Resin composition
By using monomers such as DABA, CpODA, and silicon-containing compounds, the imidization rate and silicon-containing compound ratio of the resin composition were optimized, solving the problems of insufficient varnish filtering and properties of polyimide films in display applications, and achieving higher tensile elongation and transparency.
Patent Information
- Application Number
- CN202411117752.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-05-28
- Filing Date
- 2021-05-28
- Publication Date
- 2024-12-06
AI Technical Summary
Existing polyimide films have problems with insufficient varnish filtration and poor properties in display applications, especially in terms of tensile elongation and transparency.
A resin composition containing specific structural units is used, with DABA, CpODA and silicon-containing compounds as monomers, to form a polyimide resin through a polycondensation reaction. The imidization rate and the proportion of silicon-containing compounds are controlled to optimize the performance of the polyimide film.
It improves the tensile elongation and transparency of polyimide films in display applications, enhances mechanical properties and heat resistance, and improves the viscosity stability and filterability of varnishes.
Smart Images

Figure CN119081111A_ABST
Abstract
Description
[0001] This application is a divisional application of the Chinese patent application with an application date of May 28, 2021, application number 202180038523.3, and invention name “Resin Composition”. Technical Field
[0002] The present invention relates to a resin composition containing a polyimide precursor / polyimide and a polyimide film, and also relates to a method for producing the resin composition containing a polyimide precursor / polyimide, and a method for producing a polyimide film, a display, a laminate and a flexible device. Background Art
[0003] Polyimide resin is an insoluble, infusible, super heat-resistant resin having excellent properties such as heat oxidation resistance, heat resistance, radiation resistance, low temperature resistance, and chemical resistance. Therefore, polyimide resin is used in a wide range of fields including electronic materials. Examples of the application of polyimide resin in the field of electronic materials include insulating coating materials, insulating films, semiconductors, and electrode protective films of thin film transistor liquid crystal displays (TFT-LCDs). Recently, the lightness and flexibility of polyimide films have been used to replace glass substrates used in the field of display materials and used as flexible substrates.
[0004] Patent document 1 describes a polyimide film, which is obtained as follows: polyimide is synthesized using 3,5-diaminobenzamide (hereinafter also referred to as DABA), a compound of the following structural formula (hereinafter also referred to as CpODA) and other compounds as monomers, a crosslinking agent is added to the obtained polyimide varnish, and the film is coated and dried.
[0005]
[0006] Patent Document 1 also describes that the film has excellent gas separation performance. Patent Document 2 describes a transparent polyimide film obtained by coating and drying a polyimide varnish using DABA, TFMB (2,2'-bis(trifluoromethyl)benzidine) or the like as a diamine and CpODA as an acid dianhydride.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent No. 6551640
[0010] Patent Document 2: International Publication No. 2019 / 211972 Summary of the invention
[0011] Problem that the invention aims to solve
[0012] The polyimide film described in Patent Document 1 is used as a gas separation membrane, and has not been studied as an optical material.
[0013] In addition, the present inventors have found that when DABA, TFMB, CpODA, silicon-containing compounds, etc. are used as monomers and a polyimide varnish is synthesized in the same manner as described in the above-mentioned Patent Document 2, the varnish filterability required in the varnish production process is insufficient, and the polyimide film obtained by coating and heating the polyimide varnish is insufficient in the properties required for display applications (tensile elongation, etc.). On the other hand, the present inventors have found that a polyimide obtained by using DABA, 3,3'-diaminodiphenyl sulfone (33DAS), 4,4'-diaminodiphenyl sulfone (44DAS), diamines such as 9,9-bis(4-aminophenyl)fluorene (BAFL), CpODA, 4,4'-oxydiphthalic anhydride (ODPA), acid dianhydrides such as 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF), and other silicon-containing compounds as monomers is excellent in the properties required for display applications.
[0014] Therefore, the present invention has been made in view of the above circumstances, and its object is to provide a polyimide film having excellent properties both in the production process of a resin composition containing a polyimide precursor and / or polyimide and in other properties sought for display applications, and a resin composition for forming the same.
[0015] Solutions for solving problems
[0016] The above problems can be solved by the following technical means.
[0017] [First method]
[0018] <1> A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7),
[0019]
[0020] {In the formula, P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer.}
[0021]
[0022] {In the formula, P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer.}
[0023] The aforementioned P5 or P6 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10),
[0024]
[0025] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group, anhydride group, isocyanate group, carboxyl group, acid ester group, acyl halide group, hydroxyl group, epoxy group or mercapto group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0026] Furthermore, the resin composition contains 25% by mass or less of the silicon-containing compound based on the total mass of the resin.
[0027] <2> A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7),
[0028]
[0029] {In the formula, P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer.}
[0030]
[0031] {In the formula, P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer.}
[0032] The aforementioned P5 or P6 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10),
[0033]
[0034] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group, anhydride group, isocyanate group, carboxyl group, acid ester group, acyl halide group, hydroxyl group, epoxy group or mercapto group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0035] Furthermore, the imidization rate of the resin is 50% or more.
[0036] <3> The resin composition according to item 1, wherein the imidization ratio of the resin is 50% or more.
[0037] <4> A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7),
[0038]
[0039] {In the formula, P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer.}
[0040]
[0041] {In the formula, P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer.}
[0042] The aforementioned P5 or P6 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10),
[0043]
[0044] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group, anhydride group, isocyanate group, carboxyl group, acid ester group, acyl halide group, hydroxyl group, epoxy group or mercapto group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0045] Furthermore, the resin composition satisfies any of the following (i) or (ii),
[0046] (i) the aforementioned P3 and / or P5 contain a structural unit derived from a compound represented by the following general formula (8),
[0047] or
[0048] (ii) the aforementioned P4 and / or P6 contain a structural unit derived from a compound represented by the following general formula (9),
[0049]
[0050] <5> A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7),
[0051]
[0052] {In the formula, P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer.}
[0053]
[0054] {In the formula, P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer.}
[0055] The aforementioned P5 or P6 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10),
[0056]
[0057] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group, anhydride group, isocyanate group, carboxyl group, acid ester group, acyl halide group, hydroxyl group, epoxy group or mercapto group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0058] Furthermore, the aforementioned P3 and / or P5 each independently comprises at least one structural unit derived from 3,3'-diaminodiphenyl sulfone (33DAS), 4,4'-diaminodiphenyl sulfone (44DAS) or 9,9-bis(4-aminophenyl)fluorene (BAFL).
[0059] <6> A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7),
[0060]
[0061] {In the formula, P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer.}
[0062]
[0063] {In the formula, P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer.}
[0064] The aforementioned P5 or P6 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10),
[0065]
[0066] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group, anhydride group, isocyanate group, carboxyl group, acid ester group, acyl halide group, hydroxyl group, epoxy group or mercapto group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0067] Furthermore, the aforementioned P3 and / or P5 each independently comprises at least one structural unit derived from 2,2′-bis(trifluoromethyl)-4,4′-diaminodiphenyl ether (6FODA).
[0068] <7> A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7),
[0069]
[0070] {In the formula, P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer.}
[0071]
[0072] {In the formula, P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer.}
[0073] The aforementioned P5 or P6 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10),
[0074]
[0075] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0076] Furthermore, when A (mass %) is the ratio of the diamine of the general formula (10) among the diamines constituting P5 in the general formula (7), and B (mass %) is the ratio of the diamine of the general formula (10) among the diamines constituting P3 in the general formula (6), BA is greater than 0 and less than 60.
[0077] <8> The resin composition according to item 7, wherein the diamine is at least one compound selected from the group consisting of a compound represented by the following general formula (8), 3,3'-diaminodiphenyl sulfone (33DAS), 4,4'-diaminodiphenyl sulfone (44DAS) and 9,9-bis(4-aminophenyl)fluorene (BAFL).
[0078]
[0079] <9> The resin composition according to any one of items 1 to 8, wherein in the general formula (6) and / or the general formula (7), P4 and / or P6 each independently contain at least one structural unit derived from various compounds of 4,4'-oxydiphthalic anhydride (ODPA) or 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF).
[0080] <10> The resin composition according to any one of items 1 to 9, wherein the functional group equivalent of the silicon-containing compound represented by the general formula (10) is 800 or more.
[0081] <11> The resin composition according to any one of items 1 to 10,
[0082] The aforementioned P5 comprises a structural unit derived from the compound represented by the aforementioned general formula (10), and
[0083] In the aforementioned general formula (10), the aforementioned L1 and L2 are each independently an amino group.
[0084] <12> The resin composition according to any one of items 4 and 9 to 11, wherein the compound represented by the general formula (8) is more than 50 mol % when all diamines (excluding the compound represented by the general formula (10)) are taken as 100 mol %.
[0085] <13> The resin composition according to any one of items 1 to 12, wherein P3 or P5 each independently contains a structural unit derived from a compound represented by the following formula (BisAM).
[0086]
[0087] <14> The resin composition according to any one of items 1 to 13, wherein the P4 or P6 each independently comprises a compound (BzDA) derived from 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride, represented by the following formula:
[0088]
[0089] Or the compound represented by the following formula (BNBDA)
[0090]
[0091] structural unit.
[0092] <15> The resin composition according to any one of items 1 to 14, wherein a polyimide resin film obtained by heating the resin is used for a flexible substrate.
[0093] <16> The resin composition according to any one of items 1 to 15, wherein a polyimide resin film obtained by curing the resin is used for a flexible display.
[0094] <17> A method for producing a resin composition, comprising:
[0095] After polyimide is obtained by polycondensation reaction of diamine or acid dianhydride with a silicon-containing compound represented by the following general formula (10),
[0096] Allowing it to undergo a polycondensation reaction with other compounds to provide a resin composition comprising a resin comprising a polyimide precursor and a polyimide,
[0097]
[0098] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group, anhydride group, isocyanate group, carboxyl group, acid ester group, acyl halide group, hydroxyl group, epoxy group or mercapto group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0099] The resin composition contains 25% by mass or less of the silicon-containing compound based on the total mass of the resin.
[0100] <18> A method for producing a resin composition, comprising:
[0101] After polyimide is obtained by polycondensation reaction of diamine or acid dianhydride with a silicon-containing compound represented by the following general formula (10),
[0102] Allowing it to undergo a polycondensation reaction with other compounds to provide a resin composition comprising a resin comprising a polyimide precursor and a polyimide,
[0103]
[0104] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group, anhydride group, isocyanate group, carboxyl group, acid ester group, acyl halide group, hydroxyl group, epoxy group or mercapto group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0105] The imidization rate of the resin is 50% or more.
[0106] <19> A method for producing a resin composition, comprising:
[0107] After polyimide is obtained by polycondensing the compound represented by the following general formula (8) or the compound represented by the following general formula (9) with the silicon-containing compound represented by the following general formula (10) and other compounds,
[0108] The polyimide precursor is subjected to polycondensation reaction with other compounds to provide a resin composition containing a polyimide precursor and a polyimide.
[0109]
[0110] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group, anhydride group, isocyanate group, carboxyl group, acid ester group, acyl halide group, hydroxyl group, epoxy group or mercapto group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0111] <20> A method for producing a resin composition, comprising:
[0112] At least one compound selected from 3,3'-diaminodiphenyl sulfone (33DAS), 4,4'-diaminodiphenyl sulfone (44DAS) and 9,9-bis(4-aminophenyl)fluorene (BAFL) is subjected to a polycondensation reaction with a silicon-containing compound represented by the following general formula (10) and other compounds to obtain a polyimide,
[0113] The polyimide precursor is subjected to polycondensation reaction with other compounds to provide a resin composition containing a polyimide precursor and a polyimide.
[0114]
[0115] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group, anhydride group, isocyanate group, carboxyl group, acid ester group, acyl halide group, hydroxyl group, epoxy group or mercapto group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0116] <21> A method for producing a resin composition, comprising:
[0117] At least one compound selected from 4,4'-oxydiphthalic anhydride (ODPA) and 9,9-bis(3,4-dicarboxyphenyl)fluorene anhydride (BPAF) is subjected to polycondensation reaction with a silicon-containing compound represented by the following general formula (10) and other compounds to obtain a polyimide,
[0118] The polyimide precursor is subjected to polycondensation reaction with other compounds to provide a resin composition containing a polyimide precursor and a polyimide.
[0119]
[0120] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group, anhydride group, isocyanate group, carboxyl group, acid ester group, acyl halide group, hydroxyl group, epoxy group or mercapto group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0121] <22> A method for producing a polyimide resin film, comprising:
[0122] A step of coating the resin composition according to any one of items 1 to 16 or the resin composition obtained by the method according to any one of items 17 to 21 on the surface of a support;
[0123] A film-forming step of heating the resin composition to form a polyimide resin film; and
[0124] A peeling step of peeling the polyimide resin film from the support.
[0125] <23> The method for producing a polyimide resin film according to item 22, comprising:
[0126] Prior to the peeling step, an irradiation step of irradiating the resin composition with laser light from the support side is performed.
[0127] <24> A method for manufacturing a display, comprising:
[0128] A step of coating the resin composition according to any one of items 1 to 16 or the resin composition obtained by the method according to any one of items 17 to 21 on the surface of a support;
[0129] A film-forming step of heating the resin composition to form a polyimide resin film;
[0130] an element forming step of forming an element on the polyimide resin film; and
[0131] A peeling step of peeling the polyimide resin film on which the element is formed from the support.
[0132] <25> A method for manufacturing a laminate, comprising:
[0133] A step of coating the resin composition according to any one of items 1 to 16 or the resin composition obtained by the method according to any one of items 17 to 21 on the surface of a support;
[0134] A film-forming step of heating the resin composition to form a polyimide resin film; and
[0135] The step of forming an element on the polyimide resin film is followed by a step of forming an element.
[0136] <26> The method for manufacturing a laminate according to item 25, further comprising:
[0137] a step of peeling the polyimide resin film on which the element is formed from the support.
[0138] <27> A method for manufacturing a flexible device, comprising:
[0139] The laminate is manufactured by the method described in item 25 or 26.
[0140] [Second Method]
[0141] <28> A resin composition comprising a resin having a structural unit represented by the following general formula (1) or (2):
[0142]
[0143] {In the formula, P1 represents a divalent organic group; P2 represents a tetravalent organic group; and p represents a positive integer.}
[0144]
[0145] {In the formula, P1 represents a divalent organic group; P2 represents a tetravalent organic group, and p represents a positive integer.}
[0146] The aforementioned P1 comprises a structural unit derived from a compound represented by the following general formula (3),
[0147]
[0148] Furthermore, the aforementioned P1 or P2 includes a structural unit derived from a silicon-containing compound represented by the following general formula (5):
[0149]
[0150] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50; and the functional group equivalent is 800 or more.}
[0151] <29> The resin composition according to item 28, wherein P2 contains a structural unit derived from a compound represented by the following general formula (4).
[0152]
[0153] <30> A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7),
[0154]
[0155] {In the formula, P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer; P3 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA).}
[0156]
[0157] {In the formula, P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer; P5 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA).}
[0158] The aforementioned P3 or P4 includes a structural unit derived from a silicon-containing compound represented by the following general formula (10).
[0159]
[0160] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0161] <31> A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7),
[0162]
[0163] {In the formula, P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer; P3 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA).}
[0164]
[0165] {In the formula, P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer; P5 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA).}
[0166] The aforementioned P3 or P4 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10),
[0167]
[0168] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0169] Furthermore, the resin composition satisfies any of the following (i) or (ii),
[0170] (i) the aforementioned P3 and / or P5 contain a structural unit derived from a compound represented by the following general formula (8),
[0171] or
[0172] (ii) The aforementioned P4 and / or P6 contain a structural unit derived from a compound represented by the following general formula (9).
[0173]
[0174] <32> A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7),
[0175]
[0176] {In the formula, P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer; P3 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA).}
[0177]
[0178] {In the formula, P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer; P5 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA).}
[0179] The aforementioned P3 or P4 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10),
[0180]
[0181] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0182] Furthermore, the aforementioned P3 and / or P5 include at least one structural unit derived from various compounds selected from 3,3′-diaminodiphenyl sulfone (33DAS) or 4,4′-diaminodiphenyl sulfone (44DAS).
[0183] <33> A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7),
[0184]
[0185] {In the formula, P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer; P3 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA).}
[0186]
[0187] {In the formula, P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer; P5 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA).}
[0188] The aforementioned P3 or P4 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10),
[0189]
[0190] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0191] Furthermore, the aforementioned P3 and / or P5 include at least one structural unit derived from 9,9-bis(4-aminophenyl)fluorene (BAFL) or a compound of the following general formula (BisAM).
[0192]
[0193] <34> A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7),
[0194]
[0195] {In the formula, P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer; P3 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA).}
[0196]
[0197] {In the formula, P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer; P5 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA).}
[0198] The aforementioned P3 or P4 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10),
[0199]
[0200] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0201] Furthermore, the aforementioned P4 and / or P6 comprises at least one
[0202] 4,4'-oxydiphthalic anhydride (ODPA),
[0203] 4,4'-(Hexafluoroisopropylidene)diphthalic anhydride (6FDA),
[0204] 9,9-bis(3,4-dicarboxyphenyl)fluorene anhydride (BPAF),
[0205] The compound of the following general formula (BzDA),
[0206]
[0207] Or the compound of the following general formula (BNBDA)
[0208]
[0209] The structural units of various compounds.
[0210] <35> The resin composition according to any one of Items 30 to 34,
[0211] The aforementioned P3 comprises a structural unit derived from the compound represented by the aforementioned general formula (10),
[0212] The functional group equivalent of the silicon-containing compound represented by the general formula (10) is 800 or more.
[0213] <36> The resin composition according to any one of Items 30 to 35,
[0214] The aforementioned P3 comprises a structural unit derived from the compound represented by the aforementioned general formula (10), and
[0215] In the aforementioned general formula (10), the aforementioned L1 and L2 are each independently an amino group.
[0216] <37> The resin composition according to any one of items 28, 29 and 31, wherein the compound represented by the general formula (3) or (8) is more than 50 mol % when all diamines (excluding the compound represented by the general formula (5) or (10)) are taken as 100 mol %.
[0217] <38> The resin composition according to any one of Items 28 to 37, wherein a polyimide resin film obtained by heating the resin is used for a flexible substrate.
[0218] <39> The resin composition according to any one of Items 28 to 38, wherein a polyimide resin film obtained by curing the resin is used for a flexible display.
[0219] <40> A method for producing a resin composition, comprising:
[0220] A polyimide precursor and / or polyimide is provided by polycondensing a compound represented by the following general formula (3), at least one diamine selected from 3,3'-diaminodiphenyl sulfone (33DAS) and 4,4'-diaminodiphenyl sulfone (44DAS) and an acid dianhydride with a silicon-containing compound represented by the following general formula (5) and other compounds.
[0221]
[0222] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0223] <41> A method for producing a resin composition, comprising:
[0224] After polycondensing a diamine (excluding 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA)) with an acid dianhydride to obtain a polyimide,
[0225] A resin composition containing a polyimide precursor and a polyimide is provided by subjecting a silicon-containing compound represented by the following general formula (5) to a polycondensation reaction with other compounds.
[0226]
[0227] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0228] <42> A method for producing a resin composition, comprising:
[0229] A compound represented by the following general formula (3), at least one diamine selected from 3,3'-diaminodiphenyl sulfone (33AS) and 4,4'-diaminodiphenyl sulfone (44DAS), an acid dianhydride and other compounds are subjected to polycondensation reaction to obtain a polyimide,
[0230] A resin composition containing a polyimide precursor and a polyimide is provided by subjecting a silicon-containing compound represented by the following general formula (5) to a polycondensation reaction with other compounds.
[0231]
[0232] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0233] <43> A method for producing a polyimide resin film, comprising:
[0234] A step of coating the resin composition described in any one of items 28 to 39 or the resin composition obtained by the method described in any one of items 40 to 42 on the surface of a support;
[0235] A film-forming step of heating the resin composition to form a polyimide resin film; and
[0236] A peeling step of peeling the polyimide resin film from the support.
[0237] <44> The method for producing a polyimide resin film according to item 43, comprising:
[0238] Prior to the peeling step, an irradiation step of irradiating the resin composition with laser light from the support side is performed.
