Method for producing vinyl silicone oil by continuous method and application
Through continuous production of vinyl silicone oil, the combination of reactor, film evaporator and molecular evaporator is used to solve the problems of low production efficiency and poor stability of traditional silicone oil, and the efficient production and low energy consumption of different levels of volatile components are achieved, avoiding the use of high-quality volatile components. The emergence of mixed layers.
Patent Information
- Application Number
- CN202411075109.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-12-06
AI Technical Summary
Traditional silicone oil production process is low efficiency and poor product stability, making it difficult to meet different volatile components needs, and mixing layers are easily generated when switching different varieties.
The vinyl silicone oil is produced by continuous method. The volatile components are reduced step by step by step by step by step by the use of a catalyst and a neutralizing agent. The use of catalyst and neutralizing agent is ensured. Silicone oil stability.
It realizes efficient production of volatile silicone oil of different grades, with good stability of silicone oil, reduced energy consumption by 20%, and reduced equipment cost by 30%. It is suitable for low-level factories and avoids the mixed layer problem when switching different varieties.
Smart Images

Figure CN119081119A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicone oil production, and particularly relates to a method for continuously producing vinyl silicone oil and its application. Background Art
[0002] Silicone oil is a general term for organic silicon compounds containing silicon oxygen bonds (-Si-O-Si-), and there are many types of silicone oil. Among them, vinyl silicone oil mainly includes vinyl-terminated polydimethylsiloxane and vinyl-terminated polymethylvinylsiloxane, and products with different viscosities and vinyl contents can be provided according to needs.
[0003] Traditional silicone oil production can be done in two ways: intermittent and continuous. Indirect production, i.e., using kettle reaction, has low efficiency and cannot guarantee quality. Continuous production, i.e., using pipelines, evaporators and other equipment for continuous production, will produce a large number of intermediate layers when switching between different types of silicone oils, and silicone oils with different levels of volatility cannot be obtained well. In short, the production process of silicone oil has problems such as complicated process, low production efficiency, high product energy consumption, poor product batch stability, and cannot meet customers' needs for silicone oils with different volatile contents.
[0004] Therefore, there is an urgent need to provide a method for continuously producing vinyl silicone oil, which can produce silicone oils with different levels of volatility, has good silicone oil stability, and does not have the problem of mixed layers when switching between different types of silicone oil products. Summary of the invention
[0005] The present invention aims to solve one or more technical problems existing in the above-mentioned prior art, and at least provide a beneficial choice or create conditions. Specifically, the present invention provides a method for continuously producing vinyl silicone oil, which can produce silicone oil with different levels of volatility, and the silicone oil has good stability, and there is no problem of mixed layer when switching different varieties of silicone oil products.
[0006] The inventive concept of the present invention is as follows: the present invention adopts a continuous method to produce vinyl silicone oil, firstly, a dimethylcyclosiloxane mixture and a vinyl capping agent are mixed, heated, a catalyst is added, a first reaction is carried out, then a neutralizing agent is added, a second reaction is carried out, and a reduced pressure distillation is carried out to obtain silicone oil 1; then silicone oil 1 is added to a thin film evaporator, degassing treatment is carried out to obtain silicone oil 2; then silicone oil 2 is added to a molecular evaporator, degassing treatment is carried out to obtain silicone oil 3. The present invention uses reduced pressure distillation in a reaction kettle, a thin film evaporator and a molecular evaporator in combination, and the fraction removed is continuously increased, and the volatile matter is reduced step by step to obtain silicone oil 1, silicone oil 2 and silicone oil 3 with different levels of volatile matter, and the silicone oil has good stability and low energy consumption, and there is no problem of mixed layer when switching different varieties of silicone oil products.
[0007] Therefore, a first aspect of the present invention provides a method for producing vinyl silicone oil in a continuous process.
[0008] Specifically, a method for continuously producing vinyl silicone oil comprises the following steps:
[0009] (1) mixing a dimethylcyclosiloxane mixture and a vinyl capping agent, heating, adding a catalyst, performing a first reaction, then adding a neutralizing agent, performing a second reaction, and performing reduced pressure distillation to obtain silicone oil 1;
[0010] (2) adding the silicone oil 1 obtained in step (1) into a thin film evaporator for degassing to obtain silicone oil 2;
[0011] (3) Add the silicone oil 2 obtained in step (2) into a molecular evaporator and perform degassing to obtain silicone oil 3.
