold crystallization temperature peak), and Tm (melting peak). Since pure PET is a semi-crystalline polyester, it shows the unique characteristics of polyester; while only one Tg (glass transition temperature) is seen in the heating curve of PET-CaSIPE, and both the cold crystallization peak and the melting peak disappear. This is attributed to the molecular structure characteristics of Ca-SIPE. Due to its large molecular structure, the introduction of Ca-SIPE into the molecular chain completely destroys the regularity of the molecular chain of the entire polyester, and increases the amorphous area in the polyester molecular chain. Therefore, the DSC heating curve shows no crystallization peak and melting peak, indicating that the amorphous copolyester has been successfully prepared.
[0062] Figure 4 TG curve comparison diagram of the amorphous polyester prepared in Example 1 and pure polyester (PET).
[0063] Figure 5 The DTG curve comparison diagram of the amorphous polyester prepared in Example 1 and pure polyester (PET) is shown in FIG.
[0064] The following table shows the thermal data of amorphous polyester tested by TGA.
[0065] Sample <![CDATA[T 5% (℃)]]> <![CDATA[T 10% (℃)]]> <![CDATA[T max (℃)]]> Residue(%) PET 395.5 403.2 436.2 10.1 Example 1 382.3 396.3 430.2 12.7
[0066] In the table, T 5% , T 10% Represent the temperatures when the weight loss is 5% and 10%, respectively.
[0067] As you can see, Figure 4 The TG curves show that the PET-CaSIPE prepared in Example 1 has similar thermal stability and decomposition tendency as PET. With the addition of Ca-SIPE, the initial decomposition temperature of PET-CaSIPE decreases slightly. Similarly, the maximum decomposition temperature (T max ) also decreased slightly, from 436.2℃ of PET to 430.2℃.
[0068] In addition, with the addition of Ca-SIPE, the weight percentage of the highest temperature residue (Residue) of the modified polyester obtained in Example 1 is 12.7%, which is 2.6% higher than the 10.1% of pure polyester, indicating that the sulfonic acid group can promote the formation of a dense carbon layer in PET. This dense carbon layer can prevent heat and oxygen transfer to a certain extent, thereby improving the flame retardant properties of the material. At the same time, the formation of this carbon layer can increase the melt viscosity and strength of the material at high temperatures, reduce the droplet phenomenon during the combustion process, and improve the mechanical strength of the polyester.
[0069] Comparative Example 1
[0070] This comparative example provides a method for preparing an amorphous copolyester. Compared with Example 1, the only difference is that in the transesterification reaction of step S2, the catalyst Mn(OAc) 2 Replaced by Zn(OAc) 2 ; Other experimental parameters and conditions are basically the same as those in Example 1 and will not be repeated here.
[0071] The following table shows the experimental data of Example 1 and Comparative Example 1:
[0072] project catalyst Measured transesterification rate / % Example 1 <![CDATA[Mn(OAc) 2 ]]> 96.8 Comparative Example 1 <![CDATA[Zn(OAc) 2 ]]> 72.6
[0073] It can be seen that the use of Zn(OAc) 2 The transesterification rate of the product obtained as the catalyst was only 72.6%, which was much lower than that in Example 1.
[0074] Examples 2-5 and Comparative Examples 2-7
[0075] Compared with Example 1, the main difference is that the Na-SIPM and CaCl in step S1 are changed 2 The molar ratio of the Ca-SIPM salt and ethylene glycol in step S2, the amount of the third monomer Ca-SIPE added in step S4, and other experimental parameters and conditions are basically the same as those in Example 1 and will not be repeated here. The details are shown in the following table.
[0076]
[0077]
[0078] Experiments show that when Na-SIPM and CaCl 2 When the molar ratio of is less than 1:0.7 (Comparative Example 7), since the molar ratios on both sides are not carried out according to the conventional reaction ratio, the reaction will have an excess of Na-SIPM and CaCl 2 The insufficient problem results in incomplete ion exchange between the two sides, which causes the failure of the next reaction.