[0239] <45> A method for manufacturing a display, comprising:
[0240] A step of coating the resin composition according to any one of items 28 to 39 or the resin composition obtained by the method according to any one of items 40 to 42 on the surface of a support;
[0241] A film-forming step of heating the resin composition to form a polyimide resin film;
[0242] an element forming step of forming an element on the polyimide resin film; and
[0243] A peeling step of peeling the polyimide resin film on which the element is formed from the support.
[0244] <46> A method for manufacturing a laminate, comprising:
[0245] A step of coating the resin composition described in any one of items 28 to 39 or the resin composition obtained by the method described in any one of items 40 to 42 on the surface of a support;
[0246] A film-forming step of heating the resin composition to form a polyimide resin film; and
[0247] The step of forming an element on the polyimide resin film is followed by a step of forming an element.
[0248] <47> The method for manufacturing a laminate according to item 46, further comprising:
[0249] a step of peeling the polyimide resin film on which the element is formed from the support.
[0250] <48> A method for manufacturing a flexible device, comprising:
[0251] The laminate is manufactured by the method described in item 46 or 47.
[0252] Effects of the Invention
[0253] According to the present invention, DABA, CpODA and other silicon-containing compounds are first used as monomers, and a polyimide precursor or a polyimide resin composition having excellent characteristics required for display applications can be provided.
[0254] According to the present invention, DABA, silicon-containing compounds and other compounds are used as monomers, or DABA, silicon-containing compounds and other compounds are used as monomers, and 3,3'-diaminodiphenyl sulfone (33DAS) and / or 4,4'-diaminodiphenyl sulfone (44DAS) and silicon-containing compounds and other compounds are used as monomers, so that a polyimide precursor or polyimide resin composition with excellent properties sought for display applications can be provided.
[0255] It should be noted that the above description cannot be regarded as disclosing all the embodiments of the present invention and all the advantages of the present invention. Further embodiments of the present invention and their advantages can be clarified by referring to the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0256] Figure 1 This is a schematic diagram showing the structure of a top emission type flexible organic EL display as an example of the display according to the present embodiment, above the polyimide substrate. DETAILED DESCRIPTION
[0257] Hereinafter, an exemplary embodiment of the present invention (hereinafter referred to as "this embodiment") is described in detail. The present invention is not limited to this embodiment, and various modifications can be made within the scope of the present invention. In the present application specification, the upper limit and the lower limit of each numerical range can be arbitrarily combined.
[0258] [First method]
[0259] 《Resin composition》
[0260] 〈Resin / polyimide precursor / polyimide〉
[0261] The resin composition of the present embodiment includes a resin having a structural unit represented by the following general formula (6) and (7), and may also include a partially imidized polyimide precursor.
[0262]
[0263] {In the formula, P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer.}
[0264]
[0265] {In the formula, P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer.}
[0266] P5 or P6 contains a structural unit derived from a silicon-containing compound represented by the following general formula (10).
[0267]
[0268] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group, anhydride group, isocyanate group, carboxyl group, acid ester group, acyl halide group, hydroxyl group, epoxy group or mercapto group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0269] In the case of such a partially imidized polyimide precursor, the viscosity stability of the composition is excellent compared with a complete polyimide precursor, and it is excellent from the viewpoint of ease of synthesis of a polyimide (polyimide precursor) compared with a complete polyimide.
[0270] Based on the total mass of the resin, the proportion of the silicon-containing compound is 25% by mass or less. From the viewpoint of the viscosity storage stability and filterability of the varnish, the proportion of the silicon-containing compound in the total resin is preferably 20% by mass or less, more preferably 10% by mass or less, and particularly preferably 5% by mass or less. As such, the mechanism by which the viscosity storage stability and filterability of the varnish are better as the proportion of the silicon-containing compound in the resin is smaller is still uncertain, and it can be considered that it is related to the aggregation of the dissociated silicon-containing compound.
[0271] On the other hand, from the viewpoint of residual stress of the obtained polyimide film, the ratio of the silicon-containing compound is preferably 5 mass % or more, more preferably 10 mass % or more, and particularly preferably 15 mass % or more.
[0272] The appropriate ratio of the silicon-containing compound in the entire resin varies depending on the type and ratio of the diamine monomer / acid dianhydride monomer used, and needs to be determined by comprehensively considering the residual stress of the polyimide film, the viscosity storage stability of the varnish, filterability, etc.
[0273] The imidization rate of the resin is 50% or more. From the viewpoint of the viscosity storage stability of the varnish, the imidization rate of the resin is preferably 60% or more, more preferably 70% or more, further preferably 80% or more, and particularly preferably 90% or more. As described above, the mechanism by which the viscosity storage stability of the varnish is improved as the imidization rate increases is not clear, but it is believed that it is related to the depolymerization of the amide part during storage of the varnish.
[0274] On the other hand, from the viewpoint of hygroscopic turbidity of the varnish, the imidization rate of the resin is preferably 90% or less, more preferably 80% or less, and further preferably 70% or less. As such, the mechanism by which the varnish is less likely to become hygroscopically turbid as the imidization rate decreases is not clear, but it is believed to be related to the solvent solubility of the polyimide / polyamide.
[0275] The appropriate imidization ratio of the resin also varies depending on the type and ratio of the diamine monomer / acid dianhydride monomer used, and needs to be determined by comprehensively considering the viscosity storage stability of the varnish, the hygroscopic turbidity of the varnish, and the like.
[0276] The difference between the imide unit and the amide unit in the ratio of the silicon-containing compound in the diamine monomer of the resin is greater than 0 and is not more than 60. The difference between the imide unit and the amide unit in the ratio of the silicon-containing compound in the diamine monomer of the resin is obtained by the following formula.
[0277] A: Ratio of silicon-containing compound in diamine of imide unit (mass %) = silicon-containing compound used in imidization step / total mass of diamine monomer (including silicon-containing compound) used in imidization step × 100
[0278] B: Ratio of silicon-containing compound in diamine of amide unit (mass %) = total mass of silicon-containing compound used in imidization step / mass of diamine monomer (including silicon-containing compound) used in amidation step × 100
[0279] Here, A may also be referred to as "the ratio (mass %) of the diamines of the general formula (10) among the diamines constituting P5 in the general formula (7)". In addition, B may also be referred to as "the ratio (mass %) of the diamines of the general formula (10) among the diamines constituting P3 in the general formula (6)".
[0280] The difference between the imide unit and the amide unit in the ratio of the silicon-containing compound in the diamine is BA using the above-mentioned A and B.
[0281] The difference between the ratio of silicon-containing compounds in the diamine monomer and the imide unit and the amide unit indicates: in a polyimide precursor (polyamide-imide) resin having a structure derived from a silicon-containing compound and partially imidized, the ratio of the silicon-containing compound of the imide unit and the amide unit, the greater the value, the more it can be said that the imide unit has a structure derived from a silicon-containing compound. The greater the value, the better the residual stress of the polyimide film becomes. If the value is small, the foaming / filterability of the varnish / the haze (turbidity) of the polyimide film becomes good. And, when the value is in the above range, it is possible to take into account various characteristics such as the foaming / filterability of the varnish / the residual stress / haze (turbidity) of the polyimide film, so it is preferred.
[0282] In addition, when the diamine used in the above-mentioned resin is at least one compound selected from the group consisting of the compound represented by the following general formula (8), 3,3'-diaminodiphenyl sulfone (33DAS), 4,4'-diaminodiphenyl sulfone (44DAS) and 9,9-bis(4-aminophenyl)fluorene (BAFL), the characteristics of the varnish / polyimide are further improved, which is preferred.
[0283]
[0284] In addition, the resin composition according to another embodiment of the present invention may include a polyimide precursor which includes structural units represented by the following general formulae (6) and (7) and is partially imidized.
[0285]
[0286] {In the formula, P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer.}
[0287]
[0288] {In the formula, P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer.}
[0289] P5 or P6 may include a structural unit derived from a silicon-containing compound represented by the following general formula (10),
[0290]
[0291] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group, anhydride group, isocyanate group, carboxyl group, acid ester group, acyl halide group, hydroxyl group, epoxy group or mercapto group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50.}
[0292] Furthermore, the resin composition may satisfy any of the following (i) or (ii),
[0293] (i) the aforementioned P3 and / or P5 contain a structural unit derived from a compound represented by the following general formula (8),
[0294] or
[0295] (ii) The aforementioned P4 and / or P6 contain a structural unit derived from a compound represented by the following general formula (9).
[0296]
[0297] Diamine
[0298] The resin composition contains at least one structural unit selected from various diamine compounds including a compound of the following general formula (8), 3,3'-diaminodiphenyl sulfone (33DAS), 4,4'-diaminodiphenyl sulfone (44DAS), 9,9-bis(4-aminophenyl)fluorene (BAFL) or 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA).
[0299]
[0300] Among the diamine compounds represented by general formula (8), 3,5-diaminobenzoic acid (DABA) is preferred from the viewpoint of transparency and YI of the polyimide film. By using at least one selected from DABA, 33DAS, 44DAS, BAFL and 6FODA as the diamine compound, the mechanical properties of the polyimide film are improved (especially tensile elongation), and the heat resistance can be improved, so it is preferred.
[0301] The content of DABA in all diamines (including compounds in which L1 and L2 in the general formula (10) are amino groups) may be more than 50 mol%, more than 55 mol%, or more than 70 mol%, or more than 90 mol%, or more than 95 mol%. The greater the amount of DABA, the greater the tensile elongation of the polyimide film, which is preferred.
[0302] Examples of diamines other than the general formula (8) include p-phenylenediamine (PDA), m-phenylenediamine, 2,2'-dimethylbenzidine (mTB), 4,4'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 4,4'-diaminobiphenyl, 3,4'-diaminobiphenyl, 3,3'-diaminobiphenyl, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, bis(4-(4-aminophenoxy)benzene), and bis(4-(4-aminophenoxy)benzene). 4,4-bis(4-aminophenoxy)biphenyl, 4,4-bis(3-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 9,10-bis(4-aminophenyl)anthracene, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl)propane, 2,2-bis[4-(4-aminophenoxy)phenyl)hexafluoropropane and 1,4-bis(3-aminopropyldimethylsilyl)benzene, 1,3-bis[1-(4-aminophenyl)-1-methylethyl]benzene](BiSAM), etc.
[0303] The diamine other than the general formula (8) is preferably at least one selected from the group consisting of 1,3-bis[1-(4-aminophenyl)-1-methylethyl]benzene] (BisAM) and 1,4-cyclohexanediamine (CHDA).
[0304] Acid dianhydride
[0305] The resin composition contains at least one structural unit selected from various acid dianhydride compounds such as a compound represented by the following general formula (9) (also referred to as CpODA), 4,4'-oxydiphthalic anhydride (ODPA) or 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF).
[0306]
[0307] The presence of these structural units is preferred because the transparency, YI, and heat-resistant mechanical properties of the polyimide film obtained can be improved.
[0308] The content of CpODA, ODPA and BPAF in all acid dianhydrides (including compounds in which L1 and L2 in the general formula (10) are anhydride groups) can be 50 mol% or more, 60 mol% or more, or 70 mol% or more, or 90 mol% or more, or 95 mol% or more. The greater the amount of CpODA, ODPA and BPAF, the higher the transparency of the polyimide film, so it is preferred.
[0309] Examples of the acid dianhydride other than the general formula (9) include pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,2',3,3'-biphenyltetracarboxylic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA), 5-(2,5-dioxotetrahydro-3-furyl)-3-methyl-cyclohexene-1,2-dicarboxylic anhydride, 1,2,3,4-benzenetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, and methylenediaminetetracarboxylic acid dianhydride. 1,1-ethylene-4,4'-diphthalic anhydride, 2,2-propylene-4,4'-diphthalic anhydride, 1,2-ethylene-4,4'-diphthalic anhydride, 1,3-trimethylene-4,4'-diphthalic anhydride, 1,4-tetramethylene-4,4'-diphthalic anhydride, 1,5-pentamethylene-4,4'-diphthalic anhydride, 4,4'-oxydiphthalic anhydride, p-phenylene ditrimellityl anhydride, thio-4,4'-diphthalic anhydride, sulfonyl-4,4'-diphthalic anhydride, 1,3 -Bis(3,4-dicarboxyphenyl)phthalic anhydride, 1,3-bis(3,4-dicarboxyphenoxy)phthalic anhydride, 1,4-bis(3,4-dicarboxyphenoxy)phthalic anhydride, 1,3-bis[2-(3,4-dicarboxyphenyl)-2-propyl]phthalic anhydride, 1,4-bis[2-(3,4-dicarboxyphenyl)-2-propyl]phthalic anhydride, bis[3-(3,4-dicarboxyphenoxy)phenyl]methane dianhydride, bis[4-(3,4-dicarboxyphenoxy)phenyl]methane dianhydride, 2,2-bis[3-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl] ] propane dianhydride, bis(3,4-dicarboxyphenoxy)dimethylsilane dianhydride, 1,3-bis(3,4-dicarboxyphenyl)-1,1,3,3-tetramethyldisiloxane dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride and 1,2,7,8-phenanthrenetetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride (HPMDA) and 1,2,3,4-cyclobutanetetracarboxylic dianhydride (CBDA), a compound of the following structure (BzDA);
[0310]
[0311] The compound with the following structure (BNBDA), etc.
[0312]
[0313] The acid dianhydride other than the above general formula (9) is preferably at least one selected from the group consisting of BzDA, BNBDA, and 1,2,4,5-cyclohexanetetracarboxylic dianhydride (HPMDA). The acid dianhydride may be used alone or in combination of two or more.
[0314] 〈Silicon-containing compounds〉
[0315] The polyimide precursor in the present embodiment can have the structure shown in the above formula (6) and the structure shown in the above formula (7) together. Taking the mass of the polyimide precursor as a benchmark, the content ratio of the structure derived from the silicon-containing compound in the polyimide precursor is preferably more than 5% by mass and less than 40% by mass. If the polyimide precursor includes a structure derived from a silicon-containing compound within the numerical range, it is possible to take into account low residual stress and high transparency and heat resistance in the resulting polyimide film, so it is preferred. Taking the mass of the polyimide precursor as a benchmark, the content ratio of the structure derived from the silicon-containing compound can be more than 6% by mass or more than 7% by mass, and in addition, it can be less than 30% by mass or less than 25% by mass.
[0316] The polyimide / polyimide precursor in the present embodiment has a structure derived from a silicon-containing compound. Therefore, the silicon-containing compound used in the synthesis of the polyimide precursor in the present embodiment may be a compound having a reactive group capable of co-condensing with at least one of tetracarboxylic dianhydride and diamine.
[0317] Examples of such silicon-containing compounds include compounds represented by the following formula (10).
[0318]
[0319] {where,
[0320] R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms,
[0321] R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of R2 and R3 is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms,
[0322] R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of R4 and R5 is a monovalent aromatic group having 6 to 10 carbon atoms,
[0323] R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of R6 and R7 is an organic group containing an unsaturated aliphatic hydrocarbon group having 2 to 10 carbon atoms.
[0324] L1 and L2 are each independently a monovalent organic group containing an acid anhydride structure, an amino group, an isocyanate group, a carboxyl group, an alkoxycarbonyl group, a halogenated carbonyl group, a hydroxyl group, an epoxy group or a mercapto group,
[0325] i and j are each independently an integer of 1 to 200,
[0326] k is an integer from 0 to 200, and
[0327] Satisfies the relationship 0.05≤j / (i+j+k)≤0.50.}
[0328] R1 in formula (10) is independently a single bond or a divalent organic group having 1 to 10 carbon atoms. The divalent organic group having 1 to 10 carbon atoms may be any of linear, cyclic and branched, and may be saturated or unsaturated. Examples of the divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms include linear or branched alkylene groups such as methylene, ethylene, n-propylene, isopropylene, n-butylene, sec-butylene, tert-butylene, n-pentylene, neopentylene, n-hexylene, n-heptylene, n-octylene, n-nonylene, and n-decylene; and cycloalkylene groups such as cyclopropylene, cyclobutylene, cyclopentylene, cyclohexylene, cycloheptylene, and cyclooctylene. The divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms is preferably at least one selected from the group consisting of ethylene, n-propylene, and isopropylene.
[0329] In the formula (10), R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of them is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms.
[0330] The monovalent organic group having 1 to 10 carbon atoms may be any of linear, cyclic, and branched, and may be saturated or unsaturated. For example, as the monovalent organic group having 1 to 10 carbon atoms, there can be listed linear or branched alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, neopentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl; cycloalkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, and cyclooctyl; aromatic groups such as phenyl, tolyl, xylyl, α-naphthyl, and β-naphthyl.
[0331] The monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms may be any of linear, cyclic, and branched, and may be saturated or unsaturated. For example, as the monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms, there can be listed linear or branched alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, and neopentyl; and cycloalkyl groups such as cyclopropyl, cyclobutyl, and cyclopentyl. As the monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms, it is preferably at least one selected from the group consisting of methyl, ethyl, and n-propyl.
[0332] R4 and R5 in formula (10) are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of them is a monovalent aromatic group having 6 to 10 carbon atoms. The monovalent organic group having 1 to 10 carbon atoms may be any of linear, cyclic, and branched, and may be saturated or unsaturated. For example, as the monovalent organic group having 1 to 10 carbon atoms, there can be listed linear or branched alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, neopentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl; cycloalkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, and cyclooctyl; aromatic groups such as phenyl, tolyl, xylyl, α-naphthyl, and β-naphthyl; and the like. Examples of the monovalent aromatic group having 6 to 10 carbon atoms include phenyl, tolyl, xylyl, α-naphthyl, β-naphthyl and the like, and preferably phenyl, tolyl or xylyl.
[0333] R6 and R7 in formula (10) are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of them is an organic group having an unsaturated aliphatic hydrocarbon group. The monovalent organic group having 1 to 10 carbon atoms may be any of linear, cyclic, and branched. Examples of the monovalent organic group having 1 to 10 carbon atoms include linear or branched alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, neopentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl; cycloalkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, and cyclooctyl; and aromatic groups such as phenyl, tolyl, xylyl, α-naphthyl, and β-naphthyl. As the monovalent organic group having 1 to 10 carbon atoms, at least one selected from the group consisting of methyl, ethyl, and phenyl is preferred.
[0334] The organic group having an unsaturated aliphatic hydrocarbon group may be an unsaturated aliphatic hydrocarbon group having 3 to 10 carbon atoms, and may be any of a straight chain, a cyclic, or a branched chain. As the unsaturated aliphatic hydrocarbon group having 3 to 10 carbon atoms, for example, vinyl, allyl, 1-propenyl, 3-butenyl, 2-butenyl, pentenyl, cyclopentenyl, hexenyl, cyclohexenyl, heptenyl, octenyl, nonenyl, decenyl, ethynyl, propynyl, butynyl, pentynyl, hexynyl, etc. may be cited. As the unsaturated aliphatic hydrocarbon group having 3 to 10 carbon atoms, at least one selected from the group consisting of vinyl, allyl, and 3-butenyl may be preferred.
[0335] In the formula (10), some or all of the hydrogen atoms in R1 to R7 may be substituted with a substituent such as a halogen atom such as F, Cl, or Br, or may be unsubstituted.
[0336] L1 and L2 in formula (10) are each independently a monovalent organic group containing an acid anhydride structure (also referred to as an acid anhydride group), an amino group, an isocyanate group, a carboxyl group, an alkoxycarbonyl group, a halogenated carbonyl group, a hydroxyl group, an epoxy group or a mercapto group.
[0337] As a monovalent organic group including an acid anhydride structure, a 2,5-dioxotetrahydrofuran-3-yl group represented by the following formula can be mentioned, for example.
[0338]
[0339] {In the above formula, "*" represents a connecting bond.}
[0340] Among these, an amino group and an acid anhydride group are preferred, and an amino group is more preferred from the viewpoint of viscosity stability of the resin composition.
[0341] The alkoxy group in the alkoxycarbonyl group may be an alkoxy group having 1 to 6 carbon atoms, and examples thereof include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, and tert-butoxy.
[0342] The halogen atom in the halocarbonyl group is preferably a halogen atom other than a fluorine atom, and more preferably a chlorine atom or an iodine atom.