[0012] Specifically, step (1) is carried out in a reactor, and by utilizing the principle that the fractions removed from the reactor, thin film evaporator and molecular evaporator are continuously increasing, the volatile matter is reduced step by step, and different grades of volatile silicone oil can be produced. The reactor can achieve a volatile matter of less than or equal to 1.5%, step (2) can achieve a volatile matter of less than 1%, and step (3) can achieve a volatile matter of less than 0.5%. The silicone oil has good stability, and there is no mixed layer during switching. At the same time, the energy consumption of the system is greatly reduced, which can be reduced by about 20% compared with the kettle reaction in the prior art. In addition, by vacuum distillation, the evaporation efficiency is improved, and the area of the thin film evaporator and the molecular evaporator can be greatly reduced, and the corresponding supporting equipment, such as a receiving tank, a transfer pump, etc., can be reduced, and the equipment cost can be reduced by about 30%. At the same time, due to the reduction in the area of the thin film evaporator and the molecular evaporator, their installation height is reduced, and the height of the factory building can be reduced, which is suitable for low-level factories.
[0013] Preferably, the dimethylcyclosiloxane mixture (DMC) includes hexamethylcyclotrisiloxane (D3), octamethylcyclotetrasiloxane (D4), decamethylcyclopentasiloxane (D5), and dodecamethylcyclohexasiloxane (D6); and / or the vinyl capping agent includes vinyl silicone oil.
[0014] Preferably, the vinyl silicone oil comprises a mixture of vinyl-terminated polydimethylsilanes having a viscosity of 4-10 mm / s.
[0015] Preferably, the dimethylcyclosiloxane mixture is dehydrated before mixing, the temperature of the dehydration treatment is 45-65°C, and the time of the dehydration treatment is 0.9-2.2h; further preferably, the temperature of the dehydration treatment is 50-60°C, and the time of the dehydration treatment is 1-2h.
[0016] Preferably, the small molecules removed after the de-low molecular weight treatment in steps (2) and (3) (referred to as recovered low molecular weight) can be returned to the reactor and reused as raw materials. Step (1) is specifically as follows: the dimethylcyclosiloxane mixture, the vinyl capping agent and the recovered low molecular weight are mixed, heated, a catalyst is added, a first reaction is carried out, a neutralizing agent is added, a second reaction is carried out, and a reduced pressure distillation is performed to obtain silicone oil 1.
[0017] Preferably, the mass ratio of DMC, vinyl capping agent and recovered low molecular weight after dehydration treatment is 3880: (70-90): (270-360); further preferably, the mass ratio of DMC, vinyl capping agent and recovered low molecular weight after dehydration treatment is 3880: (75-85): (300-330); further preferably, the mass ratio of DMC, vinyl capping agent and recovered low molecular weight after dehydration treatment is 3880: 80: 316.
[0018] Specifically, the recovered low-molecular-weight substances include small-molecule silicone oil and DMC.
[0019] Preferably, in step (1), after mixing, the temperature is first raised to 110-130°C, and then the catalyst is added; further preferably, after mixing, the temperature is first raised to 115-125°C, and then the catalyst is added; further preferably, after mixing, the temperature is first raised to 120°C, and then the catalyst is added.
[0020] Preferably, in step (1), the catalyst comprises a basic catalyst.
[0021] Preferably, the alkaline catalyst comprises potassium hydroxide alkali gel.
[0022] Preferably, the mass ratio of the catalyst to the recovered low-molecular weight is 6:(70,000-90,000); further preferably, the mass ratio of the catalyst to the recovered low-molecular weight is 6:(75,000-85,000); further preferably, the mass ratio of the catalyst to the recovered low-molecular weight is 6:79,000.
[0023] Preferably, in step (1), the reaction temperature of the first reaction is 130-160° C., and the reaction time of the first reaction is 3-5 h; and / or, the reaction temperature of the second reaction is 130-160° C., and the reaction time of the second reaction is 0.8-1.5 h.
[0024] Further preferably, in step (1), the reaction temperature of the first reaction is 140-150°C, and the reaction time of the first reaction is 3.5-4.5h; and / or, the reaction temperature of the second reaction is 140-150°C, and the reaction time of the second reaction is 0.9-1.2h.