[0079] When Na-SIPM and CaCl 2 When the molar ratio is greater than 2:1.1 (Comparative Example 6), the excess substrate may cause side reactions, especially when one of the substrates has been completely reacted, the remaining substrate may react with other reactants or products in an undesirable manner.
[0080] When the amount of the third monomer added is greater than 3% of the molar amount of the first monomer (Comparative Example 3), specifically, when the amount of the third monomer added is 4% of the molar amount of the first monomer, the polyester is also amorphous, but the addition of too much third monomer will cause the melting point and Tg of the material to drop particularly sharply.
[0081] When the amount of the third monomer added is 0.125% of the molar amount of the first monomer, if the amount of the third monomer added is too small, it will not have a significant effect on the crystallinity of the pure polyester, and the key point of amorphous polyester is crystallinity. Only when the polyester does not crystallize or has poor crystallization ability will it be amorphous. That is, if the amount of the third monomer added is too small, amorphous polyester cannot be obtained.
[0082] When the molar ratio of Ca-SIPM salt to ethylene glycol is less than 1:15.4 (Comparative Example 5), the large amount of excess EG will lead to inaccurate judgment of the reaction endpoint, and dehydration reaction will occur between ethylene glycol molecules, which will greatly reduce the purity of the product.
[0083] When the molar ratio of Ca-SIPM salt to ethylene glycol is 1:8, the substrate ratio will affect the position of the chemical equilibrium, making the reaction incomplete and affecting the yield of the product. According to Le Chatelier's principle, if the concentration of the reactant increases, the equilibrium will move in the direction of the forward reaction to reduce the concentration of the reactant; conversely, if the concentration of the product increases, the equilibrium will move in the direction of the reverse reaction.
[0084] Comparison of the transparency and mechanical strength of the modified polyester prepared in Examples 1-4 with pure polyester (PET) shows that Figure 6 , Figure 7 shown.
[0085] The transparency test method is: use a flat vulcanizer to melt and press the polyester chips, the experimental temperature is 260℃, and then cool to room temperature. Then compare and analyze the pressed samples.
[0086] The mechanical strength test method is: the universal testing machine Instron is used to test on a dumbbell-shaped sample with a size of 25 mm (neck length) × 4 mm (neck width) × 2 mm (thickness), and the tensile rate is 50 mm / min. Each sample is tested 5 times in parallel and the average value is taken.
[0087] Figure 6 The PET-CaSIPE polyester flakes prepared in Examples 1-4 and pure polyester (PET) flakes are shown in Figure 1. It can be seen that the transparency of the PET-CaSIPE polyester flakes prepared in Examples 1-4 is improved compared to pure polyester (PET).
[0088] Figure 7The tensile stress-strain curve comparison diagram of the PET-CaSIPE polyester prepared in Example 1 and pure polyester (PET) is shown in FIG. It can be seen that the tensile strength of the PET-CaSIPE polyester prepared in Example 1 is higher than that of the pure polyester (PET).
[0089] Specifically, the tensile strength of the pure polyester strip is 30.4 MPa, and the tensile strength of the modified polyester obtained in Example 1 is higher than that of pure PET, which is 36.9 MPa.
[0090] Figure 8 The XRD diagrams of the PET-CaSIPE polyester flakes and pure polyester (PET) prepared in Examples 1 to 4 show that the crystal form of pure PET is triclinic, and the modified polyester obtained by adding the third monomer Ca-SIPE still maintains the original crystal form, indicating that the addition of the third monomer will not affect the crystal shape of the polyester.