[0343] From the viewpoint of the filterability of the resin composition, the functional group equivalent of the silicon-containing compound shown in formula (10) is preferably 800 or more, more preferably 1000 or more, and further preferably 1500 or more. On the other hand, when the functional group equivalent is 500 or less, the filterability sometimes deteriorates. Here, the functional group equivalent is the molecular weight of the silicon-containing compound per 1 mol of functional group (unit: g / mol). The functional group equivalent can be measured using a known method. In addition, when the functional group equivalent of the silicon-containing compound is 800 or more, the residual stress of the polyimide film under a nitrogen atmosphere is small, so it is preferred. As a reason for this, it can be considered that this is because: when the functional group equivalent is above a specific value, the organosilicon domain increases and the stress is relieved.
[0344] It should be noted that the functional group equivalent can be measured according to existing standards and the like.
[0345] i in formula (10) is an integer of 1 to 200, preferably an integer of 2 to 100, more preferably an integer of 4 to 80, and further preferably an integer of 8 to 40. j and k are each independently an integer of 0 to 200, preferably an integer of 0 to 50, more preferably an integer of 0 to 20, and further preferably an integer of 0 to 50.
[0346] If the polyimide in the resin composition has a structure derived from formula (10), the residual stress of the polyimide film measured in a nitrogen atmosphere is good (small), so it is preferred. The reason for measuring in a nitrogen atmosphere is that in the process of display, when an inorganic film such as SiO, SiN, etc. is formed on the polyimide film, it is sometimes exposed to a nitrogen atmosphere, and it is sought to have a small residual stress in a nitrogen atmosphere.
[0347] [Second Method]
[0348] 《Resin composition》
[0349] 〈Resin / polyimide precursor / polyimide〉
[0350] The resin composition of the present embodiment includes a resin having a structural unit represented by the following general formula (1) or (2), and may include a polyimide precursor (hereinafter also referred to as a full polyimide precursor) or a polyimide (hereinafter also referred to as a full polyimide).
[0351]
[0352] {In the formula, P1 represents a divalent organic group; P2 represents a tetravalent organic group; and p represents a positive integer.}
[0353]
[0354] {In the formula, P1 represents a divalent organic group; P2 represents a tetravalent organic group; and p represents a positive integer.}
[0355] P1 includes a structural unit derived from a compound represented by the following general formula (3), and, if desired, P2 may include a structural unit derived from a compound represented by the following general formula (4).
[0356]
[0357]
[0358] In addition, P1 or P2 includes a structural unit derived from a silicon-containing compound represented by the following general formula (5).
[0359]
[0360] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50; and the functional group equivalent is 8000 or more.}
[0361] The polyimide can be obtained by thermally imidizing a polyimide precursor, or chemically imidizing the polyimide precursor. Thermal imidization is preferred from the viewpoint of transparency of the obtained polyimide film.
[0362] Moreover, from the viewpoint of viscosity stability of the composition, the polyimide resin composition is more preferable than the polyimide precursor resin composition.
[0363] In addition, the resin composition according to another embodiment of the present invention may include a polyimide precursor which includes structural units represented by the following general formulae (6) and (7) and is partially imidized.
[0364]
[0365] {In the formula, P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer; P3 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA) or a structural unit derived therefrom.}
[0366]
[0367] {In the formula, P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer; P5 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA) or a structural unit derived therefrom.}
[0368] P3 and / or P5 may include a structural unit derived from a compound represented by the following general formula (8).
[0369]
[0370] In addition, P3 and / or P5 may include at least one structural unit derived from various compounds of 3,3′-diaminodiphenyl sulfone (33DAS) or 4,4′-diaminodiphenyl sulfone (44DAS).
[0371] In addition, P3 and / or P5 may include at least one structural unit derived from 9,9-bis(4-aminophenyl)fluorene (BAFL) or a compound of the following general formula (BisAM).
[0372]
[0373] Among these, from the viewpoint of the elongation and mechanical properties of the polyimide film, the compound of the general formula (8), 3,3'-diaminodiphenyl sulfone (33DAS) and / or 4,4'-diaminodiphenyl sulfone (44DAS) are preferred. On the other hand, from the viewpoint of the viscosity stability and filterability of the varnish and the viewpoint of foreign matter generated during imidization, 6FODA is not preferably used as P3 and / or P5.
[0374] P4 and / or P6 may contain a structural unit derived from a compound represented by the following general formula (9).
[0375]
[0376] Additionally, P4 and / or P6 may comprise at least one compound derived from:
[0377] 4,4'-oxydiphthalic anhydride (ODPA),
[0378] 4,4'-(Hexafluoroisopropylidene)diphthalic anhydride (6FDA),
[0379] 9,9-bis(3,4-dicarboxyphenyl)fluorene anhydride (BPAF),
[0380] The compound of the following general formula (BzDA),
[0381]
[0382] And the compound of the following general formula (BNBDA),
[0383]
[0384] The structural unit of the compound in.
[0385] Among these, the compound represented by the general formula (9) and ODPA are preferred from the viewpoint of viscosity stability and filterability of the varnish and transparency of the polyimide film.
[0386] In one embodiment, P3 or P4 includes a structural unit derived from a silicon-containing compound represented by the following general formula (10).
[0387]
[0388] {In the formula, R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group, anhydride group, isocyanate group, carboxyl group, acid ester group, acyl halide group, hydroxyl group, epoxy group or mercapto group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50; and the functional group equivalent is 8000 or more.}
[0389] In the case of such a partially imidized polyimide precursor, the viscosity stability of the composition is excellent compared with the above-mentioned full polyimide precursor, and it is excellent from the viewpoint of ease of synthesis of the polyimide (polyimide precursor) compared with the above-mentioned full polyimide.
[0390] In the general formula (10), L1 and L2 are each independently an amino group, an acid anhydride group, an isocyanate group, a carboxyl group, an acid ester group, an acid halide group, a hydroxyl group, an epoxy group or a mercapto group, and among these, an amino group is preferred from the viewpoint of resin properties or film properties.
[0391] Diamine
[0392] The resin composition contains a structural unit derived from a diamine compound represented by the following general formula (3).
[0393]
[0394] Among the diamine compounds shown in the general formula (3), 3,5-diaminobenzoic acid (DABA) is preferred from the perspective of the transparency and YI of the polyimide film. If this structural unit is present, the mechanical properties of the resulting polyimide film are improved (especially tensile elongation), and heat resistance can be improved, so it is preferred. The reason for this improvement in properties is not clear, but it can be considered that it is because: intermolecular interactions are exerted by the action of the carboxyl group.
[0395] The content of DABA in all diamines (including compounds in which L1 and L2 in the above general formula (5) and (10) are amino groups) may be more than 50 mol%, more than 55 mol%, or more than 70 mol%, or more than 90 mol%, or more than 95 mol%. The larger the amount of DABA, the greater the tensile elongation of the polyimide film, which is preferred.
[0396] The resin composition contains structural units derived from 33DAS and / or 44DAS. From the viewpoint of achieving both Rth (retardation) in the thickness direction of the polyimide film and mechanical properties, 33DAS and 44DAS are preferably used in the form of a mixture of 33DAS and 44DAS.
[0397] The total content of 33DAS and / or 44DAS in all diamines (including compounds in which L1 and L2 in the above general formula (5) and (10) are amino groups) may be more than 50 mol%, more than 55 mol%, or more than 70 mol%, or more than 90 mol%, or more than 95 mol%. The greater the amount of 33DAS and / or 44DAS, the higher the mechanical strength of the polyimide film, which is preferred.
[0398] Examples of diamines other than general formula (3) include p-phenylenediamine (PDA), m-phenylenediamine, 2,2'-dimethylbenzidine (mTB), 4,4'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 4,4'-diaminobiphenyl, 3,4'-diaminobiphenyl, 3,3'-diaminobiphenyl, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, bis[4-(4-aminophenoxy)phenyl]sulfone, 4,4 -Bis(4-aminophenoxy)biphenyl, 4,4-bis(3-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 9,10-bis(4-aminophenyl)anthracene, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl)propane, 2,2-bis[4-(4-aminophenoxy)phenyl)hexafluoropropane and 1,4-bis(3-aminopropyldimethylsilyl)benzene, 9,9-bis(4-aminophenyl)fluorene (BAFL), 1,3-bis[1-(4-aminophenyl)-1-methylethyl]benzene] (BiSAM), etc.
[0399] Among these, at least one selected from the group consisting of 9,9-bis(4-aminophenyl)fluorene (BAFL), 1,3-bis[1-(4-aminophenyl)-1-methylethyl]benzene] (BiSAM) and 1,4-cyclohexanediamine (CHDA) is preferred.
[0400] From the viewpoint of heat resistance and mechanical strength of the obtained polyimide resin film, the diamine other than 33DAS and / or 44DAS of the general formula (3) is more preferably at least one selected from the group consisting of 9,9-bis(4-aminophenyl)fluorene (BAFL) and 1,3-bis[1-(4-aminophenyl)-1-methylethyl]benzene] (BiSAM).
[0401] Acid dianhydride
[0402] The resin composition contains a structural unit derived from a compound represented by the following general formula (4) (also referred to as CpODA).
[0403]
[0404] The presence of such a structural unit is preferred because the transparency, YI, and heat-resistant mechanical properties of the polyimide film to be obtained can be improved.
[0405] The content of CpODA in all acid dianhydrides (including compounds in which L1 and L2 in the above general formula (5) and (10) are acid anhydride groups) can be 50 mol% or more, 60 mol% or more, or 70 mol% or more, or 90 mol% or more, or 95 mol% or more. The greater the amount of CpODA, the higher the transparency of the polyimide film, so it is preferred.
[0406] The resin composition further includes a structural unit derived from ODPA. The presence of such a structural unit is preferred because the transparency of the obtained polyimide film can be improved from the viewpoint of the viscosity stability and filterability of the varnish.
[0407] The content of ODPA in all acid dianhydrides (including compounds in which L1 and L2 in the above general formula (5) and (10) are acid anhydride groups) can be 50 mol% or more, 60 mol% or more, or 70 mol% or more, or 90 mol% or more, or 95 mol% or more. The greater the amount of ODPA, the higher the transparency of the polyimide film, so it is preferred.
[0408] Examples of the acid dianhydride other than the general formula (4) include pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,2',3,3'-biphenyltetracarboxylic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA), 5-(2,5-dioxotetrahydro-3-furyl)-3-methyl-cyclohexene-1,2-dicarboxylic anhydride, 1,2,3,4-benzenetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, and methylene-4,4'-diphthalic anhydride. Formic acid dianhydride, 1,1-ethylene-4,4'-diphthalic dianhydride, 2,2-propylene-4,4'-diphthalic dianhydride, 1,2-ethylene-4,4'-diphthalic dianhydride, 1,3-trimethylene-4,4'-diphthalic dianhydride, 1,4-tetramethylene-4,4'-diphthalic dianhydride, 1,5-pentamethylene-4,4'-diphthalic dianhydride, 4,4'-oxydiphthalic dianhydride, p-phenylenebis-trimellitic anhydride, thio-4,4'-diphthalic dianhydride, sulfonyl-4,4'-diphthalic dianhydride, 1,3-bis(3,4-dicarboxyphenyl)phthalic anhydride, 1,3-bis( 3,4-dicarboxyphenoxy) phthalic anhydride, 1,4-bis(3,4-dicarboxyphenoxy) phthalic anhydride, 1,3-bis[2-(3,4-dicarboxyphenyl)-2-propyl]phthalic anhydride, 1,4-bis[2-(3,4-dicarboxyphenyl)-2-propyl]phthalic anhydride, bis[3-(3,4-dicarboxyphenoxy)phenyl]methane dianhydride, bis[4-(3,4-dicarboxyphenoxy)phenyl]methane dianhydride, 2,2-bis[3-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, bis(3,4-dicarboxyphenoxy)dimethylsilane dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)phenyl 4-dicarboxyphenyl)-1,1,3,3-tetramethyldisiloxane dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride and 1,2,7,8-phenanthrenetetracarboxylic dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF), 4,4'-oxydiphthalic anhydride (ODPA), 1,2,4,5-cyclohexanetetracarboxylic dianhydride (HPMDA) and 1,2,3,4-cyclobutanetetracarboxylic dianhydride (CBDA), a compound having the following structure (BzDA);
[0409]
[0410] The compound with the following structure (BNBDA), etc.
[0411]
[0412] The acid dianhydride other than the above general formula (4) is preferably at least one selected from the group consisting of 6FDA, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF), BzDA, BNBDA, and 1,2,4,5-cyclohexanetetracarboxylic dianhydride (HPMDA). The acid dianhydride may be used alone or in combination of two or more.
[0413] 〈Silicon-containing compounds〉
[0414] The polyimide precursor in the present embodiment can have the structure shown in the above formula (1) and the structure shown in the above formula (2) together. Taking the mass of the polyimide precursor as a benchmark, the content ratio of the structure derived from the silicon-containing compound in the polyimide precursor is preferably more than 5% by mass and less than 40% by mass. If the polyimide precursor includes a structure derived from a silicon-containing compound within the numerical range, it is possible to take into account low residual stress and high transparency and heat resistance in the resulting polyimide film, so it is preferred. Taking the mass of the polyimide precursor as a benchmark, the content ratio of the structure derived from the silicon-containing compound can be more than 6% by mass or more than 7% by mass, and in addition, it can be less than 30% by mass or less than 25% by mass.
[0415] The polyimide / polyimide precursor in the present embodiment has a structure derived from a silicon-containing compound. Therefore, the silicon-containing compound used in the synthesis of the polyimide precursor in the present embodiment may be a compound having a reactive group capable of co-condensing with at least one of tetracarboxylic dianhydride and diamine.
[0416] Examples of such silicon-containing compounds include compounds represented by the following formula (5).
[0417]
[0418] {where,
[0419] R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms,
[0420] R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of R2 and R3 is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms,
[0421] R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of R4 and R5 is a monovalent aromatic group having 6 to 10 carbon atoms,
[0422] R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of R6 and R7 is an organic group containing an unsaturated aliphatic hydrocarbon group having 2 to 10 carbon atoms.
[0423] L1 and L2 are each independently a monovalent organic group containing an acid anhydride structure, an amino group, an isocyanate group, a carboxyl group, an alkoxycarbonyl group, a halogenated carbonyl group, a hydroxyl group, an epoxy group or a mercapto group,
[0424] i and j are each independently an integer of 1 to 200,
[0425] k is an integer from 0 to 200, and
[0426] Satisfies the relationship 0.05≤j / (i+j+k)≤0.50.}
[0427] R1 in formula (5) is independently a single bond or a divalent organic group having 1 to 10 carbon atoms. The divalent organic group having 1 to 10 carbon atoms may be any of linear, cyclic and branched, and may be saturated or unsaturated. Examples of divalent aliphatic hydrocarbon groups having 1 to 10 carbon atoms include linear or branched alkylene groups such as methylene, ethylene, n-propylene, isopropylene, n-butylene, sec-butylene, tert-butylene, n-pentylene, octylene, n-hexylene, n-heptylene, n-octylene, n-nonylene, and n-decylene; and cycloalkylene groups such as cyclopropylene, cyclobutylene, cyclopentylene, cyclohexylene, cycloheptylene, and cyclooctylene. As the divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, at least one selected from the group consisting of ethylene, n-propylene and isopropylene may be mentioned.
[0428] In the formula (5), R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of them is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms.
[0429] The monovalent organic group having 1 to 10 carbon atoms may be any of linear, cyclic, and branched, and may be saturated or unsaturated. For example, as the monovalent organic group having 1 to 10 carbon atoms, there can be listed linear or branched alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, neopentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl; cycloalkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, and cyclooctyl; aromatic groups such as phenyl, tolyl, xylyl, α-naphthyl, and β-naphthyl.
[0430] The monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms may be any of linear, cyclic, and branched, and may be saturated or unsaturated. For example, as the monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms, there can be listed linear or branched alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, and neopentyl; and cycloalkyl groups such as cyclopropyl, cyclobutyl, and cyclopentyl. As the monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms, it is preferably at least one selected from the group consisting of methyl, ethyl, and n-propyl.
[0431] R4 and R5 in formula (5) are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of them is a monovalent aromatic group having 6 to 10 carbon atoms. The monovalent organic group having 1 to 10 carbon atoms may be any of linear, cyclic, and branched, and may be saturated or unsaturated. For example, as the monovalent organic group having 1 to 10 carbon atoms, there can be listed linear or branched alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, neopentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl; cycloalkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, and cyclooctyl; aromatic groups such as phenyl, tolyl, xylyl, α-naphthyl, and β-naphthyl; and the like. Examples of the monovalent aromatic group having 6 to 10 carbon atoms include phenyl, tolyl, xylyl, α-naphthyl, β-naphthyl and the like, and preferably phenyl, tolyl or xylyl.
[0432] R6 and R7 in formula (5) are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of them is an organic group having an unsaturated aliphatic hydrocarbon group. The monovalent organic group having 1 to 10 carbon atoms may be any of linear, cyclic, and branched. Examples of the monovalent organic group having 1 to 10 carbon atoms include linear or branched alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, neopentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl; cycloalkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, and cyclooctyl; and aromatic groups such as phenyl, tolyl, xylyl, α-naphthyl, and β-naphthyl. As the monovalent organic group having 1 to 10 carbon atoms, at least one selected from the group consisting of methyl, ethyl, and phenyl is preferred.
[0433] The organic group having an unsaturated aliphatic hydrocarbon group may be an unsaturated aliphatic hydrocarbon group having 3 to 10 carbon atoms, and may be any of a straight chain, a cyclic, or a branched chain. As the unsaturated aliphatic hydrocarbon group having 3 to 10 carbon atoms, for example, vinyl, allyl, 1-propenyl, 3-butenyl, 2-butenyl, pentenyl, cyclopentenyl, hexenyl, cyclohexenyl, heptenyl, octenyl, nonenyl, decenyl, ethynyl, propynyl, butynyl, pentynyl, hexynyl, etc. may be cited. As the unsaturated aliphatic hydrocarbon group having 3 to 10 carbon atoms, at least one selected from the group consisting of vinyl, allyl, and 3-butenyl may be preferred.
[0434] Some or all of the hydrogen atoms in R1 to R7 in the formula (5) may be substituted with a substituent such as a halogen atom such as F, Cl, or Br, or may be unsubstituted.
[0435] L1 and L2 in formula (5) are each independently a monovalent organic group containing an acid anhydride structure (also referred to as an acid anhydride group), an amino group, an isocyanate group, a carboxyl group, an alkoxycarbonyl group, a halogenated carbonyl group, a hydroxyl group, an epoxy group or a mercapto group. Among them, L1 and L2 are preferably an amino group from the viewpoint of resin properties or film properties.
[0436] As a monovalent organic group including an acid anhydride structure, a 2,5-dioxotetrahydrofuran-3-yl group represented by the following formula can be mentioned, for example.
[0437]
[0438] {In the above formula, "*" represents a connecting bond.}
[0439] Among these, an amino group and an acid anhydride group are preferred, and an amino group is more preferred from the viewpoint of viscosity stability of the resin composition.
[0440] The alkoxy group in the alkoxycarbonyl group may be an alkoxy group having 1 to 6 carbon atoms, and examples thereof include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, and tert-butoxy.
[0441] The halogen atom in the halocarbonyl group is preferably a halogen atom other than a fluorine atom, and more preferably a chlorine atom or an iodine atom.
[0442] From the viewpoint of the filterability of the resin composition, the functional group equivalent of the silicon-containing compound shown in formula (5) is preferably 800 or more, more preferably 1000 or more, and further preferably 1500 or more. On the other hand, when the functional group equivalent is 500 or less, the filterability sometimes deteriorates. Here, the functional group equivalent is the molecular weight of the silicon-containing compound per 1 mol of functional group (unit: g / mol). The functional group equivalent can be measured using a known method. In addition, when the functional group equivalent of the silicon-containing compound is 800 or more, the residual stress of the polyimide film under a nitrogen atmosphere is small, so it is preferred. As a reason for this, it can be considered that this is because: when the functional group equivalent is above a specific value, the organosilicon domain increases and the stress is relieved.
[0443] It should be noted that the functional group equivalent can be measured according to existing standards and the like.
[0444] i in formula (5) is an integer of 1 to 200, preferably an integer of 2 to 100, more preferably an integer of 4 to 80, and further preferably an integer of 8 to 40. j and k are each independently an integer of 0 to 200, preferably an integer of 0 to 50, more preferably an integer of 0 to 20, and further preferably an integer of 0 to 50.