[0025] Preferably, the neutralizing agent comprises phosphate acid gum.
[0026] Specifically, the phosphate ester acid gel is obtained by the reaction of phosphoric acid and octamethylcyclotetrasiloxane; the role of the neutralizer is to neutralize the alkaline catalyst by adding an acidic neutralizer after the reaction 1 is completed, so as to achieve the purpose of removing the catalyst.
[0027] Preferably, the mass ratio of the catalyst to the neutralizer is 1:1-2; further preferably, the mass ratio of the catalyst to the neutralizer is 1:1.2-1.7; further preferably, the mass ratio of the catalyst to the neutralizer is 1:1.5.
[0028] Preferably, in step (1), the temperature of the reduced pressure distillation is 160-190°C, the time of the reduced pressure distillation is 2.5-4.5h, and the vacuum degree of the reduced pressure distillation is above 100Pa; further preferably, the temperature of the reduced pressure distillation is 170-180°C, the time of the reduced pressure distillation is 3-4h, and the vacuum degree of the reduced pressure distillation is greater than 100Pa and less than or equal to 500Pa.
[0029] Specifically, the reduced pressure distillation is a de-lowering treatment, i.e., removing low molecular weight molecules. After the de-lowering is completed, the low molecular weight molecules enter a low molecular weight tank and can be recycled to continue to participate in the reaction of step (1) as the recycled low molecular weight molecules.
[0030] Preferably, in step (2), the temperature of the desulfurization treatment is 160-190°C, and the vacuum degree of the desulfurization treatment is above 50Pa; and / or, in step (3), the temperature of the desulfurization treatment is 160-190°C, and the vacuum degree of the desulfurization treatment is above 50Pa.
[0031] Further preferably, in step (2), the temperature of the degassing treatment is 170-180°C, and the vacuum degree of the degassing treatment is greater than 50Pa and less than or equal to 100Pa; and / or, in step (3), the temperature of the degassing treatment is 170-180°C, and the vacuum degree of the degassing treatment is greater than 50Pa and less than or equal to 100Pa.
[0032] Specifically, after the de-lowering treatment in step (2), the low molecular weight substances continuously flow into the low molecular weight tank through the condenser, and after the de-lowering treatment in step (3), the low molecular weight substances continuously flow into the low molecular weight tank through the cold hydrazine.
[0033] Preferably, the volatile content of the silicone oil 1 is 1-1.5%; the volatile content of the silicone oil 2 is greater than 0.5% and less than 1%; and the volatile content of the silicone oil 3 is 0.05-0.5%.
[0034] Further preferably, the volatile content of the silicone oil 1 is 1-1.4%; the volatile content of the silicone oil 2 is greater than 0.55% and less than 0.9%; and the volatile content of the silicone oil 3 is 0.05-0.4%.
[0035] More preferably, the volatile content of the silicone oil 1 is 1.1%; the volatile content of the silicone oil 2 is 0.8%; and the volatile content of the silicone oil 3 is 0.2%.
[0036] Specifically, if a silicone oil with a volatile content of 1-1.5% is required, then after obtaining silicone oil 1, the cold oil valve of the reactor jacket is opened to cool down. After cooling to 100°C, the silicone oil is pressed into a qualified product tank with nitrogen, and the silicone oil is filtered and packaged. If a silicone oil with a volatile content of more than 0.5% and less than 1% is required, then step (2) is continued, and after obtaining silicone oil 2, the silicone oil is pumped into a finished product tank, cooled, and packaged. If a silicone oil with a volatile content of 0.05-0.5% is required, then step (3) is continued to obtain silicone oil 3, which is a silicone oil with a volatile content of 0.05-0.5%. By using a reactor, a thin film evaporator, and a molecular evaporator to reduce the volatile content step by step, silicone oils of different grades of volatile content can be produced to meet the different needs of customers.
[0037] The second aspect of the present invention provides an application of the method for continuously producing vinyl silicone oil according to the first aspect of the present invention in the field of silicone oil production.