[0091] In summary, the preparation method of the amorphous copolyester of the present invention firstly uses the monomer dimethyl isophthalate-5-sodium sulfonate and CaCl 2 The reaction is carried out in water to obtain a Ca-SIPM salt containing a divalent metal ion coordination. Subsequently, the Ca-SIPM salt is subjected to an ester exchange reaction with ethylene glycol to obtain a new polyester precursor, namely Ca-SIPE. Finally, a new completely amorphous polyethylene terephthalate is successfully synthesized by copolymerizing Ca-SIPE with a dibasic acid and a diol. Because the molecular structure of Ca-SIPE is large, the introduction of Ca-SIPE into the molecular chain completely destroys the regularity of the molecular chain of the entire polyester, thereby increasing the amorphous region in the polyester molecular chain. This preparation method not only realizes the amorphization of polyester materials, but also realizes the complete amorphization of polyester with a minimum addition of a third monomer. Compared with the prior art, the addition of the third monomer must exceed 9% or 20% to achieve the amorphous nature of the polyester, which significantly reduces the production cost.
[0092] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A method for preparing an amorphous copolyester, characterized in that: The following steps are involved: S1, dissolving sodium dimethyl 5-sulfonate and CaCl2 in a molar ratio of 2:(1.1-1.4) in deionized water in a reactor and mixing; stirring the obtained mixture magnetically at room temperature for 2-3 days, then collecting the precipitate by filtration, and drying until a constant weight is reached to obtain Ca-SIPM salt; S2, in a nitrogen environment, Ca-SIPM salt and ethylene glycol are subjected to an ester exchange reaction at a molar ratio of 1:(10.4-15.4) to obtain a transparent liquid product, named Ca-SIPE; the catalyst used in the ester exchange reaction is Mn(OAc)2; the mass fraction of the Mn(OAc)2 is 0.3%-0.6%; S3, using terephthalic acid as the first monomer and ethylene glycol as the second monomer, the first monomer and the second monomer are put into a reaction kettle for esterification reaction; when the water output reaches the theoretical water output, the esterification reaction is completed; S4, after the esterification is completed, the third monomer Ca-SIPE obtained in step S2 is added, and the mixture is reacted at normal pressure for 0.5 to 1 hour, and then a polycondensation reaction is carried out. The obtained copolymer is pelletized to obtain an amorphous copolyester.
2. The method for preparing the amorphous copolyester according to claim 1, characterized in that: In step S4, the amount of the third monomer added is 0.25-3% of the molar amount of the first monomer.
3. The method for preparing the amorphous copolyester according to claim 1, characterized in that: In step S3, the molar ratio of the first monomer to the second monomer is 1:(1.2-1.6).
4. The method for preparing the amorphous copolyester according to claim 1, characterized in that: In step S2, the reaction temperature of the transesterification reaction is 160-200°C, and the reaction time is 3.5-4.5 hours.
5. The method for preparing the amorphous copolyester according to claim 1, characterized in that: In step S2, the end point of the transesterification reaction is when no methanol is distilled out.
6. The method for preparing the amorphous copolyester according to claim 1, characterized in that: In step S4, the specific process of the polycondensation reaction is: first, slowly evacuate to 80-100 Pa within 1-3 hours for pre-polycondensation treatment, then heat the system to 260-280° C., and continue the reaction for 1-2 hours.
7. The method for preparing the amorphous copolyester according to claim 1, characterized in that: In step S3, during the esterification reaction, the reaction temperature is 240-260° C., the reaction time is 2-4 hours, and the pressure in the reactor is 100 kPa-360 kPa.
8. The method for preparing the amorphous copolyester according to claim 1, characterized in that: In step S3, the catalyst added to the esterification reaction is Sb2O3, and the amount of the catalyst added is 400-600 ppm.
9. An amorphous copolyester, characterized in that: The amorphous copolyester is prepared by the preparation method of any one of claims 1 to 8.
Citation Information
Patent Citations
Moisture-absorption copolyester and preparation method thereof
CN102838739A
Biodegradable aromatic-aliphatic copolyester and preparation method thereof
CN103087305A
Amorphous copolyester and preparation method thereof
CN106866948A
Polyester FDY hot melting fiber and preparation method thereof
CN110923843A
Process for the preparation of modified polybutylene terephthalate resin