[0445] If the polyimide in the resin composition has a structure derived from formula (5), the residual stress of the polyimide film measured in a nitrogen atmosphere is good (small), so it is preferred. The reason for measuring in a nitrogen atmosphere is that in the process of display, when an inorganic film such as SiO, SiN, etc. is formed on the polyimide film, it is sometimes exposed to a nitrogen atmosphere, and it is sought to have a small residual stress in a nitrogen atmosphere.
[0446] [Common components and preferred embodiments of the first and second aspects]
[0447] Hereinafter, the common components of the first and second aspects of the present invention and preferred embodiments of the present invention will be described. It should be noted that the components of the first and second aspects may be interchangeable or combined.
[0448] 〈Silicon-containing diamine〉
[0449] The silicon-containing compound of the above-described general formula (5) or (10) is preferably a silicon-containing diamine from the viewpoints of the type and cost of the monomer and the molecular weight of the obtained polyimide precursor. The silicon-containing diamine is preferably a diamino (poly)siloxane represented by the following formula (11).
[0450]
[0451] {In the formula, P5 each independently represents a divalent hydrocarbon group, which may be the same or different, P3 and P4 are the same as R2 and R3 defined in the general formula (5) or (10), and l represents an integer of 1 to 200.}
[0452] Preferred structures of P3 and P4 in the general formula (11) include methyl, ethyl, propyl, butyl and phenyl groups, among which methyl is preferred.
[0453] In the general formula (11), l is an integer of 1 to 200, and is preferably an integer of 3 to 200 from the viewpoint of heat resistance of a polyimide obtained by using the silicon-containing diamine represented by the formula (11).
[0454] The preferred range of the functional group equivalent of the compound represented by the general formula (11) is the same as that of the silicon-containing compound represented by the general formula (10).
[0455] The copolymerization ratio of silicon-containing diamine is preferably 0.5 to 30 mass %, more preferably 1.0 mass % to 25 mass %, and further preferably 1.5 mass % to 20 mass % relative to the total mass of polyimide precursor / polyimide. When the silicon-containing diamine is 0.5 mass % or more, the residual stress generated between the support body can be effectively reduced. When the silicon-containing diamine is 30 mass % or less, the transparency (especially low haze) of the obtained polyimide film is good, which is preferred from the viewpoint of achieving high total light transmittance and high glass transition temperature.
[0456] As described above, the silicon-containing compound as a monomer used in the polyimide precursor / polyimide can be synthesized using the technical common sense at the time of application, or commercial products can be used. Commercial products include methylphenyl silicone oil modified with amine at both ends (manufactured by Shin-Etsu Chemical Co., Ltd.: X22-1660B-3 (functional group equivalent is 2200), X22-9409 (functional group equivalent is 670)), methylphenyl silicone oil modified with anhydride at both ends (manufactured by Shin-Etsu Chemical Co., Ltd.: X22-168-P5-B (functional group equivalent is 2100)), methylphenyl silicone oil modified with epoxy at both ends (manufactured by Shin-Etsu Chemical Co., Ltd.: X22-2000 (functional group equivalent is 670)). Functional group equivalent weight is 620)), dimethyl silicone modified with amino groups at both ends (Shin-Etsu Chemical Co., Ltd.: PAM-E (functional group equivalent weight is 130), X22-161A (functional group equivalent weight is 800), X22-161B (functional group equivalent weight is 1500), KF8012 (functional group equivalent weight is 2200), BY16-853U (functional group equivalent weight is 450) manufactured by Dow Corning Toray, Silaplane FM3311 (number average molecular weight of 1000)), dimethyl silicone oil modified with epoxy at both ends (manufactured by Shin-Etsu Chemical Co., Ltd.: X-22-163A (functional group equivalent of 1750), dimethyl silicone oil modified with alicyclic epoxy at both ends (manufactured by Shin-Etsu Chemical Co., Ltd.: X-22-169B (functional group equivalent of 1700)), dimethyl silicone oil modified with hydroxyl at both ends (manufactured by Shin-Etsu Chemical Co., Ltd.: KF-6000), dimethyl silicone oil modified with mercapto at both ends (manufactured by Shin-Etsu Chemical Co., Ltd.: X-22-167B (functional group equivalent of 1700)), dimethyl silicone oil modified with anhydride at both ends (manufactured by Shin-Etsu Chemical Co., Ltd.: X-22-168A (functional group equivalent of 1000)), etc. Among these, dimethyl silicone oil modified with amine at both ends is preferred from the viewpoints of price, improvement of chemical resistance and improvement of Tg.
[0457] 〈Solvent〉
[0458] Typically, the resin composition includes a solvent. As a solvent, a solvent having good solubility of polyimide / polyimide precursor and being able to appropriately control the solution viscosity of the resin composition is preferred, and the reaction solvent of the polyimide precursor can be used as a solvent for the composition. Among them, N-methyl-2-pyrrolidone (NMP), γ-butyrolactone (GBL), the compound represented by the above general formula (9) described in the first embodiment, and the compound represented by the above general formula (4) described in the second embodiment are preferred. As a specific example of the solvent composition, N-methyl-2-pyrrolidone (NMP) alone or a mixed solvent of N-methyl-2-pyrrolidone (NMP) and γ-butyrolactone (GBL) can be listed. The mass ratio of NMP to GBL can be, for example, NMP:GBL (mass ratio) = 10:90 to 90:10.
[0459] 〈Additional ingredients〉
[0460] The resin composition of the present embodiment may further contain an additional component in addition to the polyimide / polyimide precursor, the low molecular weight cyclic siloxane, and the solvent. Examples of the additional component include a surfactant and an alkoxysilane compound.
[0461] Surfactants
[0462] By adding a surfactant to the resin composition of the present embodiment, the coating properties of the resin composition can be improved. Specifically, it is possible to prevent streaks from being generated in the coating film.
[0463] Examples of such surfactants include silicone surfactants, fluorine surfactants, and other nonionic surfactants. Examples of silicone surfactants include organosiloxane polymers KF-640, 642, 643, KP341, X-70-092, X-70-093 (trade names, manufactured by Shin-Etsu Chemical Co., Ltd.); SH-28PA, SH-190, SH-193, SZ-6032, SF-8428, DC-57, DC-190 (trade names, manufactured by Toray Dow Corning Silicones Co., Ltd.); SILWETL-77, L-7001, FZ-2105, FZ-2120, FZ -2154, FZ-2164, FZ-2166, L-7604 (trade name, made by Unicharm Co., Ltd. of Japan); DBE-814, DBE-224, DBE-621, CMS-626, CMS-222, KF-352A, KF-354L, KF-355A, KF-6020, DBE-821, DBE-712 (Gelest), BYK-307, BYK-310, BYK-378, BYK-333 (trade name, made by BYK-Chemie Japan); GRANOL (trade name, made by Kyoeisha Chemical Co., Ltd.), etc. As fluorine-based surfactants, for example, Megafac F171, F173, R-08 (manufactured by Dainippon Ink & Chemicals Co., Ltd., trade names); Fluorad FC4430, FC4432 (trade names by Sumitomo 3M Co., Ltd.), etc. As nonionic surfactants other than these, for example, polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, polyoxyethylene octylphenol ether, etc. can be mentioned.
[0464] Among these surfactants, silicone surfactants and fluorine surfactants are preferred from the viewpoint of coating properties of the resin composition (suppression of streaks), and silicone surfactants are preferred from the viewpoint of reducing the influence of oxygen concentration on YI value and total light transmittance during the curing process. When a surfactant is used, its blending amount is preferably 0.001 to 5 parts by mass, more preferably 0.01 to 3 parts by mass, relative to 100 parts by mass of the polyimide precursor in the resin composition.
[0465] Alkoxysilane compounds
[0466] When the polyimide film obtained by the resin composition of the present embodiment is used for a flexible substrate, etc., from the viewpoint of obtaining good adhesion between the support and the polyimide film in the manufacturing process, the resin composition may contain 0.01 to 20 parts by mass of an alkoxysilane compound relative to 100 parts by mass of the polyimide precursor. By making the content of the alkoxysilane compound 0.01 parts by mass or more relative to 100 parts by mass of the polyimide precursor, it is possible to obtain good adhesion between the support and the polyimide film. In addition, from the viewpoint of the storage stability of the resin composition, the content of the alkoxysilane compound is preferably 20 parts by mass or less. The content of the alkoxysilane compound is preferably 0.02 to 15 parts by mass, more preferably 0.05 to 10 parts by mass, and further preferably 0.1 to 8 parts by mass relative to 100 parts by mass of the polyimide precursor. By using an alkoxysilane compound, the above-mentioned adhesion is improved, the coating property of the resin composition is improved (uneven streaks are suppressed), and the influence of the oxygen concentration during curing on the YI value of the polyimide film can be reduced.
[0467] Examples of the alkoxysilane compound include 3-ureidopropyltriethoxysilane, bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltripropoxysilane, γ-aminopropyltributoxysilane, γ-aminoethyltriethoxysilane, γ-aminoethyltripropoxysilane, γ-aminoethyltributoxysilane, γ-aminobutyltriethoxysilane, γ-aminobutyltrimethoxysilane, γ-aminobutyltripropoxysilane, γ-aminobutyltributoxysilane, phenylsilanetriol, trimethoxyphenylsilane, trimethoxy(p-tolyl)silane, diphenylsilanediol, dimethoxydiphenylsilane, diethoxydiphenylsilane, dimethoxydi-p-tolylsilane, triphenylsilanol, and alkoxysilane compounds each having the following structure.
[0468]
[0469] The alkoxysilane compounds may be used alone or in combination of two or more.
[0470] 《Method for producing resin composition》
[0471] The method for producing the resin composition in the present embodiment is not particularly limited, and for example, the following method can be used.
[0472] 〈Purification of Silicon-Containing Compounds〉
[0473] The resin composition of the present embodiment can be manufactured by subjecting the polycondensation components containing acid dianhydride, diamine and silicon-containing compound to polycondensation reaction. As a method for reducing the total amount of cyclic silicon-containing compounds contained in the resin composition of the present embodiment, for example, before the polycondensation reaction, the silicon-containing compound is purified to reduce the total amount of the cyclic silicon-containing compounds. Alternatively, the resin composition can be purified after the polycondensation reaction to reduce the total amount of the cyclic silicon-containing compounds.
[0474] As a method for purifying silicon-containing compounds, there can be cited the following: for example, in any container, stripping the silicon-containing compound while blowing an inert gas, such as nitrogen, into the silicon-containing compound. As the temperature of the stripping, it is preferably above 200°C and below 300°C, more preferably above 220°C and below 300°C, and further preferably above 240°C and below 300°C. As the vapor pressure of the stripping, the lower the better, it is preferably below 1000Pa, more preferably below 300Pa, further preferably below 200Pa, and further preferably below 133.32Pa (1mmHg). As the time of the stripping, it is preferably above 4 hours and below 12 hours, and more preferably above 6 hours and below 10 hours. By adjusting to the above conditions, monocyclic silicon-containing compounds can be effectively removed, and the total amount of cyclic silicon-containing compounds can be controlled to a preferred range.
[0475] 〈Synthesis of polyimide / polyimide precursor〉
[0476] The polyimide precursor of the present embodiment can be synthesized by subjecting a polycondensation component including an acid dianhydride, a diamine, and a silicon-containing compound to a polycondensation reaction.
[0477] Regarding the synthesis of the polyimide / polyimide precursor according to the first aspect, there is provided a method for producing a resin composition including, for example, the following arbitrary steps.
[0478] A step of subjecting the compound represented by the general formula (8) or the compound represented by the general formula (9) described above to a polycondensation reaction with a silicon-containing compound represented by the general formula (10) to obtain a polyimide, and then subjecting the polyimide to a polycondensation reaction with another compound to provide a resin composition comprising a polyimide precursor and a polyimide;
[0479] A step of subjecting the above-described diamine or acid dianhydride to a polycondensation reaction with a silicon-containing compound represented by the general formula (10) to obtain a polyimide, and then subjecting the polycondensation reaction to another compound to provide a resin composition containing a polyimide precursor and a polyimide.
[0480] Regarding the synthesis of the polyimide / polyimide precursor according to the second embodiment, there is provided a method for producing a resin composition including, for example, the following arbitrary steps.
[0481] A step of subjecting the compound represented by the general formula (3) and the compound represented by the general formula (4) and the silicon-containing compound represented by the general formula (5) described above and other compounds to polycondensation reaction to provide a resin composition containing a polyimide precursor or a polyimide;
[0482] A step of subjecting the compound represented by the general formula (3) described above and other compounds and the compound represented by the general formula (4) described above and other compounds to polycondensation reaction to obtain a polyimide, and then subjecting the silicon-containing compound represented by the general formula (5) described above and other compounds to polycondensation reaction to provide a resin composition containing a polyimide precursor and a polyimide; or
[0483] After the diamine described above is subjected to polycondensation reaction with an acid dianhydride to obtain a polyimide, a step of subjecting a silicon-containing compound represented by the general formula (5) to polycondensation reaction with other compounds to provide a resin composition containing a polyimide precursor and a polyimide.
[0484] In addition, the silicon-containing compound is preferably a substance obtained by the above purification. In a preferred embodiment, the polycondensation component is formed by an acid dianhydride, a diamine and a silicon-containing compound. The polycondensation reaction is preferably carried out in an appropriate solvent. Specifically, for example, a method in which a predetermined amount of a diamine component and a silicon-containing compound are dissolved in a solvent, a predetermined amount of an acid dianhydride is added to the obtained diamine solution, and the mixture is stirred.
[0485] Regarding the molar ratio of the acid dianhydride to the diamine when synthesizing the polyimide / polyimide precursor, from the viewpoint of the high molecular weight of the polyimide precursor resin and the slit coating characteristics of the resin composition, the range of acid dianhydride: diamine = 100:90 to 100:110 (0.90 to 1.10 mol parts of diamine relative to 1 mol part of acid dianhydride) is preferred, and the range of 100:95 to 100:105 (0.95 to 1.05 mol parts of diamine relative to 1 mol part of acid dianhydride) is more preferred.
[0486] The molecular weight of the polyimide / polyimide precursor can be controlled by adjusting the types of acid dianhydride, diamine and silicon-containing compound, the molar ratio of acid dianhydride to diamine, adding a capping agent, adjusting the reaction conditions, etc. The closer the molar ratio of the acid dianhydride component to the diamine component is to 1:1 and the less the amount of the capping agent is used, the higher the molecular weight of the polyimide precursor can be.
[0487] As the acid dianhydride component and the diamine component, it is recommended to use a high-purity product. As its purity, it is preferably 98% by mass or more, more preferably 99% by mass or more, and further preferably 99.5% by mass or more. By reducing the water content in the acid dianhydride component and the diamine component, it is also possible to highly purify. When using a variety of acid dianhydride components and / or a variety of diamine components, it is preferred that the acid dianhydride component as a whole and the diamine component as a whole have the above-mentioned purity, and it is more preferred that all types of acid dianhydride components and diamine components used have the above-mentioned purity respectively.
[0488] As the solvent of the reaction, there is no particular limitation as long as it is a solvent that can dissolve the acid dianhydride component and the diamine component, and the generated polyimide / polyimide precursor, and can obtain a high molecular weight polymer. As such solvent, for example, aprotic solvents, phenolic solvents, ethers, and glycol solvents can be cited.
[0489] Examples of aprotic solvents include N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N-methyl-2-pyrrolidone (NMP), N-methylcaprolactam, 1,3-dimethylimidazolidinone, tetramethylurea, and amide solvents of the following general formula; lactone solvents such as γ-butyrolactone and γ-valerolactone; phosphorus-containing amide solvents such as hexamethylphosphoramide and hexamethylphosphinetriamide; sulfur-containing solvents such as dimethyl sulfone, dimethyl sulfoxide, and cyclopentane; ketone solvents such as cyclohexanone and methylcyclohexanone; tertiary amine solvents such as methylpyridine and pyridine; ester solvents such as (2-methoxy-1-methylethyl) acetate, and the like.
[0490]
[0491] {In the formula, R 12 = Ecoamide M100 (trade name: manufactured by Idemitsu Kosan Co., Ltd.) represented by methyl group and R 12 = Ecoamide B100 (trade name: manufactured by Idemitsu Kosan Co., Ltd.) represented by n-butyl
[0492] Examples of the phenolic solvent include phenol, o-cresol, m-cresol, p-cresol, 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, and 3,5-xylenol.
[0493] Examples of the ether and glycol solvents include 1,2-dimethoxyethane, bis(2-methoxyethyl)ether, 1,2-bis(2-methoxyethoxy)ethane, bis[2-(2-methoxyethoxy)ethyl]ether, tetrahydrofuran, and 1,4-dioxane.
[0494] These solvents may be used alone or in combination of two or more.
[0495] The boiling point of the solvent used in the synthesis of the polyimide / polyimide precursor at normal pressure is preferably 60 to 300°C, more preferably 140 to 280°C, and further preferably 170 to 270°C. By making the boiling point of the solvent less than 300°C, the drying process becomes short. If the boiling point of the solvent is above 60°C, it is not easy to cause roughness on the surface of the resin film, mixing of bubbles into the resin film, etc. during the drying process, and a more uniform film can be obtained. In particular, from the viewpoint of solubility and reducing edge abnormalities during coating, it is preferred to use a solvent having a boiling point of 170 to 270°C and / or a vapor pressure of 250 Pa or less at 20°C. More specifically, it is preferably selected from one or more of the group consisting of N-methyl-2-pyrrolidone (NMP), γ-butyrolactone (GBL) and the compound represented by the general formula (6) described in the first and second embodiments.
[0496] In order to carry out polycondensation reaction well, the water content in the solvent is preferably, for example, less than 3,000 mass ppm. In the resin composition of the present embodiment, the content of molecules with a molecular weight less than 1,000 is preferably less than 5 mass %. It is believed that the presence of molecules with a molecular weight less than 1,000 in the resin composition is because: it is related to the moisture content of the solvent and raw materials (acid dianhydride, diamine) used during synthesis. That is, it can be considered that this is because: the anhydride gene of a part of the acid dianhydride monomer is hydrolyzed by moisture to form a carboxyl group, which will not be high molecular weight, but will remain in a low molecular state. Therefore, the less the moisture content of the solvent used in the above-mentioned polycondensation reaction, the more preferred. The moisture content of the solvent is preferably set to less than 3,000 mass ppm, and more preferably set to less than 1,000 mass ppm. Similarly, about the moisture content contained in the raw material, it is also preferably set to less than 3,000 mass ppm, and more preferably set to less than 1,000 mass ppm.
[0497] It is believed that the water content of the solvent is related to the grade of the solvent used (dehydrated grade, general grade, etc.), the solvent container (bottle, 18L can, small can, etc.), the storage state of the solvent (whether a rare gas is sealed, etc.), the time from opening to use (whether it is used immediately after opening, or whether it is used after a certain period of time after opening, etc.). It is also believed that it is related to the rare gas replacement of the reactor before synthesis, whether the rare gas is circulated during synthesis, etc. Therefore, it is recommended to use a high-purity product as a raw material and a solvent with a small amount of water when synthesizing a polyimide precursor, and to take measures to prevent moisture from the environment from mixing into the system before and during the reaction.
[0498] When each polycondensation component is dissolved in a solvent, heating may be performed as needed. From the viewpoint of obtaining a polyimide precursor with a high degree of polymerization, the reaction temperature when synthesizing the polyimide precursor may preferably be 0° C. to 120° C., 40° C. to 100° C., or 60° C. to 100° C., and the polymerization time may preferably be 1 to 100 hours or 2 to 10 hours. By setting the polymerization time to more than 1 hour, a polyimide precursor with a uniform degree of polymerization is formed, and by setting it to less than 100 hours, a polyimide precursor with a high degree of polymerization can be obtained.
[0499] In the resin composition of the present embodiment, in addition to the polyimide / polyimide precursor in the present embodiment, other additional polyimide precursors may be included. However, from the viewpoint of reducing the oxygen dependence of the YI value and the total light transmittance of the polyimide film, the mass ratio of the additional polyimide / polyimide precursor relative to the total amount of the polyimide / polyimide precursor in the resin composition is preferably 30% by mass or less, and more preferably 10% by mass or less.