[0038] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:
[0039] (1) The present invention uses a combination of vacuum distillation, a thin film evaporator and a molecular evaporator in a reaction kettle to continuously increase the fraction removed, and reduce the volatile matter step by step to obtain silicone oil 1, silicone oil 2 and silicone oil 3 with different levels of volatile matter. The silicone oil has good stability and low energy consumption. At the same time, there is no problem of mixed layer when switching different types of silicone oil products.
[0040] (2) The present invention first undergoes reduced pressure distillation to improve the evaporation efficiency, which can greatly reduce the area of the thin film evaporator and the molecular evaporator, and reduce the supporting equipment of the thin film evaporator and the molecular distillation, such as the receiving tank, the transfer pump, etc., and the equipment cost is reduced by about 30%. In addition, due to the reduction in the area of the thin film evaporator and the molecular evaporator, their installation height is reduced, and the height of the factory building can be reduced, which is suitable for low-level factories.
[0041] (3) The small molecules removed after the deoxidation treatment of the present invention can be returned to the reactor as raw materials to continue to participate in the reaction, which has certain economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a process flow chart for producing vinyl silicone oil by a continuous process according to Example 1 of the present invention. DETAILED DESCRIPTION
[0043] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0044] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0045] Example 1
[0046] A method for continuously producing vinyl silicone oil comprises the following steps:
[0047] (1) First, DMC is pumped into the dehydration kettle through the DMC intermediate storage tank. The amount of DMC added at one time is 4 tons. The steam is turned on, the temperature is raised to 55°C, and vacuum is drawn while bubbling dry nitrogen at the bottom. The dehydration time is 1.5 hours, and the amount of DMC removed is about 3% of the amount of DMC added. The dehydrated DMC is 3880 kg (measured by a mass flow meter), which is pumped into the DMC metering tank. 80 kg of the capping agent (low-viscosity vinyl silicone oil) is pumped into the capping agent metering tank, and 316 kg of the recovered low-molecular weight (a mixture of small-molecule silicone oil and DMC) is pumped into the low-boiling metering tank through the low-molecular weight storage tank. DMC, the capping agent, and the low-molecular weight are added to the reactor through their respective metering tanks. The stirring of the reactor is turned on, the heat transfer oil valve is opened, and the temperature is raised. When the temperature reaches At 120°C, 24g of catalyst potassium hydroxide alkali glue is added, the reaction temperature is controlled at 150°C, the reaction time is 4 hours, after the reaction is completed, 36g of neutralizing agent phosphate acid glue is added, and neutralization is carried out at 150°C for 1 hour. After the neutralization is completed, vacuum distillation is carried out, and the degassing temperature during vacuum distillation is controlled at 170°C, and the vacuum degree is 300Pa. When no liquid flows out of the receiving tank, the degassing time is 4 hours. After the degassing is completed, the low molecular weight is injected into the low molecular weight tank (which can be used as a recycled low molecular weight to return to the reactor as a raw material to participate in the reaction), and vinyl silicone oil 1 is obtained. If the volatile content of vinyl silicone oil 1 is qualified, the cold oil valve of the reactor jacket is opened to cool down. After cooling to 100°C, it is pressed into the qualified product tank with nitrogen, and filtered and packaged through a filter;
[0048] (2) If the volatile content is required to be less than 1%, the vinyl silicone oil 1 obtained in step (1) is pumped into a thin film evaporator through a metering pump to control the flow rate. The material entering the thin film evaporator is controlled at a temperature of 180° C. by a thermal oil heater. The vacuum degree of the thin film evaporator is controlled at 75 Pa. Low molecular weight materials continuously flow into a low molecular weight tank through a condenser (they can be returned to the reactor as raw materials to participate in the reaction). Each batch of low molecular weight materials is 2 kg (8 kg per day, 4 batches of materials per day for 2 reactors), and vinyl silicone oil 2 is obtained. If the volatile content of vinyl silicone oil 2 is qualified, the silicone oil is pumped into a first-class product tank and packaged after cooling;
[0049] (3) If the volatile matter is required to be less than 0.3%, the vinyl silicone oil 2 in the first-grade product tank obtained in step (2) is pumped into the molecular evaporator through a metering pump to control the flow rate. The material entering the molecular evaporator is controlled to have a temperature of 180° C. by a thermal oil heater. The vacuum degree of the molecular evaporator is controlled at 75 Pa to remove low molecular weight materials. The low molecular weight materials flow into the low molecular weight tank (which can be returned to the reactor as raw materials to participate in the reaction) through cold hydrazine. Each batch of low molecular weight materials is 1 kg (4 kg per day). The condenser water is chilled water. The low molecular weight materials are pumped into the low molecular weight tank for recycling to obtain vinyl silicone oil 3. The finished silicone oil continuously flows into the transition tank and is pumped into the finished product tank by a viscosity pump to cool down. The finished product is pumped into the filter by a pump for filtration and packaging.
[0050] The process flow chart of the continuous process for producing vinyl silicone oil in Example 1 of the present invention is as follows: Figure 1 shown.
[0051] Comparative Example 1
[0052] A method for continuously producing vinyl silicone oil comprises the following steps:
[0053] First, DMC is pumped into the dehydration kettle through the DMC intermediate storage tank. The amount of DMC added at one time is 4 tons. The steam is turned on, the temperature is raised to 55°C, and the vacuum is drawn while the bottom is bubbled with dry nitrogen. The dehydration time is 1.5 hours, and the amount of DMC removed is about 3% of the amount of DMC added. The dehydrated DMC is 3880kg (measured by a mass flow meter), which is pumped into the DMC metering tank. 80kg of the capping agent (low-viscosity vinyl silicone oil) is pumped into the capping agent metering tank, and 316kg of low molecular weight is pumped into the low-boiling metering tank through the low molecular weight storage tank. DMC, capping agent, low molecular weight, and The tank is added to the reactor; the stirring of the reactor is turned on, the heat transfer oil valve is opened, and the temperature is increased. When the temperature reaches 120°C, 24g of potassium hydroxide alkali glue as a catalyst is added, the reaction temperature is controlled at 150°C, and the reaction time is 4 hours. After the reaction is completed, 36g of phosphate acid glue as a neutralizing agent is added, and neutralization is carried out at 150°C for 1 hour. After the neutralization is completed, the product obtained is pumped into the thin film evaporator through a metering pump to control the flow rate. The material entering the thin film evaporator is controlled at 180°C by a heat transfer oil heater, and the vacuum degree of the thin film evaporator is controlled at 75Pa to obtain vinyl silicone oil 4.
[0054] Comparative Example 2
[0055] A method for continuously producing vinyl silicone oil comprises the following steps:
[0056] First, DMC is pumped into the dehydration kettle through the DMC intermediate storage tank. The amount of DMC added at one time is 4 tons. The steam is turned on, the temperature is raised to 55°C, and the vacuum is drawn while the bottom is bubbled with dry nitrogen. The dehydration time is 1.5 hours, and the amount of DMC removed is about 3% of the amount of DMC added. The dehydrated DMC is 3880kg (measured by a mass flow meter), which is pumped into the DMC metering tank. 80kg of the capping agent (low-viscosity vinyl silicone oil) is pumped into the capping agent metering tank, and 316kg of low molecular weight is pumped into the low-boiling metering tank through the low molecular weight storage tank. DMC, capping agent, low molecular weight, and The tank is added to the reactor; the stirring of the reactor is turned on, the heat transfer oil valve is opened, and the temperature is increased. When the temperature reaches 120°C, 24g of potassium hydroxide alkali glue as a catalyst is added, the reaction temperature is controlled at 150°C, and the reaction time is 4 hours. After the reaction is completed, 36g of phosphate acid glue as a neutralizing agent is added, and neutralization is carried out at 150°C for 1 hour; the product obtained after the neutralization is completed is pumped into a molecular evaporator through a metering pump to control the flow rate, and the material entering the molecular evaporator is controlled at 180°C by a heat transfer oil heater, and the vacuum degree of the molecular evaporator is controlled at 75Pa to obtain vinyl silicone oil 5.
[0057] Performance Testing
[0058] The volatile matter, viscosity and vinyl content of vinyl silicone oil 1, vinyl silicone oil 2 and vinyl silicone oil 3 obtained in Example 1, vinyl silicone oil 4 obtained in Comparative Example 1 and vinyl silicone oil 5 obtained in Comparative Example 2 were measured. The test method is as follows:
[0059] Volatile matter test: The vinyl silicone oil prepared in Example 1 and Comparative Examples 1-2 was baked at 150° C. for 3 hours, blown, and the weight loss was measured.