[0500] A portion of the polyimide precursor in the present embodiment may be imidized (partially imidized). By partially imidizing the polyimide precursor, the viscosity stability during storage of the resin composition can be improved. From the viewpoint that the solubility of the polyimide precursor in the resin composition is balanced with the storage stability of the solution, the imidization rate at this time is preferably 5% or more, more preferably 8% or more, and preferably 80% or less, more preferably 70% or less, and further preferably 50% or less. The partial imidization is obtained by heating the polyimide precursor and performing dehydration ring closure. The heating can be preferably carried out at a temperature of preferably 120 to 200°C, more preferably 150 to 185°C, and further preferably 150 to 180°C for 15 minutes to 20 hours, more preferably 30 minutes to 10 hours.
[0501] As the polyimide precursor of the present embodiment, a substance obtained by adding N,N-dimethylformamide dimethyl acetal or N,N-dimethylformamide diethyl acetal to the polyimide / polyimide precursor obtained by the above reaction and heating to esterify a part or all of the carboxylic acids can be used. Viscosity stability during storage can be improved by esterification. These ester-modified polyamic acids can also be obtained by reacting the above-mentioned acid dianhydride component with a monohydric alcohol having 1 equivalent relative to the acid anhydride group, and a dehydration condensation agent such as thionyl chloride and dicyclohexylcarbodiimide, and then reacting with a diamine component to obtain the condensation reaction.
[0502] 〈Synthesis of polyimide〉
[0503] As a more preferred embodiment, the polyimide varnish can be prepared in the form of a polyimide solution (also referred to as a polyimide varnish) containing polyimide and a solvent by dissolving the acid dianhydride component and the diamine component in a solvent, such as an organic solvent, adding an azeotropic solvent such as toluene, and excluding the water generated during imidization from the system. Here, the conditions during the reaction are not particularly limited, for example, the reaction temperature is 0°C to 180°C and the reaction time is 3 to 72 hours. In order to fully react with the diamines containing a sulfonic group, it is preferred to heat the reaction at 180°C for about 12 hours. In addition, during the reaction, an inert atmosphere such as argon or nitrogen is preferably used.
[0504] <Preparation of resin composition>
[0505] When the solvent used in the synthesis of the polyimide precursor is the same as the solvent contained in the resin composition, the synthesized polyimide / polyimide precursor solution can be directly used as a resin composition. As required, by adding a further solvent and one or more of the additional components to the polyimide precursor in the temperature range of room temperature (25°C) to 80°C, and stirring and mixing, the resin composition can also be prepared. The stirring and mixing can be carried out using appropriate devices such as Three One Motor (Shinto Chemical Co., Ltd.) equipped with stirring blades, a rotation revolution stirrer, etc. As required, the resin composition can be heated to 40°C to 100°C.
[0506] On the other hand, when the solvent used in the synthesis of polyimide / polyimide precursor is different from the solvent contained in the resin composition, the polyimide / polyimide precursor can be separated by removing the solvent in the synthesized polyimide precursor solution by appropriate methods such as reprecipitation and solvent distillation. Then, the resin composition can be prepared by adding the desired solvent and the components added as needed to the separated polyimide precursor in the temperature range of room temperature (25°C) to 80°C, and stirring and mixing.
[0507] After the resin composition is prepared as described above, a portion of the polyimide precursor can be dehydrated imidized (partially imidized) to such an extent that the polymer does not precipitate by heating the resin composition at, for example, 130 to 200° C. for, for example, 5 minutes to 2 hours. The imidization rate can be controlled by controlling the heating temperature and the heating time. By partially imidizing the polyimide precursor, the viscosity stability of the resin composition when it is stored can be improved.
[0508] From the perspective of slit coating performance, the solution viscosity of the resin composition is preferably 500 to 100,000 mPa·s, more preferably 1,000 to 50,000 mPa·s, and further preferably 3,000 to 20,000 mPa·s. Specifically, from the perspective of not easily leaking from the slit nozzle, it is preferably 500 mPa·s or more, more preferably 1,000 mPa·s or more, and further preferably 3,000 mPa·s or more. From the perspective of the slit nozzle being difficult to clog, it is preferably 100,000 mPa·s or less, more preferably 50,000 mPa·s or less, and further preferably 20,000 mPa·s or less.
[0509] Regarding the solution viscosity of the resin composition when synthesizing polyimide / polyimide precursor, if it is higher than 200,000 mPa·s, it is possible to cause the problem of difficulty in stirring during synthesis. Among them, even if the solution reaches a high viscosity during synthesis, a resin composition with good handling viscosity can be obtained by adding a solvent and stirring after the reaction is completed. The solution viscosity of the resin composition in this embodiment is a value measured at 23°C using an E-type viscometer (e.g., VISCONICE HD, manufactured by Toki Sangyo Co., Ltd.).
[0510] From the viewpoint of viscosity stability during storage of the resin composition, the water content of the resin composition of the present embodiment is preferably 3,000 mass ppm or less, more preferably 2,500 mass ppm or less, further preferably 2,000 mass ppm or less, further preferably 1,500 mass ppm or less, particularly preferably 1,000 mass ppm or less, particularly preferably 500 mass ppm or less, particularly preferably 300 mass ppm or less, and particularly preferably 100 mass ppm or less.
[0511] "Polyimide film and method for producing the same"
[0512] The resin composition of the present embodiment can provide a polyimide film (hereinafter also referred to as a polyimide resin film). The method for manufacturing the polyimide film of the present embodiment includes: a coating step of coating the resin composition of the present embodiment on the surface of a support; a film forming step of heating the resin composition to form a polyimide resin film; and a stripping step of stripping the polyimide resin film from the support.
[0513] 〈Coating process〉
[0514] In the coating process, the resin composition of the present embodiment is coated on the surface of the support. The support is not particularly limited as long as it has heat resistance to the heating temperature in the subsequent film forming process (heating process) and good peeling properties in the peeling process. Examples of the support include glass substrates, such as alkali-free glass substrates; silicon wafers; resin substrates such as PET (polyethylene terephthalate), OPP (stretched polypropylene), polyethylene terephthalate, polyethylene naphthalate, polycarbonate, polyimide, polyamide-imide, polyetherimide, polyetheretherketone, polyethersulfone, polyphenylsulfone, and polyphenylene sulfide; and metal substrates such as stainless steel, alumina, copper, and nickel.
[0515] When forming a thin film of polyimide molding, a glass substrate, silicon wafer, etc. are preferred, and when forming a thick film or sheet of polyimide molding, a support formed of PET (polyethylene terephthalate), OPP (oriented polypropylene), etc. is preferred.
[0516] As coating methods, coating methods such as blade coaters, air knife coaters, roller coaters, spin coaters, flow coaters, die coaters, rod coaters, etc. can generally be listed; coating methods such as spin coating, spray coating, dip coating, etc.; printing techniques represented by screen printing and gravure printing, etc. The resin composition of this embodiment is preferably coated based on slit coating. The coating thickness should be appropriately adjusted according to the desired thickness of the resin film and the content of the polyimide precursor in the resin composition, preferably about 1 to 1,000 μm. The temperature in the coating process can be room temperature, and the resin composition can be heated to, for example, 40 to 80°C in order to reduce the viscosity and improve workability.
[0517] <Optional drying process>
[0518] The drying process can be followed by the coating process, or the drying process can be omitted and the subsequent film forming process (heating process) can be directly advanced. The drying process is carried out for the purpose of removing the organic solvent in the resin composition. In the case of the drying process, suitable devices such as a heating plate, a box-type dryer, and a conveyor-type dryer can be used. The temperature of the drying process is preferably 80 to 200° C., more preferably 100 to 150° C. The implementation time of the drying process is preferably 1 minute to 10 hours, more preferably 3 minutes to 1 hour. As above, a coating film containing a polyimide precursor is formed on the support.
[0519] 〈Film forming process〉
[0520] Next, a film forming process (heating process) is performed. The heating process is a process for removing the organic solvent contained in the above-mentioned coating film and performing an imidization reaction of the polyimide precursor in the coating film to obtain a polyimide resin film. The heating process can be performed using devices such as an inert gas oven, a hot plate, a box-type dryer, and a belt-type dryer. This process can be performed simultaneously with the drying process, or the two processes can be performed in sequence.
[0521] The heating process can be carried out under an air atmosphere, preferably in an inert gas atmosphere from the viewpoint of obtaining safety and good transparency, low thickness retardation (Rth) and low YI value of the obtained polyimide film. As inert gas, for example nitrogen, argon, etc. can be listed. The heating temperature can be appropriately set according to the type of polyimide precursor and the type of solvent in the resin composition, preferably 250°C to 550°C, more preferably 300 to 450°C. If it is more than 250°C, imidization is well performed, and if it is less than 550°C, the transparency of the obtained polyimide film can be avoided. The heat-up time is preferably about 0.1 to 10 hours.
[0522] In this embodiment, from the viewpoint of transparency and YI value of the obtained polyimide film, the oxygen concentration of the surrounding atmosphere in the above-mentioned heating step is preferably 2,000 mass ppm or less, more preferably 100 mass ppm or less, and further preferably 10 mass ppm or less. By heating in an atmosphere with an oxygen concentration of 2,000 mass ppm or less, the YI value of the obtained polyimide film can be set to 30 or less.
[0523] 〈Peeling process〉
[0524] In the peeling step, the polyimide resin film on the support is peeled off after being cooled to, for example, about room temperature (25° C.) to about 50° C. As the peeling step, for example, the following modes (1) to (4) can be mentioned.
[0525] (1) After making a structure comprising a polyimide resin film / support body by the above method, irradiating a laser from the support body side of the structure body, abrading the interface between the support body and the polyimide resin film, and thus peeling off the polyimide resin. As the type of laser, solid (YAG) laser, gas (UV excimer) laser, etc. can be listed. Preferably, a spectrum with a wavelength of 308nm or the like is used (with reference to Japanese Patent Table 2007-512568 Gazette, Japanese Patent Table 2012-511173 Gazette, etc.).
[0526] (2) Before coating the resin composition on the support, a release layer is formed on the support, and then a structure comprising a polyimide resin film / release layer / support is obtained, and the polyimide resin film is released. As the release layer, PARYLENE (registered trademark, manufactured by Japan PARYLENE Contract Co., Ltd.) and tungsten oxide can be listed, and a release agent such as a vegetable oil-based, silicone-based, fluorine-based, or alkyd-based release agent can be used (see Japanese Patent Publication No. 2010-067957, Japanese Patent Publication No. 2013-179306, etc.).
[0527] The method (2) and the laser irradiation of the method (1) may be used in combination.
[0528] (3) A method of obtaining a polyimide resin film by etching the metal using an etchant after obtaining a structure including a polyimide resin film / support using an etchant. As the metal, for example, copper (as a specific example, electrolytic copper foil "DFF" manufactured by Mitsui Mining & Smelting Co., Ltd.), aluminum, etc. can be used. As the etchant, ferric chloride, etc. can be used for copper, and dilute hydrochloric acid, etc. can be used for aluminum.
[0529] (4) After obtaining a structure including a polyimide resin film / support body by the above method, an adhesive film is attached to the surface of the polyimide resin film, the adhesive film / polyimide resin film is separated from the support body, and then the polyimide resin film is separated from the adhesive film.
[0530] Among these stripping methods, from the viewpoint of the difference in refractive index between the front and back of the obtained polyimide resin film, the YI value and the elongation, method (1) or (2) is preferred. From the viewpoint of the difference in refractive index between the front and back of the obtained polyimide resin film, method (1), i.e., an irradiation step of irradiating a laser from the support side before the stripping step, is more preferred. It should be noted that when copper is used as a support in method (3), a tendency of increasing the YI value and decreasing the elongation of the obtained polyimide resin film is observed. This is considered to be the influence of copper ions.
[0531] The thickness of the obtained polyimide film is not limited, but is preferably 1 to 200 μm, more preferably 5 to 100 μm.
[0532] 《Application of polyimide film》
[0533] The polyimide film obtained by the resin composition of the present embodiment can be used as, for example, a semiconductor insulating film, a thin film transistor liquid crystal display (TFT-LCD) insulating film, an electrode protective film, and can also be used as a transparent substrate for display devices such as a liquid crystal display, an organic electroluminescent display, a field emission display, and electronic paper. In particular, the polyimide film obtained by the resin composition of the present embodiment can be suitably used as a substrate for a thin film transistor (TFT) substrate, a color filter substrate, a touch panel substrate, and a transparent conductive film (ITO, Indium Thin Oxide) in the manufacture of a flexible device. As a flexible device to which the polyimide film in the present embodiment can be applied, for example, a TFT device for a flexible display, a flexible solar cell, a flexible touch panel, a flexible lighting, a flexible battery, a flexible printed substrate, a flexible color filter, and a surface covering lens for smartphone use can be listed.
[0534] Typically, the process of forming TFTs on a flexible substrate using a polyimide film is performed at a wide temperature range of 150 to 650° C. Specifically, when a TFT device using amorphous silicon is produced, a process temperature of 250 to 350° C. is generally required, and the polyimide film of this embodiment needs to be able to withstand this temperature, so specifically, it is necessary to appropriately select a polymer structure having a glass transition temperature or a thermal decomposition start temperature above the process temperature.
[0535] When manufacturing TFT devices using metal oxide semiconductors (IGZO, etc.), a process temperature of 320°C to 400°C is generally required. The polyimide film of this embodiment needs to be able to withstand this temperature. Therefore, it is necessary to appropriately select a polymer structure having a glass transition temperature and a thermal decomposition start temperature that are higher than the highest temperature of the TFT manufacturing process.
[0536] In the case of making a TFT device using low-temperature polysilicon (LTPS), a process temperature of 380°C to 520°C is usually required. The polyimide film of this embodiment needs to be able to withstand this temperature. Therefore, it is necessary to appropriately select a glass transition temperature and a thermal decomposition start temperature above the highest temperature of the TFT manufacturing process. On the other hand, due to these thermal histories, there is a tendency that the optical properties (especially light transmittance, delay characteristics, and YI value) of the polyimide film will decrease the more it is exposed to high-temperature processes. However, the polyimide obtained from the polyimide precursor of this embodiment has good optical properties even after a thermal history.
[0537] Hereinafter, as application examples of the polyimide film of the present embodiment, a method for producing a display and a laminate will be described.
[0538] <Method for manufacturing display>
[0539] The manufacturing method of the display of the present embodiment includes: a coating step of coating the resin composition of the present embodiment on the surface of a supporting body; a film forming step of heating the above-mentioned resin composition to form a polyimide resin film; an element forming step of forming an element on the above-mentioned polyimide resin film; and a peeling step of peeling the above-mentioned polyimide resin film on which the above-mentioned element is formed from the above-mentioned supporting body.
[0540] Manufacturing example of flexible organic EL display
[0541] Figure 1 Schematic diagram showing the structure of a top emission type flexible organic EL display as an example of the display of this embodiment above the polyimide substrate. Figure 1 The organic EL structure 25 of the embodiment is described. For example, an organic EL element 250a emitting red light, an organic EL element 250b emitting green light, and an organic EL element 250c emitting blue light are taken as one unit and arranged in a matrix, and a partition wall (bank) 251 is used to divide the light-emitting area of each organic EL element. Each organic EL element is composed of a lower electrode (anode) 252, a hole transport layer 253, a light-emitting layer 254, and an upper electrode (cathode) 255. On the lower layer 2a representing a CVD multilayer film (multilayer barrier layer) formed by silicon nitride (SiN) and silicon oxide (SiO), a plurality of TFTs 256 (selected from low-temperature polycrystalline silicon (LTPS), metal oxide semiconductor (IGZO, etc.)) for driving the organic EL element, an interlayer insulating film 258 having a contact hole 257, and a lower electrode 259 are provided. The organic EL element is sealed by a sealing substrate 2b, and a hollow portion 261 is formed between each organic EL element and the sealing substrate 2b.
[0542] The manufacturing process of the flexible organic EL display includes: making a polyimide film on a glass substrate support, and making a Figure 1 The process of manufacturing the organic EL substrate shown in the figure; the process of manufacturing the sealing substrate; the assembly process of bonding the two substrates together; and the peeling process of peeling the organic EL display made on the polyimide film from the glass substrate support. The organic EL substrate manufacturing process, the sealing substrate manufacturing process and the assembly process can apply known manufacturing processes. An example thereof is listed below, but it is not limited to this. The peeling process is the same as the peeling process of the polyimide film mentioned above.
[0543] For example, if you refer to Figure 1First, a polyimide film is prepared on a glass substrate support by the above method, and a multilayer barrier layer (SiN) formed of a multilayer structure of silicon nitride (SiN) and silicon oxide (SiO) is prepared on the top thereof by a CVD method or a sputtering method. Figure 1 The lower substrate 2a in the middle is used to make a metal wiring layer for driving TFT on its upper part using photoresist or the like. An active buffer layer such as SiO is made on its upper part using CVD method, and a TFT device such as metal oxide semiconductor (IGZO) or low temperature polycrystalline silicon (LTPS) is made on its upper part ( Figure 1 After the TFT substrate for the flexible display is manufactured, an interlayer insulating film 258 having a contact hole 257 is formed by using a photosensitive acrylic resin or the like. An ITO film is formed by a sputtering method or the like to form a lower electrode 259 in a manner matching the TFT.
[0544] Next, after forming a partition wall (bank) 251 using photosensitive polyimide or the like, a hole transport layer 253 and a light-emitting layer 254 are formed in each space divided by the partition wall. An upper electrode (cathode) 255 is formed so as to cover the light-emitting layer 254 and the partition wall (bank) 251. Thereafter, an organic EL material (which is the same as the red light) emitting layer is evaporated using a known method using a fine metal mask or the like as a mask. Figure 1 The organic EL element 250a emitting red light in the embodiment corresponds to the organic EL element 250a emitting red light), the organic EL material emitting green light (corresponding to the organic EL element 250a emitting red light in the embodiment Figure 1 The organic EL element 250b emitting green light in the embodiment corresponds to the organic EL element 250b emitting green light and the organic EL material emitting blue light (corresponding to Figure 1 The organic EL substrate is manufactured by using a sealing film, etc. ( Figure 1 The organic EL substrate is sealed by using the sealing substrate 2b in the embodiment, and the device above the polyimide substrate is peeled off from the glass substrate support by a known peeling method such as laser peeling, thereby making a top-emitting flexible organic EL display. When the polyimide of this embodiment is used, a transparent (see-through) flexible organic EL display can be made. A bottom-emitting flexible organic EL display can also be made by a known method.
[0545] Manufacturing example of flexible liquid crystal display
[0546] The polyimide film of this embodiment can be used to make a flexible liquid crystal display. As a specific production method, a polyimide film is produced on a glass substrate support using the above method, and a TFT substrate formed of, for example, amorphous silicon, a metal oxide semiconductor (IGZO, etc.) and low-temperature polycrystalline silicon is produced using the above method. Separately, according to the coating process and film forming process of this embodiment, a polyimide film is produced on a glass substrate support, and a color filter glass substrate (CF substrate) having a polyimide film is produced according to a known method and using a color photoresist, etc. On one of the TFT substrate and the CF substrate, a sealing material including a thermosetting epoxy resin or the like is applied by screen printing into a partially defective frame pattern of a liquid crystal injection port, so that the other substrate maintains a diameter equivalent to the thickness of the liquid crystal layer, and spherical spacers formed of plastic or silicon dioxide are dispersed.
[0547] Next, the TFT substrate and the CF substrate are bonded together to solidify the sealing material. Furthermore, a liquid crystal material is injected into the space surrounded by the TFT substrate, the CF substrate and the sealing material by a decompression method, a thermosetting resin is applied to the liquid crystal injection port, and the liquid crystal material is sealed by heating to form a liquid crystal layer. Finally, the glass substrate on the CF side and the glass substrate on the TFT side are peeled off at the interface between the polyimide film and the glass substrate by a laser lift-off method, etc., thereby making a flexible liquid crystal display.
[0548] <Method for producing laminate>
[0549] The method for manufacturing the laminate of the present embodiment includes: a coating step of coating the resin composition of the present embodiment on the surface of a support; a film forming step of heating the resin composition to form a polyimide resin film; and an element forming step of forming an element on the polyimide resin film.
[0550] As the element in the laminate, the elements exemplified in the manufacture of the above-mentioned flexible device can be cited. As the support, for example, a glass substrate can be used. The preferred specific steps of the coating process and the film-forming process are the same as those described for the method for manufacturing the above-mentioned polyimide film. In the element forming process, the above-mentioned element is formed on the polyimide resin film as a flexible substrate formed on the support. Thereafter, the polyimide resin film and the element can be optionally peeled off from the support in the peeling process.
[0551] Example
[0552] Hereinafter, although embodiment of this invention is demonstrated concretely by an Example and a comparative example, this invention is not limited to these Examples and comparative examples.
[0553] [First method]
[0554] 《Measurement and evaluation methods》
[0555] 〈Weight average molecular weight〉
[0556] The weight average molecular weight (Mw) and the number average molecular weight (Mn) were measured by gel permeation chromatography (GPC) under the following conditions.
[0557] As a solvent, NMP (manufactured by Wako Pure Chemical Industries, Ltd., for high performance liquid chromatography, obtained by adding and dissolving 24.8 mmol / L of lithium bromide monohydrate (manufactured by Wako Pure Chemical Industries, Ltd., purity 99.5%) and 63.2 mmol / L of phosphoric acid (manufactured by Wako Pure Chemical Industries, Ltd., for high performance liquid chromatography) immediately before measurement) was used. A calibration curve for calculating the weight average molecular weight was prepared using standard polystyrene (manufactured by Tosoh Corporation).
[0558] Column: Shodex KD-806M (Showa Denko Co., Ltd.)
[0559] Flow rate: 1.0mL / min
[0560] Column temperature: 40°C
[0561] Pump: PU-2080Plus (manufactured by JASCO)
[0562] Detector: RI-2031 Plus (RI: differential refractometer, manufactured by JASCO) and UV-2075 Plus (UV-VIS: ultraviolet visible spectrophotometer, manufactured by JASCO)
[0563] <Evaluation of Viscosity Stability of Composition (Varnish)>
[0564] The resin compositions prepared in the examples and comparative examples were placed in an atmosphere of 23°C and 50% RH for 24 hours, and the initial (0-day) viscosity of the resin compositions was measured using a viscometer with a temperature controller (VISCOMATER TVE-35H manufactured by Toki Sangyo Co., Ltd.). In addition, the resin compositions were placed in an atmosphere of 23°C and 50% RH for 10 days, and the viscosity was measured after 10 days in the same manner as at the beginning. Next, the viscosity stability shown in the following formula was calculated.
[0565] Viscosity stability (% / day) = |(initial viscosity (mPa·s)) - (viscosity after 10 days (mPa·s)) | / (initial viscosity (mPa·s)) × 100 / 10 (day)
[0566] The viscosity stability was evaluated according to the following criteria.
[0567] A: Viscosity stability is below 2% / day, "Excellent"
[0568] B: Viscosity stability is more than 4% / day and less than 7% / day "good"
[0569] C: Viscosity stability is more than 6% / day and less than 10% / day "OK"
[0570] D: Viscosity stability over 8% / day "OK"
[0571] <Evaluation of Filterability of Composition (Varnish)>
[0572] The resin compositions prepared in the examples and comparative examples were filtered under pressure at 23°C and 50% RH using a polyethylene membrane filter having a size of 900 mmφ and a unit area weight of 0.2 μm at a pressure of 0.25 MPa. The mass of the resin composition filtered out at this time was measured and the filtration rate was calculated. The filterability was evaluated according to the following criteria.
[0573] A: Filtration rate is above 1700g / hr "Excellent"
[0574] B: Filtration rate is less than 1700 g / hr and above 1500 g / hr "good"
[0575] C: Filtration rate is less than 1500g / hr and above 500g / hr "OK"
[0576] D: Filtration rate less than 500g / hr "Not allowed"
[0577] <Evaluation of Tensile Elongation of Polyimide Resin Film>
[0578] As a support, a 6-inch silicon wafer substrate with an aluminum vapor-deposited layer on the surface is used, and the resin composition prepared in the embodiment and the comparative example is spin-coated on the surface of the aluminum vapor-deposited layer in a manner that the film thickness of the polyimide resin film becomes 10 μm to form a coating. After the coating is pre-baked at 100° C. for 6 minutes, a vertical curing furnace (Koyo Thermo System Co., Ltd., model name "VF-2000B") in which the oxygen concentration in the warehouse is adjusted to less than 10 mass ppm is used, and heated at 400° C. for 1 hour to form a polyimide film on the wafer. Then, a dicing saw (DISCO Co., Ltd., product name "DAD 3350") is used to scratch the obtained polyimide film into a 3 mm wide scratch, and then the wafer with the polyimide film is immersed in a dilute hydrochloric acid aqueous solution for one night, and the polyimide film sheet is peeled off and dried to obtain a 3 mm wide polyimide sheet. It is cut into 50 mm long to obtain a 3 mm wide and 50 mm long polyimide measurement sample. The tensile elongation of the polyimide resin film was measured using TENSILON (Orientec Corporation, model name "UTM-II-20") at a test speed of 40 mm / min and an initial load of 0.5 fs. The tensile elongation was evaluated according to the following criteria.
[0579] A: Tensile elongation over 40% "Excellent"
[0580] B: Tensile elongation is more than 30% and less than 40% "good"
[0581] C: Tensile elongation is more than 20% and less than 30% "OK"
[0582] D: Tensile elongation less than 20% "Not allowed"
[0583] <Evaluation of Residual Stress of Polyimide Resin Film>
[0584] The resin composition prepared in the embodiment and the comparative example was applied to a 6-inch silicon wafer with a thickness of 625 μm ± 25 μm and a pre-measured "warpage amount" using a spin coater, and pre-baked at 100° C. for 7 minutes. Thereafter, a vertical curing furnace (manufactured by Koyo Lindberg, model name: VF-2000B) was used to adjust the oxygen concentration in the chamber to 10 mass ppm or less, and a heat curing treatment (curing treatment) was performed at 400° C. for 1 hour to produce a silicon wafer with a polyimide resin film having a film thickness of 10 μm after curing.
[0585] The amount of warpage of the wafer was measured using a residual stress measuring device (manufactured by Tencor Corporation, model name: FLX-2320), and the residual stress generated between the silicon wafer and the resin film “under a nitrogen atmosphere” was evaluated.
[0586] A: Residual stress is less than 35MPa "good"
[0587] B: Residual stress is above 35MPa and less than 45MPa "OK"
[0588] C: Residual stress is 45MPa or above "Not allowed"
[0589] <Ratio of Silicon-Containing Compounds in All Resins>
[0590] The ratio (mass %) of the silicon-containing compound in the total mass of all resins in the resin composition of Examples / Comparative Examples was calculated as follows.
[0591] Ratio of silicon-containing compound (mass %) = mass of silicon-containing compound (g) / total mass of each monomer (acid dianhydride monomer, diamine monomer, silicon-containing compound) (g) × 100
[0592] The ratio of the silicon-containing compound can be determined by the following method using a varnish.
[0593] An appropriate amount of water is added to the varnish, and a heating treatment is performed at 80°C for 3 days to depolymerize the acid component, the amine component, and the depolymerization component to produce an acid monomer and an amine monomer. Thereafter, the solvent is distilled off to obtain a powder mixed with the acid monomer and the amine monomer, and an acetonitrile solution is prepared and measured by high performance liquid chromatography mass spectrometry (LC / MS). In addition, the peak area of each monomer can be calculated based on the peak area ratio.
[0594] <Imidization rate>
[0595] The imidization ratio (%) of the resin of Examples / Comparative Examples was calculated as follows.
[0596] (When L1 and L2 in the general formula (10) are amino groups)
[0597] Imidization rate (%) =
[0598] Total moles of diamine monomers (including silicon-containing compounds in which L1 and L2 of the general formula (10) are amino groups) in the imidization step / {total moles of diamine monomers (including silicon-containing compounds in which L1 and L2 of the general formula (10) are amino groups) in the imidization step + total moles of diamine monomers (including silicon-containing compounds in which L1 and L2 of the general formula (10) are amino groups) in the amidation step}×100
[0599] For example, in the case of Example I-1,
[0600] Total molar number of diamine monomers (including silicon-containing compounds in which L1 and L2 of the general formula (10) are amino groups) in the imidization step: 93.6 mmol
[0601] Total molar number of diamine monomers (including silicon-containing compounds in which L1 and L2 of the general formula (10) are amino groups) in the amidation step: 111.9 mmol
[0602] The imidization rate was 83.7%.
[0603] (When L1 and L2 in the general formula (10) are anhydride groups)
[0604] Imidization rate (%) =
[0605] Total moles of acid dianhydride monomers (including silicon-containing compounds in which L1 and L2 of the general formula (10) are acid anhydride groups) in the imidization step / {total moles of acid anhydride monomers (including silicon-containing compounds in which L1 and L2 of the general formula (10) are acid anhydride groups) in the imidization step + total moles of acid dianhydride monomers (including silicon-containing compounds in which L1 and L2 of the general formula (10) are acid anhydride groups) in the amidation step}×100
[0606] In addition, the imidization ratio can be determined by the following method using a varnish.
[0607] An appropriate amount of water is added to the varnish, and a heating treatment is performed at 80°C for 3 days to depolymerize the acid component, the amine component, and the depolymerization component to produce an acid monomer and an amine monomer. Thereafter, the solvent is distilled off to obtain a powder mixed with the acid monomer and the amine monomer, and an acetonitrile solution is prepared and measured by high performance liquid chromatography mass spectrometry (LC / MS). In addition, the peak area of each monomer can be calculated based on the peak area ratio.
[0608] In addition, the imidization rate can also be measured using an IR (infrared spectrophotometer). After the varnish is reprecipitated using an aqueous solvent, the powder is separated and dried, and then KBr is added to form a pellet, which is used as a sample. In addition, the infrared absorption spectrum of the resin layer is measured using a single reflection ATR method, so that the infrared absorption spectrum of the resin layer can be measured at 1009 cm -1 The benzene ring carbon-hydrogen bond is used as the benchmark, according to 1778cm -1 Here, the imidization rate of the polyimide film after the varnish was heat-treated at 400° C. for 1 hour was set to 100%.
[0609] <Difference between the ratio of imide units and amide units of silicon-containing compounds in diamine>
[0610] The difference between the imide unit and the amide unit in the ratio of the silicon-containing compound in the diamine of the resin of the Examples and Comparative Examples was determined according to the following formula.
[0611] A: Ratio of silicon-containing compound in diamine of imide unit (mass %) = silicon-containing compound used in imidization step / total mass of diamine monomer (including silicon-containing compound) used in imidization step × 100
[0612] B: Ratio of silicon-containing compound in diamine of amide unit (mass %) = total mass of silicon-containing compound used in imidization step / mass of diamine monomer (including silicon-containing compound) used in amidation step × 100
[0613] A may also be referred to as "the ratio (mass %) of the diamine of the general formula (10) in the diamine constituting P5 in the general formula (7)".
[0614] In addition, B can also be referred to as "the ratio (mass %) of the diamine of the general formula (10) in the diamine constituting P3 in the general formula (6)".
[0615] In addition, regarding the ratio of the silicon-containing compound in the diamine, the difference between the imide unit and the amide unit is shown as "BA".
[0616] Table 5 shows the BA values of Examples I-14, I-16, I-17, and Comparative Examples I-4 to I-6, and the properties of the varnishes and polyimide films thereof.
[0617] 《Example I-1》
[0618] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (189 g) as a solvent, toluene (19 g), DABA (73.0 mmol, 11.1 g) as a diamine, and a silicon-containing compound (2) (6.699 mmol, 10.72 g) were added while stirring as described in Tables 1 and 2, and then CpODA (38.4 g) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 160°C, and reflux was heated at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was restored to room temperature. Then, DABA (18.3 mmol, 2.8 g) as a diamine was added while stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution (hereinafter also referred to as varnish) of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0619] 《Example I-2》
[0620] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (191 g) as a solvent, toluene (19 g), DABA (13.6 g) as a diamine, and a silicon-containing compound (1) (10.82 g) were added while stirring as described in Tables 1 and 2, and then CpODA (38.4 g) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 160°C, and refluxed at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was restored to room temperature. Then, DABA (0.7 g) as a diamine was added while stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0621] 《Example I-3》
[0622] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (191 g) as a solvent, toluene (19 g), DABA (7.3 g) as a diamine, and a silicon-containing compound (3) (10.85 g) were added while stirring as described in Tables 1 and 2, and then CpODA (38.4 g) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 160°C, and refluxed at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was restored to room temperature. Then, DABA (7.3 g) as a diamine was added while stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0623] 《Example I-4》
[0624] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (191 g) as a solvent, toluene (19 g), DABA (8.7 g) as a diamine, and a silicon-containing compound (4) (10.85 g) were added while stirring as described in Tables 1 and 2, and then CpODA (38.4 g) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 160°C, and refluxed at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was restored to room temperature. Then, DABA (5.8 g) as a diamine was added while stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0625] 《Example I-5》
[0626] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (186 g) as a solvent, toluene (19 g), and DABA (14.9 g) as a diamine were added while stirring as described in Tables 1 and 2, and then CpODA (32.8 g) as an acid dianhydride and a silicon-containing compound (5) (10.51 g) were added at room temperature. Thereafter, the internal temperature was raised to 160°C, and reflux was heated at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was restored to room temperature. Then, CpODA (3.6 g) as an acid dianhydride was added while stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0627] 《Example I-6》
[0628] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (184 g), toluene (18 g), DABA (12.9 g) as a diamine, and silicon-containing compound (1) (10.44 g) as a solvent were added while stirring as described in Tables 1 and 2, and then CpODA (28.8 g) and ODPA (7.8 g) as acid dianhydrides were added at room temperature. Thereafter, the internal temperature was raised to 160°C, and refluxed at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was restored to room temperature. Then, DABA (1.4 g) as a diamine was added while stirring. The molar ratio of acid dianhydride to diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0629] 《Example I-7》
[0630] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (194 g), toluene (19 g), DABA (11.1 g) as a diamine, and a silicon-containing compound (2) (11.02 g) as a solvent were added while stirring as described in Tables 1 and 2, and then CpODA (28.8 g) and 6FDA (11.1 g) as an acid dianhydride were added at room temperature. Thereafter, the internal temperature was raised to 160°C, and refluxed at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was restored to room temperature. Then, DABA (2.8 g) as a diamine was added while stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0631] 《Example I-8》
[0632] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (197 g), toluene (20 g), DABA (8.6 g) as a diamine, and silicon-containing compound (1) (11.19 g) as a solvent were added while stirring as described in Tables 1 and 2, and then CpODA (28.8 g) and BPAF (11.5 g) as acid dianhydrides were added at room temperature. Thereafter, the internal temperature was raised to 160°C, and reflux was heated at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was restored to room temperature. Then, DABA (5.7 g) as a diamine was added while stirring. The molar ratio of acid dianhydride to diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0633] 《Example I-9》
[0634] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (193 g), toluene (19 g), DABA (7.2 g) as a diamine, and silicon-containing compound (1) (10.92 g) as a solvent were added while stirring as described in Tables 1 and 2, and then CpODA (28.8 g) and BzDA (10.1 g) as acid dianhydrides were added at room temperature. Thereafter, the internal temperature was raised to 160°C, and refluxed at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was restored to room temperature. Then, DABA (7.2 g) as a diamine was added while stirring. The molar ratio of acid dianhydride to diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0635] 《Example I-10》
[0636] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (170 g), toluene (17 g), DABA (13.3 g) as a diamine, and silicon-containing compound (2) (9.62 g) as a solvent were added while stirring as described in Tables 1 and 2, and then CpODA (28.8 g) and BNBDF (4.1 g) as acid dianhydride were added at room temperature. Thereafter, the internal temperature was raised to 160°C, and refluxed at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was restored to room temperature. Then, DABA (0.7 g) as a diamine was added while stirring. The molar ratio of acid dianhydride to diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0637] 《Example I-11》
[0638] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (204 g) as a solvent, toluene (20 g), DABA (10.3 g) as a diamine, BAFL (5.9 g), and a silicon-containing compound (1) (11.57 g) were added while stirring as described in Tables 1 and 2, and then CpODA (38.4 g) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 160°C, and reflux was heated at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was returned to room temperature. Then, DABA (1.1 g) and BAFL (0.7 g) as diamines were added while stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0639] 《Example I-12》
[0640] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (202 g) as a solvent, toluene (20 g), DABA (5.5 g) as a diamine, BisAM (3.1 g), and a silicon-containing compound (2) (11.42 g) were added while stirring as described in Tables 1 and 2, and then CpODA (38.4 g) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 160°C, and refluxed at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was returned to room temperature. Then, DABA (5.5 g) and BisAM (3.1 g) as diamines were added while stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0641] 《Example I-13》
[0642] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (218 g) as a solvent, toluene (22 g), DABA (5.9 g) as a diamine, BAFL (9.4 g), and a silicon-containing compound (1) (12.35 g) were added while stirring as described in Tables 1 and 2, and then CpODA (38.4 g) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 160°C, and reflux was heated at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was returned to room temperature. Then, DABA (2.5 g) and BAFL (4.0 g) as diamines were added while stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0643] Comparative Example I-1
[0644] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (208 g) as a solvent, toluene (21 g), DABA (10.22 g) and TFMB (16.0 g) as a diamine were added while stirring as described in Tables 1 and 2, and then CpODA (27.7 g), BPDA (5.3 g) and a silicon-containing compound (6) (9.95 g) as an acid dianhydride were added at room temperature. The molar ratio of the acid dianhydride to the diamine was 100:100. Thereafter, the internal temperature was raised to 160°C, and reflux was heated at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After 12 hours of reaction, the oil bath was removed and the temperature was restored to room temperature to obtain an NMP solution of a polyimide resin (functional groups other than silicon-containing compounds: imide groups; functional groups of silicon-containing compounds: imide groups). The obtained varnish was stored in a freezer (set to -20°C, the same below) and thawed for use in evaluation.
[0645] Comparative Examples I-2, I-3
[0646] In Comparative Example I-1, except that the types and amounts of the solvent, the acid dianhydride, and the diamine were changed to those described in Tables 1 and 2, the same procedures as in Comparative Example I-1 were carried out.
[0647] 《Example I-14》
[0648] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod, nitrogen was introduced, and NMP (177 g) as a solvent, toluene (18 g), a silicon-containing compound (2) (4.12 g), 33DAS (8.5 g), and 44DAS (12.8 g) as diamines were added with stirring as described in Tables 3 and 4, and then ODPA (31.0 g) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 160°C, and reflux was performed at 160°C for 1 hour to perform imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while toluene was removed. After the reaction for 12 hours, the oil bath was removed and the temperature was returned to room temperature. Then, 33DAS (0.9 g) and 44DAS (1.4 g) as diamines were added with stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0649] 《Example I-15》
[0650] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod, nitrogen was introduced, and NMP (170 g) as a solvent, toluene (17 g), a silicon-containing compound (2) (1.70 g), 33DAS (8.7 g), and 44DAS (13.0 g) as diamines were added with stirring as described in Tables 3 and 4, and then ODPA (31.0 g) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 160°C, and reflux was performed at 160°C for 1 hour to perform imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was returned to room temperature. Then, 33DAS (1.0 g) and 44DAS (1.4 g) as diamines were added with stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0651] 《Example I-16》
[0652] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (204 g), toluene (20 g), a silicon-containing compound (2) (16.36 g), and DABA (12.0 g) as a solvent were added while stirring as described in Tables 3 and 4, and then CpODA (38.4 g) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 160°C, and refluxed at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was restored to room temperature. Then, DABA (1.3 g) as a diamine was added while stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0653] 《Example I-17》
[0654] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (259 g), toluene (26 g), a silicon-containing compound (1) (15.54 g), and BAFL (29.1 g) as a solvent were added while stirring as described in Tables 3 and 4, and then CpODA (38.4 g) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 160°C, and reflux was heated at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was restored to room temperature. Then, BAFL (3.2 g) as a diamine was added while stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0655] 《Example I-18》
[0656] Into a separable flask equipped with a Dean-Stark tube and a reflux tube and a stirring rod, nitrogen was introduced, and NMP (232 g) as a solvent, toluene (23 g), silicon-containing compound (1) (7.73 g), 33DAS (8.5 g), and 44DAS (12.8 g) as diamines were added with stirring as shown in Tables 3 and 4, and then BPAF (45.8 g) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 160°C, and reflux was performed at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was returned to room temperature. Then, 33DAS (0.9 g) and 44DAS (1.4 g) as diamines were added with stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0657] 《Example I-19》
[0658] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (235 g), toluene (24 g), a silicon-containing compound (1) (7.84 g), and 6FODA (28.9 g) as a solvent were added while stirring as described in Tables 3 and 4, and then CpODA (38.4 g) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 160°C, and reflux was heated at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was restored to room temperature. Then, 6FODA (3.2 g) as a diamine was added while stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: imide group).