[0060] Viscosity measurement: Fourier RVDV-1 viscometer was used to test at 25°C.
[0061] Determination of vinyl content: Determine in accordance with GB / T 36691-2018.
[0062] The test results of the volatile matter, viscosity and vinyl content of the vinyl silicone oils prepared in Example 1 and Comparative Examples 1-2 are shown in Table 1.
[0063] Table 1: Volatile matter, viscosity, and vinyl content test results of the vinyl silicone oils prepared in Example 1 and Comparative Examples 1-2
[0064]
[0065]
[0066] As can be seen from Table 1, the combination of vacuum distillation, thin film evaporator and molecular evaporator can reduce the volatile matter step by step to obtain silicone oil 1, silicone oil 2 and silicone oil 3 with different levels of volatile matter, which can meet different requirements for the volatile matter of silicone oil.
[0067] Comparative Example 1 did not undergo vacuum distillation and molecular evaporation, so that the volatile matter of the prepared vinyl silicone oil was 1.5%, which was relatively large. Comparative Example 2 did not undergo vacuum distillation and thin film evaporation, so that the volatile matter of the prepared vinyl silicone oil was 1.3%, which was relatively large.
[0068] In summary, the present invention uses vacuum distillation, a thin film evaporator and a molecular evaporator in a reactor to continuously increase the fraction, reduce the volatile matter step by step, and obtain vinyl silicone oil 1, vinyl silicone oil 2 and vinyl silicone oil 3 with different levels of volatile matter. The reactor can achieve a volatile matter of less than or equal to 1.5%, the thin film evaporator can achieve a volatile matter of less than 1%, and the molecular evaporator can achieve a volatile matter of less than or equal to 0.5%, which can meet the different needs of customers, and the silicone oil has good stability and low energy consumption. At the same time, there is no problem of mixed layer when switching different types of silicone oil products.
[0069] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for continuously producing vinyl silicone oil, characterized in that: The following steps are involved: (1) mixing a dimethylcyclosiloxane mixture and a vinyl capping agent, heating, adding a catalyst, performing a first reaction, then adding a neutralizing agent, performing a second reaction, and performing reduced pressure distillation to obtain silicone oil 1; (2) adding the silicone oil 1 obtained in step (1) into a thin film evaporator for degassing to obtain silicone oil 2; (3) Add the silicone oil 2 obtained in step (2) into a molecular evaporator for degassing to obtain silicone oil 3.
2. The method according to claim 1, characterized in that The dimethylcyclosiloxane mixture includes hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, and dodecamethylcyclohexasiloxane; and / or the vinyl capping agent includes vinyl silicone oil.
3. The method according to claim 1, characterized in that The dimethylcyclosiloxane mixture is first dehydrated before mixing, the temperature of the dehydration treatment is 45-65° C., and the time of the dehydration treatment is 0.9-2.2 h.
4. The method according to claim 1, characterized in that: In step (1), the mixture is heated to 110-130° C. after mixing, and then the catalyst is added.
5. The method according to claim 1, characterized in that In step (1), the catalyst comprises a basic catalyst.
6. The method according to claim 1, characterized in that In step (1), the reaction temperature of the first reaction is 130-160° C., and the reaction time of the first reaction is 3-5 h; and / or the reaction temperature of the second reaction is 130-160° C., and the reaction time of the second reaction is 0.8-1.5 h.
7. The method according to claim 1, characterized in that In step (1), the temperature of the reduced pressure distillation is 160-190° C., the time of the reduced pressure distillation is 2.5-4.5 h, and the vacuum degree of the reduced pressure distillation is above 100 Pa.
8. The method according to claim 1, characterized in that In step (2), the temperature of the desulfurization treatment is 160-190°C, and the vacuum degree of the desulfurization treatment is above 50Pa; and / or, in step (3), the temperature of the desulfurization treatment is 160-190°C, and the vacuum degree of the desulfurization treatment is above 50Pa.
9. The method according to claim 1, characterized in that: The volatile content of the silicone oil 1 is 1-1.5%; the volatile content of the silicone oil 2 is greater than 0.5% and less than 1%; and the volatile content of the silicone oil 3 is 0.05-0.5%.
10. Application of the method for producing vinyl silicone oil by continuous method according to any one of claims 1 to 9 in the field of silicone oil production.