[0659] Comparative Example I-4
[0660] As described in Tables 3 and 4, BPADA 200 g (0.384 mol) was dispersed in 1101 g of 1,2-bis (2-methoxyethoxy) ethane (triethylene glycol dimethyl ether) and maintained at 80°C. 172 g (0.115 mol) of the silicon-containing compound X-22-9409 (manufactured by Shin-Etsu Chemical Co., Ltd., two ends: amino, functional group equivalent: 670) was added thereto and stirred evenly for 30 minutes. Then, it was heated to 140°C and stirred for 1 hour. After the reaction was completed, the temperature was raised to 180°C and heated to reflux for 3 hours. After the reaction was completed, it was cooled to room temperature and 27.7 g (1.54 mol) of water was added. After uniform stirring for 30 minutes, it was heated to 80°C and heated to reflux for 3 hours. In this way, a solution in which imidized tetracarboxylic acid (terminal tetracarboxylic acid siloxane imide oligomer) was dissolved was obtained.
[0661] Next, the solution was cooled to room temperature, 99.7 g (0.230 mol) of mBAPS was added, and the mixture was uniformly stirred at room temperature for 1 hour to obtain a resin composition solution.
[0662] Comparative Example I-5
[0663] As described in Tables 3 and 4, a nitrogen inlet tube, a thermometer, and a spherical condenser equipped with a moisture separation collector were installed in a three-necked separable flask. 15 g of triethylene glycol dimethyl ether (triglyme), 35 g of γ-butyrolactone (GBL), 20.0 g of toluene, and 10.86 g (35.00 mmol) of ODPA were added at room temperature of 25°C and stirred until uniform. Thereafter, the temperature was raised to 80°C, and 11.30 g (13.78 mmol) of a silicon-containing compound KF-8010 (manufactured by Shin-Etsu Chemical Co., Ltd., both ends: amino groups, functional group equivalent: 430) was added. After further stirring for 0.5 hours, the temperature was raised to 170°C and heated for 4 hours. During the reaction, the by-produced water and toluene were azeotropically co-existed, and dehydration was performed under reflux using a spherical condenser equipped with a moisture separation collector. After removing the by-produced water, the reflux was stopped and all the toluene was removed. After cooling the system to 100° C., 0.14 g of maleic anhydride was added, followed by stirring for 0.5 hours.
[0664] The mixture was left to stand at room temperature of 25°C for 12 hours and then cooled, and then 6.00 g (20.52 mmol) of APB was added to obtain a resin composition.
[0665] Comparative Example I-6
[0666] As shown in Tables 3 and 4, 27.0 g (0.0802 mol) of 6FODA and 56.000 g of NMP were added to a 500 mL 5-necked round-bottom flask equipped with a stainless steel half-moon-shaped stirring blade, a nitrogen inlet pipe, a Dean Stark equipped with a condenser, a thermometer, and a glass tube end cap, and stirred at a temperature of 70° C. in the system, at a nitrogen atmosphere, and at a rotation speed of 200 rpm to obtain a solution.
[0667] After adding CpODA19.2g (0.050 mol) and NMP 14.000g to the solution, 0.253g of TEA as an imidization catalyst was added, and the temperature in the reaction system was raised to 190°C in about 20 minutes by heating with a hood heater. The distilled components were captured, the rotation speed was adjusted as the viscosity increased, and the temperature in the reaction system was maintained at 190°C and refluxed for 1 hour. Thereafter, 85.806g of NMP was added, and the temperature in the reaction system was cooled to 50°C to obtain a solution containing an oligomer having an imide repeating structural unit.
[0668] 9.7 g (0.033 mol) of BPDA and 7.527 g of NMP were added to the obtained solution, and the mixture was stirred at 50° C. for 5 hours. Thereafter, 100.000 g of NMP was added and homogenized, and then a mixed solution of 13.2 g (0.003 mol) of X-22-1660B-3 (modified silicone oil, functional group equivalent: 2200, Shin-Etsu Chemical Co., Ltd.) dissolved in 16.667 g of NMP was added, and the mixture was stirred for about 1 hour to obtain an NMP solution (hereinafter also referred to as varnish) of a partially imidized polyimide precursor (functional groups other than silicon-containing compounds: amide groups or imide groups; functional groups of silicon-containing compounds: amide groups).
[0669] The viscosity stability and filterability were evaluated using the resin compositions of Examples and Comparative Examples, and the tensile elongation and residual stress were evaluated using the obtained polyimide resin films. The evaluation results are shown in Tables 1 to 4.
[0670] The abbreviations in Examples and Comparative Examples are as follows.
[0671] 〈Acid dianhydride〉
[0672] CpODA: Compound of the following general formula
[0673]
[0674] ODPA: 4,4'-oxydiphthalic anhydride
[0675] 6FDA: 4,4'-(hexafluoroisopropylidene) diphthalic anhydride
[0676] BPAF: 9,9-bis(3,4-dicarboxyphenyl)fluorene anhydride
[0677] BzDA: a compound of the following general formula
[0678]
[0679] BNBDA: a compound of the following general formula
[0680]
[0681] BPADA: 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (diamine)
[0682] DABA: 3,5-diaminobenzoic acid
[0683] 3,3'-Diaminodiphenyl sulfone (33DAS)
[0684] 4,4'-Diaminodiphenylsulfone (44DAS)
[0685] BAFL: 9,9-bis(4-aminophenyl)fluorene
[0686] BisAM: a compound of the following general formula
[0687]
[0688] TFMB: diaminobis(trifluoromethyl)biphenyl
[0689] BAPP: Compound of the following general formula
[0690]
[0691] mBAPS: bis[4-(3-aminophenoxy)phenyl]sulfone
[0692] APB: 1,3-bis(3-aminophenoxy)benzene
[0693] 〈Silicon-containing compounds〉
[0694] Silicon-containing compound (1): (in the general formula (10), L1 and L2 are amino groups (-NH2), R1 is a trimethylene group (-CH2CH2CH2-), R2 and R3 are methyl groups, j and k are 0, and the functional group equivalent is 1500)
[0695] Silicon-containing compound (2): (in the general formula (10), L1 and L2 are amino groups (-NH2), R1 is trimethylene (-CH2CH2CH2-), R2 and R3 are methyl groups, j and k are 0, and the functional group equivalent is 800)
[0696] Silicon-containing compound (3): (in the general formula (10), L1 and L2 are amino groups (-NH2), R1 is trimethylene (-CH2CH2CH2-), R2 and R3 are methyl groups, j and k are 0, and the functional group equivalent is 2200)
[0697] Silicon-containing compound (4): In the general formula (10), L1 and L2 are amino groups, R1 is -CH2CH2CH2-, R2, R3, R6, and R7 are methyl groups, R4 and R5 are phenyl groups, j / (i+j+k)=0.15, and the functional group equivalent is 2200
[0698] Silicon-containing compound (5): (in the general formula (10), L1 and L2 are anhydride groups (-CH(C=O)2O), R1 is a trimethylene group (-CH2CH2CH2-), R2 and R3 are methyl groups, j and k are 0, and the functional group equivalent is 1000)
[0699] Silicon-containing compound (6): (in the general formula (10), L1 and L2 are anhydride groups (-CH(C=O)2O), R1 is a trimethylene group (-CH2CH2CH2-), R2 and R3 are methyl groups, j and k are 0, and the functional group equivalent is 500) [Table 1]
[0700]
[0701] [Table 2]
[0702]
[0703] [Table 3]
[0704]
[0705] [Table 4]
[0706]
[0707] [Table 5]
[0708]
[0709] [Second Method]
[0710] 《Measurement and evaluation methods》
[0711] 〈Weight average molecular weight〉
[0712] The weight average molecular weight (Mw) and the number average molecular weight (Mn) were measured by gel permeation chromatography (GPC) under the following conditions.
[0713] As a solvent, NMP (manufactured by Wako Pure Chemical Industries, Ltd., for high performance liquid chromatography, obtained by adding and dissolving 24.8 mmol / L of lithium bromide monohydrate (manufactured by Wako Pure Chemical Industries, Ltd., purity 99.5%) and 63.2 mmol / L of phosphoric acid (manufactured by Wako Pure Chemical Industries, Ltd., for high performance liquid chromatography) immediately before measurement) was used. A calibration curve for calculating the weight average molecular weight was prepared using standard polystyrene (manufactured by Tosoh Corporation).
[0714] Column: Shodex KD-806M (Showa Denko Co., Ltd.)
[0715] Flow rate: 1.0mL / min
[0716] Column temperature: 40°C
[0717] Pump: PU-2080Plus (manufactured by JASCO)
[0718] Detector: RI-2031 Plus (RI: differential refractometer, manufactured by JASCO) and UV-2075 Plus (UV-VIS: ultraviolet visible spectrophotometer, manufactured by JASCO)
[0719] <Evaluation of Viscosity Stability of Composition (Varnish)>
[0720] The resin compositions prepared in the examples and comparative examples were placed in an atmosphere of 23°C and 50% RH for 24 hours, and the initial (0-day) viscosity of the resin compositions was measured using a viscometer with a temperature controller (VISCOMATER TVE-35H manufactured by Toki Sangyo Co., Ltd.). In addition, the resin compositions were placed in an atmosphere of 23°C and 50% RH for 7 days, and the viscosity was measured after 7 days in the same manner as at the beginning. Next, the viscosity stability shown in the following formula was calculated.
[0721] Viscosity stability (% / day) = |(initial viscosity (mPa·s)) - (viscosity after 7 days (mPa·s)) | / (initial viscosity (mPa·s)) × 100 / 7 (day)
[0722] The viscosity stability was evaluated according to the following criteria.
[0723] A: Viscosity stability is below 1% / day, "Excellent"
[0724] B: Viscosity stability is more than 1% / day and less than 3% / day "good"
[0725] C: Viscosity stability is more than 3% / day and less than 5% / day "OK"
[0726] D: Viscosity stability over 5% / day "OK"
[0727] <Evaluation of Filterability of Composition (Varnish)>
[0728] The resin compositions prepared in the examples and comparative examples were filtered under pressure at 23°C and 50% RH using a polyethylene membrane filter having a size of 900 mmφ and a unit area weight of 0.2 μm at a pressure of 0.25 MPa. The mass of the resin composition filtered out at this time was measured and the filtration rate was calculated. The filterability was evaluated according to the following criteria.
[0729] A: Filtration rate is above 2000g / hr "Excellent"
[0730] B: Filtration rate is less than 2000g / hr and above 1500g / hr "good"
[0731] C: Filtration rate is less than 1500g / hr and above 1000g / hr "OK"
[0732] D: Filtration rate less than 1000g / hr "Not allowed"
[0733] <Evaluation of Tensile Elongation of Polyimide Resin Film>
[0734] As a support, a 6-inch silicon wafer substrate with an aluminum vapor-deposited layer on the surface is used, and the resin composition prepared in the embodiment and the comparative example is spin-coated on the surface of the aluminum vapor-deposited layer in a manner that the film thickness of the polyimide resin film becomes 10 μm to form a coating. After the coating is pre-baked at 100° C. for 6 minutes, a vertical curing furnace (Koyo Thermo System Co., Ltd., model name "VF-2000B") in which the oxygen concentration in the warehouse is adjusted to less than 10 mass ppm is used to heat at 400° C. for 1 hour to form a polyimide film on the wafer. Then, a dicing saw (DISCO Co., Ltd., product name "DAD 3350") is used to scratch the obtained polyimide film into a 3 mm wide scratch, and then the wafer with the polyimide film is immersed in a dilute hydrochloric acid aqueous solution for one night, and the polyimide film sheet is peeled off and dried to obtain a 3 mm wide polyimide sheet. It is cut into 50 mm long to obtain a 3 mm wide and 50 mm long polyimide measurement sample. The tensile elongation of the polyimide resin film was measured using TENSILON (Orientec Corporation, model name "UTM-II-20") at a test speed of 40 mm / min and an initial load of 0.5 fs. The tensile elongation was evaluated according to the following criteria.
[0735] A: Tensile elongation over 50% "Excellent"
[0736] B: Tensile elongation is more than 40% and less than 50% "good"
[0737] C: Tensile elongation is more than 30% and less than 40% "OK"
[0738] D: Tensile elongation less than 30% "Not allowed"
[0739] <Evaluation of Residual Stress of Polyimide Resin Film>
[0740] The resin composition prepared in the embodiment and the comparative example was applied to a 6-inch silicon wafer with a thickness of 625 μm ± 25 μm and a pre-measured "warpage amount" using a spin coater, and pre-baked at 100° C. for 7 minutes. Thereafter, a vertical curing furnace (manufactured by Koyo Lindberg, model name: VF-2000B) was used to adjust the oxygen concentration in the chamber to 10 mass ppm or less, and a heat curing treatment (curing treatment) was performed at 400° C. for 1 hour to produce a silicon wafer with a polyimide resin film having a film thickness of 10 μm after curing.
[0741] The amount of warpage of the wafer was measured using a residual stress measuring device (manufactured by Tencor Corporation, model name: FLX-2320), and the residual stress generated between the silicon wafer and the resin film “under a nitrogen atmosphere” was evaluated.
[0742] A: Residual stress is less than 30MPa "good"
[0743] B: Residual stress is above 30MPa and less than 40MPa "OK"
[0744] C: Tensile elongation of 40 MPa or more "Not allowed"
[0745] 《Example II-1》
[0746] In a 3L separable flask with a stirring rod, nitrogen was introduced and NMP (191 g) as a solvent, DABA (14.4 g) as a diamine and a silicon-containing compound (1) (10.82 g) were added while stirring as described in Tables 6 and 7, and then CpODA (38.4 g) as an acid dianhydride was added. The molar ratio of the acid dianhydride to the diamine was 100:98. The mixture was stirred at room temperature for 48 hours to obtain a transparent polyimide precursor (functional groups other than the silicon-containing compound: amide group; functional groups of the silicon-containing compound: amide group) NMP solution (hereinafter also referred to as varnish). The obtained varnish was stored in a freezer (set to -20°C, the same below) and thawed for use when evaluating.
[0747] 《Example II-2》
[0748] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (191 g), toluene (19 g), DABA (14.4 g) as a diamine, and silicon-containing compound (1) (10.82 g) as a solvent were added while stirring as described in Tables 6 and 7, and then CpODA (38.4 g) as an acid dianhydride was added at room temperature. The molar ratio of the acid dianhydride to the diamine was 100:98. Thereafter, the internal temperature was raised to 160°C, and refluxed at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was restored to room temperature to obtain an NMP solution of a polyimide resin (functional groups other than the silicon-containing compound: imide group; functional groups of the silicon-containing compound: imide group). The obtained varnish was stored in a freezer (set to -20°C, and the same applies to lower temperatures), and was thawed and used for evaluation.
[0749] 《Example II-3》
[0750] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (189 g) as a solvent, toluene (19 g), DABA (13.9 g) as a diamine were added while stirring as described in any one of Tables 6 to 9, and then CpODA (38.4 g) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 160°C, and refluxed at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was restored to room temperature. Then, a silicon-containing compound (2) (10.72 g) was added while stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution (hereinafter also referred to as varnish) of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: amide group).
[0751] 《Example II-16》
[0752] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod, nitrogen was introduced, and NMP (177 g) as a solvent, toluene (18 g), 33DAS (8.5 g) and 44DAS (12.8 g) as diamines were added while stirring as described in Tables 8 and 9, and then ODPA (31.0 g) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 160°C, and reflux was heated at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and the temperature was returned to room temperature. Then, 33DAS (0.9 g) and 44DAS (1.4 g) as diamines, and a silicon-containing compound (2) (4.12 g) were added while stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution (hereinafter also referred to as varnish) of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: amide group).
[0753] 《Example II-17》
[0754] Into a separable flask equipped with a Dean Stark tube and a reflux tube and a stirring rod at the top, nitrogen was introduced, and NMP (173 g), toluene (17 g), and DABA (13.0 g) as a solvent were added while stirring as described in Tables 8 and 9, and then CpODA (38.4 g) as an acid dianhydride was added at room temperature. Thereafter, the internal temperature was raised to 160°C, and refluxed at 160°C for 1 hour to carry out imidization. After the imidization was completed, the temperature was raised to 180°C, and the reaction was continued while taking out toluene. After reacting for 12 hours, the oil bath was removed and returned to room temperature. Then, DABA (1.4 g) as a diamine and a silicon-containing compound (2) (4.80 g) were added while stirring. The molar ratio of the acid dianhydride to the diamine was 100:98. Then, the mixture was stirred at room temperature for 48 hours to obtain an NMP solution (hereinafter also referred to as varnish) of a partially imidized polyimide precursor (functional groups other than the silicon-containing compound: amide group or imide group; functional groups of the silicon-containing compound: amide group).
[0755] Comparative Example II-4
[0756] As shown in Tables 8 and 9, 27.0 g (0.0802 mol) of 6FODA and 56.000 g of NMP were added to a 500 mL 5-necked round-bottom flask equipped with a stainless steel half-moon-shaped stirring blade, a nitrogen inlet pipe, a Dean Stark equipped with a condenser, a thermometer, and a glass tube end cap, and stirred at a temperature of 70° C. in the system, under a nitrogen atmosphere, and a rotation speed of 200 rpm to obtain a solution.
[0757] After adding CpODA19.2g (0.050 mol) and NMP 14.000g to the solution, TEA0.253g as an imidization catalyst was added, and the temperature in the reaction system was raised to 190°C in about 20 minutes by heating with a hood heater. The distilled components were captured, the rotation speed was adjusted as the viscosity increased, and the temperature in the reaction system was maintained at 190°C and refluxed for 1 hour. Thereafter, NMP 85.806g was added, and the temperature in the reaction system was cooled to 50°C to obtain a solution containing an oligomer having an imide repeating structural unit.
[0758] 9.7 g (0.033 mol) of BPDA and 7.527 g of NMP were added to the obtained solution, and the mixture was stirred at 50° C. for 5 hours. After that, 100.000 g of NMP was added and homogenized, and then a mixed solution of 13.2 g (0.003 mol) of X-22-1660B-3 (modified silicone oil, functional group equivalent: 2200, Shin-Etsu Chemical) dissolved in 16.667 g of NMP was added, and the mixture was further stirred for about 1 hour to obtain an NMP solution (hereinafter also referred to as varnish) of a partially imidized polyimide precursor (functional groups other than silicon-containing compounds: amide groups or imide groups; functional groups of silicon-containing compounds: amide groups).
[0759] "Examples II-4, II-5, II-7, II-9, II-10, II-12, II-14, II-15"
[0760] In Example II-3, except that the types and amounts of the solvent, acid dianhydride, diamine, and silicon-containing compound were changed to those described in Tables 6 and 7, the same procedures as in Example II-3 were carried out.
[0761] Reference Example II-6, Examples II-8, II-11, II-13, Comparative Examples II-1 to II-3
[0762] In Example II-2, except that the types and amounts of the solvent, acid dianhydride, diamine, and silicon-containing compound were changed to those described in Tables 6 and 7, the same procedures as in Example II-2 were carried out.
[0763] The viscosity stability and filterability were evaluated using the resin compositions of Examples and Comparative Examples, and the tensile elongation and residual stress were evaluated using the obtained polyimide resin films. The evaluation results are shown in Tables 6 to 9.
[0764] The abbreviations in Examples and Comparative Examples are as follows.
[0765] 〈Acid dianhydride〉
[0766] CpODA: Compound of the following general formula
[0767]
[0768] ODPA: 4,4'-oxydiphthalic anhydride
[0769] 6FDA: 4,4'-(hexafluoroisopropylidene) diphthalic anhydride
[0770] BPAF: 9,9-bis(3,4-dicarboxyphenyl)fluorene anhydride
[0771] BzDA: a compound of the following general formula
[0772]
[0773] BNBDA: a compound of the following general formula
[0774]
[0775] 〈Diamine〉
[0776] DABA: 3,5-diaminobenzoic acid
[0777] BAFL: 9,9-bis(4-aminophenyl)fluorene
[0778] BisAM: a compound of the following general formula
[0779]
[0780] TFMB: diaminobis(trifluoromethyl)biphenyl
[0781] BAPP: Compound of the following general formula
[0782]
[0783] 33DAS: 3,3'-diaminodiphenyl sulfone
[0784] 44DAS: 3,3'-diaminodiphenyl sulfone
[0785] 6FODA: 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether
[0786] 〈Silicon-containing compounds〉
[0787] Silicon-containing compound (1): (in the general formula (5) and (10), L1 and L2 are amino groups (-NH2), R1 is trimethylene (-CH2CH2CH2-), R2 and R3 are methyl groups, j and k are 0, and the functional group equivalent is 1500)
[0788] Silicon-containing compound (2): (in the general formula (5) and (10), L1 and L2 are amino groups (-NH2), R1 is trimethylene (-CH2CH2CH2-), R2 and R3 are methyl groups, j and k are 0, and the functional group equivalent is 800)
[0789] Silicon-containing compound (3): (in the general formula (5) and (10), L1 and L2 are amino groups (-NH2), R1 is trimethylene (-CH2CH2CH2-), R2 and R3 are methyl groups, j and k are 0, and the functional group equivalent is 2200)
[0790] Silicon-containing compound (4): In the general formula (5) and (10), L1 and L2 are amino groups, R1 is -CH2CH2CH2-, R2, R3, R6, and R7 are methyl groups, R4 and R5 are phenyl groups, j / (i+j+k)=0.15, and the functional group equivalent is 2200
[0791] Silicon-containing compound (5): (In the general formula (5) and (10), L1 and L2 are anhydride groups (-CH(C=O)2O), R1 is a trimethylene group (-CH2CH2CH2-), R2 and R3 are methyl groups, j and k are 0, and the functional group equivalent is 1000)
[0792] Silicon-containing compound (6): (in the general formula (5) and (10), L1 and L2 are anhydride groups (-CH(C=O)2O), R1 is a trimethylene group (-CH2CH2CH2-), R2 and R3 are methyl groups, j and k are 0, and the functional group equivalent is 500) [Table 6]
[0793]
[0794] [Table 7]
[0795]
[0796] [Table 8]
[0797]
[0798] [Table 9]
[0799]
[0800] Description of Reference Numerals
[0801] 2a lower base plate
[0802] 2b Sealing substrate
[0803] 25 Organic EL structure
[0804] 250a Organic EL element emitting red light
[0805] 250b Organic EL element emitting green light
[0806] 250c Organic EL element that emits blue light
[0807] 251 Dividing wall (embankment)
[0808] 252 lower electrode (anode)
[0809] 253 Hole transport layer
[0810] 254 Luminous Layer
[0811] 255 Upper electrode (cathode)
[0812] 256 TFT
[0813] 257 Contact hole
[0814] 258 interlayer insulation film
[0815] 259 Lower electrode
[0816] 261 Hollow
Claims
1. A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7), In formula (6), P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer, In formula (7), P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer, The P5 or P6 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10), In formula (10), R1 is independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are independently an amino group, an acid anhydride group, an isocyanate group, a carboxyl group, an acid ester group, an acyl halide group, a hydroxyl group, an epoxy group or a mercapto group; i is an integer of 1 to 200; j and k are independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50, Furthermore, the resin composition contains 25% by mass or less of the silicon-containing compound based on the total mass of the resin. The resin is a condensation reaction product of polyimide and other ingredients.
2. The resin composition according to claim 1, wherein The resin composition contains 5 mass % or more of the silicon-containing compound based on the total mass of the resin.
3. The resin composition according to claim 1 or 2, wherein The imidization rate of the resin is 50% or more.
4. A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7), In formula (6), P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer, In formula (7), P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer, The P5 or P6 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10), In formula (10), R1 is independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are independently an amino group, an acid anhydride group, an isocyanate group, a carboxyl group, an acid ester group, an acyl halide group, a hydroxyl group, an epoxy group or a mercapto group; i is an integer of 1 to 200; j and k are independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50, Furthermore, the imidization rate of the resin is 50% or more, The resin is a condensation reaction product of polyimide and other ingredients.
5. A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7), In formula (6), P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer, In formula (7), P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer, The P5 or P6 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10), In formula (10), R1 is independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are independently an amino group, an acid anhydride group, an isocyanate group, a carboxyl group, an acid ester group, an acyl halide group, a hydroxyl group, an epoxy group or a mercapto group; i is an integer of 1 to 200; j and k are independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50, Furthermore, the resin composition satisfies any of the following (i) or (ii), (i) P3 and / or P5 contain structural units derived from the compound represented by the following general formula (8), or (ii) P4 and / or P6 contain structural units derived from the compound represented by the following general formula (9): The resin is a condensation reaction product of polyimide and other ingredients.
6. A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7), In formula (6), P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer, In formula (7), P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer, The P5 or P6 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10), In formula (10), R1 is independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are independently an amino group, an acid anhydride group, an isocyanate group, a carboxyl group, an acid ester group, an acyl halide group, a hydroxyl group, an epoxy group or a mercapto group; i is an integer of 1 to 200; j and k are independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50, Furthermore, P3 and / or P5 each independently contain at least one structural unit derived from various compounds selected from 3,3'-diaminodiphenyl sulfone (33DAS), 4,4'-diaminodiphenyl sulfone (44DAS) or 9,9-bis(4-aminophenyl)fluorene (BAFL), The resin is a condensation reaction product of polyimide and other ingredients.
7. A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7), In formula (6), P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer, In formula (7), P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer, The P5 or P6 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10), In formula (10), R1 is independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are independently an amino group, an acid anhydride group, an isocyanate group, a carboxyl group, an acid ester group, an acyl halide group, a hydroxyl group, an epoxy group or a mercapto group; i is an integer of 1 to 200; j and k are independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50, Furthermore, P3 and / or P5 each independently comprises at least one structural unit derived from 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA), The resin is a condensation reaction product of polyimide and other ingredients.
8. A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7), In formula (6), P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer, In formula (7), P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer, The P5 or P6 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10), In formula (10), R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50, Furthermore, when A (mass %) is the ratio of the diamine of the general formula (10) among the diamines constituting P3 in the general formula (6), and B (mass %) is the ratio of the diamine of the general formula (10) among the diamines constituting P5 in the general formula (7), BA is greater than 0 and less than 60.
9. The resin composition according to claim 8, wherein The diamine comprises at least one compound selected from the group consisting of a compound represented by the following general formula (8), 3,3'-diaminodiphenyl sulfone (33DAS), 4,4'-diaminodiphenyl sulfone (44DAS) and 9,9-bis(4-aminophenyl)fluorene (BAFL), 10. The resin composition according to any one of claims 1 to 9, wherein In the general formula (6) and / or the general formula (7), P4 and / or P6 each independently comprises at least one structural unit derived from various compounds of 4,4'-oxydiphthalic anhydride (ODPA) or 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF).
11. The resin composition according to any one of claims 1 to 10, wherein The functional group equivalent of the silicon-containing compound represented by the general formula (10) is 800 or more.
12. The resin composition according to claim 11, wherein The functional group equivalent of the silicon-containing compound represented by the general formula (10) is 1500 or more.
13. The resin composition according to any one of claims 1 to 12, wherein The P5 comprises a structural unit derived from the compound represented by the general formula (10), and In the general formula (10), L1 and L2 are each independently an amino group.
14. The resin composition according to any one of claims 5 and 10 to 13, wherein When all diamines excluding the compound represented by the general formula (10) are taken as 100 mol %, the compound represented by the general formula (8) is more than 50 mol %.
15. The resin composition according to claim 5, 9 or 14, wherein The compound represented by the general formula (8) is 3,5-diaminobenzoic acid (DABA).
16. The resin composition according to any one of claims 1 to 15, wherein The P3 or P5 each independently comprises a structural unit derived from a compound (BisAM) represented by the following formula:
17. The resin composition according to any one of claims 1 to 16, wherein The P4 or P6 each independently comprises a compound (BzDA) derived from 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride, represented by the following formula: Or the compound represented by the following formula (BNBDA) structural unit.
18. The resin composition according to any one of claims 1 to 17, wherein A polyimide resin film obtained by heating the resin is used for a flexible substrate.
19. The resin composition according to any one of claims 1 to 18, wherein A polyimide resin film obtained by curing the resin is used in a flexible display.
20. A method for producing a resin composition, comprising: After polyimide is obtained by polycondensation reaction of diamine or acid dianhydride with a silicon-containing compound represented by the following general formula (10), Allowing it to undergo a polycondensation reaction with other compounds to provide a resin composition comprising a resin comprising a polyimide precursor and a polyimide, In formula (10), R1 is independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are independently an amino group, an acid anhydride group, an isocyanate group, a carboxyl group, an acid ester group, an acyl halide group, a hydroxyl group, an epoxy group or a mercapto group; i is an integer of 1 to 200; j and k are independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50, The resin composition contains 25% by mass or less of the silicon-containing compound based on the total mass of the resin.
21. A method for producing a resin composition, comprising: After polyimide is obtained by polycondensation reaction of diamine or acid dianhydride with a silicon-containing compound represented by the following general formula (10), Allowing it to undergo a polycondensation reaction with other compounds to provide a resin composition comprising a resin comprising a polyimide precursor and a polyimide, In formula (10), R1 is independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are independently an amino group, an acid anhydride group, an isocyanate group, a carboxyl group, an acid ester group, an acyl halide group, a hydroxyl group, an epoxy group or a mercapto group; i is an integer of 1 to 200; j and k are independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50, The imidization rate of the resin is 50% or more.
22. A method for producing a resin composition, comprising: After polyimide is obtained by polycondensing the compound represented by the following general formula (8) or the compound represented by the following general formula (9) with the silicon-containing compound represented by the following general formula (10) and other compounds, The polyimide precursor and the polyimide are subjected to polycondensation reaction with other compounds to provide a resin composition comprising a polyimide precursor and a polyimide. In formula (10), R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group, an acid anhydride group, an isocyanate group, a carboxyl group, an acid ester group, an acyl halide group, a hydroxyl group, an epoxy group or a mercapto group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.
50.
23. A method for producing a resin composition, comprising: At least one compound selected from 3,3'-diaminodiphenyl sulfone (33DAS), 4,4'-diaminodiphenyl sulfone (44DAS) and 9,9-bis(4-aminophenyl)fluorene (BAFL) is subjected to a polycondensation reaction with a silicon-containing compound represented by the following general formula (10) and other compounds to obtain a polyimide, The polyimide precursor and the polyimide are subjected to polycondensation reaction with other compounds to provide a resin composition comprising a polyimide precursor and a polyimide. In formula (10), R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group, an acid anhydride group, an isocyanate group, a carboxyl group, an acid ester group, an acyl halide group, a hydroxyl group, an epoxy group or a mercapto group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.
50.
24. A method for producing a resin composition, comprising: At least one compound selected from 4,4'-oxydiphthalic anhydride (ODPA) and 9,9-bis(3,4-dicarboxyphenyl)fluorene anhydride (BPAF) is subjected to polycondensation reaction with a silicon-containing compound represented by the following general formula (10) and other compounds to obtain a polyimide, The polyimide precursor and the polyimide are subjected to polycondensation reaction with other compounds to provide a resin composition comprising a polyimide precursor and a polyimide. In formula (10), R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group, an acid anhydride group, an isocyanate group, a carboxyl group, an acid ester group, an acyl halide group, a hydroxyl group, an epoxy group or a mercapto group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.
50.
25. A method for producing a polyimide resin film, comprising: A step of coating the resin composition according to any one of claims 1 to 19 or the resin composition obtained by the method according to any one of claims 20 to 24 on the surface of a support; A film-forming step of heating the resin composition to form a polyimide resin film; and A peeling step of peeling the polyimide resin film from the support.
26. The method for producing a polyimide resin film according to claim 25, comprising: Prior to the peeling step, an irradiation step of irradiating the resin composition with laser light from the support side is performed.
27. A method for manufacturing a display, comprising: A step of coating the resin composition according to any one of claims 1 to 19 or the resin composition obtained by the method according to any one of claims 20 to 24 on the surface of a support; A film-forming step of heating the resin composition to form a polyimide resin film; an element forming step of forming an element on the polyimide resin film; and A peeling step of peeling the polyimide resin film on which the element is formed from the support.
28. A method for manufacturing a laminate, comprising: A step of coating the resin composition according to any one of claims 1 to 19 or the resin composition obtained by the method according to any one of claims 20 to 24 on the surface of a support; A film-forming step of heating the resin composition to form a polyimide resin film; and The step of forming an element on the polyimide resin film is followed by a step of forming an element.
29. The method for manufacturing a laminate according to claim 28, further comprising: a step of peeling the polyimide resin film on which the element is formed from the support.
30. The manufacturing method according to any one of claims 25 to 29, wherein: In the film forming step, the heating temperature is 250° C. to 550° C., and the oxygen concentration of the surrounding atmosphere is 2,000 mass ppm or less.
31. A method for manufacturing a flexible device, comprising: The laminate is produced by the method according to claim 28 or 29.
32. A resin composition comprising a resin having a structural unit represented by the following general formula (1) or (2): In formula (1), P1 represents a divalent organic group; P2 represents a tetravalent organic group; and p represents a positive integer, In formula (2), P1 represents a divalent organic group; P2 represents a tetravalent organic group, and p represents a positive integer. The P1 comprises a structural unit derived from a compound represented by the following general formula (3), Furthermore, the P1 or P2 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (5): In formula (5), R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50; and the functional group equivalent is 800 or more.
33. The resin composition according to claim 32, wherein The compound represented by the general formula (3) is 3,5-diaminobenzoic acid (DABA).
34. The resin composition according to claim 32 or 33, wherein The P2 comprises a structural unit derived from a compound represented by the following general formula (4), 35. A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7), In formula (6), P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer; P3 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA), In formula (7), P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer; P5 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA), The P3 or P4 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10), In formula (10), R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.
50.
36. A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7), In formula (6), P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer; P3 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA), In formula (7), P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer; P5 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA), The P3 or P4 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10), In formula (10), R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50, Furthermore, the resin composition satisfies any of the following (i) or (ii), (i) P3 and / or P5 contain structural units derived from the compound represented by the following general formula (8), or (ii) P4 and / or P6 contain structural units derived from the compound represented by the following general formula (9):
37. A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7): In formula (6), P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer; P3 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA), In formula (7), P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer; P5 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA), The P3 or P4 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10), In formula (10), R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50, Furthermore, the P3 and / or P5 comprises at least one structural unit derived from various compounds of 3,3'-diaminodiphenyl sulfone (33DAS) or 4,4'-diaminodiphenyl sulfone (44DAS).
38. A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7), In formula (6), P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer; P3 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA), In formula (7), P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer; P5 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA), The P3 or P4 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10), In formula (10), R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50, Furthermore, the P3 and / or P5 contain at least one structural unit derived from 9,9-bis(4-aminophenyl)fluorene (BAFL) or a compound of the following general formula (BisAM), 39. A resin composition comprising a resin having structural units represented by the following general formulae (6) and (7), In formula (6), P3 represents a divalent organic group; P4 represents a tetravalent organic group; and p represents a positive integer; P3 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA), In formula (7), P5 represents a divalent organic group; P6 represents a tetravalent organic group; and q represents a positive integer; P5 does not contain 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA), The P3 or P4 comprises a structural unit derived from a silicon-containing compound represented by the following general formula (10), In formula (10), R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.50, Furthermore, P4 and / or P6 contain at least one 4,4'-oxydiphthalic anhydride (ODPA), 4,4'-(Hexafluoroisopropylidene)diphthalic anhydride (6FDA), 9,9-bis(3,4-dicarboxyphenyl)fluorene anhydride (BPAF), The compound of the following general formula (BzDA), Or the compound of the following general formula (BNBDA) The structural units of various compounds.
40. The resin composition according to any one of claims 35 to 39, wherein The P3 comprises a structural unit derived from the compound represented by the general formula (10), The functional group equivalent of the silicon-containing compound represented by the general formula (10) is 800 or more.
41. The resin composition according to any one of claims 35 to 40, wherein The P3 comprises a structural unit derived from the compound represented by the general formula (10), and In the general formula (10), L1 and L2 are each independently an amino group.
42. The resin composition according to any one of claims 32, 34 and 36, wherein When all diamines excluding the compound represented by the general formula (5) or (10) are taken as 100 mol %, the compound represented by the general formula (3) or (8) is more than 50 mol %.
43. The resin composition according to any one of claims 32 to 42, wherein A polyimide resin film obtained by heating the resin is used for a flexible substrate.
44. The resin composition according to any one of claims 32 to 43, wherein A polyimide resin film obtained by curing the resin is used in a flexible display.
45. A method for producing a resin composition, comprising: A polyimide precursor and / or a polyimide is provided by subjecting a compound represented by the following general formula (3), at least one diamine selected from 3,3'-diaminodiphenyl sulfone (33DAS) and 4,4'-diaminodiphenyl sulfone (44DAS) and an acid dianhydride, a silicon-containing compound represented by the following general formula (5) and other compounds to a condensation reaction, In formula (5), R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.
50.
46. A method for producing a resin composition, comprising: After polyimide is obtained by polycondensation reaction of diamine and acid dianhydride, A silicon-containing compound represented by the following general formula (5) is subjected to a polycondensation reaction with other compounds to provide a resin composition containing a polyimide precursor and a polyimide, Wherein, the diamine does not include 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA), In formula (5), R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.
50.
47. A method for producing a resin composition, comprising: A compound represented by the following general formula (3), at least one diamine selected from 3,3'-diaminodiphenyl sulfone (33AS) and 4,4'-diaminodiphenyl sulfone (44DAS), an acid dianhydride and other compounds are subjected to polycondensation reaction to obtain a polyimide, A silicon-containing compound represented by the following general formula (5) is subjected to a polycondensation reaction with other compounds to provide a resin composition containing a polyimide precursor and a polyimide, In formula (5), R1 is each independently a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, at least one of which is a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms; L1 and L2 are each independently an amino group; i is an integer of 1 to 200; j and k are each independently an integer of 0 to 200; 0≤j / (i+j+k)≤0.
50.
48. A method for producing a polyimide resin film, comprising: A coating step of coating the resin composition according to any one of claims 32 to 44 or the resin composition obtained by the method according to any one of claims 45 to 47 on the surface of a support; A film-forming step of heating the resin composition to form a polyimide resin film; and A peeling step of peeling the polyimide resin film from the support.
49. The method for producing a polyimide resin film according to claim 48, comprising: Prior to the peeling step, an irradiation step of irradiating the resin composition with laser light from the support side is performed.
50. A method for manufacturing a display, comprising: A coating step of coating the resin composition according to any one of claims 32 to 44 or the resin composition obtained by the method according to any one of claims 45 to 47 on the surface of a support; A film-forming step of heating the resin composition to form a polyimide resin film; an element forming step of forming an element on the polyimide resin film; and A peeling step of peeling the polyimide resin film on which the element is formed from the support.
51. A method for manufacturing a laminate, comprising: A coating step of coating the resin composition according to any one of claims 32 to 44 or the resin composition obtained by the method according to any one of claims 45 to 47 on the surface of a support; A film-forming step of heating the resin composition to form a polyimide resin film; and The step of forming an element on the polyimide resin film is followed by a step of forming an element.
52. The method for manufacturing a laminate according to claim 51, further comprising: a step of peeling the polyimide resin film on which the element is formed from the support.
53. A method for manufacturing a flexible device, comprising: A laminate is produced by the method according to claim 51 or 52.
Citation Information
Patent Citations
Active matrix displays and other electronic devices with plastic substrates
JP2007512568A
Substrate structure applied in flexible electronic device and fabrication method thereof
JP2010067957A
Electronic devices with plastic substrates
JP2012511173A
Light-emitting device manufacturing method
JP2013179306A
Polyimide resin, polyimide varnish, and polyimide film
WO2019211972A1